Composite separator and battery

MYPI2025004871A0Undetermined Publication Date: 2024-09-16SHENZHEN SENIOR TECH MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004871
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-16
Filing Date
2023-04-04
Publication Date
2024-09-16

AI Technical Summary

Technical Problem

After the separator prepared by the dry process is stretched in one direction in the longitudinal direction, the longitudinal internal stress is not completely released, which causes the separator to easily wrinkle on the membrane surface, affecting the performance and safety of the battery. In addition, the air permeability increase of the existing coated separator is large. Affect battery electrical performance.

Method used

An adhesive coating consisting of polyethylene wax particles and inorganic particles is used. The adhesive coating is located on the outermost layer of the composite separator. By adjusting the weight ratio and particle size distribution of polyethylene wax particles and inorganic particles, the reduction in temperature before and after the coating is reduced. The increase in air permeability improves battery performance.

Benefits of technology

It can effectively prevent dimensional changes caused by the release of internal stress, improve the wrinkle problem of the separator, reduce the air permeability increase of the composite separator before and after hot pressing, and improve the electrical performance and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004871_DRAWING_001
    Figure PI2025004871_DRAWING_001
Patent Text Reader

Abstract

This application provides a composite separator and a battery. In a first aspect, this application provides a composite separator, which includes a base film and an adhesive coating. The adhesive coating includes polyethylene wax particles and inorganic particles. The polyethylene wax particles can play a good adhesive role, prevent dimensional changes caused by release of internal stress, and improve the problem of wrinkling of the separator upon electrolyte injection. The inorganic particles play a supporting role. By adjusting the weight ratio and the size ratio of the polyethylene wax particles and the inorganic particles, and the weight of the polyethylene wax particles per unit area, the air permeability increase before and after providing the adhesive coating and the air permeability increase of the composite separator before and after hot pressing can be reduced on the basis of ensuring the adhesion force of the composite separator, and the electrical performance of the battery can be improved. Fig 1.
Need to check novelty before this filing date? Find Prior Art

Description

Composite diaphragm and battery

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on March 16, 2023, with application number 2023102562159 and application name “A Composite Diaphragm and Battery”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to a composite diaphragm and a battery, and relates to the technical field of batteries. Background Art

[0003] The diaphragm is a thin film with a microporous structure. As one of the four core materials of a battery, it plays a vital role in its performance and safety. Currently, the preparation processes for diaphragms mainly include wet and dry processes. The dry process, in which a polymer, additives, and other raw materials are mixed to form a uniform melt, is then stretched and heat-set at a certain temperature. Due to its pollution-free preparation process, mature technology, and low production costs, it holds a high share of the diaphragm market.

[0004] However, since the dry process is characterized by longitudinal unidirectional stretching, the longitudinal internal stress is not completely released, resulting in wrinkles on the membrane surface after the electrolyte is injected. As the battery is charged and discharged, solid precipitation will appear at the wrinkles, affecting the performance and safety of the battery.

[0005] The problem of membrane surface wrinkles can be addressed to some extent by coating the membrane surface after dry stretching. For example, Chinese invention patent publication number CN 114374058A discloses a coated membrane comprising a base membrane and an adhesive coating formed by applying an aqueous slurry of polyethylene wax powder. However, the coated membrane provided in this patent exhibits a significant increase in air permeability before and after application of the adhesive coating. Furthermore, the coated membrane prepared by this method also exhibits a significant increase in air permeability before and after hot pressing, seriously impacting the electrical performance of downstream batteries.

[0006] Summary of the Invention

[0007] The present application provides a composite diaphragm including an adhesive coating, which reduces the air permeability increment before and after the adhesive coating is provided and before and after the composite diaphragm is hot-pressed while ensuring the adhesive strength of the composite diaphragm, thereby improving the electrical performance of the battery.

[0008] A first aspect of the present application provides a composite membrane, comprising a base membrane and an adhesive coating, wherein the adhesive coating is located on the outermost layer of the composite membrane, and the adhesive coating comprises polyethylene wax particles and inorganic particles;

[0009] The weight of the polyethylene wax particles per unit area of ​​the adhesive coating is 0.2-4 g / m2 ;

[0010] The ratio of D90 of the inorganic particles to D90 of the polyethylene wax particles is (0.3-0.85):1;

[0011] The weight of the inorganic particles is 5-75 wt % of the total weight of the polyethylene wax particles and the inorganic particles.

[0012] The present application provides a composite separator, comprising a base film and an adhesive coating, wherein the base film is prepared using a conventional dry uniaxial stretching process in the art, and the adhesive coating is located as the outermost layer of the composite separator, capable of bonding to the positive electrode sheet and / or the negative electrode sheet. In a specific embodiment, the adhesive coating can be directly disposed on the upper and / or lower surface of the base film, or another coating can be disposed between the base film and the adhesive coating, depending on actual needs.

