Oil-resistant paper, packaging material, and package
Patent Information
- Application Number
- MYPI2025005334
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-03-07
- Publication Date
- 2024-09-15
AI Technical Summary
Conventional non-fluorine-based oil-resistant papers lack sufficient high-temperature oil resistance and air permeability, making them unsuitable for packaging high-temperature foods like fried foods, and often require excessive coating which impairs air permeability.
Developing an oil-proof paper with a paper base material composed mainly of pulp, an oil-resistant agent composition containing hydrophobized starch, crosslinking agents, fatty acids, and fatty acid salts, where at least part of the composition is impregnated into the paper base material to achieve low air permeability and high-temperature oil resistance without forming a surface coating that impairs air permeability.
The solution results in oil-proof paper with excellent low air permeability and high-temperature oil resistance, suitable for packaging high-temperature foods, while maintaining air permeability to prevent steam buildup and ensuring the paper does not easily tear during processing.
Abstract
Description
Greaseproof paper, packaging materials and packages
[0001] This application claims priority from Japanese Patent Application No. 2023-040776, filed on March 15, 2023, the contents of which are incorporated herein by reference.
[0002] Grease-resistant paper, which is paper that has been given oil resistance using an oil-resistant agent, is used for packaging food and the like. Fluorine-based grease-resistant paper using a fluorine-based grease-resistant agent has traditionally been widely used as grease-resistant paper, but in recent years, in consideration of the environment and safety, non-fluorine-based grease-resistant paper using a non-fluorine-based grease-resistant agent has come to be used. Patent Documents 1 and 2 propose grease-resistant paper using hydrophobicized starch.
[0003] Japanese Patent Application Laid-Open No. 2002-69889 International Publication No. 2005 / 014930
[0004] Conventional non-fluorine-based oil-proofing agents do not repel oil like fluorine-based oil-proofing agents, but instead physically prevent oil by forming a coating layer on the paper. Therefore, conventional non-fluorine-based grease-resistant paper generally has a high air permeability (air resistance) and does not allow steam to escape, making it unsuitable for bags for fried foods, etc. The grease-resistant paper of Patent Document 1 also requires a large amount of coating to achieve sufficient oil resistance, which causes the same problem. Patent Document 2 uses a combination of hydrophobic starch, a crosslinking agent, and a fatty acid to achieve both low air permeability and oil resistance, and applies a coating amount of 0.5 to 20 g / m 2 However, the greaseproof paper of Patent Document 2 may not have sufficient oil resistance, particularly resistance to high-temperature (e.g., 180°C) oil (high-temperature oil resistance).
[0005] An object of the present invention is to provide a low-air-permeability greaseproof paper and packaging material that are excellent in high-temperature oil resistance, and a package using this packaging material.
[0006] The present invention has the following aspects. [1] Grease-resistant paper comprising a paper base material mainly composed of pulp and an oil-resistant composition containing hydrophobized starch adhered to the paper base material, wherein at least a portion of the oil-resistant composition is impregnated into the paper base material, the total content of a crosslinking agent, a fatty acid, a fatty acid salt, and a modified fatty acid being 0.8% by mass or less relative to the mass of the grease-resistant paper, and the air permeability being 30,000 seconds or less. [2] The grease-resistant paper according to [1], wherein the paper base material does not contain a sizing agent. [3] The grease-resistant paper according to [1] or [2], wherein the content of the crosslinking agent is 0.70% by mass or less relative to the mass of the grease-resistant paper. [4] The grease-resistant paper according to any one of [1] to [3], wherein the total content of the fatty acid, the fatty acid salt, and the modified fatty acid is 0.30% by mass or less relative to the mass of the grease-resistant paper. [5] The amount of the oil-resistant composition adhered to 1 m of the grease-resistant paper. 2 In terms of the mass of the hydrophobized starch per unit area, it is 1 to 20 g / m 2 [6] The greaseproof paper according to any one of [1] to [4], wherein the basis weight is 20 to 400 g / m 2 [7] The grease-resistant paper according to any one of [1] to [5], wherein the Canadian standard freeness of the pulp obtained by disintegrating the grease-resistant paper is 150 to 500 mL. [8] The grease-resistant paper according to any one of [1] to [7], wherein one or both of the paper base material and the oil-proofing composition contain the crosslinking agent. [9] The grease-resistant paper according to [8], wherein the crosslinking agent contains an epichlorohydrin-based crosslinking agent.
[10] A packaging material comprising the grease-resistant paper according to any one of [1] to [9].
[11] A package in which an article is packaged with the packaging material according to
[10] .
[0007] According to the present invention, it is possible to provide a low-air-permeability greaseproof paper and packaging material that are excellent in high-temperature oil resistance, and a package using this packaging material.
[0008] In this specification, the term "to" indicating a range of values means that the values before and after it are included as the lower and upper limits. The lower and upper limits of the ranges disclosed in this specification can be combined in any way to form new ranges.
