Monocrystalline silicon rod and silicon wafer prepared therefrom, and battery, battery string and solar module
Patent Information
- Application Number
- MYPI2025005142
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-27
- Filing Date
- 2024-02-23
- Publication Date
- 2024-08-23
AI Technical Summary
In the field of photovoltaics, it is difficult to effectively control the resistivity of silicon wafers with existing technology, resulting in a decrease in the efficiency of solar cells, and the uneven resistivity of single crystal silicon rods increases production costs.
By reasonably controlling the concentration of antimony elements in single crystal silicon rods to ensure that it is within the range of 4E+14atom/cm3 to 2E+16atom/cm3, the resistivity uniformity of the silicon wafer is optimized, thereby improving the energy conversion efficiency and production efficiency of the battery. .
It achieves an improvement in the uniformity of the resistivity of the silicon wafer, extends the battery life, reduces energy loss and heat loss, and improves the overall efficiency of the battery and the quality of the finished product.
Smart Images

Figure PI2025005142_DRAWING_001 
Figure PI2025005142_DRAWING_002
Abstract
Description
A single crystal silicon rod and silicon wafer, battery, battery string and solar module made therefrom
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to the Chinese patent application filed with the Patent Office of China on February 23, 2023, with application number 202310158796.2, entitled “A single crystal silicon rod and silicon wafers, batteries and battery components made therefrom”, and the Chinese patent application filed with the Patent Office of China on September 27, 2023, with application number 202311267505.X, entitled “A single crystal silicon rod and silicon wafers, batteries and battery components made therefrom”, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of solar photovoltaics, and in particular to a single crystal silicon rod and silicon wafers, batteries, battery strings and solar modules made therefrom. Background Art
[0004] With the development of high-efficiency cell structures such as HJT and TOPCon, demand for N-type silicon wafers in the crystalline silicon photovoltaic market has increased dramatically. To further improve cell conversion efficiency, it is necessary to determine the optimal resistivity range for silicon wafers. Higher resistivity increases the series resistance of solar cell devices, while lower resistivity leads to severe carrier Auger recombination, both of which reduce solar cell efficiency. Therefore, for photovoltaics, ensuring that the resistivity of silicon wafers is within an optimal range can significantly improve cell conversion efficiency.
[0005] Furthermore, for mass-produced silicon wafers, improved resistivity concentration in monocrystalline silicon rods significantly improves back-end cell conversion efficiency. Currently, N-type silicon rods and wafers used in photovoltaic cells are primarily phosphorus-doped single crystals, resulting in significant resistivity differences between the head and tail of the N-type monocrystalline silicon rods. In the actual Cz crystal pulling process, achieving a narrower resistivity range is typically achieved by shortening the rod length, which increases actual crystal pulling costs.
[0006] Summary of the Invention
[0007] While exploring an excellent resistivity range for silicon wafers, this application controls the concentration of antimony in single crystal silicon rods to obtain single crystal silicon rods with an excellent resistivity range and resistivity concentration, thereby improving the overall finished product quality of single crystal silicon rods and achieving higher energy conversion efficiency for photovoltaic cells.
[0008] In order to solve the above technical problems, this application is implemented as follows:
[0009] The present application provides a single crystal silicon rod, wherein the single crystal silicon rod contains antimony element, and the concentration of the antimony element is 4E+14atom / cm 3 to 2E+16atom / cm 3 , the preferred concentration of antimony is 4.3E+14cm -3 to 1.9E+16cm -3 , further preferably the concentration of antimony element is 4.45E+14cm -3 to 1.87E+16cm -3 .
[0010] In the present application, since the concentration of antimony elements in the above-mentioned single crystal silicon rods is reasonably controlled, the resistivity of the silicon wafer or bare silicon wafer itself is made uniform. Preparing batteries with such silicon wafers can reduce the lateral transmission resistance of carriers and ultimately achieve an increase in battery efficiency.
[0011] Optionally, the concentration of antimony in the single crystal silicon rod is 0.15E+16atom / cm 3 to 1.95E+16atom / cm 3 .
[0012] Optionally, the concentration of antimony in the single crystal silicon rod is 0.4E+16atom / cm 3 to 1.05E+16atom / cm 3 .
[0013] Optionally, the concentration of antimony in the single crystal silicon rod is 0.5E+16atom / cm 3 to 0.7E+16 atom / cm 3 .
[0014] In the present application, by further controlling the concentration range of antimony elements, the formation of vacancy defects in silicon crystals can be further suppressed. On the one hand, less oxygen precipitates are formed after oxygen enters the silicon crystal; on the other hand, Auger recombination is reduced, the minority carrier lifetime of the silicon wafer is increased, the short-circuit current of the prepared battery is improved, and the battery efficiency is further improved.
[0015] Optionally, the single crystal silicon rod satisfies the following conditions: (the concentration of antimony at the tail end face of the single crystal silicon rod - the concentration of antimony at the head end face of the single crystal silicon rod) / the concentration of antimony at the tail end face of the single crystal silicon rod ≤10%, preferably (the concentration of antimony at the tail end face of the single crystal silicon rod - the concentration of antimony at the head end face of the single crystal silicon rod) / the concentration of antimony at the tail end face of the single crystal silicon rod ≤5%, further preferably (the concentration of antimony at the tail end face of the single crystal silicon rod - the concentration of antimony at the head end face of the single crystal silicon rod) / the concentration of antimony at the tail end face of the single crystal silicon rod ≤2%.
[0016] Optionally, the single crystal silicon rod satisfies the following conditions: (maximum antimony element concentration of the single crystal silicon rod - minimum antimony element concentration of the single crystal silicon rod) / maximum antimony element concentration of the single crystal silicon rod ≤ 10%, preferably (maximum antimony element concentration of the single crystal silicon rod - minimum antimony element concentration of the single crystal silicon rod) / maximum antimony element concentration of the single crystal silicon rod ≤ 5%, further preferably (maximum antimony element concentration of the single crystal silicon rod - minimum antimony element concentration of the single crystal silicon rod) / maximum antimony element concentration of the single crystal silicon rod ≤ 2%.
[0017] Optionally, the tail end face of the single crystal silicon rod satisfies the following conditions: -15%≤(concentration of antimony element in the center of the tail end face - concentration of antimony element at the edge of the tail end face) / concentration of antimony element in the center of the tail end face ≤15%, preferably -10%≤(concentration of antimony element in the center of the tail end face - concentration of antimony element at the edge of the tail end face) / concentration of antimony element in the center of the tail end face ≤10%, further preferably -5%≤(concentration of antimony element in the center of the tail end face - concentration of antimony element at the edge of the tail end face) / concentration of antimony element in the center of the tail end face ≤5%.
[0018] Optionally, the resistivity of the single crystal silicon rod is 0.2 to 10 Ω·cm, preferably 0.3 to 3 Ω·cm, and more preferably 0.5 to 1.2 Ω·cm; or the resistivity of the single crystal silicon rod is 0.3 to 10 Ω·cm, preferably 0.4 to 8 Ω·cm; and more preferably 0.5 to 6 Ω·cm.
[0019] In this application, by controlling the doping concentration distribution of the entire silicon rod, the resistivity concentration of the single crystal silicon rod is improved, the length of the crystal pulling rod can be increased, and costs can be saved; for the battery end, first, it can provide more stable and reliable battery performance, and consistent resistivity can ensure that each component is in similar working conditions, thereby reducing energy loss and efficiency loss, which is crucial to the performance and life of the battery; second, it can provide higher battery efficiency, and consistent resistivity enables the battery to better distribute and transmit electrical energy during operation, reducing electrical energy loss and improving the energy conversion efficiency of the battery. This can extend the battery's service life, reduce the number of charging times, and improve the energy efficiency of the entire system; furthermore, it can also reduce the heat loss of the battery. The battery will generate a certain amount of heat when working, and heat loss will reduce the efficiency of the battery. Due to the good resistivity concentration of the single crystal silicon rod, the transmission and distribution of electrical energy are more uniform, and the heat can also be better diffused and dispersed, thereby reducing heat loss and improving the energy conversion efficiency of the battery.
[0020] The present application also provides a silicon wafer, wherein the silicon wafer is a silicon wafer made according to the above-mentioned single crystal silicon rod, and the silicon wafer contains antimony element, and the concentration of the antimony element is 0.04E+16atom / cm 3 to 2.00E+16atom / cm 3, the preferred concentration of antimony is 4.30E+14cm -3 to 1.90E+16cm -3 , further preferably the concentration of antimony element is 4.45E+14cm -3 to 1.87E+16cm -3 .
[0021] In this application, by rationally controlling the antimony concentration of the silicon wafer, uniform doping is achieved, resulting in a uniform resistivity across the silicon wafer or bare silicon wafer itself. Using such a wafer in a battery can reduce the lateral carrier transport resistance, ultimately increasing battery efficiency. Furthermore, the silicon wafers used in this application exhibit a higher minority carrier lifetime, resulting in improved short-circuit current and further enhanced battery efficiency.
[0022] Optionally, the concentration of the antimony element is 0.15E+16atom / cm 3 to 1.95E+16atom / cm 3 .
[0023] Optionally, the concentration of the antimony element is 0.40E+16atom / cm 3 to 1.05E+16atom / cm 3 .
[0024] Optionally, the concentration of the antimony element is 0.50E+16atom / cm 3 to 0.70E+16 atom / cm 3 .
[0025] Optionally, the silicon wafer satisfies the following conditions: -15%≤(concentration of antimony element in the center of the radial cross section - concentration of antimony element at the edge of the radial cross section) / concentration of antimony element in the center of the radial cross section≤15%, preferably -10%≤(concentration of antimony element in the center of the radial cross section - concentration of antimony element at the edge of the radial cross section) / concentration of antimony element in the center of the radial cross section≤10%, further preferably -5%≤(concentration of antimony element in the center of the radial cross section - concentration of antimony element at the edge of the radial cross section) / concentration of antimony element in the center of the radial cross section≤5%.
[0026] In practical applications, radial concentration gradients can lead to differences in carrier concentration and resistivity across the cell plane. This in turn causes radial internal currents to flow during cell operation. This current is leakage current, which reduces the cell's opening voltage. In this application, the narrower the radial concentration range on the silicon wafer, the less carrier recombination occurs, the higher the open-circuit voltage, and the higher the cell efficiency.
[0027] Optionally, the silicon wafer further includes at least one of phosphorus, gallium, and germanium.
[0028] In the present application, when phosphorus is included in the silicon wafer, due to the difference in evaporation rates of antimony and phosphorus during the doping process, only a single phosphorus dopant is effective in the later stage of crystal pulling, thereby making the resistivity of the head and tail of the crystal ingot closer, thereby improving the uniformity of the axial resistivity, and the resistivity uniformity in the corresponding silicon wafer is also improved; when gallium is included in the silicon wafer, the longitudinal resistivity distribution of the prepared single crystal silicon rod is more uniform, thereby extending the length of the single crystal silicon rod in production, and further improving the resistivity uniformity in the silicon wafer prepared by cutting the silicon rod; when germanium is included in the silicon wafer, the effect of germanium and point defects (self-interstitial silicon atoms, vacancies) can be used to suppress native micro-defects in the silicon single crystal, especially void defects, which can effectively improve the quality and yield of the silicon single crystal, suppress native defects, and improve crystal quality.
[0029] Optionally, the margin of the silicon wafer is greater than 156 mm.
[0030] Because the doping concentration in the silicon rod is controlled in this application, the resistivity of the silicon wafers produced from the silicon rods is uniform, and large-sized silicon wafers can be produced. For example, the margin of the large-sized silicon wafer is greater than or equal to 156 mm.
[0031] Optionally, the silicon wafer is rectangular, one side of the rectangle is 156 mm to 300 mm, and the other side of the rectangle is 83 mm to 300 mm.
[0032] In the present application, since the silicon wafer is set to a rectangle, the rectangular silicon wafer of the present application can be a rectangular wafer obtained by machining and slicing the silicon rod, or it can be a rectangular wafer obtained by cutting the square / rectangular silicon wafer in half / slicing. Among them, one side of the rectangular silicon wafer or silicon substrate is controlled at 156mm to 300mm, and the other side is controlled at 83mm to 300mm. Compared with the square cell, the rectangular cell has a larger area, so the area that can be used to receive light is also larger, so that it can have a higher photoelectric conversion efficiency. Moreover, the cell provided in the embodiment of the present application is easier to transport after typesetting, which is conducive to improving the utilization rate of the container and thus improving the efficiency of transportation.
[0033] Optionally, the silicon wafer further includes a chamfer connecting two adjacent sides of the silicon wafer, and the arc length projection length of the chamfer is 1 mm to 10 mm.
[0034] In this application, setting chamfers on the silicon wafers is also beneficial to reducing damage to the silicon wafers during transportation and processing, improving the yield of subsequent processes, reducing the fragmentation rate, and reducing waste in production costs.
[0035] Optionally, the thickness of the silicon wafer is 40 μm to 170 μm, preferably 70 μm to 160 μm, and more preferably 80 μm to 140 μm.