[0013] The adhesive coating includes polyethylene wax particles, which can play a good bonding role, prevent dimensional changes caused by internal stress release, and improve the problem of wrinkling of the diaphragm after injecting electrolyte, while the inorganic particles play a supporting role. By adjusting the weight ratio, size ratio and weight of polyethylene wax particles per unit area of ​​​​the polyethylene wax particles and inorganic particles, it is possible to reduce the increase in air permeability before and after the adhesive coating is set and before and after the hot pressing of the composite diaphragm while ensuring the bonding strength of the composite diaphragm, thereby improving the electrical performance of the battery.

[0014] In one embodiment, Figure 1 is a schematic structural diagram of a composite diaphragm provided in an embodiment of the present application. As shown in Figure 1, the composite diaphragm includes a base membrane 1 and an adhesive coating 2 arranged on the upper and lower surfaces of the base membrane. The adhesive coating 2 is located on the outermost layer of the composite diaphragm and can contact the positive electrode sheet and the negative electrode sheet; wherein, the base membrane 1 is prepared by a conventional dry process in the field, such as a PP microporous base membrane, a PE microporous base membrane, a PP double-layer base membrane, a PP / PP / PP three-layer co-extruded microporous base membrane, and a PP / PE / PP three-layer co-extruded microporous base membrane.

[0015] Furthermore, the base membrane 1 has a thickness of 4-25 μm, a maximum pore size of 20-60 nm, and a porosity of 20-60%; wherein the definition of thickness is the same as the conventional definition in the art, that is, the distance between the upper surface and the lower surface of the base membrane for setting the adhesive coating; the maximum pore size refers to the maximum diameter of the pores of the base membrane, which can be obtained by measuring with a PMI instrument; the porosity refers to the percentage of the total volume of all pores in the base membrane to the total volume of the base membrane. During the test, in accordance with the provisions of GB / T 6673-2001 and GB / T 6672-2001, the length, width, and thickness of the diaphragm are measured, and the mass of the sample is weighed using an analytical balance with a resolution of 0.0001 g, and calculated according to Formula 1: P = (1-m / (L*b*d*ρ))*100% Formula 1

[0016] In formula 1, P is the porosity of the diaphragm, in %; m is the mass of the diaphragm, in g; L is the length of the diaphragm, in cm; b is the width of the diaphragm, in cm; d is the thickness of the diaphragm, in μm; ρ is the density of the raw material, in g / cm 2 .

[0017] Figure 2 is an electron microscope image of the adhesive coating provided in an embodiment of the present application. As shown in Figure 2, the adhesive coating 2 includes polyethylene wax particles and inorganic particles. The polyethylene wax particles can play a good bonding role, prevent dimensional changes caused by internal stress release, and improve the problem of wrinkling of the diaphragm after injecting electrolyte, while the inorganic particles play a supporting role, preventing the polyethylene wax particles from being squeezed and deformed during hot pressing to block the pores of the base membrane and reduce the permeability increase.

[0018] It can be understood that the polyethylene wax particles and inorganic particles are in granular form. When the adhesive coating is directly set on the surface of the base film, the particles close to the surface of the base film will partially enter the pores of the base film. At the same time, the polyethylene wax particles and inorganic particles are not limited to spherical forms, and can also exist in various forms such as ellipsoids and irregular spheres.

[0019] In the present application, by adjusting the weight ratio, size ratio and weight of polyethylene wax particles per unit area of ​​the polyethylene wax particles and the inorganic particles, the permeability increment before and after the adhesive coating is set and before and after the hot pressing of the composite diaphragm can be effectively reduced, thereby improving the electrical performance of the battery.

[0020] Specifically, the weight of the polyethylene wax particles per unit area of ​​the adhesive coating is 0.2-4 g / m 2 , specifically selected from 0.2g / m 2 , 0.5g / m 2 , 1.0g / m 2 , 1.5g / m 2 , 1.8g / m 2 , 2.0g / m2 , 2.5g / m 2 3.0g / m 2 3.5g / m 2 , 4.0g / m 2 or any two thereof; further, in the adhesive coating per unit area, the weight of the polyethylene wax particles is 0.3-1.5 g / m 2 By limiting the total weight of polyethylene wax particles per square meter of the adhesive coating, it is possible to take into account the adhesive strength of the adhesive coating and the air permeability increment before and after the adhesive coating and before and after the hot pressing of the composite diaphragm.

[0021] Specifically, in order to ensure the bonding force between the adhesive coating and the electrode, the D90 of the inorganic particles should be smaller than the D90 of the polyethylene wax particles; further, the ratio of the D90 of the inorganic particles to the D90 of the polyethylene wax particles is (0.3-0.85):1, specifically selected from the range of 0.3:1, 0.5:1, 0.55:1, 0.7:1, 0.8:1, 0.85:1 or any two thereof; further, the ratio of the D90 of the inorganic particles to the D90 of the polyethylene wax particles is (0.5-0.85):1; D90 refers to the particle size corresponding to when the cumulative particle size distribution number of polyethylene particles / inorganic particles reaches 90%, which can be obtained according to GB / T 19077.1-2008 test.

