Surface-treated aluminum material, method of manufacturing the same, and member for semiconductor-processing apparatus
Patent Information
- Application Number
- MYPI2025005177
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-10
AI Technical Summary
Components for semiconductor processing equipment with anodic oxide films face low durability against corrosive gases and plasma due to incomplete pore closure, leading to potential cracks and foreign matter generation, necessitating improved heat resistance and corrosion resistance.
A surface-treated aluminum material with a protective film comprising aluminum oxide and hydrated oxide, formed by anodizing and sealing the anodic oxide film in hot water under specific temperature and time conditions to achieve a thickness of 2 μm or more, with a hydrogen-to-aluminum mass ratio within 0.2 to 0.7, enhancing corrosion resistance and suppressing crack occurrence.
The surface-treated aluminum material exhibits excellent corrosion resistance against corrosive gases and plasma, while preventing cracks, making it suitable for semiconductor manufacturing equipment components.
Smart Images

Figure PI2025005177_DRAWING_001
Abstract
Description
Surface-treated aluminum material, its manufacturing method, and semiconductor processing equipment component
[0001] The present invention relates to a surface-treated aluminum material, a method for producing the same, and a member for semiconductor manufacturing equipment.
[0002] Aluminum materials made of aluminum or aluminum alloys are used in a variety of applications, and an anodized coating is sometimes provided on the surface of these aluminum materials for purposes such as surface protection.
[0003] For example, Patent Document 1 describes a component for a substrate processing apparatus that performs plasma processing on a substrate, characterized in that the component is connected to the anode of a DC power supply and has a coating formed on the surface of the component by anodizing, in which the component is immersed in a solution mainly containing an organic acid, and the coating is subjected to a semi-sealing treatment using boiling water.
[0004] Japanese Patent Application Laid-Open No. 2008-81815
[0005] However, the component of Patent Document 1 has a problem in that the pores of the anodized film are not completely closed, resulting in low durability against corrosive gases and plasma.
[0006] On the other hand, in order to improve the durability of the component disclosed in Patent Document 1 against corrosive gases and plasma, a method of completely blocking the pores in the anodized film is conceivable. However, in this case, cracks are likely to occur in the anodized film when the temperature rises, and there is a risk of generating foreign matter consisting of small pieces of the anodized film. To prevent the generation of such foreign matter, it is desirable to further improve the heat resistance of aluminum materials having an anodized film on their surfaces.
[0007] The present invention has been made in view of the above background, and aims to provide a surface-treated aluminum material that has excellent corrosion resistance against corrosive gases and plasma and can suppress the occurrence of cracks, a method for manufacturing the same, and a component for semiconductor manufacturing equipment.
[0008] One aspect of the present invention is a method for manufacturing a protective coating film comprising: a base material made of aluminum or an aluminum alloy; and a protective coating film containing an oxide and a hydrated oxide of aluminum, the protective coating film having a thickness of 2 μm or more; and when the mass ratios of elements in the protective coating film are analyzed in the depth direction by glow discharge optical emission spectroscopy, the integral value C of the mass ratio of aluminum atoms in the range from the surface of the protective coating to a depth of 1 μm is 0.05 μm or more. Al The integral value C of the mass ratio of hydrogen atoms to H Ratio C H / C Al The surface-treated aluminum material has a surface roughness of 0.2 or more and 0.7 or less.
[0009] Another aspect of the present invention is a method for producing a surface-treated aluminum material according to the above aspect, comprising: an anodizing treatment step of anodizing the base material to form an anodized film having pores on the base material; and a sealing step of subsequently immersing the base material in hot water to seal the pores in the anodized film, thereby forming the protective film on the base material, wherein the product of the hot water temperature T [°C] and the immersion time t [hours] in the sealing step is more than 20°C·hours and less than 75°C·hours.
[0010] The surface of the base material in the surface-treated aluminum material (hereinafter referred to as "aluminum material") is provided with a protective coating having a thickness of 2 μm or more and containing an oxide and a hydrated oxide of aluminum. The oxide and the hydrated oxide are analyzed in the depth direction of the protective coating by glow discharge optical emission spectroscopy, and the integrated value C of the mass ratio of aluminum atoms in the protective coating is Al The integral value C of the mass ratio of hydrogen atoms to H Ratio C H / C Al is distributed so as to be within the above-mentioned specific range. By providing such a protective coating on the base material, the aluminum material has high corrosion resistance and can suppress the occurrence of cracks.