[0036] In the present application, the thickness of the silicon wafer is set to 40 to 170 μm. First, the silicon wafer has higher strength, reduces the fragmentation rate of the silicon wafer, and is conducive to extending the service life of the silicon wafer. Secondly, when the thickness of the silicon wafer is 60 to 140 μm, the silicon wafer is easy to process and has a large production capacity, which can reduce production costs. That is, controlling the silicon wafer within a smaller thickness range is also conducive to reducing the production cost of the silicon wafer.
[0037] The present application also provides a battery, comprising the silicon wafer as described above or the silicon wafer made from the single crystal silicon rod as described above, wherein the battery comprises a silicon substrate, a doped region is provided on at least one surface of the silicon substrate, the silicon substrate contains antimony, the doped region is doped with a doping element, and the doping element is selected from a Group III element or a Group V element.
[0038] The doping concentration of antimony element in the silicon substrate is 4E+14cm -3 to 2E+16cm -3 , preferably 4.3E+14cm -3 to 1.9E+16cm -3 ; More preferably 4.45E+14cm -3 to 1.87E+16cm -3 .
[0039] In the present application, since the above-mentioned silicon substrate reasonably controls the concentration of antimony elements and achieves uniform doping, thereby making the resistivity of the silicon wafer or bare silicon wafer itself uniform, preparing batteries with such silicon wafers can reduce the lateral transmission resistance of carriers and ultimately achieve an increase in battery efficiency; in addition, the antimony atoms in the antimony-doped silicon wafer can capture and neutralize radiation-induced defects, thereby reducing the formation and diffusion of defects. Therefore, antimony-doped silicon wafers usually have better radiation stability after being made into batteries than phosphorus-doped silicon wafers.
[0040] Optionally, a doped region is provided in the surface of at least one side of the silicon substrate, or at least one doped passivation layer is provided on the surface of at least one side of the silicon substrate.
[0041] Because single-element doping can cause lattice distortion, which typically occurs in crystalline silicon, heavily doped areas often contain defects. In this application, the antimony atoms in antimony-doped silicon wafers can capture and neutralize radiation-induced defects, thereby reducing the formation and spread of defects. Therefore, antimony-doped silicon wafers typically exhibit better radiation stability when fabricated into solar cells than phosphorus-doped silicon wafers.
[0042] Optionally, the concentration of the antimony element in the doped region is substantially constant in the thickness direction of the silicon substrate.
[0043] Therefore, during the drawing process of the antimony-doped silicon rod, the doping atoms and silicon atoms are dissolved in the crystal lattice, so the concentration of antimony elements in the doped area remains basically unchanged along the thickness direction of the silicon substrate, thereby overcoming the crystalline silicon lattice distortion caused by single element doping, which results in many defects in the heavily doped area, and can also improve light absorption and increase battery efficiency.
[0044] Optionally, in the doping region, the sum of the concentration of antimony element and the concentration of doping element is less than or equal to 1E+21cm -3 .
[0045] The battery of the present application controls the range of the sum of the concentration of the doping region and the concentration of the doping element, thereby facilitating the separation of carriers, while reducing carrier recombination and improving short-circuit current and open-circuit voltage.
[0046] Optionally, when the doping element is a Group III element, the thickness of the doping region is in the range of 30 to 650 nm; or
[0047] When the doping element is a Group V element, the thickness of the doping region ranges from 100 to 200 nm.
[0048] Optionally, the doping region includes a first doping region and a second doping region,
[0049] An interface passivation layer and a doping passivation layer are sequentially stacked on the surface of the first doped region on the side away from the silicon substrate,
[0050] doping a first doping element in the doped passivation layer,
[0051] The second doping region on the silicon substrate is further doped with a second doping element,
[0052] The first doping region and the second doping region have opposite conductivity types.
[0053] In practical applications, single-element doping can lead to lattice distortion. This typically results in crystalline silicon lattice distortion, leading to numerous defects in heavily doped regions. In this application, by providing two doping regions, doping the doped passivation layer with a first doping element, and further doping the second doping element with a second doping element in the second doping region on the silicon substrate, the battery of this application can effectively prevent lattice distortion.
[0054] Optionally, the first doping element is a Group V element, the second doping element is a Group III element,
[0055] In the doped passivation layer, the concentration of the first doping element at a first preset depth from the surface of the doped passivation layer on a side away from the silicon substrate is greater than the concentration of the second doping element at the same first preset depth from the surface of the second doping region. The thickness of the doped passivation layer ranges from 100 to 400 nm, and the first preset depth is less than or equal to the thickness of the doped passivation layer.
[0056] In this approach, because the concentration of the first doping element is greater than that of the second doping element, free-carrier Auger recombination can be further reduced, further improving short-circuit current. Furthermore, this can be achieved without compromising the passivation effect of the tunneling layer, further improving short-circuit current, open-circuit voltage, and battery efficiency.
[0057] Optionally, the first doping element is a Group V element, the second doping element is a Group III element,
[0058] An interface passivation layer and a doping passivation layer are sequentially stacked on a surface of the second doped region on a side away from the silicon substrate;
[0059] In the doped passivation layer, the concentration of the first doping element at a first preset depth from the surface of the doped passivation layer on the side away from the silicon substrate in the first doping region is greater than the concentration of the second doping element at a first preset depth from the surface of the doped passivation layer on the side away from the silicon substrate in the second doping region, the thickness of the doped passivation layer on the first doping region ranges from 100 to 400 nm, the thickness of the doped passivation layer on the second doping region ranges from 100 to 400 nm, and the first preset depth is less than or equal to the thickness of the doped passivation layer on the first doping region.
[0060] In the present application, the thickness of the doped passivation layer on the first doped region and the second doped region is controlled in the range of 100 to 400 nm, so as to further reduce the free carrier Auger recombination and further improve the short-circuit current.
[0061] Optionally, a first doping element is doped into the interface passivation layer,
[0062] In the direction from the doped passivation layer to the interface passivation layer, in the interface passivation layer, the concentration of the first doping element at a second preset depth from the surface of the doped passivation layer away from the silicon substrate is greater than the concentration of the second doping element at a second preset depth from the surface of the second doping region, the thickness range of the interface passivation layer is 0.5 to 5 nm, and the second preset depth is less than or equal to the sum of the thicknesses of the doped passivation layer and the interface passivation layer.
[0063] In this application, the thickness of the interfacial passivation layer is controlled within the range of 0.5 to 5 nm, which is beneficial for reducing free carrier Auger recombination and further improving short-circuit current. In addition, since the concentration of the first doping element is greater than the concentration of the second doping element, free carrier Auger recombination can be further reduced, further improving short-circuit current.
[0064] Optionally, the interface passivation layer of the first doping region is doped with a first doping element, and the interface passivation layer of the second doping region is doped with a second doping element.
[0065] In the direction from the doped passivation layer to the interface passivation layer, in the interface passivation layer, the concentration of the first doping element at a second preset depth on the surface of the doped passivation layer away from the silicon substrate in the first doping region is greater than the concentration of the second doping element at a second preset depth on the surface of the doped passivation layer away from the silicon substrate in the second doping region, the thickness of the interface passivation layer on the first doping region ranges from 0.5 to 5 nm, the thickness of the interface passivation layer on the second doping region ranges from 0.5 to 5 nm, and the second preset depth is less than or equal to the sum of the thicknesses of the doped passivation layer and the interface passivation layer on the first doping region.
[0066] Optionally, in the direction from the doped passivation layer to the surface of the first doped region, in the silicon substrate, the concentration of the first doping element at a third preset depth from the surface of the doped passivation layer on the side away from the silicon base is greater than the concentration of the second doping element at a third preset depth from the surface of the second doped region, the thickness range of the first doped region is 30 to 100 nm, and the third preset depth is less than or equal to the sum of the thicknesses of the doped passivation layer, the interface passivation layer and the first doped region.
[0067] Optionally, in the direction from the doped passivation layer to the surface of the first doped region, in the silicon substrate, the concentration of the first doping element at a third preset depth from the surface of the doped passivation layer of the first doped region away from the silicon substrate is greater than the concentration of the second doping element at a third preset depth from the surface of the doped passivation layer of the second doped region away from the silicon substrate, the thickness range of the first doped region is 30 to 100 nm, and the third preset depth is less than or equal to the sum of the thicknesses of the doped passivation layer, the interface passivation layer and the first doped region on the first doped region.
[0068] Optionally, when the doping element is a Group III element, the thickness of the doping region is in the range of 80 to 180 nm;
[0069] When the doping element is a Group V element, the thickness of the doping region ranges from 30 to 100 nm.
[0070] In the present application, large-sized antimony atoms will cause lattice distortion, but have the effect of suppressing vacancy defects; by controlling the doping concentration of antimony element within the above range, the incorporation of large-sized antimony atoms can play a role in reducing the concentration of vacancy defects and reducing the formation of oxygen precipitation.
[0071] Optionally, the battery includes an electrode formed on a light absorber, the electrode including a metal crystal portion in contact with the light absorber, the metal crystal portion including antimony element, wherein the light absorber includes a silicon substrate and a region for separating carriers generated by the silicon substrate.
[0072] Since the metal crystal portion of the electrode of the battery of the present application contains antimony element, the contact resistance of the battery can be reduced, and the contact resistance of the battery can be further reduced.
[0073] Optionally, the metal crystal portion further includes a doping element, and the concentration of the doping element is greater than the concentration of the antimony element.
[0074] By controlling the antimony concentration within the above range, the carrier recombination effect and the antimony self-doping effect can be reduced, the original and expected characteristics of the battery structure layer can be maintained, good film quality can be formed, and the battery conversion efficiency can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0075] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, a brief introduction will be given below to the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0076] FIG1 is a schematic diagram of a battery structure (TOPCon structure) provided in this application.
[0077] Figure 2 is a schematic diagram of the battery stringing process.
[0078] Figure 3 is another schematic diagram of the battery stringing process.
[0079] FIG4 is a schematic diagram of a specific structure of the component.
[0080] FIG5 is another specific structural diagram of the assembly. Specific embodiments
[0081] The specific embodiments of the present application will be described in more detail below. Although the specific embodiments of the present application are shown below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.
[0082] It should be noted that the following description is for the purpose of describing preferred embodiments of the present invention, but the description is for the purpose of explaining the general principles of the specification and is not intended to limit the scope of the present invention. The scope of protection of the present invention shall be determined by the scope defined in the claims.
[0083] In the present application, the concentration of antimony in the silicon rod or silicon wafer can be detected by any method known to those skilled in the art. Those skilled in the art can make a selection based on demand, for example, it can be detected by SIMS, ICP-MS, GDMS and other methods, preferably by ICP-MS method. It will be understood by those skilled in the art that the concentration of antimony in the silicon rod or silicon wafer can refer to the concentration of antimony at any site on the surface of the silicon rod or silicon wafer, in the middle of the silicon rod or silicon wafer, and of course it can also be the average value of the antimony concentration at multiple locations or the average value of the antimony concentration on the entire silicon rod or silicon wafer. Those skilled in the art can select any of the above-mentioned sites for detection based on actual conditions based on the detection conditions and the instruments used, or can calculate the average value of multiple sites after detecting multiple sites as the concentration of antimony.
[0084] In the present application, the resistivity of a silicon rod or a silicon wafer can be detected by any method known to those skilled in the art, and those skilled in the art can select based on demand, for example, by a four-probe tester test, or can be detected by methods such as a non-contact eddy current method (for example, from a terahertz offline two-dimensional imaging device), and in a specific manner by a four-probe tester test. Those skilled in the art will understand that the resistivity of a silicon rod or a silicon wafer can refer to the resistivity detection data of any site on the surface of the silicon rod or the silicon wafer, the middle of the silicon rod or the silicon wafer, and of course, it can also be the average value of the resistivity detection data of multiple positions or the average value of the resistivity on the entire silicon rod or silicon wafer. Those skilled in the art can select the above-mentioned arbitrary site for detection based on the actual situation based on the conditions of detection and the instrument used, or can calculate the average value of multiple sites after detecting multiple sites as the resistivity of the silicon wafer.
[0085] Those skilled in the art will understand that silicon wafers generally refer to raw material bare silicon wafers, and silicon substrates generally refer to the parts formed by silicon wafers in batteries. Light absorbers generally refer to functional bodies in batteries for absorbing photons, generating photogenerated carriers and separating photogenerated carriers, which include silicon substrates and regions for separating carriers generated by silicon substrates (such as tunneling layers and doped polycrystalline layers in TOPCON structures), wherein the silicon substrate is used to absorb light and generate photogenerated carriers. It is understandable that simple emission-reducing layers, other functional layers, and electrodes do not belong to light absorbers. Those skilled in the art will understand that light absorbers or silicon substrates can be recovered from batteries, and the silicon substrate defined in this application can be obtained by peeling off different stacked structures.
[0086] In the present application, the doped region can also be used to separate photogenerated carriers, such as the region in which the third main group element (boron element) is diffused in the TOPCon cell described below.