[0022] In a specific embodiment of the present application, the D90 of the polyethylene wax is 1-10 μm, specifically selected from the range of 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm or any two thereof; further, the D90 of the polyethylene wax is 2-5 μm; by controlling the D90 of the polyethylene wax particles, on the one hand, it is possible to avoid the D90 being too large, resulting in an excessive thickness of the adhesive coating, and on the other hand, it is possible to avoid the problem of D90 being too small, resulting in clogging of the base membrane pores, and to avoid an increase in the permeability increment before and after the adhesive coating is set and before and after the hot pressing of the composite diaphragm.

[0023] In a specific embodiment of the present application, the D10 of the polyethylene wax particles should be greater than the maximum pore size of the base membrane. Furthermore, the ratio of the D10 of the polyethylene wax particles to the maximum pore size of the base membrane is 3-50. Furthermore, the ratio of the D10 of the polyethylene wax particles to the maximum pore size of the base membrane is 25-40. D10 refers to the particle size corresponding to when the cumulative particle size distribution number of the polyethylene wax particles reaches 10%. By controlling the D10 of the polyethylene wax particles, the polyethylene wax can be effectively prevented from clogging the pores of the base membrane, resulting in an increase in the air permeability before and after the adhesive coating is set and before and after the hot pressing of the composite diaphragm.

[0024] Furthermore, the specific value of D10 of the polyethylene wax particles can be determined according to the maximum pore size of the base film.

[0025] In addition, it should be noted that when the polyethylene wax particles and inorganic particles are irregular in shape, the particle sizes involved are all equivalent particle sizes.

[0026] In a specific embodiment of the present application, the melting point of the polyethylene wax particles is 90-130°C, and the melting point refers to the temperature at which the polyethylene wax particles change from solid to liquid, specifically selected from 90°C, 100°C, 103°C, 105°C, 108°C, 110°C, 112°C, 115°C, 110°C, 118°C, 120°C, 130°C or a range consisting of any two of them; further, the melting point of the polyethylene wax particles is 100-120°C; by controlling the melting point of the polyethylene wax microspheres, it is possible to ensure that the polyethylene wax particles do not melt during the preparation and hot pressing process, thereby avoiding the problem of clogging the pores of the base membrane, avoiding excessive increase in the permeability of the adhesive coating and the diaphragm, and avoiding too high a melting point resulting in small deformation of the polyethylene wax particles, resulting in less than expected bonding effect.

[0027] In a specific embodiment of the present application, the number average molecular weight is directly related to the melting point of the polyethylene wax particles. Therefore, the present application further limits the number average molecular weight of the polyethylene wax. Specifically, the number average molecular weight of the polyethylene wax particles is 500-20000. Further, the number average molecular weight of the polyethylene wax particles is 1000-5000. The number average molecular weight can be obtained according to GB / T36214.4-2018 test.

[0028] Specifically, the weight of the inorganic particles is 5-75wt% of the total weight of the polyethylene wax particles and the inorganic particles, that is, the weight of the inorganic particles / (the weight of the inorganic particles+the weight of the polyethylene wax particles)*100%=5-75wt%, specifically selected from 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt% or a range consisting of any two of them; further, the weight of the inorganic particles is 25-60wt% of the total weight of the polyethylene wax particles and the inorganic particles; the inorganic particles mainly play a supporting role. If the weight of the inorganic particles is too low, the polyethylene wax particles may be deformed too much during the hot pressing process, thereby blocking the pores on the surface of the base film, affecting the air permeability increment before and after the adhesive coating is set and before and after the hot pressing of the composite diaphragm, and affecting the electrical performance of the battery.

[0029] In a specific embodiment of the present application, the inorganic particles may be one or more of alumina, boehmite, silica, magnesium oxide, and titanium dioxide.

[0030] The adhesive coating provided in the present application also includes one or more of an adhesive, a surfactant, and a dispersant. The adhesive is used to bond the polyethylene wax and inorganic particles to the surface of the base film, the dispersant is used to ensure the dispersion of each component in the adhesive coating, and the surfactant is used to improve the leveling of the slurry during the coating process.

[0031] The adhesive, surfactant and dispersant can all be conventional materials in the art. Specifically, the adhesive is one or more of polyacrylate, polyacrylamide, polymethyl methacrylate, polybutyl methacrylate, polyethyl acrylate, styrene acrylic latex, polyvinyl acetate, styrene-butadiene latex, ethylene-vinyl acetate copolymer, and polyvinyl pyrrolidone; the surfactant is one or more of polyether-modified polysiloxane, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ether, fatty amine polyoxyethylene ether, and fluoroalkyl ethoxy alcohol ether; the dispersant is one or more of sodium polyacrylate, ammonium polyacrylate, carboxylate, and sulfonate. Furthermore, the dispersant is one or both of ammonium polyacrylate and sodium polyacrylate.

[0032] Furthermore, the weight of the adhesive is 2-10 wt% of the total weight of the polyethylene wax particles and the inorganic particles; furthermore, the weight of the adhesive is 3-5 wt% of the total weight of the polyethylene wax particles and the inorganic particles.

[0033] Furthermore, the weight of the dispersant is 0.2-5 wt % of the total weight of the inorganic particles. Furthermore, the weight of the dispersant is 0.5-2 wt % of the total weight of the inorganic particles.