[0009] <Grease-resistant paper> The grease-resistant paper according to one embodiment of the present invention comprises a paper substrate and an oil-proofing composition adhered to the paper substrate. The paper substrate is mainly composed of pulp. The oil-proofing composition contains hydrophobized starch. The paper substrate and the oil-proofing composition may each contain at least one selected from the group consisting of a crosslinking agent, a fatty acid, a fatty acid salt, and a modified fatty acid (hereinafter, these are also collectively referred to as "additive A"). Additive A, the paper substrate, and the oil-proofing composition will be described in detail later.
[0010] In greaseproof paper, at least a portion of the oilproofing composition is impregnated into the paper substrate. That is, at least a portion of the oilproofing composition is located inside the surface of the paper substrate. While a portion of the oilproofing composition may be located on the surface of the paper substrate, not all of the oilproofing composition is located on the surface of the paper substrate. If all of the oilproofing composition is located on the surface of the paper substrate, the surface of the paper substrate may be covered with a layer of the oilproofing composition, which may impair the low air permeability of the paper substrate. By impregnating at least a portion of the oilproofing composition into the paper substrate, the low air permeability of the paper substrate is less likely to be impaired. Greaseproof paper in which at least a portion of the oilproofing composition is impregnated into the paper substrate is typically obtained by applying a coating liquid containing the oilproofing composition and water to the paper substrate and drying it. Details will be described later. The oilproofing composition corresponds to the solid content of the coating liquid and does not include water.
[0011] The amount of oil-resistant composition attached to the oil-resistant paper is 2 1 to 20 g / m in terms of the mass of hydrophobized starch derived from the oil-proofing composition per unit area. 2 is preferred, and 1 to 10 g / m 2 More preferably, 2 to 6 g / m 2 When the amount of the oil-proofing composition deposited in terms of hydrophobicized starch is at least the above lower limit, the oil-proofing composition exhibits a sufficient effect of improving oil resistance, and when it is at most the above upper limit, the oil-resistant paper has better low air permeability and high-temperature oil resistance.
[0012] When the amount of the oil-proofing composition deposited in terms of hydrophobicized starch is within the above range, the thickness of the oil-proofing composition deposited on the fiber surface of the paper substrate is thought to be about 5 μm or less, but is not particularly limited. The thickness of the oil-proofing composition deposited on the fiber surface can be confirmed by microscopic observation of the fiber cross section.
[0013] The content of Additive A in the grease-resistant paper, i.e., the total content of the crosslinker, fatty acid, fatty acid salt, and modified fatty acid, is 0.8% by mass or less, preferably 0.7% by mass or less, and more preferably 0.6% by mass or less, relative to the mass of the grease-resistant paper. When the content of Additive A is equal to or less than the upper limit, high-temperature oil resistance is excellent. The lower limit of the content of Additive A is not particularly limited, and may be 0% by mass relative to the mass of the grease-resistant paper. In terms of oil resistance and operability, the content of Additive A is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, relative to the mass of the grease-resistant paper. The upper and lower limits can be appropriately combined. For example, it may be 0.1 to 0.8% by mass, 0.3 to 0.7% by mass, or 0.3 to 0.6% by mass.
[0014] The content of the crosslinking agent in Additive A is preferably 0.70% by mass or less, more preferably 0.6% by mass or less, and even more preferably 0.5% by mass or less, relative to the mass of the grease-resistant paper. When the content of the crosslinking agent is equal to or less than the upper limit, the high-temperature oil resistance is superior. The lower limit of the content of the crosslinking agent is not particularly limited and may be 0% by mass relative to the mass of the grease-resistant paper. When the grease-resistant paper contains a crosslinking agent, the content of the crosslinking agent is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, relative to the mass of the grease-resistant paper. The upper and lower limits can be combined as appropriate. For example, the content may be 0.01 to 0.70% by mass, 0.1 to 0.6% by mass, or 0.1 to 0.5% by mass.
[0015] The total content of the fatty acids, fatty acid salts, and modified fatty acids in additive A is preferably 0.30% by mass or less, more preferably 0.25% by mass or less, even more preferably 0.20% by mass or less, and particularly preferably 0.09% by mass or less, relative to the mass of the grease-resistant paper. When the total content of the fatty acids, fatty acid salts, and modified fatty acids is below the upper limit, the grease-resistant paper has excellent high-temperature oil resistance. Furthermore, the surface of the grease-resistant paper is non-slip, and the grease-resistant paper or packaging materials using the grease-resistant paper are less likely to collapse when stacked. The lower limit of the total content of the fatty acids, fatty acid salts, and modified fatty acids is not particularly limited, and may be 0% by mass relative to the mass of the grease-resistant paper. When the grease-resistant paper contains at least one selected from the group consisting of fatty acids, fatty acid salts, and modified fatty acids, the total content of the fatty acids, fatty acid salts, and modified fatty acids is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, relative to the mass of the grease-resistant paper. The upper and lower limits can be combined as appropriate. For example, it may be 0 to 0.30% by mass, 0.01 to 0.25% by mass, 0.05 to 0.20% by mass, or 0.05 to 0.09% by mass.