[0087] That is, the silicon substrate is obtained from a bare silicon wafer, and the silicon substrate includes a silicon base portion and a doped region portion. The silicon base portion is the body region that is undoped during the battery process and has the same performance as the raw material bare silicon wafer. The doped region can be a doped region that is basically the same as the body region except for the doping element, such as a doped region formed by direct doping or internal diffusion doping within the bare silicon wafer. In addition, in some cases, the doped region is antimony or a doping element, such as a Group III element or a Group V element, specifically a place where B or P is concentrated. In some cases, the doped region may be basically the same as the body region, that is, it mainly includes an antimony doped region.
[0088] In a structural cell having at least part of TOPCon (e.g., a TOPCon cell, a local TOPCon cell, a back contact hybrid cell, and a TBC cell), the silicon substrate generally includes a doped region formed within the surface of at least one side of the silicon substrate, and the performance of this doped region portion is the same as that of the raw material bare silicon wafer. The doped region may be substantially the same as the body region except for the doping element, that is, the antimony element concentration, resistivity change rate, resistivity offset rate, and other properties are substantially the same. Such a doped region may be formed by directly doping the bare silicon wafer as described in detail below, or by doping the doping element into the bare silicon wafer through a layer such as a doped passivation layer and an interface passivation layer. In the present application, for a structural cell having at least part of TOPCon, a doped region generally refers to a region formed by direct doping or internal doping inside the raw silicon wafer, wherein the internal doping is formed by doping polysilicon called a doping layer through a tunneling layer called a passivation layer into the interior of the bare silicon wafer.
[0089] In the case of crystalline silicon heterojunction cells (HJT / HIT) and full back electrode back contact heterojunction cells (HBC), the doped region also refers to the doped region within the internal surface of at least one side of the silicon substrate. In this case, the doped region includes antimony elements or doping elements, such as third-group elements and fifth-group elements, specifically where B or P is concentrated, or the doped region may be basically the same as the body region, that is, it mainly includes an antimony doped region. Furthermore, at least one side of the silicon substrate has a doped amorphous silicon layer as a doping layer and an intrinsic amorphous silicon layer as a passivation layer. In this case, the doping elements may or may not enter the raw silicon wafer.
[0090] In the present application, there is no further limitation on the silicon wafer itself involved in the above-mentioned present application. It can be a silicon wafer obtained after machining and slicing after the silicon rod is drawn (it can also be called a bare silicon wafer). The silicon substrate in the present application can be a part of the silicon substrate that is peeled off and recovered from the component, as long as it can have a certain shape and can be in the form of a sheet, that is, the size of one surface is larger than the size of the surface perpendicular to it, and it is flat or plate-shaped. There is no limitation on the size of the silicon wafer or silicon substrate of the present application. The silicon wafer or silicon substrate can be of any size, and the light absorber is recovered from the component and the peeled part of the silicon substrate of other layer structures is peeled off. In addition, those skilled in the art can understand that during peeling, if the doped region is partially destroyed, as long as part of the doped region still exists, it should be understood that it is the silicon substrate described in the present application, and the battery with such a silicon substrate is also a battery that meets the definition of the present application. For example, in a specific embodiment, the length of at least one side of the silicon wafer or silicon substrate of the present application (including the silicon substrate after the recovery and peeling of other layer structures) is greater than 156 mm, for example, it can be 158±2 mm, (160±2) mm, (165±2) mm, (170±2) mm, (175±2) mm, (180±2) mm, (185±2) mm, 190±2 mm, (195±2) mm, (200±2) mm, (205±2)mm, (210±2)mm, (215±2)mm, (220±2)mm, (225±2)mm, (230±2)mm, (235±2)mm, (240±2)mm, (245±2)mm, (250±2)mm, (255±2)mm, (260±2)mm, (265±2)mm, (270±2)mm, (275±2)mm, and any ranges between these values.
[0091] Because the doping concentration in the silicon rod is controlled in this application, the resistivity of the silicon wafers produced from the silicon rods is uniform, and large-sized silicon wafers can be produced. For example, the margin of the large-sized silicon wafer is greater than or equal to 156 mm.
[0092] Furthermore, in a specific embodiment, the silicon wafer or silicon substrate of the present application (including the partial silicon substrate after recovery and stripping of other layer structures) is rectangular, one side of the rectangle is 156mm to 300mm, and the other side of the rectangle is 83mm to 300mm.
[0093] In the present application, since the silicon wafer or silicon substrate (including the silicon substrate after the stripping of other layer structures is recovered and stripped) is set to a rectangle, the rectangular silicon wafer of the present application can be a rectangular piece obtained by machining and slicing the silicon rod, or it can be a rectangular piece obtained by cutting the square / rectangular silicon wafer in half / slicing. Among them, one side of the rectangular silicon wafer or silicon substrate is controlled at 156mm~300mm, and the other side is controlled at 83mm~300mm. Compared with the square battery cell, the area of the rectangular battery cell is larger, so the area that can be used to receive light is also larger, so that it can have a higher photoelectric conversion efficiency. Moreover, the battery cell provided in the embodiment of the present application is more convenient to transport after typesetting, which is conducive to improving the utilization rate of the container and thus improving the efficiency of transportation.
[0094] In a specific embodiment, the silicon wafer or optical silicon substrate of the present application (including the silicon substrate after recovery and stripping of other layer structures) also includes a chamfer connecting two adjacent sides of the silicon wafer, and the arc length projection length of the chamfer is 1mm to 10mm.
[0095] In this application, setting chamfers on the silicon wafers is also beneficial to reducing damage to the silicon wafers during transportation and processing, improving the yield of subsequent processes, reducing the fragmentation rate, and reducing waste in production costs.
[0096] In a specific embodiment, the thickness of the silicon wafer or optical silicon substrate of the present application (including the partial silicon substrate after recovery and peeling of other layer structures) is at least 40 to 170 μm, for example, it can be 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, or 160 μm.
[0097] In practical applications, the thickness of silicon wafers plays a crucial role in the light absorption capacity of solar cells. Specifically, thicker silicon wafers can accommodate more electrons, thereby increasing the generation of current and improving the output efficiency of the battery, while thinner silicon wafers can improve the light absorption efficiency of the battery. However, when the silicon wafer thickness is too small, it is more likely to have hidden cracks, resulting in an increased risk of silicon wafer fragmentation. In this application, the silicon wafer thickness is set to 40 to 170 μm. First, it ensures the strength of the silicon wafer, reduces its fragmentation rate, and helps to extend the service life of the silicon wafer. Secondly, when the silicon wafer thickness is 60 to 140 μm, the silicon wafer is easy to process and has a large production capacity, which can reduce production costs. That is, controlling the silicon wafer within a smaller thickness range is also conducive to reducing the production cost of the silicon wafer.
[0098] In a specific embodiment, the size of the silicon substrate after recovery and stripping of other layer structures can be smaller than the above-mentioned size, as long as the concentration of antimony elements and resistivity can be detected, and the resistivity change rate, resistivity average offset rate and other limitations involved in this application can be calculated.
[0099] In the present application, essentially unchanged means that the concentration of antimony elements in the thickness direction of the silicon substrate of the present application is uniform. Although the specific values may vary to a certain extent with the change of the detection site, the overall difference in antimony concentration in the thickness direction will not exceed 50%, 40%, 30%, or 20%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2% or 1%, that is, the difference between the maximum value and the minimum value will not exceed 50%, 40%, 30%, or 20% of the minimum value, or 15% of the minimum value, or 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2% or 1% of the minimum value.
[0100] In the present application, when detecting the above-mentioned antimony concentration and resistivity, if a technician in this field needs to select multiple sites to calculate the average value, he can randomly select, for example, 2 sites, 3 sites, 4 sites, 5 sites, 6 sites, 7 sites, 8 sites, 9 sites, or more than 10 sites on the silicon rod, silicon wafer, or silicon substrate for detection and calculation.
[0101] In the present application, the method for detecting whether a silicon rod, silicon wafer or silicon substrate contains a certain element can be detected by SIMS, ICP-MS, GDMS and the like, preferably by ICP-MS to detect metal elements.
[0102] In this application, the same detection and characterization methods are used for silicon wafers and silicon rods. The difference is that the silicon rods are cut into thin slices for testing, and the only difference from the finished silicon wafers is the thickness. The finished silicon wafers are generally 100-200μm thick, and the thin slices cut from the silicon rods are generally less than 3mm thick. The parameters of the silicon rods are tested based on these thin slices. Of course, those skilled in the art can also adjust the thickness and size of the cut slices according to actual conditions to facilitate testing.
[0103] If further conditions are required for the antimony concentration of a single crystal silicon rod or its tail end face, it is sufficient to detect the maximum antimony concentration or the minimum antimony concentration of the single crystal silicon rod and perform calculations. Alternatively, the antimony concentration at the center of the tail end face or the antimony concentration at the edge of the tail end face can be detected and calculated. Furthermore, the maximum and minimum antimony concentrations of a single crystal silicon rod can be detected using the above-described detection method, and the maximum and minimum values at any detected locations can be selected for calculation.
[0104] If further requirements are required for the resistivity of a single crystal silicon rod or the end face of a single crystal silicon rod to be satisfied, it is only necessary to separately test the resistivity of the head end face and the end face of the single crystal silicon rod and perform calculations. Furthermore, the maximum and minimum resistivity of a single crystal silicon rod can be measured using the above-described testing method, and the maximum and minimum values at any tested location can be selected for calculation.
[0105] In the present application, the silicon rods of the present application can be cut to a suitable length by a cutting machine, and then transferred to a square cutting machine to be processed into square rods. After the square rods are polished by a polishing machine, they are transferred to a slicer, and the silicon square rods are cut into silicon wafers of the present application by diamond wire.
[0106] In the present application, the arc length projection length of the chamfer connecting two adjacent sides of the silicon wafer can also be detected by a length measurement method commonly used by those skilled in the art, for example, it can be measured by a micrometer.
[0107] In the present application, there is no further limitation on the silicon wafer itself involved in the present application. It can be a silicon wafer obtained after machining and slicing after the silicon rod is drawn (also called a bare silicon wafer), or a silicon wafer obtained after doping, or a partial silicon wafer peeled and recovered from a component, as long as it can have a certain shape and can be in the form of a sheet, that is, the size of one surface is larger than the size of the surface perpendicular to it, and it is flat or plate-shaped. There is no limitation on the size of the silicon wafer. The silicon wafer can be of any size, and the partial silicon wafer after peeling and other layer structures are recovered from the component. In addition, those skilled in the art will understand that when peeling, if some areas are destroyed, but as long as there is still part of the substrate structure of the battery, it should also be understood as the silicon wafer or substrate described in this application. For example, in a specific embodiment, the length of at least one side of the silicon wafer of the present application (including the silicon wafer after the recovery and stripping of other layer structures) is greater than 156 mm, for example, it can be 158 ± 2 mm, (160 ± 2) mm, (165 ± 2) mm, (170 ± 2) mm, (175 ± 2) mm, (180 ± 2) mm, (185 ± 2) mm, 190 ± 2 mm, (195 ± 2) mm, (200 ± 2) mm, (20 2)mm, (250±2)mm, (255±2)mm, (260±2)mm, (265±2)mm, (270±2)mm, (275±2)mm, and any ranges between these values.
[0108] In a specific embodiment, the thickness of the silicon wafer of the present application (including the portion of the silicon wafer after recovery and stripping of other layer structures) is at least 40 to 170 μm, for example, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm. In a specific embodiment, the size of the portion of the silicon wafer after recovery and stripping of other layer structures can be smaller than the above size, as long as the concentration of antimony, mechanical strength, type of doping element, etc. can be tested for it within the limits of the present application.
[0109] In a specific embodiment of the present application, only antimony is doped as a Group V doping element in the silicon wafer of the present application to replace phosphorus. In this case, those skilled in the art will understand that, depending on the source of the silicon wafer raw materials or by additional addition to the crystal pulling raw materials, the prepared silicon wafer may also contain other elements, such as any one, two, or three of phosphorus, gallium, and germanium, but only antimony is actively doped as a Group V doping element to replace phosphorus.
[0110] In one specific embodiment, phosphorus is included in the molten silicon used to manufacture silicon wafers, resulting in silicon wafers containing both phosphorus and antimony. Due to the different evaporation rates of antimony and phosphorus during the doping process, both dopants contribute to the resistivity of the silicon ingot in the early stages of crystal pulling. Over time, the contribution of antimony decreases. Once all antimony evaporates, i.e., in the later stages of crystal pulling, only the phosphorus dopant remains active, resulting in closer resistivity at the head and tail of the ingot. This improves axial resistivity uniformity, and consequently, resistivity uniformity across the silicon wafer.
[0111] In one specific embodiment, gallium is included in the molten silicon used to manufacture silicon wafers, resulting in silicon wafers containing both gallium and antimony. Specifically, in the method for preparing single-crystal silicon, on the one hand, an appropriate amount of gallium is doped into the polycrystalline silicon material to introduce majority holes, thereby producing single-crystal silicon with a predetermined resistivity. On the other hand, an appropriate amount of antimony is doped into the polycrystalline silicon material to introduce free electrons, thereby compensating for holes in the silicon crystal, particularly at the tail of the single-crystal silicon rod, and reducing the concentration of holes at the tail of the single-crystal silicon rod. This results in a more uniform longitudinal resistivity distribution of the produced single-crystal silicon rod, thereby extending the length of the single-crystal silicon rod during production and improving the resistivity uniformity of the silicon wafers cut from the silicon rod.