[0011] In addition, in the method for producing an aluminum material according to the above aspect, the base material is anodized to form an anodized film, and then the pores in the anodized film are sealed under the specific conditions, thereby forming the protective film on the base material, thereby easily obtaining the aluminum material.
[0012] As described above, according to the above-described aspects, it is possible to provide a surface-treated aluminum material that has excellent corrosion resistance against corrosive gases and plasma and can suppress the occurrence of cracks, a method for manufacturing the same, and a member for semiconductor manufacturing equipment.
[0013] Fig. 1 is a cross-sectional view showing a main part of an aluminum material in an example. Fig. 2 is a cross-sectional view showing a main part of a base material after an anodizing treatment process is completed in the manufacturing process of the aluminum material in an example. Fig. 3 is an explanatory diagram showing a depth profile of the mass ratio of hydrogen atoms in the protective coating of test material S1.
[0014] (Aluminum Material) The material of the base material in the aluminum material can be appropriately selected from the group consisting of aluminum and aluminum alloys depending on the application of the aluminum material. For example, when attempting to reduce outgassing from the aluminum material, it is preferable that the base material be composed of 1000 series aluminum or 3000 series aluminum alloy. As the 3000 series aluminum alloy, for example, an aluminum alloy containing 1.0 mass% to 1.5 mass% Mn (manganese) and one or more elements selected from the group consisting of Si (silicon), Fe (iron), Cu (copper), Mg, Cr (chromium), Zn (zinc), and Ti (titanium) as optional components, with the remainder being Al and unavoidable impurities, can be used.
[0015] More specifically, as the 1000 series aluminum constituting the base material of the aluminum material, for example, aluminum having a chemical component represented by alloy number AA1100, AA1100A, AA1200, AA1200A, AA1300, AA1110, AA1120, AA1230, AA1230A, AA1235, AA1435, AA1145, AA1345, AA1445, AA1150, AA1350, AA1350A, AA1450, AA1370, AA1275, AA1185, AA1285, AA1385, AA1188, AA1190, AA1290, AA1193, AA1198, or AA1199 can be used.
[0016] Examples of the 3000 series aluminum alloys constituting the base material of the aluminum material include alloy numbers AA3002, AA3102, AA3003, AA3103, AA3103A, AA3103B, AA3203, AA3403, AA3004, AA3004A, AA3104, AA3204, AA3304, AA3005, AA3005A, AA3105, AA3105A, AA3105B, AA3007, and AA3107. , AA3207, AA3207A, AA3307, AA3009, AA3010, AA3110, AA3011, AA3012, AA3012A, AA3013, AA3014, AA3015, AA3016, AA3017, AA3019, AA3020, AA3021, AA3025, AA3026, AA3030, AA3130, or AA3065 can be used.
[0017] Furthermore, when increasing the strength of an aluminum material, it is preferable that the base material be composed of a 5000-series aluminum alloy or a 6000-series aluminum alloy. Examples of the 5000-series aluminum alloy include an aluminum alloy containing 0.5% by mass to 5.0% by mass of magnesium (Mg), optionally containing one or more elements selected from the group consisting of Si, Fe, Cu, Mn, Cr, Zn, and Ti, with the balance consisting of Al and unavoidable impurities. Examples of the 6000-series aluminum alloy include an aluminum alloy containing 0.3% by mass to 1.5% by mass of magnesium, 0.2% by mass to 1.2% by mass of Si, optionally containing one or more elements selected from the group consisting of Fe, Cu, Mn, Cr, Zn, and Ti, with the balance consisting of Al and unavoidable impurities.