[0034] During the preparation of the composite membrane, polyethylene wax particles and inorganic particles in emulsion form are dispersed in an aqueous solvent to prepare an adhesive coating slurry, which is then coated on the surface of a base film obtained by dry uniaxial stretching and dried to obtain the composite membrane.

[0035] Specifically, the total weight of the polyethylene wax particles and the inorganic particles is 2-50 wt % of the weight of the adhesive coating slurry, and further, the total weight of the polyethylene wax particles and the inorganic particles is 5-20 wt % of the weight of the adhesive coating slurry. The weight of the polyethylene wax particles and the inorganic particles is carried out according to the aforementioned weight ratio.

[0036] When the adhesive coating includes an adhesive, a surfactant and a dispersant, the weights of the adhesive and the dispersant are as described above, the weight of the surfactant is 0.1-1 wt% of the total weight of the adhesive coating slurry, and further, the weight of the surfactant is 0.2-0.5 wt% of the total weight of the adhesive coating slurry.

[0037] In a specific embodiment of the present application, the preparation process of the adhesive coating slurry is as follows:

[0038] Step 1: adding a dispersant and inorganic particles to deionized water in sequence and dispersing to obtain a first preform;

[0039] Step 2: mixing polyethylene wax particles and deionized water, and dispersing them to obtain a second preform;

[0040] Step 3: Mix the first preform and the second preform in proportion and continue to disperse to obtain a first mixture;

[0041] Step 4: adding the adhesive and the surfactant to the first mixture and dispersing them evenly to obtain an adhesive coating slurry;

[0042] Furthermore, the dispersion speed of each of the above steps is 500-3000 rpm, the dispersion time is 5-60 min, and the dispersion temperature is 10-30°C;

[0043] Step 5: Prepare a dry uniaxially stretched base film according to conventional methods in the art, apply the adhesive coating slurry on the surface of the base film, dry it in an oven at 40-70°C, and then roll it up to obtain a composite diaphragm containing an adhesive coating; further, control the baking temperature to 50-60°C.

[0044] In a specific embodiment, the D10 and D90 of the polyethylene wax particles and the inorganic particles can be achieved by adjusting the particle size distribution; the number average molecular weight and melting point of the polyethylene wax particles can be prepared according to conventional technical means in the field; the weight of the polyethylene wax particles per unit area of ​​the adhesive coating can be adjusted by the coating thickness or surface density.

[0045] In summary, the present application provides a composite diaphragm, which includes a microporous base film obtained by dry uniaxial stretching and an adhesive coating. The adhesive coating includes polyethylene wax particles, which can play a good bonding role, prevent dimensional changes caused by internal stress release, and improve the problem of wrinkling of the diaphragm after injection of electrolyte, while the inorganic particles play a supporting role. By adjusting the weight ratio, size ratio and weight of polyethylene wax particles per unit area of ​​the polyethylene wax particles and the inorganic particles, it is possible to reduce the air permeability increment before and after the adhesive coating is set and before and after the hot pressing of the composite diaphragm on the basis of ensuring the bonding strength of the composite diaphragm, thereby improving the electrical performance of the battery.

[0046] A second aspect of the present application provides a battery, comprising any of the composite diaphragms described above.

[0047] Based on the characteristics of the composite membrane of the first aspect of the present application, the composite membrane provided by the present application helps to improve the electrical performance of the battery.

[0048] In a specific embodiment, the battery provided in the present application further includes a positive electrode sheet, a negative electrode sheet and an electrolyte, the positive electrode sheet includes a positive electrode collector and a positive electrode active layer arranged on the surface of the positive electrode collector, and the positive electrode active layer includes a positive electrode active material, a conductive agent and a binder; the negative electrode sheet includes a negative electrode collector and a negative electrode active layer arranged on the surface of the negative electrode collector, and the negative electrode active layer includes a negative electrode active material, a conductive agent and a binder.

[0049] The selection of positive electrode active materials, negative electrode active materials, conductive agents, and binders is not special and can be conventionally selected in the art. Taking lithium-ion batteries as an example, the positive electrode active material is selected from one or more of lithium cobalt phosphate, lithium nickel cobalt manganese oxide, lithium iron phosphate, lithium nickel cobalt aluminum oxide, and lithium iron manganese phosphate; the negative electrode active material is selected from one or more of artificial graphite, natural graphite, hard carbon, mesophase carbon microbeads, lithium titanate, silicon carbon, and silicon dioxide; the conductive agent is selected from one or more of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, single-walled carbon nanotubes, multi-walled carbon nanotubes, and carbon fiber; and the binder is selected from one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and lithium polyacrylate (PAALi).

[0050] The electrolyte is a conventional electrolyte known in the art comprising a lithium salt and a solvent, wherein the solvent contains ethylene carbonate (abbreviated as EC), diethyl carbonate (abbreviated as DEC), propylene carbonate (abbreviated as PC), and fluoroethylene carbonate (abbreviated as FEC).