[0112] In a specific embodiment, germanium is included in the molten silicon used to manufacture silicon wafers, and silicon wafers containing both germanium and antimony are obtained. Antimony is doped in the process of preparing single-crystalline silicon. Antimony has a high volatilization rate and a large atomic radius, which leads to lattice changes. A trace amount of germanium is doped. The number of outermost electrons of the germanium element is the same as that of the silicon element, which is 4, and will not affect the electrical properties of the silicon material. Instead, the effect of germanium and point defects (self-interstitial silicon atoms, vacancies) can be used to suppress native micro-defects in the silicon single crystal, especially void defects, which can effectively improve the quality and yield of the silicon single crystal, suppress native defects, and improve the crystal quality.
[0113] Usually the concentration of phosphorus in silicon wafers does not exceed 3E+16atom / cm 3 ; The concentration of gallium will not exceed 7E+16atom / cm 3 , the concentration of germanium will not exceed 1E+19atom / cm 3 When doping simultaneously, the above concentration limits refer to the concentration limits of each element.
[0114] In this application, the mechanical strength testing method for silicon wafers or silicon substrates is based on GB / T 6569-2006, Test Method for Bending Strength of Fine Ceramics. In this test method, bending strength refers to the maximum stress at which a material breaks under bending load. This method can also be used to test the curvature of batteries.
[0115] In this application, the mechanical strength dispersion of a silicon wafer or silicon substrate is used to characterize the strength uniformity of different silicon wafers produced using the same process. Lower dispersion indicates smaller strength differences between different silicon wafers. This can be tested using testing methods known in the art, such as using a single-column electronic universal testing machine.
[0116] In the present application, the margin and thickness of the silicon wafer can be detected by methods for measuring length and thickness known in the art, for example, by measuring with a micrometer.
[0117] In the present application, the mechanical strength of the silicon wafer is greater than or equal to 70 MPa, and / or the dispersion of the mechanical strength of the silicon wafer is less than or equal to 0.9.
[0118] In actual production and application, when the thickness of silicon wafers is thinned to a certain level, the mechanical properties of the silicon wafers are affected, and defective solar cells are easily produced. When the mechanical strength of the silicon wafers is greater than or equal to 70MPa, the mechanical properties of the silicon wafers can be maintained at a good level, which can inhibit excessive bending of the solar cells when stringing, making it less likely to produce fragments, thereby improving the battery yield and ensuring product quality.
[0119] It should be noted that, when the size of the silicon wafer is fixed, the mechanical strength of the silicon wafer increases with the increase of the thickness of the silicon wafer.
[0120] When conducting strength tests, a horizontal testing platform is set up and two support beams are installed on the horizontal testing platform. The silicon wafer is placed on the two support beams. The span between the two support beams is 60mm. The thickness of the silicon wafer is 40um~170um. Then, a thrust is applied to the silicon wafer from top to bottom. The specific data of the applied pressure and the thrust distance are recorded by the sensor, and the mechanical strength of the silicon wafer is measured to be 60~500Mpa.
[0121] The mechanical strength of the silicon wafer can be, for example, 70 MPa, 80 MPa, 90 MPa, 100 MPa, 110 MPa, 120 MPa, 140 MPa, 160 MPa, 180 MPa, 200 MPa, 210 MPa, 230 MPa, 250 MPa, 280 MPa, 300 MPa, 310 MPa, 320 MPa, 330 MPa, 340 MPa, 350 MPa, 360 MPa, 370 MPa, 380 MPa, 400 MPa, 500 MPa, and any range between these values.
[0122] As competition in the photovoltaic industry becomes increasingly fierce, low cost has become the core key. Thinning can effectively reduce the cost of silicon wafers, reduce battery light decay, and the prepared batteries have good flexibility; however, the absorption of light becomes poor and they are very prone to warping. This is mainly because the mechanical strength is greatly reduced during thinning. The silicon wafer of this application effectively hinders lattice slip by controlling the concentration of antimony element, plays the role of pinning dislocation movement, and thus improves the mechanical strength of the silicon wafer.
[0123] In a specific embodiment, the discreteness of the mechanical strength of the silicon wafer is less than 0.9, for example, it can be 0.89, 0.85, 0.8, 0.75, 0.7, 0.65, 0.6, 0.55, 0.5, 0.45, 0.4, 0.35, 0.3, 0.25, 0.2, 0.15, 0.1, and any range between these values.
[0124] The present application relates to a battery prepared using the above-mentioned silicon wafer.
[0125] In this application, because the silicon wafers described above rationally control the concentration of antimony, achieving uniform doping and thus uniform resistivity across the silicon wafer or bare silicon wafer itself, using such wafers to fabricate batteries can reduce the lateral carrier transport resistance, ultimately increasing battery efficiency. Furthermore, the silicon wafers described in this application exhibit a higher minority carrier lifetime, resulting in improved short-circuit current and further enhanced battery efficiency.
[0126] The above description of the silicon wafer in this application is applicable to the silicon substrate in the battery of this application.
[0127] In a specific embodiment, the silicon wafer of the present application can be used as a silicon substrate for various types of solar cells. Various types of solar cells include aluminum back surface field cells (Al-BSF), passivated emitter and back contact cells (PERC), metal wrap-through cells (MWT); passivated emitter back localized diffused cells (PERL), passivated emitter back fully diffused cells (PERT), emitter wrap-through cells (EWT), tunneling oxide passivated cells (TOPCon), interdigitated back contact cells (IBC), crystalline silicon heterojunction cells (HJT / HIT), and full back electrode back contact heterojunction cells (HBC).
[0128] Another aspect of the present application relates to a solar cell, which includes the case where the silicon wafer described in detail in the present application is used in the solar cell. The detailed description of the silicon wafer is basically applicable. Specifically, the solar cell of the present application includes a silicon substrate, wherein a doped region is provided on at least one surface of the silicon substrate, the silicon substrate contains antimony, the doped region is doped with a doping element, the doping element is selected from the third main group element or the fifth main group element, and the concentration of the antimony element in the silicon substrate is 4E+14cm -3 to 2E+16cm -3 , preferably 4.3E+14cm -3 to 1.9E+16cm -3 ; More preferably 4.45E+14cm -3 to 1.87E+16cm -3 .
[0129] In the present application, the concentration of the antimony element is controlled so that the antimony atoms in the antimony-doped silicon wafer can capture and neutralize radiation-induced defects, thereby reducing the formation and diffusion of defects. Therefore, the battery made using the silicon wafer has better radiation stability; in addition, controlling the concentration of the antimony element within the above range can improve the contact resistance between the metal and the silicon substrate, and can more effectively collect charges, thereby improving the performance of the solar cell; at the same time, it can reduce the recombination loss of carriers and improve the efficiency of the battery.
[0130] Those skilled in the art will understand that the silicon substrate is the structure formed after the silicon wafer of the present application is prepared into a cell. Those skilled in the art will understand that the solar cell mentioned above encompasses all solar cells that can be applied to the silicon wafer of the present application, such as crystalline silicon heterojunction cells (HJT / HIT), full back electrode back contact heterojunction cells (HBC), TOPCon cells, partial TOPCon cells, back contact hybrid cells and TBC cells, as well as any cell form well known to those skilled in the art.
[0131] In the above-mentioned battery form, at least one doped layer is provided on the surface of at least one side of the silicon substrate. Specifically, depending on the battery form, the doped layer can be selected based on requirements, for example, it can be an n-type amorphous or polycrystalline silicon carbide layer, such as phosphorus-doped silicon carbide or nitrogen-doped silicon carbide; it can be n-type amorphous or polycrystalline silicon, such as phosphorus-doped amorphous silicon or nitrogen-doped phosphorus-doped silicon; or it can be n-type amorphous or polycrystalline diamond-like carbon, such as nitrogen-doped diamond-like carbon. Those skilled in the art are fully free to make their selections as required, and as long as the requirements of this application are met, at least a portion of the surface of at least one side of the silicon substrate can have one doped layer, and other regions can have another doped layer.
[0132] In the above-described battery configuration, at least one passivation layer is provided between the doped layer and the doped region of the silicon substrate. Specifically, the passivation layer can be selected based on specific requirements, depending on the battery configuration. Generally, the thickness of the passivation layer should be less than 10 nm. Due to its very small thickness, there are no requirements for the conductivity of the passivation layer. Due to its small thickness, there are no absorption limitations. Commonly used passivation layers include silicon oxide, silicon nitride, intrinsic amorphous silicon, aluminum oxide, aluminum nitride, phosphorus nitride, titanium nitride, and the like. Those skilled in the art are fully free to select a passivation layer based on their requirements, as long as it meets the requirements of this application.
[0133] In one specific embodiment, the solar cell is a heterojunction cell, such as a crystalline silicon heterojunction cell (HJT / HIT) or a full back electrode back contact heterojunction cell (HBC). When the silicon wafer of the present application forms a silicon substrate for use as a heterojunction cell or a full back electrode back contact heterojunction cell, even after a heterojunction layer is stacked on the silicon substrate, the antimony concentration and resistivity change rate described in detail for the silicon wafer are still met, that is, after the heterojunction layer is stacked, the antimony concentration in the silicon substrate is 4E+14 cm -3 to 2E+16cm -3 All the above descriptions of the antimony concentration and resistivity change rate in the silicon wafer are applicable to this method.
[0134] For crystalline silicon heterojunction cells (HJT / HIT) and full back electrode back contact heterojunction cells (HBC), an intrinsic amorphous silicon layer and a doped amorphous silicon are usually further stacked on the silicon substrate of the present application, wherein the intrinsic amorphous silicon layer serves as a passivation layer. Due to the characteristics of the Sb element itself, the antimony element in the silicon substrate will not enter the doped amorphous silicon layer through the passivation layer. The doped amorphous silicon layer basically does not contain Sb, that is, the silicon substrate contains antimony element, while the doped amorphous silicon layer or the intrinsic amorphous silicon layer contains doping elements but does not contain Sb.
[0135] More specifically, for crystalline silicon heterojunction cells (HJT / HIT) and full back contact heterojunction cells (HBC), the concentration of antimony in the silicon substrate is 4.3E+14 cm -3 to 1.9E+16cm -3 More specifically, the concentration of antimony in the silicon substrate is 4.45E+14 cm -3 to 1.87E+16cm -3 .
[0136] In a specific embodiment, when the solar cell is a TOPCon cell, a local TOPCon cell, a back contact hybrid cell, or a TBC cell, the solar cell of the present application includes a silicon substrate, a doped region is formed in at least one surface of the silicon substrate, the entire silicon substrate contains antimony, and the doped region is doped with a doping element, the doping element is selected from the third main group element or the fifth main group element, and the concentration of the antimony element in the silicon substrate is 4E+14cm -3 to 2E+16cm -3 , preferably 4.3E+14cm -3 to 1.9E+16cm -3 ; More preferably 4.45E+14cm -3 to 1.87E+16cm -3 .
[0137] More specifically, for TOPCon cells, local TOPCon cells, back contact hybrid cells, and TBC cells, the concentration of antimony in the silicon substrate is 4.3E+14 cm -3 to 1.9E+16cm -3 More specifically, the concentration of antimony in the silicon substrate is 4.45E+14 cm -3 to 1.87E+16cm -3 .
[0138] In a specific embodiment, for TOPCon cells, local TOPCon cells, back contact hybrid cells and TBC cells, the doped region contains doping elements as described above, and the concentration of antimony elements in the doped region is basically unchanged in the thickness direction of the silicon substrate. As a result, during the drawing process of the antimony-doped silicon rod, the doping atoms and silicon atoms are solid-dissolved in the lattice, so the concentration of antimony elements in the doped region is basically unchanged along the thickness direction of the silicon substrate, thereby overcoming the crystalline silicon lattice distortion caused by single element doping, resulting in many defects in the heavily doped region, and also improving light absorption and improving battery efficiency; in addition, the original and expected characteristics of different battery structures can be maintained, forming good film quality, which is also conducive to improving battery conversion efficiency. Those skilled in the art will understand that for TOPCon cells, local TOPCon cells, back contact hybrid cells and TBC cells, the doped region in this application refers to the region formed by direct doping inside the raw silicon wafer or indirectly doped through other layer structures. Therefore, in this case, the doped region is formed in the silicon substrate by the doping element entering the silicon wafer. An interface passivation layer and a doped passivation layer can be further stacked on at least one side of the silicon substrate. In addition, those skilled in the art will also understand that as long as the solar cell structure has the structure described in detail in this application, any difference in its name also falls within the scope of protection of this application.
[0139] In this application, an interfacial passivation layer refers to a layer that has a passivating effect and allows the passage of dopant elements, such as a tunneling layer. A doped passivation layer is a layer that forms a PN junction or a high-low junction with the silicon substrate. Examples include a doped amorphous silicon layer or a doped polysilicon layer.