[0018] More specifically, examples of the 5000 series aluminum alloys constituting the base material of the aluminum material include alloy numbers AA5182, AA5183, AA5005, AA5005A, AA5205, AA5305, AA5505, AA5605, AA5006, AA5106, AA5010, AA5110, AA5110A, AA5210, AA5310, AA5016, AA5017, AA5018, AA5018A, AA5019, AA5019A, and AA5 119, AA5119A, AA5021, AA5022, AA5023, AA5024, AA5026, AA5027, AA5028, AA5040, AA5140, AA5041, AA5042, AA5043, AA5049, AA5149, AA5249, AA5349, AA5449, AA5449A, AA5050, AA5050A, AA5050C, AA5150, AA5051, AA5051A, AA5151, AA5251, AA5251A, AA5351, AA5451, AA5052, AA5252, AA5352, AA5154, AA5154A, AA5154B, AA5154C, AA5254, AA5354, AA5454, AA5554, AA5654, AA 5654A, AA5754, AA5854, AA5954, AA5056, AA5356, AA5356A, AA5456, AA5456A, AA5456B, AA5556, AA5556A, AA5556B, AA5556C, Aluminum alloys having a chemical composition represented by AA5257, AA5457, AA5557, AA5657, AA5058, AA5059, AA5070, AA5180, AA5180A, AA5082, AA5182, AA5083, AA5183, AA5183A, AA5283, AA5283A, AA5283B, AA5383, AA5483, AA5086, AA5186, AA5087, AA5187, or AA5088 can be used.
[0019] Examples of the 6000 series aluminum alloys constituting the base material of the aluminum material include alloy numbers AA6101, AA6101A, AA6101B, AA6201, AA6201A, AA6401, AA6501, AA6002, AA6003, AA6103, AA6005, AA6005A, AA6005B, AA6005C, AA6105, AA6205, AA6305, AA6006, AA6106, AA6206, AA6306, AA6008, AA6009, AA6010, AA6110, AA6110A, AA6011, AA6111, AA6012, AA6012A, AA6013, AA6113, AA6014, AA6015, AA6016 , AA6016A, AA6116, AA6018, AA6019, AA6020, AA6021, AA6022, AA6023, AA6024, AA6025, AA6026, AA6027, AA6028, AA6031, AA6032, AA6033, AA6040, AA6041, AA6042, AA6043, AA6151, AA6351, AA6351A, AA6451, AA6951, AA6053, AA6055, AA6056, AA6156, AA6060, AA6160, AA6260, AA6360, AA6460, AA6460B, AA6560, AA6660, AA6061, AA6061A, AA6261, AA6361, AA6162, Aluminum alloys having a chemical composition represented by AA6262, AA6262A, AA6063, AA6063A, AA6463, AA6463A, AA6763, A6963, AA6064, AA6064A, AA6065, AA6066, AA6068, AA6069, AA6070, AA6081, AA6181, AA6181A, AA6082, AA6082A, AA6182, AA6091, or AA6092 can be used.
[0020] A protective coating containing aluminum oxide and hydrated oxide is provided on the base material. The protective coating can be obtained, for example, by anodizing the base material to form a porous anodic oxide coating made of aluminum oxide and having numerous pores on the surface of the base material, followed by a pore-sealing treatment to block the pores in the anodic oxide coating with hydrated aluminum oxide.
[0021] The thickness of the protective coating is 2 μm or more. This protects the base material from corrosive gases and plasma, and improves the corrosion resistance of the aluminum material. From the viewpoint of corrosion resistance, there is no particular upper limit on the thickness of the protective coating, and the thicker the protective coating, the more the corrosion resistance of the aluminum material can be improved. From this viewpoint, the thickness of the protective coating is preferably 5 μm or more, and more preferably 10 μm or more. Note that the upper limit of the thickness of the protective coating from a manufacturing standpoint is, for example, 200 μm. From the viewpoint of suppressing the occurrence of cracks in the protective coating, the thickness of the protective coating is preferably 100 μm or less.
[0022] The oxide and hydrated oxide of aluminum in the protective film are determined by analyzing the mass ratio of elements in the protective film in the depth direction by glow discharge optical emission spectrometry, and the integral value C of the mass ratio of aluminum atoms in the range from the surface of the protective film to a depth of 1 μm is used. Al The integral value C of the mass ratio of hydrogen atoms to H Ratio C H / C Al The integral ratio C is distributed so that the integral ratio C is 0.20 or more and 0.70 or less. H / C Al indicates the amount of hydrated oxide present near the surface of the protective coating, and the ratio C H / C Al A higher value means that the amount of hydrated oxide present near the surface of the protective coating is greater.
[0023] Therefore, the ratio of the integral values C H / C Al In a protective film having a ratio C of 0.20 or more, it is believed that the pores generated by the anodizing treatment are sufficiently blocked by hydrated oxides. H / C Al By making the ratio of integral values C 0.20 or more, it is possible to suppress the intrusion of corrosive gases, plasma, etc. into the pores, and to improve the corrosion resistance of the aluminum material. H / C AlThe value of is preferably 0.22 or more, more preferably 0.24 or more, even more preferably 0.26 or more, particularly preferably 0.28 or more, and most preferably 0.30 or more.