[0016] When the oil-proofing composition contains Additive A, the proportion of Additive A derived from the oil-proofing composition relative to 100 parts by mass of the paper substrate is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 1 part by mass, and even more preferably 0.1 to 0.8 parts by mass. When the proportion of Additive A derived from the oil-proofing composition is the above upper limit or less, the oil resistance tends to be excellent.
[0017] The air permeability of the grease-resistant paper is 30,000 seconds or less, preferably 20,000 seconds or less, more preferably 10,000 seconds or less, and even more preferably 5,000 seconds or less. The air permeability of the paper substrate is lower than that of the grease-resistant paper. When the air permeability of the grease-resistant paper is below the above upper limit, the paper substrate has low air permeability, so that the coating liquid containing the oil-proofing composition easily penetrates into the paper substrate. Therefore, a coating layer that significantly impairs air permeability is unlikely to be formed on the surface of the paper substrate, and oil resistance can be imparted while maintaining low air permeability. Furthermore, when the air permeability of the grease-resistant paper is below the above upper limit, steam can easily escape, making it applicable to packaging of high-temperature fried foods, etc. In terms of oil resistance, the air permeability of the grease-resistant paper is preferably 200 seconds or more, more preferably 500 seconds or more. The above upper limit and lower limit can be combined as appropriate. The air permeability is measured according to J. TAPPI Paper and Pulp Test Methods No. 5-2:2000 (Paper and paperboard - Smoothness and air permeability test methods - Part 2: Oken method). The air permeability of grease-resistant paper can be adjusted by the air permeability of the paper substrate, the amount of oil-proofing composition attached, the type of hydrophobic starch, etc. For example, the air permeability of grease-resistant paper tends to be lower when the amount of oil-proofing composition attached is smaller.
[0018] The basis weight of the greaseproof paper is 20 to 400 g / m 2 is preferred, and 25 to 100 g / m 2 More preferably, 30 to 70 g / m 2 is more preferable. When the basis weight of the grease-resistant paper is equal to or greater than the above lower limit, the tear strength of the grease-resistant paper is increased, making it less likely to break during processing, and improving processability. When the basis weight of the grease-resistant paper is equal to or less than the above upper limit, the entire paper substrate is easily impregnated with the oil-proofing agent composition. In addition, processing such as folding is easier, improving processability. The basis weight of the grease-resistant paper is measured in accordance with JIS P 8124:2011.
[0019] The Canadian Standard Freeness (hereinafter also referred to as "disaggregated freeness") of the pulp obtained by disaggregating the grease-resistant paper is preferably 150 to 500 mL, more preferably 200 to 400 mL, and even more preferably 250 to 350 mL. When the disaggregated freeness is within the above range, the grease-resistant paper has high tear strength and excellent processability. Furthermore, when the disaggregated freeness is equal to or greater than the above lower limit, the coating liquid containing the oil-proofing composition easily penetrates into the paper substrate, and the high-temperature oil resistance tends to be better. Disaggregation of the grease-resistant paper is carried out in accordance with JIS P 8220-1:2012. The Canadian Standard Freeness is measured in accordance with JIS P 8121-2:2012. The disaggregated freeness can be adjusted by the beating degree of the pulp.
[0020] The tear strength of the grease-resistant paper is preferably 150 mN or more, more preferably 180 mN or more, and even more preferably 200 mN or more. The higher the tear strength, the better, and there is no particular upper limit, but it is, for example, 3000 mN. When the tear strength is equal to or greater than the above lower limit, the grease-resistant paper has excellent processability. Tear strength is measured in accordance with JIS P 8116:2000. The tear strength of the grease-resistant paper can be adjusted by the tear strength of the paper substrate, the components of the coating liquid, etc. Note that grease-resistant paper coated with a coating liquid containing hydrophobic starch tends to have lower tear strength than the paper substrate before coating.
[0021] (Additive A) Additive A is at least one selected from the group consisting of a crosslinking agent, a fatty acid, a fatty acid salt, and a modified fatty acid. Additive A contributes to improving oil resistance when combined with hydrophobized starch. Hereinafter, fatty acids, fatty acid salts, and modified fatty acids are also collectively referred to as "fatty acids."
[0022] The crosslinking agent crosslinks hydrophobized starch particles with each other or between the hydrophobized starch and the cellulose in the paper substrate, thereby contributing to improving oil resistance and suppressing elution of the hydrophobized starch into water. The crosslinking agent is not particularly limited as long as it can crosslink the hydrophobized starch. Examples include epichlorohydrin-based crosslinking agents such as polyamide epichlorohydrin resin and epichlorohydrin, glyoxal, dialdehyde, polyacrolein, N-methylol urea, N-methylol melamine, activated vinyl compounds, various esters, and diisocyanates. Among these, epichlorohydrin-based crosslinking agents are preferred in terms of economic efficiency and their superior effect on food.