[0051] The present application provides a composite diaphragm, which includes a microporous base film obtained by dry uniaxial stretching and an adhesive coating located on the surface of the base film. The adhesive coating includes polyethylene wax particles, which can play a good bonding role, prevent dimensional changes caused by internal stress release, and improve the problem of diaphragm wrinkling after electrolyte injection. The inorganic particles play a supporting role. By adjusting the weight ratio, size ratio and weight of the polyethylene wax particles per unit area of ​​the polyethylene wax particles and the inorganic particles, it is possible to reduce the air permeability increment before and after the adhesive coating is set and before and after the hot pressing of the composite diaphragm on the basis of ensuring the bonding strength of the composite diaphragm, thereby improving the electrical performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, a brief introduction will be given below to the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0053] FIG1 is a schematic structural diagram of a composite diaphragm provided in one embodiment of the present application;

[0054] FIG2 is an electron microscope image of an adhesive coating provided in one embodiment of the present application.

[0055] Description of reference numerals: 1 - base film; 2 - adhesive coating layer. DETAILED DESCRIPTION

[0056] To make the purpose, technical solutions, and advantages of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0057] Example 1

[0058] The diaphragm provided in this embodiment includes a PP microporous membrane and an adhesive coating on the surface of the PP microporous membrane, wherein the PP microporous membrane has a thickness of 14 μm, a maximum pore size of 30 nm, and a porosity of 40%; the adhesive coating includes polyethylene wax particles, boehmite, ammonium polyacrylate, polyethyl acrylate, and polyether-modified polysiloxane. The parameters of the polyethylene wax particles and boehmite are shown in Table 1.

[0059] The method for preparing the diaphragm provided in this embodiment includes the following steps:

[0060] Step 1: Prepare adhesive coating slurry:

[0061] Ammonium polyacrylate was added to deionized water and dispersed at a speed of 1500 rpm for 10 minutes; then boehmite powder with a D90 of 2.4 μm was added and dispersed at a speed of 3000 rpm for 40 minutes to obtain a first preform; polyethylene wax particle emulsion was added to deionized water, dispersed at a speed of 2000 rpm and a dispersion time of 20 minutes to obtain a second preform; the second preform was added to the first preform, dispersed at a speed of 3000 rpm and a dispersion time of 30 minutes to obtain a first mixture; polyethyl acrylate was added to the first mixture, dispersed at a speed of 1500 rpm and a dispersion time of 30 minutes to obtain a second mixture; polyether modified polysiloxane was added to the second mixture, dispersed at a speed of 1000 rpm and a dispersion time of 20 minutes to obtain an adhesive coating slurry; in the above preparation process, the dispersion temperature was set to 15°C.

[0062] In the adhesive coating slurry, the total weight of polyethylene wax particles and boehmite is 8wt% of the slurry system, the weight of boehmite is 40wt% of the total weight of polyethylene wax particles and boehmite, the weight of ammonium polyacrylate is 2wt% of the weight of boehmite, the weight of polyethyl acrylate is 3wt% of the total weight of polyethylene wax particles and boehmite, and the weight of polyether-modified polysiloxane is 0.3wt% of the slurry system.

[0063] Step 2: Apply the adhesive coating slurry on the surface of a uniaxially stretched PP microporous membrane with a thickness of 14 μm, a maximum pore size of 30 nm, and a porosity of 40%. The weight of the polyethylene wax particles per unit area in the coating is 0.6 g / m 2 After drying in an oven at 50°C, the membrane is rolled up to obtain a separator.

[0064] Example 2

[0065] The diaphragm provided in this embodiment and the preparation method thereof can refer to Example 1, except that the D10 of the polyethylene wax particles is 0.75 μm.

[0066] Example 3

[0067] The diaphragm provided in this embodiment and the preparation method thereof can refer to Example 1, except that the D10 of the polyethylene wax particles is 1.2 μm.

[0068] Example 4

[0069] The diaphragm provided in this embodiment and the preparation method thereof can refer to Example 1, except that the D10 of the polyethylene wax particles is 1.5 μm.

[0070] Example 5

[0071] The diaphragm provided in this embodiment and the preparation method thereof can refer to Example 1, except that the D10 of the polyethylene wax particles is 0.12 μm.

[0072] Example 6

[0073] The diaphragm provided in this embodiment and the preparation method thereof can refer to Example 1, except that the D10 of the polyethylene wax particles is 1.56 μm.

[0074] Example 7

[0075] The diaphragm provided in this embodiment and its preparation method can refer to Example 1, except that the maximum pore size of the base membrane is 25 nm, the D10 of the polyethylene wax particles is 0.6 μm, the D90 is 1 μm, and the D90 of boehmite is 0.8 μm.

[0076] Example 8

[0077] The diaphragm provided in this embodiment and its preparation method can refer to Example 7, except that the D90 of the polyethylene wax particles is 2 μm, and the D90 of the boehmite is 1.6 μm.

[0078] Example 9

[0079] The diaphragm provided in this embodiment and the preparation method thereof can refer to Example 7, except that the D90 of the polyethylene wax particles is 5 μm and the D90 of the boehmite is 4 μm.

[0080] Example 10

[0081] The diaphragm provided in this embodiment and the preparation method thereof can refer to Example 7, except that the D90 of the polyethylene wax particles is 10 μm and the D90 of the boehmite is 8 μm.