[0024] On the other hand, the ratio of the integral values C H / C Al If the ratio is less than 0.20, the pores are likely to be insufficiently blocked, which may result in a decrease in the corrosion resistance of the aluminum material.
[0025] Furthermore, the ratio C of the integral values H / C Al If the value of integral ratio C becomes excessively high, cracks may easily occur in the protective coating when the temperature of the aluminum material rises. The reason for this is not entirely clear, but the following may be considered, for example. H / C Al If the value of C is excessively high, it is considered that the protective film contains an excessively large amount of hydrated oxide or the crystalline state of the hydrated oxide is excessively high. H / C Al If the value of is excessively high, the difference in the thermal expansion coefficients between the base material, the aluminum oxide, and the aluminum hydrate oxide will cause uneven thermal expansion within the protective coating, making it more likely to crack when the temperature rises.
[0026] From the viewpoint of suppressing the occurrence of cracks in the protective coating, the ratio of integral values C H / C Al From the same viewpoint, the value of the ratio C H / C Al The value of is preferably 0.68 or less, more preferably 0.66 or less, and even more preferably 0.64 or less.
[0027] Ratio of integral values in the protective coating C H / C Al In determining the preferable range of the integral ratio C H / C Al The upper and lower limits of the integral ratio C can be arbitrarily combined. H / C AlThe preferred range of may be 0.22 or more and 0.68 or less, 0.24 or more and 0.68 or less, 0.26 or more and 0.66 or less, 0.28 or more and 0.66 or less, or 0.30 or more and 0.64 or less.
[0028] The ratio C of the integral values in the protective coating H / C Al Specifically, the calculation method is as follows. First, the surface of the aluminum material is cleaned, and then a glow discharge optical emission spectrometer (for example, "GD750" manufactured by SPECTRUMA Analytik GmbH) is used to obtain a profile of the emission intensity of aluminum atoms and hydrogen atoms in the depth direction of the protective coating. At this time, the measurement conditions for the glow discharge optical emission spectrometer are an anode diameter of 2.5 mm, an output of 25 W, a gas pressure of 3.5 hPa, and an emission intensity acquisition interval of 0.2 to 0.24 seconds. When measured under these conditions, the sputtering rate of the protective coating is approximately 50 to 90 nm / second.
[0029] The thus obtained profile of the emission intensity of aluminum atoms and hydrogen atoms in the depth direction is converted into a profile of mass ratio based on a calibration curve prepared in advance. Then, the mass ratio of each atom is integrated over a range from the surface of the protective coating to a depth of 1 μm, and the integral value C of the mass ratio of hydrogen atoms is obtained. H and the integral value C of the mass ratio of aluminum atoms Al The integral value C of the mass ratio of hydrogen atoms obtained above is calculated. H The integral value C of the mass ratio of aluminum atoms Al By dividing by this, the ratio of the integral values C H / C Al can be calculated.
[0030] When a sealing test was performed according to the method specified in JIS H8683-2:2013, the mass loss per unit area of the aluminum material was 0.2 g / dm 2 In this case, the corrosion resistance of the aluminum material can be further improved.
[0031] The specific method for the pore sealing test is as follows. First, 35 mL of phosphoric acid and 20 g of chromic anhydride are dissolved in water to prepare 1 L of test solution. Next, a test piece including a protective coating is taken from the aluminum material, and the area of the protective coating on the test piece is measured. After removing any dirt from the surface of this test piece, the mass of the test piece is measured. Thereafter, the test piece is immersed in the test solution maintained at a temperature of 38°C ± 1°C for 15 minutes ± 5 seconds.
[0032] After the test piece has been immersed in the test solution, it is washed with running water and then with deionized or distilled water. After the test piece has been washed, it is thoroughly dried and its mass is measured.
[0033] The area A (unit: dm 2 ), the mass m of the test piece before immersion in the test liquid 1 (unit: g) and the mass m of the test piece after immersion in the test liquid 2 (unit: g) and calculated the mass loss per unit area δ based on the following formula (1): A (unit: g / dm 2 ) can be calculated. A = (m 1 -m 2 ) / A...(1)
[0034] As mentioned above, the aluminum material has excellent corrosion resistance against corrosive gases, plasma, etc., and can suppress the occurrence of cracks in protective coatings even when temperatures rise. Therefore, the aluminum material is suitable for applications such as covers installed around fans in cooking appliances and components for semiconductor manufacturing equipment. More specifically, the aluminum material is suitable for use in, for example, chambers in semiconductor manufacturing equipment such as film deposition equipment and etching equipment, and components placed within the chambers. Examples of film deposition equipment include PVD (physical vapor deposition) equipment and CVD (chemical vapor deposition) equipment. Examples of etching equipment include dry etching equipment.