[0023] Examples of fatty acids include saturated fatty acids, unsaturated fatty acids, distilled fatty acids, and hardened fatty acids. The fatty acids may be vegetable or animal fatty acids. The carbon number of the fatty acid is, for example, 8 to 30. Examples of salts of fatty acid salts include sodium salts and potassium salts. Modified fatty acids include various fatty acids modified to impart functionality, such as fatty acids modified with epichlorohydrin-based agents (epichlorohydrin-based agent-modified fatty acids), fatty acid amides, and fatty acid esters. Examples of epichlorohydrin-based agents include epichlorohydrin. Here, "modified with epichlorohydrin-based agents" refers not only to fatty acids in which a structure derived from epichlorohydrin-based agents has been introduced, but also to fatty acids to which epichlorohydrin-based agents have been added in some form, such as when epichlorohydrin-based agents are used as dispersants for fatty acids. The fatty acids may also be fatty acid sizing agents. Fatty acid sizing agents include fatty acids, fatty acid salts, or modified fatty acids to which cationic fixing agents such as polyamine-based agents have been added, and some are epoxidized with epichlorohydrin-based agents. All of these are preferably used as fatty acids. As fatty acids, epichlorohydrin-based modified fatty acids are preferred because of their superior oil resistance. Additive A may be used alone or in combination of two or more.
[0024] (Paper base material) The paper base material is composed mainly of pulp. Here, "composed mainly of pulp" means that the pulp content of the paper base material is 70% by mass or more. The paper base material may be a commonly used paper, for example, a paper base material composed mainly of wood pulp. Specific examples of paper base materials include bleached kraft paper, unbleached kraft paper, fine paper, paperboard, liner paper, coated paper, one-side glazed paper, glassine paper, and graphene paper. Among these, bleached kraft paper, unbleached kraft paper, coated paper, and one-side glazed paper are preferred in terms of the heat sealability of the heat seal paper.
[0025] Examples of pulp include chemical pulps such as bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), bleached hardwood sulfite pulp (LBSP), and bleached softwood sulfite pulp (NBSP). Other examples include unbleached pulp, semi-bleached pulp, and bleached pulp such as stone ground pulp (GP), pressurized stone ground pulp (PGW), refiner ground pulp (RGP), chemi-ground pulp (CGP), thermomechanical pulp (TMP), and chemi-thermomechanical pulp (CTMP). Other examples include sulfite pulp and recycled paper pulp.
[0026] In order to improve printability, the pulp preferably contains hardwood pulp such as bleached hardwood kraft pulp (LBKP) or bleached hardwood sulfite pulp (LBSP). The content of the hardwood pulp is preferably 50% by mass or more, more preferably 70% by mass or more, and may be 100% by mass, based on the total mass of the pulp.
[0027] In order to increase tear strength, the pulp preferably contains softwood pulp such as bleached softwood kraft pulp (NBKP) or bleached softwood sulfite pulp (NBSP). The content of the softwood pulp is preferably 10% by mass or more, more preferably 50% by mass or more, and may be 100% by mass, based on the total mass of the pulp.
[0028] Hardwood pulp and softwood pulp may be used in combination. In the paper base material, the hardwood pulp content is preferably 0 to 90% by mass and the softwood pulp content is preferably 10 to 100% by mass, and more preferably 0 to 70% by mass and 30 to 100% by mass, based on the total mass of pulp.
[0029] The paper base material may contain additive A as an internal additive. When the paper base material contains additive A, additive A in the paper base material is preferably a crosslinking agent. Because crosslinking agents function as wet strength agents, adding a crosslinking agent to the paper base material can increase the wet strength of the paper base material. If the wet strength of the paper base material is low, the paper base material may tear when impregnated with an oil-proofing composition. As the crosslinking agent in the paper base material, an epichlorohydrin-based crosslinking agent is preferred, and a polyamide-epichlorohydrin resin is more preferred. The content of the crosslinking agent in the paper base material can be appropriately set within a range that does not exceed the above-mentioned upper limit of the content of additive A in the grease-resistant paper; for example, 0.1 to 0.7 parts by mass, and more preferably 0.2 to 0.6 parts by mass, per 100 parts by mass of pulp is preferred. When the crosslinking agent in the paper base material contains an epichlorohydrin-based crosslinking agent, the content of the epichlorohydrin-based crosslinking agent is preferably 50% by mass or more, more preferably 70% by mass or more, and may be 100% by mass, based on the total mass of the crosslinking agent in the paper base material. From the viewpoints of air permeability and ease of impregnation with the oil-proofing composition, it is preferable that the paper base material does not contain fatty acids.
[0030] The paper base material may further contain internal additives other than Additive A. Examples of internal additives other than Additive A include sizing agents, fillers, paper strength agents, retention aids, pH adjusters, drainage improvers, water-resistant agents, softeners, antistatic agents, antifoaming agents, slime control agents, dyes, and pigments.