[0082] Example 11

[0083] The diaphragm provided in this embodiment and its preparation method can refer to Example 1, except that the maximum pore size of the base film is 35 nm, the D10 of the polyethylene wax particles is 0.8 μm, the D90 is 3 μm, the D90 of the boehmite is 2.4 μm, and the weight of the polyethylene wax particles per unit area in the coating is 0.2 g / m 2 .

[0084] Example 12

[0085] The diaphragm provided in this embodiment and its preparation method can refer to Example 11, except that the weight of the polyethylene wax particles per unit area of ​​the adhesive coating is 0.6 g / m 2 .

[0086] Example 13

[0087] The diaphragm provided in this embodiment and its preparation method can refer to Example 11, except that the weight of the polyethylene wax particles per unit area of ​​the adhesive coating is 1.5 g / m 2 .

[0088] Example 14

[0089] The diaphragm provided in this embodiment and its preparation method can refer to Example 11, except that the weight of the polyethylene wax particles per unit area of ​​the adhesive coating is 4 g / m 2 .

[0090] Example 15

[0091] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the D90 of boehmite is 0.9 μm.

[0092] Example 16

[0093] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the D90 of boehmite is 1.8 μm.

[0094] Example 17

[0095] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the D90 of boehmite is 2.55 μm.

[0096] Example 18

[0097] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the melting point of the polyethylene wax particles is 85°C.

[0098] Example 19

[0099] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the melting point of the polyethylene wax particles is 135°C.

[0100] Example 20

[0101] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the melting point of the polyethylene wax particles is 90°C.

[0102] Example 21

[0103] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the melting point of the polyethylene wax particles is 100°C.

[0104] Example 22

[0105] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the melting point of the polyethylene wax particles is 120°C.

[0106] Example 23

[0107] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the melting point of the polyethylene wax particles is 130°C.

[0108] Example 24

[0109] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the weight of the boehmite is 5 wt% of the total weight of the polyethylene wax particles and the boehmite.

[0110] Example 25

[0111] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the weight of the boehmite is 25 wt % of the total weight of the polyethylene wax particles and the boehmite.

[0112] Example 26

[0113] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the weight of boehmite is 60 wt % of the total weight of the polyethylene wax particles and the boehmite.

[0114] Example 27

[0115] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the weight of the boehmite is 75 wt % of the total weight of the polyethylene wax particles and the boehmite.

[0116] Comparative Example 1

[0117] The diaphragm provided in this comparative example and its preparation method can refer to Example 7, except that the D90 of the polyethylene wax particles is 0.8 μm, and the D90 of the boehmite is 0.64 μm.

[0118] Comparative Example 2

[0119] The diaphragm provided in this comparative example and its preparation method can refer to Example 7, except that the D90 of the polyethylene wax particles is 11 μm, and the D90 of the boehmite is 8.8 μm.

[0120] Comparative Example 3

[0121] The diaphragm provided in this comparative example and its preparation method can refer to Example 12, except that the particle sizes of the polyethylene wax particles and boehmite are different, as shown in Table 1.

[0122] Comparative Example 4

[0123] The diaphragm and its preparation method provided in this comparative example can refer to Example 12, except that the weight of the polyethylene wax particles per unit area of ​​the adhesive coating is 0.15 g / m 2 .

[0124] Comparative Example 5

[0125] The diaphragm and its preparation method provided in this comparative example can refer to Example 12, except that the weight of the polyethylene wax particles per unit area of ​​the adhesive coating is 4.5 g / m 2 .

[0126] Comparative Example 6

[0127] The diaphragm and preparation method thereof provided in this comparative example can refer to Example 12, except that the D90 of the boehmite is 0.6 μm.

[0128] Comparative Example 7

[0129] The diaphragm provided in this comparative example and its preparation method can refer to Example 12, except that the D90 of boehmite is 2.7 μm.

[0130] Comparative Example 8

[0131] The diaphragm and its preparation method provided in this comparative example can refer to Example 18, except that the weight of boehmite is 0, that is, the weight of boehmite is 0wt% of the total weight of polyethylene wax particles and boehmite. The weight of polyethylene wax particles per unit area of ​​the adhesive coating is 4.5g / m 2 .

[0132] Comparative Example 9

[0133] The diaphragm provided in this comparative example and its preparation method can refer to Example 19, except that the weight of boehmite is 85wt% of the total weight of polyethylene wax particles and boehmite, and the weight of polyethylene wax particles per unit area of ​​the adhesive coating is 0.15g / m 2 .

[0134] Comparative Example 10

[0135] The diaphragm provided in this embodiment and its preparation method can refer to Example 12, except that the weight of boehmite is 80 wt % of the total weight of the polyethylene wax particles and the boehmite.

[0136] Comparative Example 11

[0137] A uniaxially stretched PP microporous membrane with a thickness of 14 μm, a maximum pore size of 35 nm, and a porosity of 40% was used as a comparison sample.