[0140] In the present application, essentially unchanged means that the concentration of antimony elements in the thickness direction of the silicon substrate of the present application is uniform. Although the specific values may vary to a certain extent with the change of the detection site, the overall difference in antimony concentration in the thickness direction will not exceed 50%, 40%, 30%, or 20%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2% or 1%, that is, the difference between the maximum value and the minimum value will not exceed 50%, 40%, 30%, or 20% of the minimum value, or 15% of the minimum value, or 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2% or 1% of the minimum value.
[0141] Those skilled in the art will understand that, depending on the different application requirements of the silicon wafer, for example, when the silicon wafer is used in various solar cells, the silicon wafer can be further doped with various doping elements to form one or more doping regions. These doping elements can be Group III elements, such as boron, aluminum, gallium, indium, and thallium, or Group V elements, such as nitrogen, phosphorus, arsenic, antimony, and bismuth.
[0142] In the present application, the antimony element concentration and the like described for the above-mentioned silicon wafer are also applicable to the silicon substrate that has been installed in the solar cell as part of the light absorber. At this time, the above-mentioned parameters described for the antimony element concentration in the silicon wafer are applicable to the entire silicon substrate, that is, they are applicable to the body region that contains only antimony element doping, the doped region, and the body region and the doped region as a whole. Those skilled in the art will understand that when the above-mentioned detection is performed only on the body region, the results of the measured or calculated antimony element concentration, resistivity, resistivity change rate, and resistivity average offset rate are within the scope of the above-mentioned detailed description of the present application. When the above-mentioned detection is performed only on the doped region, the results of the measured or calculated antimony element concentration are within the scope of the above-mentioned detailed description of the present application. When the boundary between the doped region and the body region is ignored and any position of the entire silicon substrate is detected, the above-mentioned results can also be obtained.
[0143] In a specific embodiment, the doping element can be doped into the doping region by direct doping, that is, the doping element is doped directly into the doping region without passing through other layer structures of the battery. The direct doping method can also be various methods known in the art, such as thermal diffusion, ion implantation, or coating a slurry containing a dopant and incorporating the dopant by a driving force (such as heat treatment, laser, etc.). Those skilled in the art can choose according to their needs. It also includes the case where aluminum is diffused into the silicon wafer through aluminum grid lines through heat treatment.
[0144] In a specific manner, in addition to the above-mentioned direct doping, the doping element can be doped into the doping region in such a way that the doping element (i.e., the doping element) passes through the layer structure stacked on the silicon wafer or silicon substrate and is doped into the silicon wafer or silicon substrate to form the above-mentioned doping region. Those skilled in the art will understand that, according to different application scenarios of the silicon wafer, such as when used in different solar cells, the layer structure can be adjusted accordingly. For example, the layer structure may itself contain a dopant that provides the doping element, and the doping element is doped through the layer structure. The layer structure itself may also not contain a dopant, but the adjacent area has an atmosphere that can provide the doping element, and is doped into the silicon wafer through the layer structure to form a doping region by, for example, thermal diffusion, ion implantation, etc. The above-mentioned atmosphere that can provide the doping element can be a gas atmosphere (e.g., a gas containing a dopant), a liquid (e.g., a slurry containing a dopant), or a solid (e.g., a layer including a dopant, such as a doped passivation layer, especially a doped polysilicon layer).
[0145] The layer structure can be a single layer (e.g., a passivation layer or tunneling layer) or multiple layers, such as a passivation layer and a doped layer. The layer structure can be a natural oxide layer formed by natural oxidation on a silicon substrate. Alternatively, the layer structure can be made of intrinsic amorphous silicon, i.e., intrinsic amorphous silicon is provided on one side of the silicon wafer to provide passivation.
[0146] Taking the TOPCon battery structure as an example, the layer structure may be a doped polysilicon layer (doped passivation layer), a tunneling layer (interface passivation layer), or a doped polysilicon layer and a tunneling layer acting together as a layer structure. Those skilled in the art will fully understand that the above enumeration is only illustrative, and both direct doping and doping via a layer structure are optional, and direct doping and doping via a layer structure can be targeted at a local part of one side of the silicon wafer, such as doping elements by direct doping locally, while stacking TOPCon structures on other areas of the side surface to form a local TOPCon structure or a back-contact hybrid battery with a TOPCon structure. Or even one TOPCon structure can be used locally, and another TOPCon structure can be used in other locations to achieve doping separately, such as forming a TBC battery.
[0147] Those skilled in the art will understand that in the case of a TOPCon structure, a tunneling layer and a doped polysilicon layer are further stacked on the silicon substrate, and the concentration of antimony in the silicon substrate is 4E+14cm -3 to 2E+16cm -3 , preferably 4.3E+14cm -3 to 1.9E+16cm -3 ; More preferably 4.45E+14cm -3 to 1.87E+16cm -3 .
[0148] In the present application, by controlling the doping concentration of antimony elements during the silicon rod drawing process, the resistivity uniformity of the silicon rods can be improved, and the concentration can be better. After the silicon rods are processed into silicon wafers, the antimony doping concentration of the silicon wafers can be made more appropriate, and the resistivity uniformity and concentration of the silicon wafers are also correspondingly better. In this way, during the processing stage of the battery, there is no need to use additional processes to introduce antimony elements into the silicon wafers. Compared to the conventional N-type battery, which introduces antimony elements through silver paste and ion implantation during the battery processing stage, the present application does not require additional processes to introduce antimony elements during the battery processing stage, thereby simplifying the manufacturing process of solar cells and reducing the processing cost of the battery.
[0149] In a specific embodiment, in the case of direct doping, within a range of a thickness of h from the surface of the doped region away from the silicon substrate (i.e., the doping depth of the directly doped region), the concentration of the doping element is greater than the concentration of the antimony element at the surface and at the same depth from the surface. In addition, in the doped region, the sum of the concentration of the antimony element and the concentration of the doping element is less than or equal to 1E+21 cm -3The battery of the present application controls the range of the sum of the concentration of the doping region and the concentration of the doping element, thereby facilitating the separation of carriers, while reducing carrier recombination and improving the short-circuit current and open-circuit voltage.
[0150] In a specific manner, the above-mentioned doping element is a third main group element, and the above-mentioned h ranges from 30 to 650 nm. In a specific manner, the above-mentioned doping element is a third main group element, and the above-mentioned h is greater than or equal to 400 nm. In a specific manner, the above-mentioned doping element is a third main group element, and the above-mentioned h ranges from 30 nm to 100 nm. In a specific embodiment, the above-mentioned doping element is a fifth main group element, and the above-mentioned h ranges from 100 to 200 nm. As mentioned above, the maximum range at the same depth from the above-mentioned surface should be the thickness h. For example, when the depth is 0, it is the concentration on the surface of the above-mentioned doping region. When the depth is 100 nm, for example, at a position 100 nm from the above-mentioned surface, the concentration of the doping element is greater than the concentration of the antimony element. In a specific manner, as described in Figure 1, the surface away from the side of the silicon substrate of the doping region is the front side of the doping region 2.
[0151] In a specific embodiment, the doping element is boron, and h is in the range of 30 to 650 nm or in the range of 30 nm to 100 nm. When only local doping is performed, only the location of the local doping needs to satisfy the above relationship.
[0152] In the present application, since the thickness of the doped region formed by direct doping in the silicon substrate of the solar cell is controlled, it is beneficial to the separation of carriers, while reducing carrier recombination and improving the short-circuit current and open-circuit voltage.
[0153] In some specific embodiments, if the thickness of the doped region formed by direct doping, for example, the thickness of the doped region in the case of doping the third main group element is further controlled to be even less than 100nm or even less than 50nm, the free carrier Auger recombination is further reduced and the short-circuit current is further improved. In a specific embodiment, in the case of diffusion through a layer structure, within a range of m thickness from the surface of the doped region away from the silicon substrate side (the depth of the doped region in the case of diffusion through the layer structure), the concentration of the doping element on the above surface and at the same depth from the above surface is greater than the concentration of the antimony element. In a specific embodiment, as shown in Figure 1, the surface away from the silicon substrate side of the doped region is the back side of the doped region 4.
[0154] In a specific manner, the doping element is a third main group element, and the range of m is 80 to 180 nm. In a specific embodiment, the doping element is a fifth main group element, and the range of m is 30 to 100 nm. As described above, the maximum range at the same depth from the surface should be less than or equal to m. For example, when the depth is 0, it is the concentration on the surface of the doped region. When the depth is 100 nm, for example, at a position 100 nm from the surface, the concentration of the doping element is greater than the concentration of the antimony element.
[0155] In a specific embodiment, the doping element is phosphorus, and m is in the range of 80 to 180 nm or in the range of 30 to 100 nm. When only local doping is performed, only the local doping position needs to satisfy the above relationship.
[0156] In the present application, the above-mentioned light absorber controls the thickness of the doped region formed by doping the layer structure, thereby retaining the passivation effect of the interface passivation layer and achieving effective doping of doped polysilicon, thereby increasing the short-circuit current and open-circuit voltage, and improving the efficiency of the battery.
[0157] In a specific embodiment, the solar cell of the present application is, for example, a tunneling oxide passivation cell (TOPCon cell), a local TOPCon cell, a back contact hybrid cell or a TBC cell.
[0158] In a specific embodiment, the typical structure of a TOPCon cell is shown in FIG1 , which includes, from the front to the back, a silicon substrate 1 (with a second doped region 2 and a first doped region 4 formed inside its two side surfaces), a tunneling layer 5, a doped polysilicon layer 6, a passivation layer or a high-transmission thin film layer 7, and an electrode 8. It is fully understood by those skilled in the art that although the structure of the TOPCon cell is described with the aid of FIG1 , the structure of the TOPCon cell is not limited to that of FIG1 , as long as a tunneling layer and a doped polysilicon layer are present on the silicon substrate of the cell. The TOPCon structure can be formed on the entire silicon substrate or on at least a portion of the silicon substrate.
[0159] In a specific embodiment, the second doping region 2 is directly doped with boron, and the first doping region 4 is doped with phosphorus in the silicon substrate via the tunneling layer 5 and the doped polysilicon layer 6 .
[0160] A partial TOPCon cell refers to a cell in which a TOPCon structure (i.e., a first doped region, a tunneling layer, and a doped polysilicon layer) is formed in at least a portion of one side of the cell. The first doped region, the tunneling layer, and the doped polysilicon layer are located in the first partial region, while the rest of the cell is an additional doped region. The additional doped region and the first doped region are on the same surface, and the elements doped in the additional doped region and the first doped region have the same conductivity type. However, an element with an opposite conductivity type is doped on the other side to form a second doped region.
[0161] In practical applications, single-element doping can lead to lattice distortion, which is typically caused by single-element doping of crystalline silicon, resulting in multiple defects in the heavily doped regions. In this application, by providing two doping regions, doping the doped passivation layer with a first doping element, and further doping the second doping element with a second doping element in the second doping region on the silicon substrate, the solar cell of this application can effectively prevent the occurrence of lattice distortion.
[0162] TBC battery refers to a battery with a TOPCon structure formed on the back side. There are two areas on the back side of this type of battery, each of which has a TOPCon structure with doping elements of opposite conductivity types.
[0163] A back-contact hybrid cell refers to a cell with a PERC or PERL structure in one region and a TOPCon structure in the other. For example, one region on the back has a TOPCon structure, and the other region has a PERL or PERC structure, and the two regions are doped with elements of opposite conductivity types. In some specific embodiments, when aluminum gate line doping is used, a metal layer is formed on the silicon substrate, and an alloy layer and a BSF layer are formed within the silicon substrate, where the BSF layer is the doped region. In this case, the surface of the BSF layer away from the silicon substrate on the side away from the doped region refers to the surface of the BSF layer away from the silicon substrate.
[0164] In a specific embodiment, the solar cell of the present application can be any one of the four types mentioned above, namely, TOPCon cells, local TOPCon cells, back-contact hybrid cells, and TBC cells. In these four types of cells, the doping element is doped into the silicon substrate through the layer structure on the silicon substrate to form the doped region. The doped region includes a first doping region and a second doping region. The layer structure on the silicon substrate includes a tunneling layer and a doped polysilicon layer stacked in sequence on the surface of the first doping region away from the silicon substrate. The first doping element is doped in the doped polysilicon layer, and the second doping region on the silicon substrate is also doped with the second doping element. The first doping region and the second doping region have opposite conductivity types.
[0165] In this application, the "first doping element" and the "second doping element" are different doping elements. For example, when the first doping element is a Group V element, the second doping element is a Group III element; when the first doping element is a Group III element, the second doping element is a Group V element.
[0166] In a specific embodiment, the first doping element is phosphorus, and the second doping element is boron.
[0167] When the solar cell of the present application is a TOPCon cell, a partial TOPCon cell, or a back-contact hybrid cell, the second doping region is a second doping element directly doped into the second doping region, wherein the first doping element is a Group V element (e.g., phosphorus) and the second doping element is a Group III element (e.g., boron).