[0031] The air permeability of the paper substrate is set so that the air permeability of the grease-resistant paper is 30,000 seconds or less. Since the application of an oil-proofing composition to the paper substrate increases the air permeability, from the viewpoint of keeping the air permeability of the grease-resistant paper below the upper limit, the air permeability of the paper substrate is preferably 10,000 seconds or less, more preferably 5,000 seconds or less, more preferably 1,000 seconds or less, even more preferably 500 seconds or less, and preferably 1 second or more, more preferably 10 seconds or more. The upper and lower limits can be appropriately combined. The air permeability of the paper substrate can be adjusted by the freeness of the pulp forming the paper substrate, the type and amount of internal additive, the basis weight, density, etc. of the paper substrate. For example, the higher the freeness of the pulp, the lower the air permeability tends to be. When a paper substrate does not contain a sizing agent, the air permeability tends to be lower than when a sizing agent is contained.
[0032] The paper substrate is preferably so-called unsized paper, which does not contain a sizing agent. If the paper substrate contains a sizing agent, the coating liquid does not penetrate easily when applied, so a coating layer is formed on the surface of the paper, which tends to increase the air permeability. On the other hand, the coating liquid easily penetrates unsized paper when applied, so the air permeability is not easily increased. Note that typical paper sizing agents are one or more of rosin-based sizing agents, alkyl ketene dimer-based sizing agents, and alkenyl succinic anhydride-based sizing agents. Therefore, unsized paper may be paper that does not contain a rosin-based sizing agent, an alkyl ketene dimer-based sizing agent, or an alkenyl succinic anhydride-based sizing agent.
[0033] The basis weight of the paper substrate is set in consideration of the basis weight of the greaseproof paper and the amount of the oil-proofing composition applied. From the viewpoint of keeping the basis weight of the greaseproof paper below the upper limit value, the basis weight of the paper substrate is set to 399 g / m 2 Preferably, 99 g / m or less 2 More preferably, 69 g / m or less 2 Further, from the viewpoint of increasing the tear strength of the greaseproof paper, it is more preferable that the thickness is 18 g / m or less. 2 More than 20 g / m 2 More preferably, 25 g / m or more 2 More preferably, 30 g / m or more 2The above upper limit and lower limit can be combined as appropriate.
[0034] (Oil-proofing composition) The oil-proofing composition contains a hydrophobized starch. The hydrophobized starch is starch that has been hydrophobized (hydrophobized). Examples of hydrophobization treatments include, but are not limited to, contacting starch with an aqueous organosilane solution in the presence of an alkali aluminate or alkali hydroxide, derivatizing starch with silicone or alkenyl, reacting starch with an organic acid anhydride such as octenylsuccinic anhydride or docecenylsuccinic anhydride, copolymerizing starch with a hydrophobic monomer such as acrylonitrile or a hydrophobic unsaturated monomer, imparting a hydrophobic group containing a hydrocarbon group to starch by etherification or esterification, and converting starch into alkyl succinate. Examples of starches that can be hydrophobized include, but are not limited to, tapioca starch, potato starch, corn starch, potato starch, wheat starch, and rice starch. The hydrophobic starch may be used alone or in combination of two or more kinds.
[0035] The oil-proofing composition may contain additive A. When the oil-proofing composition contains additive A, additive A contained in the paper substrate may be a crosslinking agent, a fatty acid, or both. When the oil-proofing composition contains additive A and additive A contains a crosslinking agent, the crosslinking agent is preferably an epichlorohydrin-based crosslinking agent, and more preferably a polyamide-epichlorohydrin resin. When the crosslinking agent in the oil-proofing composition contains an epichlorohydrin-based crosslinking agent, the content of the epichlorohydrin-based crosslinking agent is preferably 50% by mass or more, more preferably 70% by mass or more, and may even be 100% by mass, relative to the total mass of the crosslinking agent in the oil-proofing composition. When the oil-proofing composition contains additive A and additive A contains fatty acids, the fatty acids are preferably epichlorohydrin-based agent-modified fatty acids. When the fatty acids in the oil-proofing composition contain an epichlorohydrin-based agent-modified fatty acid, the content of the epichlorohydrin-based agent-modified fatty acid is preferably 50% by mass or more, more preferably 70% by mass or more, and may even be 100% by mass, based on the total mass of the fatty acids in the oil-proofing composition. Here, the total mass of the fatty acids is the total amount of the fatty acid, fatty acid salt, and modified fatty acid.
[0036] In a preferred embodiment, the oil-proofing composition comprises a hydrophobized starch and additive A, and additive A in the oil-proofing composition is a crosslinking agent. When additive A in the oil-proofing composition is a crosslinking agent, the high-temperature oil resistance tends to be better. It is thought that when the oil-proofing composition contains a crosslinking agent, the hydrophobized starch is easily crosslinked by the crosslinking agent, and elution of the hydrophobized starch is suppressed. Two or more crosslinking agents may be used in combination. In another preferred embodiment, the oil-proofing composition comprises a hydrophobized starch and additive A, and additive A in the oil-proofing composition is a fatty acid. When additive A in the oil-proofing composition is a fatty acid, the long-term oil resistance tends to be better. Two or more fatty acids may be used in combination.