[0035] (Method for manufacturing an aluminum material) The method for manufacturing an aluminum material includes an anodizing treatment step of anodizing the base material to form an anodized film having pores on the base material, and a sealing step of immersing the base material in hot water to seal the pores in the anodized film, thereby forming the protective film on the base material. In addition, the product of the hot water temperature T (unit: °C) and the immersion time t (unit: hours) in the sealing step is more than 20°C-hours and less than 75°C-hours.
[0036] In the anodizing process, an anodic oxide film can be formed on the surface of the base material by passing a direct current between the base material and the counter electrode while they are immersed in an electrolyte. The anodic oxide film thus formed has a dense barrier layer formed on the base material and a porous layer formed on the barrier layer and having many pores. The barrier layer and the porous layer are composed of aluminum oxide such as alumina.
[0037] The electrolytic solution used in the anodizing treatment step may be, for example, an acidic electrolytic solution containing an electrolyte such as sulfuric acid or phosphoric acid, or may be an alkaline electrolytic solution containing an electrolyte such as sodium metaborate. From the viewpoint of more easily forming an anodized film having a desired structure in the anodizing treatment step and thus more easily forming the protective film, the electrolytic solution used in the anodizing treatment step is preferably an acidic electrolytic solution, more preferably an acidic electrolytic solution containing an inorganic acid as an electrolyte, and even more preferably an acidic electrolytic solution containing sulfuric acid as an electrolyte. Note that anions derived from the electrolyte may be incorporated into the anodized film formed on the surface of the aluminum material by the anodizing treatment step; for example, an anodized film containing sulfur derived from sulfate ions is formed in an anodizing treatment using sulfuric acid.
[0038] The current density of the direct current in the anodizing treatment is, for example, 1 mA / cm 2 20mA / cm or more 2 The temperature of the electrolytic solution in the anodizing treatment step can be appropriately set within the range of 0°C or higher and 40°C or lower.
[0039] The thickness of the anodic oxide film formed in the anodizing treatment step is preferably 2 μm or more. By making the thickness of the anodic oxide film 2 μm or more, it is possible to more easily make the thickness of the protective film after the sealing step 2 μm or more.
[0040] In the sealing step, the base material on which the anodized film was formed in the anodizing treatment step is immersed in hot water. When the anodized film is immersed in hot water, the aluminum oxide that constitutes the anodized film reacts with water to form a hydrated oxide. This hydrated oxide blocks the pores in the anodized film, and the anodized film becomes the protective film.
[0041] In the sealing process, the base material is immersed in hot water so that the product of the hot water temperature T (unit: °C) and the immersion time t (unit: hours) is greater than 20°C·hours and less than 75°C·hours, preferably 21°C·hours or more and 73°C·hours or less, and more preferably 23°C·hours or more and 71°C·hours or less. Immersing the base material in hot water so that the product of the hot water temperature and the immersion time is greater than 20°C·hours allows the aluminum oxide constituting the anodized film to react sufficiently with the hot water, thereby sufficiently blocking the pores in the anodized film. This allows the formation of a protective film with excellent corrosion resistance. If the product of the hot water temperature and the immersion time is less than 20°C·hours, the reaction between the aluminum oxide and the hot water is insufficient, resulting in insufficient pore blocking. This may result in a decrease in the corrosion resistance of the aluminum material. To more reliably obtain a protective coating having excellent corrosion resistance, the product of the hot water temperature and the immersion time is preferably 21°C·hours or more, and more preferably 23°C·hours or more.
[0042] On the other hand, if the product of the hot water temperature and the immersion time is too high, cracks may easily occur in the protective coating when the temperature of the aluminum material rises. This may be caused by excessive reaction between aluminum oxide and hot water. From the viewpoint of suppressing the occurrence of cracks in the protective coating and improving the heat resistance of the aluminum material, the product of the hot water temperature and the immersion time is set to less than 75°C-hours. From the same viewpoint, the product of the hot water temperature and the immersion time is preferably 73°C-hours or less, and more preferably 71°C-hours or less.