[0168] In one specific embodiment, in the doped polysilicon layer, the concentration of the first doping element at a depth x (i.e., a first predetermined depth) from the surface of the doped polysilicon layer on the side away from the silicon substrate is greater than the concentration of the second doping element at a depth x (i.e., a first predetermined depth) from the surface of the second doping region. The thickness of the doped polysilicon layer ranges from 100 to 400 nm, where x is less than or equal to the thickness of the doped polysilicon layer. In this embodiment, since the concentration of the first doping element is greater than the concentration of the second doping element, free carrier Auger recombination can be further reduced, further improving short-circuit current. In another specific embodiment, in the tunneling layer, in the direction from the doped polysilicon layer to the tunneling layer, the concentration of the first doping element at a depth y (i.e., a second predetermined depth) from the surface of the doped polysilicon layer on the side away from the silicon substrate is greater than the concentration of the second doping element at a depth y (i.e., a second predetermined depth) from the surface of the second doping region. The thickness of the tunneling layer ranges from 0.5 to 5 nm, where y is less than or equal to the sum of the thicknesses of the doped polysilicon layer and the tunneling layer.
[0169] If a heavily doped region exists on the front surface of the cell, severe Auger recombination may occur, leading to severe light absorption and affecting cell efficiency. In this approach, since the concentration of the first doping element is greater than that of the second doping element, free-carrier Auger recombination can be further reduced, further improving short-circuit current. On the other hand, free-carrier Auger recombination can be reduced without reducing the passivation effect of the tunneling layer, further improving short-circuit current, open-circuit voltage, and cell efficiency. In one specific approach, in the direction from the doped polysilicon layer to the surface of the first doped region, in the silicon substrate, at a depth z from the surface of the doped polysilicon layer away from the silicon substrate (i.e., a third predetermined depth), the concentration of the first doping element is greater than the concentration of the second doping element at a depth z from the surface of the second doping region (i.e., a third predetermined depth). The thickness of the first doping region ranges from 30 to 100 nm, with z being less than or equal to the sum of the thicknesses of the doped polysilicon layer, the tunneling layer, and the first doping region. In this approach, since the concentration of the first doping element is greater than that of the second doping element, free-carrier Auger recombination can be further reduced, further improving short-circuit current. On the other hand, it can reduce the free carrier Auger recombination without reducing the passivation effect of the tunneling layer, further improve the short-circuit current, open-circuit voltage, and improve battery efficiency.
[0170] As described above, the element concentration distribution of the doped area of the battery silicon substrate is described in detail. With the help of the TOPCon battery shown in Figure 1, the positions of the above x, y and z are described. As shown in Figure 1, the surface of the doped polysilicon layer away from the silicon substrate is the surface shown as D, the maximum value of x is the distance between D and C; the maximum value of y is the distance between D and B; the maximum value of z is the distance between D and A.
[0171] When the solar cell of the present application is a TBC cell, the first doping element is a Group V element (for example, phosphorus), the second doping element is a Group III element (for example, boron), and the layer structure on the above-mentioned silicon substrate also includes a second layer structure, and the above-mentioned second layer structure includes a tunneling layer and a doped polysilicon layer stacked in sequence on the surface of the side of the above-mentioned second doping region away from the silicon substrate; the second doping region is a doping region formed by the second doping element passing through the second layer structure on the above-mentioned silicon substrate.
[0172] In a specific embodiment, in the doped polysilicon layer, the concentration of the first doping element at a depth x (i.e., a first preset depth) away from the surface of the silicon substrate side of the doped polysilicon layer in the first doping region is greater than the concentration of the second doping element at a depth x (i.e., a first preset depth) away from the surface of the silicon substrate side of the doped polysilicon layer in the second doping region, the thickness of the doped polysilicon layer on the first doping region is in the range of 100 to 400 nm, the thickness of the doped polysilicon layer on the second doping region is in the range of 100 to 400 nm, and x is less than or equal to the thickness of the doped polysilicon layer on the first doping region. In a specific embodiment, a first doping element is doped in the tunneling layer of the above-mentioned first doping region, and a second doping element is doped in the tunneling layer of the second doping region. In the direction from the doped polysilicon layer to the tunneling layer, in the tunneling layer, the concentration of the first doping element at a depth y (i.e., a second preset depth) from the surface of the doped polysilicon layer of the first doping region away from the silicon substrate is greater than the concentration of the second doping element at a depth y (i.e., a second preset depth) from the surface of the doped polysilicon layer of the second doping region away from the silicon substrate. The thickness of the tunneling layer on the first doping region ranges from 0.5 to 5 nm, and the thickness of the tunneling layer on the second doping region ranges from 0.5 to 5 nm, and y is less than or equal to the sum of the thicknesses of the doped polysilicon layer and the tunneling layer on the first doping region. In a specific embodiment, in the direction from the doped polysilicon layer to the surface of the above-mentioned first doped region, in the silicon substrate, the concentration of the first doping element at the depth z (i.e., the third preset depth) of the surface of the doped polysilicon layer of the first doped region away from the silicon substrate is greater than the concentration of the second doping element at the depth z (i.e., the third preset depth) of the surface of the doped polysilicon layer of the second doped region away from the silicon substrate, the thickness range of the first doped region is 30 to 100 nm, and z is less than or equal to the sum of the thicknesses of the doped polysilicon layer, the tunneling layer and the first doped region on the first doped region.
[0173] In this application, whether it is a TOPCon cell, a local TOPCon cell, a back contact hybrid cell, or a TBC cell, since the antimony element and the doping element in the silicon substrate are uniformly doped, the resistivity of the silicon substrate and the light absorber is very uniform, which can effectively reduce the lateral transmission resistance of the carriers and improve the cell efficiency.
[0174] In a specific embodiment, the battery of the present application includes an electrode formed on a light absorber, the electrode includes a metal crystal portion in contact with the light absorber, the metal crystal portion includes antimony element, wherein the light absorber includes a silicon substrate and a region for separating carriers generated by the silicon substrate.
[0175] In the present application, the above-mentioned metal crystal refers to an alloy formed by the metal and silicon in the electrode during the electrode formation process.
[0176] In a specific embodiment, the metal crystal portion further includes a doping element, and the concentration of the doping element is greater than the concentration of the antimony element.
[0177] Since the metal crystal portion of the electrode of the battery of the present application contains antimony elements, the contact resistance of the solar cell can be reduced, and the contact resistance of the component can be further reduced.
[0178] In a specific embodiment, the mechanical strength of the solar cell of the present application is greater than or equal to 50 MPa.
[0179] The present application also includes a cell string structure, comprising a plurality of the above-mentioned solar cells of the present application interconnected by conductive interconnectors.
[0180] In a specific embodiment, the conductive interconnection member may be, for example, a conductive connection line (sometimes also referred to as a metal soldering ribbon), or a conductive line in a conductive backplane.
[0181] Specifically, before forming a photovoltaic module, cells need to go through a stringing (or string welding) step. Specifically, as shown in Figure 2, multiple cells are connected via multiple conductive connecting wires, for example, in series. The connecting wires can be metal wire structures with circular or triangular cross-sections, and can be composed of a substrate and a bonding layer wrapped around the substrate.
[0182] In this application, whether the connection is made using a conductive connecting wire (metal welding ribbon) or a conductive circuit formed on a conductive backplane, as long as the battery is in contact with the conductive interconnect through the electrode and the contact part contains antimony elements, such a structure can further reduce the contact resistance of the battery string.
[0183] In the stringing step, welding is used for electrical connection, and the welding process requires a heating operation, the main purpose of which is to melt the bonding layer of the connecting wire to form an electrical connection with the battery. However, in the heating step, the stress of the battery may be uneven up and down, and this uneven pressure up and down will cause bending. However, the greater the bending during the stringing process, the greater the risk of hidden cracks and fragments in the battery during lamination. The mechanical strength of the battery involved in this application is greater than 50Mpa. Its large mechanical strength can suppress excessive bending of the battery cells when stringing, which can improve the yield of the component to a certain extent. Generally speaking, the curvature of the back-contact battery will be greater than that of the bifacial battery. This is because the stress difference between the upper and lower surfaces of the back contact will be greater. Among them, the back-contact battery refers to a battery having an electrical interconnection structure only on one side, while the bifacial battery refers to a battery having an electrical interconnection structure on both opposite sides.
[0184] Specifically, referring to Figure 2, the curvature of the back-contact battery after being heated at 165-200 degrees Celsius and strung together is less than or equal to 2mm, and the curvature after being heated at a low temperature of 100-160 degrees Celsius and strung together is less than or equal to 1.5mm; referring to Figure 3, the curvature of the bifacial battery after being heated at 165-200 degrees Celsius and strung together is less than or equal to 1.2mm, and the curvature after being heated at a low temperature of 100-160 degrees Celsius and strung together is less than or equal to 1mm. It can be seen that the specially doped battery of the present invention has a smaller curvature, which can well control the problems of hidden cracks and fragments during lamination. It should be noted that the curvature involved in this application refers to the height or depth of the bulge or depression generated on the surface of the battery when the battery is bent, which can be obtained by measuring the curvature radius of the battery edge.
[0185] The present application also relates to a solar cell assembly, comprising a plurality of cells, an encapsulation layer, a cover plate and a back plate as described above. The encapsulation layer seals the plurality of cells, and the encapsulation layer is located between the cover plate and the back plate.
[0186] The battery strings of the present application are formed into components through typesetting, stacking, lamination and other processes, and the formed components are shown in Figures 4 and 5. Among them, when performing the lamination process, it is necessary to apply pressure and heat so that the encapsulation layer melts and seals the battery string, and adheres the cover plate and the back plate, and the encapsulation layer is located between the cover plate and the back plate. In the lamination process, due to the above-mentioned pressure application and heating operations, part of the stress of the battery is released and suppressed. For the back-contact battery, see Figure 4, the curvature of the battery in the laminated assembly is less than or equal to 1.2 mm, and for the double-sided battery, see Figure 5, the curvature of the battery in the laminated assembly is less than or equal to 0.8 mm. It has been verified that the hidden cracks and fragmentation problems of the laminated batteries are significantly controlled. It can be seen from Figures 3 and 5 that the bending direction of the battery is toward the cover plate, that is, the battery protrudes toward the direction of the cover plate to form a curved shape.
[0187] Specifically, the encapsulation layer can be at least one of EVA, POE, silicone, and PVB. The cover plate is close to the light-receiving surface of the battery and is transparent organic or inorganic. It can be preferably low-iron embossed glass, and its thickness is preferably 2.0 or 3.2 mm. The back plate can be transparent or non-transparent. For double-glass modules, the back plate is a transparent material, which is preferably glass, while for single-glass modules, the back plate can be non-transparent, such as a TPC board. Furthermore, the module also includes a frame, which has a groove-shaped mounting portion for accommodating the laminate, and the edges of the cover plate and back plate are embedded in the mounting portion of the frame.
[0188] In this application, whether the connection is made using a conductive connecting wire (metal welding ribbon) or a bonding layer formed on the backplane, as long as the battery is in contact with the conductive interconnection on the metal welding ribbon or the bonding layer through the electrode, and the contact part contains antimony elements, such a structure can further reduce the contact resistance of the component.
[0189] Example 1
[0190] The polysilicon blocks are placed in the quartz crucible. For example, the solid silicon raw material is first piled into the quartz crucible, and then the quartz crucible filled with silicon material is placed in the single crystal furnace.
[0191] The single crystal furnace is vacuumed to gradually melt the solid silicon in the quartz crucible into a molten state.
[0192] Because the solid silicon material in the quartz crucible is stacked and placed, after being heated and melted, the actual volume occupied by the quartz crucible decreases, and the melted silicon material does not reach the maximum loading capacity of the quartz crucible. Therefore, it is necessary to use an external feeder, such as a quartz tube feeding barrel, to fill the quartz crucible with silicon material for a second time. During the filling process, the heater simultaneously melts the silicon material in the quartz crucible.
[0193] The Sb-containing dopant is buried in the silicon material in the barrel and is added into the quartz crucible together with the silicon material.
[0194] After all the silicon material in the quartz crucible is melted, it enters the temperature adjustment stage, inserts the seed crystal into the liquid surface, and controls the power parameters to reach the critical crystallization temperature of the liquid surface temperature.
[0195] After the seed crystal and the liquid level reach the crystallization temperature, the seed crystal is pulled upward.
[0196] When the seed crystal length reaches the required length of 15-20mm and the seed crystal diameter is within 5-10mm, the actual single crystal diameter is adjusted to the range of 252±1mm round rod diameter by adjusting parameters such as power and pulling speed; after the shoulder is placed, the shoulder rotation process is carried out to enter the silicon rod equalization process.
[0197] During the equal diameter process, adjust the pulling speed, power, etc. until the equal diameter length is 3800mm.
[0198] Silicon rod drawing is completed by reducing the diameter of the silicon rod.
[0199] The antimony concentration at the head of the obtained silicon rod is 1.87E+16atom / cm 3 The antimony concentration at the tail of the silicon rod is 1.94E+16atom / cm 3The resistivity of the silicon rod tip was measured to be 0.3Ω·cm, and the resistivity of the tail was 0.291Ω·cm. The silicon rods were further processed into silicon wafers and used to manufacture N-TOPCON cells and modules. Using standard AM1.5G photovoltaic cell efficiency testing equipment, the N-TOPCON cells achieved an average energy conversion efficiency of 24.81%.