[0037] The oil-proofing composition may further contain other components in addition to the hydrophobized starch and Additive A, as needed. Examples of such other components include a defoaming agent, a thickener, a water-retaining agent, and a pigment.
[0038] In the oil-proofing composition, the proportion of Additive A relative to 100 parts by mass of the hydrophobized starch is preferably 0.5 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and even more preferably 1 to 3 parts by mass. When the proportion of Additive A is equal to or greater than the above lower limit, the effects of Additive A are sufficiently exhibited, and when it is equal to or less than the above upper limit, excellent high-temperature oil resistance is achieved.
[0039] The total proportion of the hydrophobized starch and additive A relative to the total mass of the oil-proofing composition is preferably 50 mass% or more, more preferably 70 mass% or more, even more preferably 90 mass% or more, and may be 100 mass%.
[0040] (Method for producing greaseproof paper) The greaseproof paper according to this embodiment can be produced, for example, by applying a coating liquid containing an oilproofing composition and water to a paper substrate, followed by drying. The paper substrate and the oilproofing composition are as described above.
[0041] The paper substrate can be produced, for example, by making a wet paper using various paper machines, forming the wet paper, and drying it. The paper machine is not particularly limited. Examples include a Fourdrinier paper machine, a gap former paper machine, a cylinder paper machine, and a short wire paper machine. From the viewpoint of economy, a paper machine equipped with an on-machine coater is preferred.
[0042] To prepare a pulp slurry for papermaking, it is preferable to disaggregate the pulp and beat it using a refiner or beater to give the pulp appropriate flexibility and fluffiness. However, the pulp beating method is not particularly limited. The preferred range of disaggregated freeness, which is an index of the degree of beating of the pulp, is as described above. The beaten pulp may be mixed with an internal additive such as Additive A as needed, and dispersed in water to prepare a pulp slurry with a concentration suitable for papermaking. If the paper base material is unsized paper, no sizing agent is mixed.
[0043] The wet paper obtained by the paper machine is preferably dried using a multistage cylinder dryer, an air dryer or a Yankee dryer.
[0044] The coating solution can be prepared by mixing the materials constituting the oil-proofing agent composition with water. The coating method for the coating solution is not particularly limited, and various commonly available coating machines can be used. Examples of coating machines include blade coaters, air knife coaters, roll coaters, reverse roll coaters, bar coaters, curtain coaters, slot die coaters, gravure coaters, champlex coaters, brush coaters, slide bead coaters, two-roll size press coaters, pond size press coaters, rod metering size press coaters, blade metering size press coaters, short dwell coaters, gate roll coaters, and calendar nip coaters. Among these, on-machine coating machines are preferred from the viewpoint of productivity. Examples of on-machine coating machines that are preferred include blade coaters, bar coaters, gate roll coaters, rod metering size press coaters, blade metering size press coaters, and pond size press coaters. The coating solution may be applied to one or both sides of the paper substrate. From the viewpoint of oil resistance, it is preferable to coat both sides. The coating amount of the coating liquid is determined taking into consideration the amount of oil-proofing agent composition adhered. 2 In terms of the mass of hydrophobized starch per unit area, it is 1 to 20 g / m 2 is preferred, and 1 to 10 g / m 2 More preferably, 2 to 6 g / m 2 When the oil-proofing composition contains Additive A, the coating amount of the coating solution is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 1 part by mass, and even more preferably 0.1 to 0.8 parts by mass, calculated as the proportion of Additive A in the oil-proofing composition per 100 parts by mass of the paper substrate.
[0045] The greaseproof paper may be subjected to a smoothing treatment as needed. The smoothing treatment can be carried out on-machine or off-machine using a normal smoothing treatment device such as a super calender, gloss calender, or soft calender. The paper substrate may be subjected to a smoothing treatment before the coating liquid is applied, as long as the effects of the invention are not impaired.
[0046] The resulting greaseproof paper is wound into a roll, after which both ends of the roll may be removed using a slitter to adjust the width of the greaseproof paper to the width of the processing machine in the subsequent process.
[0047] The uses of the greaseproof paper are not particularly limited, but examples thereof include packaging materials and lining papers, and it is particularly suitable as a packaging material.
[0048] <Packaging Material> A packaging material according to one embodiment of the present invention comprises the greaseproof paper of the present invention. The greaseproof paper may be used as the packaging material as is, or may be processed to form a packaging material. Known processing methods can be applied as the processing. Examples of packaging materials made from processed greaseproof paper include bags such as gusset bags, single-opening bags, flat bags, and square-bottom bags, as well as various other containers.
[0049] Examples of items packaged with the packaging material include foods such as fried foods, confectionery, and bread, and desiccants. Among these, foods are preferred, and oil-containing foods such as fried foods and bread are more preferred, with oil-containing foods that are packaged at high temperatures (e.g., 90 to 180°C) and oil-containing foods that are heated to high temperatures after packaging being particularly preferred.