[0043] The temperature T of the hot water in the sealing step is preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher. By using high-temperature hot water in the sealing step, the immersion time required to achieve the desired degree of sealing can be easily shortened. As a result, the productivity of the aluminum material can be further improved. The upper limit of the temperature T of the hot water in the sealing step is 150°C. That is, in the sealing step, the base material may be immersed in boiling water, or superheated steam may be brought into contact with the base material.
[0044] The base material used in the anodizing treatment step may be produced by any method. For example, the method for producing an aluminum material may further include a casting step of producing an ingot made of aluminum or an aluminum alloy, a homogenization treatment step of homogenizing the ingot by holding it at a temperature of 500°C to 560°C for 5 hours to 10 hours, and a hot rolling step of hot rolling the ingot that has been subjected to the homogenization treatment at a temperature of 500°C to 560°C to produce the base material.
[0045] As a casting method in the casting step, for example, DC casting can be adopted. The thickness of the ingot obtained in the casting step is not particularly limited, but the ingot may have a thickness of, for example, 600 mm or more.
[0046] In the homogenization treatment step, the ingot obtained in the casting step is subjected to homogenization treatment by holding it at a temperature of 500° C. to 560° C. for 5 hours to 10 hours. By setting the holding temperature and holding time in the homogenization treatment within the above-mentioned specific ranges, the structure of the ingot can be sufficiently homogenized.
[0047] In the hot rolling process, the ingot that has been subjected to the homogenization treatment is hot rolled at a temperature of 500°C or higher and 560°C or lower. This allows a base material to be obtained. If the starting temperature in hot rolling is too low, the deformation resistance of the ingot increases, which may cause cracks in the ingot during rolling and lead to a decrease in productivity. On the other hand, if the starting temperature in hot rolling is too high, the ingot may locally melt due to heat generated during hot rolling.
[0048] In the manufacturing method, the base material obtained as described above may be subjected to an anodizing treatment step as it is. Furthermore, the manufacturing method may also include a heat treatment step of subjecting the base material to a heat treatment such as annealing, if necessary, after the hot rolling step and before the anodizing treatment step.
[0049] Furthermore, the manufacturing method may include a pretreatment step of pretreating the base material after the hot rolling step and before the anodizing step. Examples of pretreatments of the base material include degreasing treatments such as alkaline degreasing treatments, and polishing treatments such as mechanical polishing, chemical polishing, and electrolytic polishing. In the pretreatment step, one of the above-mentioned pretreatments may be performed alone, or two or more pretreatments may be appropriately combined, depending on the desired properties of the aluminum material.
[0050] When alkaline degreasing treatment is performed in the pretreatment step, the gloss of the anodized film obtained after anodizing treatment is reduced, and an aluminum material with a dull appearance can be obtained. Furthermore, when polishing treatment is performed in the pretreatment step, the gloss of the anodized film obtained after anodizing treatment is increased, and an aluminum material with a glossy appearance can be obtained. From the viewpoint of further increasing the gloss of the aluminum material, it is preferable to perform electrolytic polishing treatment on the base material in the pretreatment step.
[0051] An embodiment of the surface-treated aluminum material and its manufacturing method will be described with reference to Figures 1 to 3. As shown in Figure 1, the surface-treated aluminum material 1 of this embodiment has a base material 2 made of aluminum or an aluminum alloy, and a protective coating 3 containing oxides and hydrated oxides of aluminum and formed on at least a portion of the surface of the base material 2. The thickness of the protective coating 3 is 2 µm or more. When the mass ratios of elements in the protective coating 3 are analyzed in the depth direction by glow discharge optical emission spectroscopy, the integral value C of the mass ratio of aluminum atoms in the range from the surface of the protective coating 3 to a depth of 1 µm is Al The integral value C of the mass ratio of hydrogen atoms to H Ratio C H / C Al is 0.2 or more and 0.7 or less.