[0200] In this embodiment, the maximum antimony concentration of the silicon rod measured is the antimony concentration at the tail end of the silicon rod, and the minimum antimony concentration of the silicon rod measured is the antimony concentration at the head end of the silicon rod.
[0201] Example 2
[0202] The method described in Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0203] The final antimony concentration at the silicon rod head is 1.02E+16atom / cm 3 The antimony concentration at the tail of the silicon rod is 1.04E+16atom / cm 3 The silicon rods were used in N-TOPCON modules and cells in the same manner as in Example 1. The N-TOPCON cells achieved an average energy conversion efficiency of 24.86%.
[0204] Example 3
[0205] The method described in Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0206] The final antimony concentration at the silicon rod head is 0.609E+16atom / cm 3 The antimony concentration at the tail of the silicon rod is 0.619E+16atom / cm 3 The resistivity of the silicon rod head was measured to be 0.8 Ω·cm, and the resistivity of the tail was 0.812 Ω·cm. The silicon rod was used in the same manner as in Example 1 for N-TOPCON type modules and cells. The average energy conversion efficiency achieved by the N-TOPCON type cells was 24.90%.
[0207] Example 4
[0208] The method described in Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0209] The final antimony concentration at the silicon rod head is 0.4E+16atom / cm 3 The antimony concentration at the tail of the silicon rod is 0.408E+16atom / cm3 The resistivity of the silicon rod head was measured to be 1.2 Ω·cm, and the resistivity of the tail was 1.178 Ω·cm. The silicon rod was used in the same manner as in Example 1 for N-TOPCON type modules and cells. The average energy conversion efficiency achieved by the N-TOPCON type cells was 24.87%.
[0210] Example 5
[0211] The method described in Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0212] The final antimony concentration at the silicon rod head is 0.212E+16atom / cm 3 The antimony concentration at the tail of the silicon rod is 0.218E+16atom / cm 3 The resistivity of the silicon rod head was measured to be 2.2 Ω·cm, and the resistivity of the tail was 2.136 Ω·cm. The silicon rod was used in the same manner as in Example 1 for N-TOPCON type modules and cells. The average energy conversion efficiency achieved by the N-TOPCON type cells was 24.83%.
[0213] Example 6
[0214] The method described in Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0215] The final antimony concentration at the silicon rod head is 0.153E+16atom / cm 3 The concentration of antimony at the tail of the silicon rod is 0.160E+16atom / cm 3 The silicon rods were tested for their head resistivity of 3Ω·cm and tail resistivity of 2.876Ω·cm. The silicon rods were used in N-TOPCON modules and cells in the same manner as in Example 1. The N-TOPCON cells achieved an average energy conversion efficiency of 24.79%.
[0216] Example 7
[0217] The method described in Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0218] The final antimony concentration at the silicon rod head is 0.0963E+16atom / cm 3 The concentration of antimony at the tail of the silicon rod is 0.102E+16atom / cm 3The silicon rods were tested for their head resistivity of 4.8 Ω·cm and their tail resistivity of 4.47 Ω·cm. The silicon rods were used in N-TOPCON modules and cells in the same manner as in Example 1. The N-TOPCON cells achieved an average energy conversion efficiency of 24.77%.
[0219] Example 8
[0220] The method described in Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0221] The final antimony concentration at the silicon rod head is 0.0691E+16atom / cm 3 The antimony concentration at the tail of the silicon rod is 0.074E+16atom / cm 3 The resistivity of the silicon rod head was measured to be 6.5 Ω·cm, and the resistivity of the tail was 6.074 Ω·cm. The silicon rod was used in the same manner as in Example 1 for N-TOPCON type modules and cells. The average energy conversion efficiency achieved by the N-TOPCON type cells was 24.74%.
[0222] Example 9
[0223] The method described in Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0224] The final antimony concentration at the silicon rod head is 0.0531E+16atom / cm 3 The concentration of antimony at the tail of the silicon rod is 0.0576E+16atom / cm 3 The resistivity of the silicon rod head was measured to be 8.4 Ω·cm, and the resistivity of the tail was 7.767 Ω·cm. The silicon rod was used in the same manner as in Example 1 for N-TOPCON type modules and cells. The average energy conversion efficiency achieved by the N-TOPCON type cells was 24.72%.
[0225] Example 10
[0226] The method described in Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0227] The final antimony concentration at the silicon rod head is 0.0445E+16atom / cm 3 The antimony concentration at the tail of the silicon rod is 0.0484E+16atom / cm 3The resistivity of the silicon rod head was measured to be 10 Ω·cm, and the resistivity of the tail was 9.199 Ω·cm. The silicon rod was used in the same manner as in Example 1 for N-TOPCON type modules and cells. The average energy conversion efficiency achieved by the N-TOPCON type cells was 24.69%.
[0228] Comparative Example 1
[0229] The polysilicon blocks are placed in the quartz crucible. For example, the solid silicon raw material is first piled into the quartz crucible, and then the quartz crucible filled with silicon material is placed in the single crystal furnace.
[0230] The single crystal furnace is vacuumed to gradually melt the solid silicon in the quartz crucible into a molten state.
[0231] Because the solid silicon material in the quartz crucible is stacked and placed, after being heated and melted, the actual volume occupied by the quartz crucible decreases, and the melted silicon material does not reach the maximum loading capacity of the quartz crucible. Therefore, it is necessary to use an external feeder, such as a quartz tube feeding barrel, to fill the quartz crucible with silicon material for a second time. During the filling process, the heater simultaneously melts the silicon material in the quartz crucible.
[0232] The phosphorus-doped N-type master alloy is buried in the silicon material in the barrel and is added into the quartz crucible together with the silicon material.
[0233] After all the silicon material in the quartz crucible is melted, it enters the temperature adjustment stage, inserts the seed crystal into the liquid surface, and controls the power parameters to reach the critical crystallization temperature of the liquid surface temperature.
[0234] After the seed crystal and the liquid level reach the crystallization temperature, the seed crystal is pulled upward.
[0235] When the seed crystal length reaches the required length of 15-20mm and the seed crystal diameter is within 5-10mm, the actual single crystal diameter is adjusted to the range of 252±1mm round rod diameter by adjusting parameters such as power and pulling speed; after the shoulder is placed, the shoulder rotation process is carried out to enter the silicon rod equalization process.
[0236] During the equal diameter process, adjust the pulling speed, power, etc. until the equal diameter length is 3800mm.
[0237] Silicon rod drawing is completed by reducing the diameter of the silicon rod.
[0238] The antimony concentration at the head of the obtained silicon rod is 1.8E+16atom / cm 3 The concentration of antimony at the tail of the silicon rod is 4.88E+16atom / cm 3The resistivity of the silicon rod head was measured to be 0.3 Ω·cm, and the resistivity of the tail was 0.14 Ω·cm. The silicon rod was used in the same manner as in Example 1 for N-TOPCON type modules and cells. The average energy conversion efficiency achieved by the N-TOPCON type cells was 24.63%.
[0239] Comparative Example 2
[0240] The method described in Comparative Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0241] The final antimony concentration at the silicon rod head is 2.63E+16atom / cm 3 The concentration of antimony at the tail of the silicon rod is 2.88E+16atom / cm 3 The silicon rods were used in N-TOPCON modules and cells in the same manner as in Example 1. The N-TOPCON cells achieved an average energy conversion efficiency of 24.67%.
[0242] Comparative Example 3
[0243] The method described in Comparative Example 1 was adopted, and the concentration of the Sb element in the Sb-containing dopant was adjusted to complete the silicon rod drawing.
[0244] The final antimony concentration at the silicon rod head is 0.0344E+16atom / cm 3 The antimony concentration at the tail of the silicon rod is 0.038E+16atom / cm 3 The resistivity of the silicon rod head was measured to be 12.5 Ω·cm, and the resistivity of the tail was 11.5 Ω·cm. The silicon rod was used in the same manner as in Example 1 for N-TOPCON type modules and cells. The average energy conversion efficiency achieved by the N-TOPCON type cells was 24.65%.
[0245] Table 1
[0246] Table 2
[0247] Table 3
[0248] Referring to Table 1 and Table 2, as shown in Example 1 and Comparative Example 1, under the same conditions, the silicon rods and silicon wafers obtained by doping with antimony are used for N-TOPCON type batteries, and the average conversion efficiency of the obtained batteries is significantly improved compared to those doped with phosphorus, and the overall finished product quality of the obtained single crystal silicon rods is higher.
[0249] In addition, as shown in Examples 1 to 10 and Comparative Examples 2 to 3, under the same conditions, the antimony concentration has a significant impact on the resistivity and the average energy conversion efficiency of the final battery, and the optimal concentration range is 0.04E+16 atom / cm 3 to 2E+16atom / cm 3 between.
[0250] As shown in Table 3, the single crystal silicon rods claimed in the present application have excellent resistivity distribution uniformity (concentration) both in the length direction and in the radial cross-sectional direction. Combined with the resistivity ranges measured in Examples 1 to 10 above, it can be shown that the overall finished product quality of the single crystal silicon rod products in the present application is high.
[0251] In addition, the ratio of concentric circles in the radial cross section of the silicon rod in Examples 1 to 10 is also smaller than that of concentric circles in the radial cross section of the conventional phosphorus-doped silicon rod.
[0252] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-mentioned specific embodiments and application fields. The above-mentioned specific embodiments are merely illustrative and instructive, and are not restrictive. A person skilled in the art, under the guidance of this specification and without departing from the scope of protection of the claims of the present invention, can also make many forms, all of which fall within the scope of protection of the present invention.
Claims
1. A single crystal silicon rod, wherein: The single crystal silicon rod contains antimony element, and the concentration of the antimony element is 4E+14atom / cm 3 To 2E+16atom / cm 3 The preferred concentration of antimony is 4.3E+14cm -3 To 1.9E+16cm -3 The concentration of antimony is preferably 4.45E+14cm -3 To 1.87E+16cm -3 .
2. The single crystal silicon rod according to claim 1, wherein: The concentration of antimony in the single crystal silicon rod is 0.15E+16atom / cm 3 To 1.95E+16atom / cm 3 .
3. The single crystal silicon rod according to claim 1, wherein: The concentration of antimony in the single crystal silicon rod is 0.4E+16atom / cm 3 To 1.05E+16atom / cm 3 .
4. The single crystal silicon rod according to claim 1, wherein: The concentration of antimony in the single crystal silicon rod is 0.5E+16atom / cm 3 To 0.70E+16atom / cm 3 .
5. The single crystal silicon rod according to any one of claims 1 to 4, wherein: The single crystal silicon rod satisfies the following conditions: (the concentration of antimony at the tail end surface of the single crystal silicon rod - the concentration of antimony at the head end surface of the single crystal silicon rod) / the concentration of antimony at the tail end surface of the single crystal silicon rod is ≤10%, preferably (the concentration of antimony at the tail end surface of the single crystal silicon rod - the concentration of antimony at the head end surface of the single crystal silicon rod) / the concentration of antimony at the tail end surface of the single crystal silicon rod is ≤5%, and further preferably (the concentration of antimony at the tail end surface of the single crystal silicon rod - the concentration of antimony at the head end surface of the single crystal silicon rod) / the concentration of antimony at the tail end surface of the single crystal silicon rod is ≤2%.
6. The single crystal silicon rod according to any one of claims 1 to 4, wherein: The single crystal silicon rod satisfies the following conditions: (maximum antimony concentration of the single crystal silicon rod - minimum antimony concentration of the single crystal silicon rod) / maximum antimony concentration of the single crystal silicon rod ≤10%, preferably (maximum antimony concentration of the single crystal silicon rod - minimum antimony concentration of the single crystal silicon rod) / maximum antimony concentration of the single crystal silicon rod ≤5%, further preferably (maximum antimony concentration of the single crystal silicon rod - minimum antimony concentration of the single crystal silicon rod) / maximum antimony concentration of the single crystal silicon rod ≤2%.
7. The single crystal silicon rod according to any one of claims 1 to 4, wherein: The tail end face of the single crystal silicon rod satisfies the following conditions: -15%≤(the concentration of antimony element in the center of the tail end face - the concentration of antimony element at the edge of the tail end face) / the concentration of antimony element in the center of the tail end face ≤15%, preferably -10%≤(the concentration of antimony element in the center of the tail end face - the concentration of antimony element at the edge of the tail end face) / the concentration of antimony element in the center of the tail end face ≤10%, and further preferably -5%≤(the concentration of antimony element in the center of the tail end face - the concentration of antimony element at the edge of the tail end face) / the concentration of antimony element in the center of the tail end face ≤5%.
8. The single crystal silicon rod according to any one of claims 1 to 4, wherein: The resistivity of the single crystal silicon rod is 0.2 to 10Ω·cm, preferably 0.3 to 3Ω·cm, and more preferably 0.5 to 1.2Ω·cm; or the resistivity of the single crystal silicon rod is 0.3 to 10Ω·cm, preferably 0.4 to 8Ω·cm; and more preferably 0.5 to 6Ω·cm.