[0050] <Package> A package according to one embodiment of the present invention is a package in which an article is packaged with the packaging material of the present invention. Examples of the article include the same articles as those described above. As the packaging method, a known packaging method can be applied.
[0051] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following descriptions. "Parts" and "%" represent "parts by mass" and "% by mass", respectively.
[0052] (Example 1) <Production of paper base material> Pulp consisting of 60% by mass of LBKP and 40% by mass of NBKP was blended with 0.4% of an internal additive paper strength agent (trade name: Polystron OFT-5, manufactured by Arakawa Chemical Industries, Ltd.) based on the bone-dry mass of the pulp, 0.4% of a wet strength agent (epichlorohydrin-based crosslinking agent (polyamide epichlorohydrin resin), trade name: WS4024, manufactured by Seiko PMC Co., Ltd.) based on the bone-dry mass of the pulp, and 1% of aluminum sulfate based on the bone-dry mass of the pulp, and the resulting mixture was passed through a paper machine to produce a paper base material with a basis weight of 40 g / m. 2The paper base material was obtained by forming the pulp into a paper substrate. The degree of beating of the pulp was adjusted so that the resulting greaseproof paper had a disintegration freeness of 220 mL. The basis weight was measured in accordance with JIS P 8124:2011 (the same applies below).
[0053] <Preparation of Coating Solution> A coating solution (solid content concentration 15%) was prepared by dispersing hydrophobized starch (trade name: Filmkote 370, manufactured by Ingredion) and a crosslinking agent (epichlorohydrin-based crosslinking agent (polyamide epichlorohydrin resin), trade name: WS4024, manufactured by Seiko PMC Corporation) in water at a solid content ratio of 99:1.
[0054] <Coating> The coating liquid is applied to both sides of the paper substrate so that the coating amount after drying (total for both sides) is 4.6 g / m 2 The amount of the coating solution after drying corresponds to the amount of the oil-proofing agent composition adhered in terms of solid content.
[0055] Example 2 Grease-resistant paper was obtained in the same manner as in Example 1, except for the following changes to the paper base material: <Production of paper base material> Pulp consisting of 70% by mass of LBKP and 30% by mass of NBKP was blended with 0.4% of an internal additive paper strength agent (trade name: Polystron TS-1, manufactured by Arakawa Chemical Industries, Ltd.) based on the bone-dry mass of the pulp, 0.4% of a crosslinking wet strength agent (trade name: WS4024, manufactured by Seiko PMC Co., Ltd.) based on the bone-dry mass of the pulp, and 1% of aluminum sulfate based on the bone-dry mass of the pulp, and the resulting paper was processed on a paper machine to have a basis weight of 40 g / m. 2 The degree of beating of the pulp was adjusted so that the resulting grease-resistant paper had a disintegration freeness of 320 mL.
[0056] (Example 3) Grease-resistant paper was obtained in the same manner as in Example 2, except that the preparation of the coating liquid was changed as follows: <Preparation of Coating Liquid> A coating liquid (solid concentration 15%) was prepared by dispersing hydrophobic starch (trade name: Fikmkote 370, manufactured by Ingredion) and fatty acids (fatty acids modified with epichlorohydrin-based agents, trade name: PT8124, manufactured by Seiko PMC) in water at a solid content ratio of 99:1.
[0057] (Example 4) The production of the paper substrate was changed as follows, and the coating liquid was applied so that the coating amount after drying (total for both sides) was 5.0 g / m 2 Oil-resistant paper was obtained in the same manner as in Example 3, except that the coating was performed so that the resulting paper was 70% by mass of LBKP and 30% by mass of NBKP. A paper strength agent (trade name: Polystron TS-1, manufactured by Arakawa Chemical Industries, Ltd.) was blended as an internal additive in an amount of 0.4% based on the bone-dry mass of the pulp, a wet strength agent (trade name: WS4024, manufactured by Seiko PMC Co., Ltd.) was blended in an amount of 0.5% based on the bone-dry mass of the pulp as a crosslinking agent, and aluminum sulfate was blended in an amount of 1% based on the bone-dry mass of the pulp. The paper was then passed through a paper machine to produce a paper having a basis weight of 40 g / m. 2 The degree of beating of the pulp was adjusted so that the resulting grease-resistant paper had a disintegration freeness of 320 mL.
[0058] Example 5 Grease-resistant paper was obtained in the same manner as in Example 4, except that the preparation of the coating liquid was changed as follows: <Preparation of Coating Liquid> A coating liquid (solid concentration 15%) was prepared by dispersing only hydrophobicized starch (trade name: Fikmkote 370, manufactured by Ingredion) in water.