[0052] Table 1 shows specific examples of aluminum material 1 (test materials S1 to S5). Test materials S1 to S5 are manufactured, for example, as follows. First, an aluminum plate having a thickness of 1.1 mm and a chemical composition represented by alloy number A6016 is prepared as base material 2. This base material 2 is subjected to a pretreatment for anodizing. Specifically, as a pretreatment, base material 2 is first immersed in a sodium hydroxide aqueous solution with a concentration of 5% by mass and a temperature of 55°C to perform an alkali etching treatment. Subsequently, base material 2 is immersed in nitric acid with a concentration of 30% by mass to perform a desmutting treatment. Subsequently, base material 2 is immersed in a mixed solution of phosphoric acid and sulfuric acid at a volume ratio of phosphoric acid:sulfuric acid = 7:3 at a temperature of 85°C to perform a chemical polishing treatment. After the chemical polishing treatment, a desmutting treatment is again performed under the same conditions as described above.
[0053] After the base material 2 has been pretreated as described above, the base material 2 is anodized to form an anodic oxide film 30 on the surface of the base material 2. The electrolyte used in the anodizing treatment is a sulfuric acid aqueous solution with a concentration of 15% by mass, and the temperature of the electrolyte is 5°C. The current density in the anodizing treatment is 10 mA / cm 2The treatment time is 60 minutes. The anodic oxide film 30 formed in this manner is a so-called porous anodic oxide film, and as shown in Figure 2, it has a barrier layer 31 formed on the base material 2 and a porous layer 32 formed on the barrier layer 31 and having a large number of pores 321. The thickness of the anodic oxide film 30 formed by anodizing under the above-mentioned conditions is approximately 15 µm.
[0054] After anodizing, the base material is immersed in hot water under the conditions shown in Table 1 to perform a sealing treatment. In this manner, test materials S1 to S5 shown in Table 1 can be obtained. Note that test materials R1 to R3 shown in Table 1 are test materials for comparison with test materials S1 to S5. The manufacturing method for test materials R1 to R3 is the same as that for test materials S1 to S5, except that the hot water temperature and immersion time in the sealing treatment were changed as shown in Table 1.
[0055] Next, the evaluation methods for the various properties of test materials S1 to S5 and test materials R1 to R3 shown in Table 1 will be explained.
[0056] [Distribution of Hydrogen Atoms and Aluminum Atoms] After cleaning the surface of each test material, a glow discharge optical emission spectrometer ("GD750" manufactured by SPECTRUMA Analytik GmbH) was used to obtain a profile of the emission intensity of aluminum atoms and hydrogen atoms in the depth direction of the protective coating. The measurement conditions for the glow discharge optical emission spectrometer were an anode diameter of 2.5 mm, an output of 25 W, a gas pressure of 3.5 hPa, and an emission intensity capture interval of 0.2 to 0.24 seconds. Note that when measured under these conditions, the sputtering rate of the protective coating was approximately 50 to 90 nm / second.
[0057] The thus obtained profile of the emission intensity of aluminum atoms and hydrogen atoms in the depth direction is converted into a mass ratio profile based on a previously prepared calibration curve. Figure 3 shows an example of a profile of the mass ratio of hydrogen atoms in test material S1. The vertical axis of Figure 3 represents the mass ratio of hydrogen atoms (unit: mass%), and the horizontal axis represents the depth from the surface of the protective coating (unit: μm). In the profile thus obtained, the mass ratio of each atom is integrated over a range from the surface of the protective coating to a depth of 1 μm, and the integral value C of the mass ratio of hydrogen atoms is calculated. H and the integral value C of the mass ratio of aluminum atoms Al The integral value C of the mass ratio of hydrogen atoms obtained above is calculated. H The integral value C of the mass ratio of aluminum atoms Al By dividing by the ratio C H / C Al Calculate.
[0058] [Pore sealing degree of protective coating] A pore sealing degree test is carried out according to the method specified in JIS H8683-2:2013, and the mass loss per unit area of each test material is measured.
[0059] [Heat Resistance] Heat resistance is evaluated based on the exposure rate of the base material measured by the following method. First, the test material is heated for 4 hours in an oven set at 200°C. After removing the test material from the oven and cooling it to room temperature, an evaluation area is set on the protective coating, and the surface of the test material other than the evaluation area is covered with silicone resin.
[0060] Next, a 5% by weight NaCl aqueous solution and a 99.7% by weight acetic acid solution were prepared, and acetic acid was added to the NaCl aqueous solution so that the volume ratio of the NaCl aqueous solution to the acetic acid was 1000:1 to prepare a measurement solution. The test piece, counter electrode, and reference electrode electrically connected to the potentiostat were immersed in this solution and allowed to stand for 30 minutes to stabilize the potential of the measurement section. An Ag / AgCl electrode, for example, could be used as the reference electrode.