[0138] Table 1 lists the separators provided by Examples 1-27 and Comparative Examples 1-11 to make the differences between the separators provided by Examples 1-27 and Comparative Examples 1-11 more intuitive:

[0139] Table 1 Description of the composite membranes provided in Examples 1-27 and Comparative Examples 1-11

[0140] Composite membranes were provided for Examples 1-27 and Comparative Examples 1-11. The air permeability was tested before and after the adhesive coating was applied and before and after hot pressing. The air permeability increment was calculated. The adhesion and liquid injection wrinkling of the composite membranes were also tested. The test method is as follows. The test results are shown in Table 2:

[0141] Test method:

[0142] 1. Air permeability increment of the adhesive coating: Test the air permeability of the base film. After applying the adhesive coating slurry, test the air permeability of the composite membrane. The absolute value of the difference between the two air permeabilities is the air permeability increment of the adhesive coating. The air permeability test method refers to GB / T 36363-2018.

[0143] 2. Air permeability increment of the composite membrane after hot pressing: Test the air permeability of the composite membrane before hot pressing. Then, stack two flat non-woven fabrics larger than the membrane surface area on top and bottom of the composite membrane. Place the membrane in a hot press and pressurize at 80°C and 1 MPa for 60 seconds. Test the air permeability after hot pressing. Calculate the difference between the air permeability before and after hot pressing to obtain the air permeability increment of the composite membrane after hot pressing. Refer to GB / T 36363-2018 for the air permeability test method.

[0144] 3. Adhesion: Stack A4 paper, non-woven fabric, 20mm-wide positive electrode material, 15mm-wide composite separator, and 10mm-wide silicone strip in the center, bottom to top, and place on the lower platen of a hot press. The hot pressing conditions are: temperature 80°C, pressure 1MPa, and pressurization for 60s. The positive electrode sheet and composite microporous membrane are each secured to a stretching machine and peeled 180° at a speed of 200mm / min. Repeat the measurement five times and take the average value.

[0145] 4. Confirmation of wrinkles after injection: simulate the assembly of the composite diaphragm, inject the electrolyte and leave it for 5 days, disassemble the battery cell, observe and record the number of wrinkles per square meter of the composite diaphragm; if the diaphragm has no wrinkles, it is judged as excellent; if the diaphragm has 1-2 wrinkles, it is judged as good; if the diaphragm has more than 3 wrinkles, it is judged as poor.

[0146] Table 2 Test results of the diaphragms provided by Examples 1-27 and Comparative Examples 1-11

[0147] According to the data provided in Table 1-2, compared with Comparative Example 1-11, the composite diaphragm provided by Example 1-27 does not have the problem of wrinkling after liquid injection, and has good adhesion to the positive electrode plate. On this basis, the air permeability increment before and after the setting of the adhesive coating and before and after hot pressing is effectively reduced, solving the technical problem to be solved in this application.

[0148] According to the data provided in Examples 1-6, as the ratio of D10 of polyethylene wax particles to the maximum pore size of the base membrane increases, the bonding force between the composite diaphragm and the electrode continues to increase, and the incremental air permeability of the adhesive coating decreases. However, when the ratio of the two is greater than 50, the incremental air permeability of the composite diaphragm before and after hot pressing becomes larger. Therefore, the ratio of D10 of polyethylene wax particles to the maximum pore size of the base membrane should be between 3-50, and further 25-40.

[0149] The data provided in Examples 7-10 and Comparative Examples 1-2 show that as the D90 of the polyethylene wax particles increases, the incremental air permeability before and after the adhesive coating is applied decreases, as does the incremental air permeability before and after hot pressing of the composite separator. However, considering the thickness of the adhesive coating, the D90 of the polyethylene wax particles is preferably 1-10 μm, more preferably 2-5 μm. Compared to Comparative Examples 1-2, polyethylene wax particles with too low or too high a D90 are prone to high incremental air permeability, decreased adhesion of the composite separator, and wrinkles on the membrane surface.

[0150] According to the data provided in Examples 11-14 and Comparative Examples 4-5, it can be seen that as the weight of polyethylene wax particles per unit area of ​​the adhesive coating increases, the adhesive force of the adhesive coating continues to increase, but at the same time, the incremental air permeability of the adhesive coating and the composite diaphragm before and after hot pressing also continues to increase. Therefore, the weight of polyethylene wax particles per unit area of ​​the adhesive coating should be controlled within the range of 0.2-4 g / m 2 , more preferably 0.3-1.5g / m 2 Compared with Comparative Examples 4-5, if the weight of polyethylene wax particles per unit area of ​​the adhesive coating is too low, the adhesion between the composite diaphragm and the electrode will be affected, resulting in wrinkles on the membrane surface; while if the weight of polyethylene wax particles is too high, the air permeability increment will increase, affecting the air permeability of the composite diaphragm.