9. The single crystal silicon rod according to any one of claims 1 to 4, wherein: The single crystal silicon rod satisfies the following conditions: -15%≤(single crystal silicon rod head end surface resistivity - single crystal silicon rod tail end surface resistivity) / single crystal silicon rod tail end surface resistivity≤15%, preferably -10%≤(single crystal silicon rod head end surface resistivity - single crystal silicon rod tail end surface resistivity) / single crystal silicon rod tail end surface resistivity≤10%, further preferably -5%≤(single crystal silicon rod head end surface resistivity - single crystal silicon rod tail end surface resistivity) / single crystal silicon rod tail end surface resistivity≤5%.
10. The single crystal silicon rod according to any one of claims 1 to 4, wherein: The tail end face of the single crystal silicon rod satisfies the following conditions: -15%≤(tail end face edge resistivity - tail end face center resistivity) / tail end face center resistivity≤15%, preferably -10%≤(tail end face edge resistivity - tail end face center resistivity) / tail end face center resistivity≤10%, further preferably -5%≤(tail end face edge resistivity - tail end face center resistivity) / tail end face center resistivity≤5%.
11. A silicon wafer made from the single crystal silicon rod according to any one of claims 1 to 10.
12. A silicon wafer, wherein: The silicon wafer contains antimony element, and the concentration of the antimony element is 0.04E+16atom / cm 3 Up to 2.00E+16atom / cm 3 The concentration of antimony is preferably 4.30E+14cm -3 To 1.90E+16cm -3 The concentration of antimony is preferably 4.45E+14cm -3 To 1.87E+16cm -3 .
13. The silicon wafer according to claim 12, wherein: The concentration of the antimony element is 0.15E+16atom / cm 3 To 1.95E+16atom / cm 3 .
14. The silicon wafer according to claim 12, wherein: The concentration of the antimony element is 0.4E+16atom / cm 3 To 1.05E+16atom / cm 3 .
15. The silicon wafer according to claim 12, wherein: The concentration of the antimony element is 0.5E+16atom / cm 3 To 0.7E+16atom / cm 3 .
16. The silicon wafer according to any one of claims 12 to 15, wherein: The silicon wafer satisfies the following conditions: -15%≤(concentration of antimony element in the center of radial section - concentration of antimony element at the edge of radial section) / concentration of antimony element in the center of radial section≤15%, preferably -10%≤(concentration of antimony element in the center of radial section - concentration of antimony element at the edge of radial section) / concentration of antimony element in the center of radial section≤10%, further preferably -5%≤(concentration of antimony element in the center of radial section - concentration of antimony element at the edge of radial section) / concentration of antimony element in the center of radial section≤5%.
17. The silicon wafer according to any one of claims 11 to 16, wherein: The silicon wafer also includes at least one of phosphorus, gallium, and germanium.
18. The silicon wafer according to any one of claims 11 to 17, wherein: The mechanical strength of the silicon wafer is greater than or equal to 70 MPa.
19. The silicon wafer according to any one of claims 11 to 18, wherein: The margin of the silicon wafer is greater than 156 mm.
20. The silicon wafer according to any one of claims 11 to 19, wherein: The silicon wafer is rectangular, one side of the rectangle is 156 mm to 300 mm, and the other side of the rectangle is 83 mm to 300 mm.
21. The silicon wafer according to any one of claims 11 to 20, wherein: The silicon wafer also includes a chamfer connecting two adjacent sides of the silicon wafer, and the arc length projection length of the chamfer is 1 mm to 10 mm.
22. The silicon wafer according to any one of claims 11 to 21, wherein: The thickness of the silicon wafer is 40 μm to 170 μm, preferably 70 μm to 160 μm, and more preferably 80 μm to 140 μm.
23. A battery, wherein: It comprises the silicon wafer according to any one of claims 11 to 22 or a silicon wafer made from the single crystal silicon rod according to any one of claims 1 to 10.
24. The battery according to claim 23, wherein The mechanical strength of the battery is greater than or equal to 50 MPa; preferably greater than or equal to 60 MPa; preferably greater than or equal to 70 MPa.
25. The battery according to claim 23 or 24, wherein The thickness of the battery is 40 μm to 170 μm, preferably 70 μm to 160 μm, and more preferably 80 μm to 140 μm.
26. The battery according to any one of claims 23 to 25, wherein One side distance of the battery is 156 mm to 300 mm, and the other side distance of the battery is 83 mm to 300 mm.
27. The battery according to any one of claims 23 to 26, wherein The battery comprises a silicon substrate, and the resistivity of the silicon substrate is 0.3 to 10 Ω·cm, preferably 0.4 to 8 Ω·cm; and more preferably 0.5 to 6 Ω·cm.
28. A battery, wherein: comprising a silicon substrate, wherein the silicon substrate contains antimony element, The doping concentration of antimony element in the silicon substrate is 4E+14cm -3 To 2E+16cm -3 , preferably 4.3E+14cm -3 To 1.9E+16cm -3 ; More preferably 4.45E+14cm -3 To 1.87E+16cm -3 .
29. The battery according to claim 28, wherein A doped region is provided in at least one side of the surface of the silicon substrate, or at least one doped passivation layer is provided on at least one side of the surface of the silicon substrate.
30. The battery according to claim 29, wherein The concentration of antimony element in the doping region in the thickness direction of the silicon substrate remains substantially unchanged.
31. The battery according to claim 29, wherein In the doping region, the sum of the concentration of the antimony element and the concentration of the doping element is less than or equal to 1E+21cm -3 .
32. The battery according to claim 29, wherein When the doping element is a Group III element, the thickness of the doping region is in the range of 30 to 650 nm; or When the doping element is a fifth main group element, the thickness of the doping region is in the range of 100 to 200 nm.
33. The battery according to claim 29, wherein The doping region includes a first doping region and a second doping region, An interface passivation layer and a doping passivation layer are sequentially stacked on a surface of the first doped region on a side away from the silicon substrate, doping a first doping element in the doped passivation layer, The second doping region on the silicon substrate is further doped with a second doping element, The first doping region and the second doping region have opposite conductivity types.
34. The battery according to claim 33, wherein The first doping element is a fifth main group element, the second doping element is a third main group element, In the doped passivation layer, the concentration of the first doping element at a first preset depth from the surface of the doped passivation layer on one side away from the silicon substrate is greater than the concentration of the second doping element at the same first preset depth from the surface of the second doping region, the thickness range of the doped passivation layer is 100 to 400 nm, and the first preset depth is less than or equal to the thickness of the doped passivation layer.
35. The battery according to claim 33, wherein The first doping element is a fifth main group element, the second doping element is a third main group element, An interface passivation layer and a doping passivation layer are sequentially stacked on a surface of the second doped region on a side away from the silicon substrate; In the doped passivation layer, the concentration of the first doping element at a first preset depth from the surface of the doped passivation layer on the side away from the silicon substrate in the first doping region is greater than the concentration of the second doping element at a first preset depth from the surface of the doped passivation layer on the side away from the silicon substrate in the second doping region, the thickness of the doped passivation layer on the first doping region ranges from 100 to 400 nm, the thickness of the doped passivation layer on the second doping region ranges from 100 to 400 nm, and the first preset depth is less than or equal to the thickness of the doped passivation layer on the first doping region.
36. The battery according to claim 34, wherein doping a first doping element in the interface passivation layer, In the direction from the doped passivation layer to the interface passivation layer, in the interface passivation layer, the concentration of the first doping element at a second preset depth from the surface of the doped passivation layer on a side away from the silicon substrate is greater than the concentration of the second doping element at a second preset depth from the surface of the second doping region, the thickness of the interface passivation layer ranges from 0.5 to 5 nm, and the second preset depth is less than or equal to the sum of the thicknesses of the doped passivation layer and the interface passivation layer.
37. The battery according to claim 35, wherein The interface passivation layer of the first doping region is doped with a first doping element, and the interface passivation layer of the second doping region is doped with a second doping element, In the direction from the doped passivation layer to the interface passivation layer, in the interface passivation layer, the concentration of the first doping element at a second preset depth from the surface of the doped passivation layer on the side away from the silicon substrate in the first doped region is greater than the concentration of the second doping element at a second preset depth from the surface of the doped passivation layer on the side away from the silicon substrate in the second doped region, the thickness of the interface passivation layer on the first doped region ranges from 0.5 to 5 nm, the thickness of the interface passivation layer on the second doped region ranges from 0.5 to 5 nm, and the second preset depth is less than or equal to the sum of the thicknesses of the doped passivation layer and the interface passivation layer on the first doped region.
38. The battery according to claim 34, wherein In the direction from the doped passivation layer to the surface of the first doped region, in the silicon substrate, the concentration of the first doping element at a third preset depth from the surface of the doped passivation layer away from the silicon substrate is greater than the concentration of the second doping element at a third preset depth from the surface of the second doped region, the thickness of the first doped region ranges from 30 to 100 nm, and the third preset depth is less than or equal to the doped passivation layer, The sum of the thicknesses of the interface passivation layer and the first doped region.
39. The battery according to claim 35, wherein In the direction from the doped passivation layer to the surface of the first doped region, in the silicon substrate, the concentration of the first doping element at a third preset depth from the surface of the doped passivation layer of the first doped region away from the silicon substrate is greater than the concentration of the second doping element at a third preset depth from the surface of the doped passivation layer of the second doped region away from the silicon substrate, the thickness of the first doped region ranges from 30 to 100 nm, and the third preset depth is less than or equal to the sum of the thicknesses of the doped passivation layer, the interface passivation layer and the first doped region on the first doped region.
40. The battery according to claim 29, wherein When the doping element is a third main group element, the thickness of the doping region ranges from 80 to 180 nm; When the doping element is a fifth main group element, the thickness of the doping region ranges from 30 to 100 nm.
41. The battery according to any one of claims 28 to 40, wherein The battery includes an electrode formed on a light absorber, the electrode including a metal crystal portion in contact with the light absorber, the metal crystal portion including antimony element, wherein the light absorber includes a silicon substrate and a region for separating carriers generated by the silicon substrate.
42. The battery according to claim 41, wherein The metal crystal portion further includes a doping element, and a concentration of the doping element is greater than a concentration of the antimony element.
43. The battery according to any one of claims 29 to 42, wherein the mechanical strength of the battery is greater than or equal to 50 MPa, preferably greater than or equal to 60 MPa; preferably greater than or equal to 70 MPa. 44 . The battery according to claim 28 , wherein the thickness of the battery is 70 μm to 170 μm, preferably 80 μm to 160 μm, and more preferably 80 μm to 140 μm.
45. The battery according to any one of claims 28 to 44, wherein one side distance of the battery is 156 mm to 300 mm, and the other side distance of the battery is 83 mm to 300 mm.
46. The battery according to any one of claims 28 to 45, wherein the resistivity of the substrate is 0.3 to 10 Ω·cm, preferably 0.4 to 8 Ω·cm; more preferably 0.5 to 6 Ω·cm.
47. A battery string comprising a plurality of batteries interconnected by conductive interconnectors, at least one of the batteries being the battery of any one of claims 23 to 46.
48. The battery string according to claim 47, wherein: The curvature of the battery is less than or equal to 2 mm.
49. The battery string according to claim 48, wherein the conductive interconnect is a connecting wire or a conductive line in a conductive back plate, and the connecting wire is joined to the battery by welding or conductive bonding.
50. The battery string of claim 49, wherein the welding comprises a heating step.
51. The battery string according to claim 50, wherein the temperature range of the heating step is 100-160 degrees Celsius, and the curvature of the battery is less than or equal to 1.5 mm.
52. The battery string according to claim 50, wherein the temperature range of the heating step is 165-200 degrees Celsius, and the curvature of the battery is less than or equal to 2 mm.
53. The battery string according to any one of claims 47 to 52, wherein the conductive interconnect comprises an electrical contact portion contacting an electrode of the battery, the electrical contact portion comprising antimony element.
54. A solar cell assembly, comprising a plurality of cells, a packaging layer, a cover plate and a back plate, wherein the packaging layer seals the plurality of cells and the packaging layer is located between the cover plate and the back plate; the cell is the cell according to any one of claims 23 to 46.
55. The solar module of claim 54, wherein: The curvature of the battery is less than or equal to 1.2 mm.
56. The solar energy assembly according to any one of claims 54 to 55, further comprising a frame, wherein the edge of the cover plate and / or the back plate is embedded in the mounting portion of the frame.
57. The solar module according to any one of claims 54 to 56, wherein the cover plate and / or the back plate is a transparent plate.
58. The solar module according to any one of claims 54 to 56, wherein the back sheet is a non-transparent sheet.
59. The solar module according to any one of claims 54 to 58, wherein the cell protrudes toward the cover plate to form a curved shape.
60. The solar module of any one of claims 54 to 59, wherein a plurality of cells are interconnected by a conductive interconnector, the conductive interconnector comprising an electrical contact portion contacting an electrode of the cell, the electrical contact portion comprising antimony.