[0061] After the potential of the measurement section has stabilized, a voltage is applied between the test piece and the counter electrode using a potentiostat, and the potential of the measurement section is swept at a sweep rate of 20 mV / min until the potential of the measurement section reaches -2000 mV relative to the reference electrode. The polarization curve of the test material after heating is obtained by measuring the current density flowing through the measurement section at this time. In addition, the polarization curve of the base material is obtained by performing the same measurement using the base material after pre-treatment for anodizing using the method described above.
[0062] Next, the center of the potential region showing the hydrogen diffusion limiting current is determined in the polarization curve of the base material. Then, the current density at the center of the potential region is calculated. Furthermore, in the polarization curve of the heated test material, the current density at the same potential as the center of the potential region in the polarization curve of the base material is calculated.
[0063] The current density calculated based on the polarization curve of the heated test material can be used as an indicator of the contact area between the base material and the test solution in the heated test material, with a larger current density indicating a larger contact area between the base material and the test solution. Therefore, the ratio of the current density calculated using the heated test piece to the current density calculated using the base material can be used as an indicator of the increase in the exposed area of the base material due to heating. More specifically, for example, if defects such as cracks are formed in the protective coating of the heated test material, the cracks may expose the base material. Therefore, in this case, the current density ratio of the heated test material to the base material increases. Table 1 shows the current density ratios for each test material.
[0064]
[0065] As shown in Table 1, the test materials S1 to S5 were subjected to the sealing treatment so that the product of the hot water temperature and the immersion time in the sealing step was within the above-mentioned specific range. Therefore, the integral value C of the mass ratio of aluminum atoms in these test materials Al The integral value C of the mass ratio of hydrogen atoms to H Ratio C H / C Alis within the specified range. Furthermore, these test materials exhibit low mass loss in a sealing test and have excellent corrosion resistance against corrosive gases, plasma, etc. Furthermore, these test materials have a low current density ratio and can suppress the occurrence of cracks in the protective coating even when the temperature rises.
[0066] On the other hand, for test materials R1 and R3, the product of the hot water temperature and immersion time during the sealing treatment was higher than the specific range, so the hydration reaction between aluminum oxide and hot water proceeded excessively. Therefore, test materials R1 and R3 had a higher current density ratio than test materials S1 to S5, and were more likely to develop cracks when the temperature rose.
[0067] For test material R2, the product of the hot water temperature and immersion time during the sealing treatment was lower than the specified range, which resulted in insufficient sealing of the pores in the anodized coating. As a result, test material R2 experienced a higher mass loss in the sealing test than test materials S1 to S5, and was therefore inferior in corrosion resistance.
[0068] The above has described aspects of the surface-treated aluminum material and the method for manufacturing the same according to the present invention based on the examples, but the specific aspects of the surface-treated aluminum material and the method for manufacturing the same according to the present invention are not limited to the aspects of the examples, and the configuration can be changed as appropriate within the scope that does not impair the intent of the present invention.
Claims
1. A substrate made of aluminum or an aluminum alloy, and a protective film containing an oxide and a hydrated oxide of aluminum and formed on at least a part of the surface of the substrate, the protective film having a thickness of 2 μm or more, and when the mass ratio of elements in the protective film is analyzed in the depth direction by glow discharge optical emission spectrometry, the integral value C of the mass ratio of aluminum atoms in the range from the surface of the protective film to a depth of 1 μm is Al The integral value C of the mass ratio of hydrogen atoms to H Ratio C H / C Al A surface-treated aluminum material, wherein the refractive index is 0.2 or more and 0.7 or less.
2. When a sealing test was conducted according to the method specified in JIS H8683-2:2013, the mass loss per unit area was 0.2 g / dm 2 The surface-treated aluminum material according to claim 1, wherein:
3. A semiconductor manufacturing equipment component made of the surface-treated aluminum material according to claim 1 or 2.
4. A method for producing a surface-treated aluminum material as defined in claim 1 or 2, comprising: an anodizing treatment step of forming an anodized film having pores on the base material by anodizing the base material; and a sealing step of subsequently immersing the base material in hot water to seal the pores in the anodized film, thereby forming the protective film on the base material, wherein the product of the hot water temperature T [°C] and the immersion time t [hours] in the sealing step is more than 20°C-hours and less than 75°C-hours.