[0151] According to the data provided in Examples 15-17, when the particle size of the polyethylene wax particles remains unchanged, as the D90 of the inorganic particles continues to increase, the incremental air permeability of the composite diaphragm before and after the adhesive coating is set and before and after hot pressing continues to decrease, but the bonding strength of the adhesive coating decreases; referring to Comparative Examples 3 and 7, when the ratio of D90 of the inorganic particles to the polyethylene wax particles is greater than 0.85:1, it may lead to insufficient bonding area between the polyethylene wax particles and the electrode, and then lead to too little bonding strength between the composite diaphragm and the electrode, resulting in wrinkles on the membrane surface; on the contrary, referring to Comparative Example 6, when the ratio of D90 of the two is too low, the polyethylene wax particles may be deformed too much during the hot pressing process, blocking the pores on the surface of the base film and affecting the air permeability of the composite diaphragm; therefore, the ratio of D90 of the inorganic particles to the polyethylene wax particles should be between (0.3-0.85):1, and more preferably (0.5-0.85):1.

[0152] According to the data provided in Examples 18-23, as the melting point of the polyethylene wax particles increases, the incremental air permeability of the composite diaphragm before and after hot pressing continues to decrease, but the adhesion of the adhesive coating also continues to decrease. Therefore, the melting point of the polyethylene wax particles should be 90-130°C, and more preferably 100-120°C.

[0153] The data provided in Examples 24-27 show that as the weight fraction of inorganic particles increases, the incremental air permeability of the composite diaphragm before and after hot pressing decreases, but the incremental air permeability before and after the application of the adhesive coating increases continuously. Compared to Comparative Example 10, when the weight fraction of inorganic particles exceeds 75wt%, the incremental air permeability of the adhesive coating increases sharply, resulting in an excessively low weight of polyethylene wax particles per unit area of ​​the adhesive coating, affecting the adhesion between the composite diaphragm and the electrode. Therefore, the weight of the inorganic particles is controlled to be 5-75wt% of the total weight of the polyethylene wax particles and inorganic particles, and more preferably 25-60wt%.

[0154] In summary, the composite diaphragm containing polyethylene wax particles and inorganic particles provided in the present application not only ensures the bonding force between the composite diaphragm and the electrode and solves the problem of wrinkles on the surface of the diaphragm, but also reduces the problem of a large increase in air permeability caused by setting an adhesive coating and a large increase in air permeability before and after hot pressing of the composite diaphragm, thereby helping to improve the electrical performance of the battery.

[0155] It should be noted that the same effect can be achieved by replacing the base film in the above embodiments with a PE microporous film, a PP double-layer film, a PP / PP / PP three-layer co-extruded microporous film, and a PP / PE / PP three-layer co-extruded microporous film; similarly, the same effect can be achieved by replacing the inorganic particles in the above embodiments with alumina, silica, magnesium oxide, titanium dioxide, etc.

[0156] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A composite diaphragm, wherein: The composite diaphragm comprises a base film and an adhesive coating, wherein the adhesive coating is located at the outermost layer of the composite diaphragm, and the adhesive coating comprises polyethylene wax particles and inorganic particles; In the adhesive coating per unit area, the weight of the polyethylene wax particles is 0.2-4 g / m 2 ; The ratio of D90 of the inorganic particles to D90 of the polyethylene wax particles is (0.3-0.85):1; The weight of the inorganic particles is 5-75 wt % of the total weight of the polyethylene wax particles and the inorganic particles.

2. The composite diaphragm according to claim 1, wherein: The melting point of the polyethylene wax particles is 90-130°C.

3. The composite diaphragm according to claim 1, wherein: The number average molecular weight of the polyethylene wax particles is 500-20000.

4. The composite diaphragm according to claim 1, wherein: The polyethylene wax particles at least meet one or more of the following combinations: a. The D10 of the polyethylene wax particles is greater than the maximum pore size of the base film; b. The D90 of the polyethylene wax particles is 1-10 μm.

5. The composite diaphragm according to claim 1, wherein: The ratio of D10 of the polyethylene wax particles to the maximum pore size of the base film is 3-50.

6. The composite diaphragm according to any one of claims 1 to 5, wherein: The inorganic particles are one or more of alumina, boehmite, silica, magnesium oxide, and titanium dioxide.

7. The composite diaphragm according to any one of claims 1 to 6, wherein: The adhesive coating further comprises one or more of an adhesive, a surfactant, and a dispersant; Wherein, the adhesive is one or more of polyacrylate, polyacrylamide, polymethyl methacrylate, polybutyl methacrylate, polyethyl acrylate, styrene acrylic latex, polyvinyl acetate, styrene butadiene latex, ethylene-vinyl acetate copolymer, and polyvinyl pyrrolidone; The surfactant is one or more of polyether-modified polysiloxane, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ether, fatty amine polyoxyethylene ether, and fluoroalkyl ethoxy alcohol ether; The dispersant is one or more of sodium polyacrylate, ammonium polyacrylate, carboxylate, sulfonate kind.

8. The composite diaphragm according to claim 7, wherein: At least one or more of the following combinations are met: a. The weight of the dispersant is 0.2-5wt% of the total weight of the inorganic particles; b. The weight of the adhesive is 2-10wt% of the total weight of the polyethylene wax particles and the inorganic particles.

9. The composite diaphragm according to any one of claims 1 to 8, wherein: The base film has a thickness of 4-25 μm, a maximum pore diameter of 20-60 nm, and a porosity of 20-60%.

10. A battery, wherein: The composite diaphragm comprises the composite diaphragm according to any one of claims 1 to 9.