[0059] Example 6 Grease-resistant paper was obtained in the same manner as in Example 5, except that the preparation of the paper base material was changed as follows: <Preparation of paper base material> A paper strength agent (trade name: Polystron TS-1, manufactured by Arakawa Chemical Industries, Ltd.) was blended as an internal additive in an amount of 0.4% based on the bone-dry mass of the pulp, and aluminum sulfate was blended in an amount of 1% based on the bone-dry mass of the pulp, and the paper was processed on a paper machine to obtain a paper with a basis weight of 40 g / m. 2 The degree of beating of the pulp was adjusted so that the resulting grease-resistant paper had a disintegration freeness of 320 mL.
[0060] Comparative Example 1 Greaseproof paper was obtained in the same manner as in Example 1, except that the preparation of the paper base material was changed as follows: <Preparation of Paper Base Material> Pulp consisting of 80% by mass of LBKP and 20% by mass of NBKP was blended with 0.3% by bone-dry mass of pulp of a sizing agent (rosin-based sizing agent, product name: Sizepine G, manufactured by Arakawa Chemical Industries, Ltd.) as an internal additive, 1.4% by bone-dry mass of pulp of a cationized starch (product name: P-3E, manufactured by Pillar Starch Co., Ltd.), 0.4% by bone-dry mass of a wet strength agent (product name: WS4024, manufactured by Seiko PMC Co., Ltd.) as a crosslinking agent, and 1.0% by bone-dry mass of aluminum sulfate, and the resulting paper was passed through a paper machine to obtain a paper with a basis weight of 50 g / m. 2 The degree of beating of the pulp was adjusted so that the resulting greaseproof paper had a disintegration freeness of 140 mL.
[0061] Comparative Example 2 Grease-resistant paper was obtained in the same manner as in Example 1, except that the preparation of the coating liquid was changed as follows: <Preparation of Coating Liquid> A coating liquid (solid concentration 15%) was prepared by dispersing hydrophobicized starch (trade name: Filmkote 370, manufactured by Ingredion), a crosslinking agent (trade name: WS4024, manufactured by Seiko PMC), and a fatty acid (trade name: PT8124, manufactured by Seiko PMC) in water to a solid content ratio of 86.4:8.6:5.
[0062] Comparative Example 3 Grease-resistant paper was obtained in the same manner as in Comparative Example 1, except that the coating liquid was changed to the same one as in Comparative Example 2.
[0063] (Evaluation) The obtained greaseproof paper was subjected to the following measurements and evaluations. The results are shown in Table 1.
[0064] <Measurement of Air Permeability> The air permeability of the greaseproof paper was measured in accordance with J. TAPPI Paper and Pulp Test Methods No. 5-2:2000 (Paper and paperboard - Smoothness and air permeability test methods - Part 2: Oken method).
[0065] <Measurement of disintegrated freeness> Greaseproof paper was disintegrated in accordance with JIS P 8220-1, and the freeness (Canadian standard freeness) of the obtained pulp was measured in accordance with JIS P 8121-2:2012, and the value was taken as the disintegrated freeness.
[0066] <Evaluation of Oil Resistance (Kit)> The oil resistance (Kit) of the oil-resistant paper was evaluated in accordance with "Paper and paperboard - Oil repellency test method - Kit method" specified in J. TAPPI No. 41:2000.
[0067] <Evaluation of high-temperature oil resistance> Salad oil at 180°C was dropped onto greaseproof paper and wiped off after 15 seconds. The greaseproof paper was then visually inspected and the high-temperature oil resistance was evaluated according to the following criteria: ○: No stains. ○-: Dotted stains present. △: Round marks from the oil droplets remain. ×: Oil bleeds through to the other side.
[0068] <Evaluation of long-term oil resistance> Salad oil at 25°C (room temperature) was dropped onto greaseproof paper and wiped off after 24 hours. The greaseproof paper was then visually inspected and the long-term oil resistance was evaluated according to the following criteria: ○: No stains. ○-: Dotted stains present. △: Round marks from the oil droplets remain. ×: Oil bleeds through to the other side.
[0069] <Evaluation of static friction coefficient> The static friction coefficient between greaseproof papers was measured in accordance with ISO 15359. The static friction coefficient was determined as the average of the first and third measurements.
[0070]
[0071] The grease-resistant papers of Examples 1 to 6 had low air permeabilities of 30,000 seconds or less. They also had excellent high-temperature oil resistance, and good oil resistance (kit) at room temperature and long-term oil resistance. In particular, the grease-resistant papers of Examples 1 to 2 and 5 to 6, which did not contain fatty acids, had a high static friction coefficient and excellent surface slip resistance. On the other hand, the grease-resistant paper of Comparative Example 1, which used the same coating liquid as Examples 1 and 2 but changed the paper substrate to a sized one, had high air permeability. It also had poor oil resistance (kit), high-temperature oil resistance, and long-term oil resistance. The grease-resistant paper of Comparative Example 2, which used the same paper substrate as Example 1 but increased the content of Additive A in the coating liquid to exceed 0.8% by mass, had poor high-temperature oil resistance. The grease-resistant paper of Comparative Example 3, which used the same coating liquid as Comparative Example 2 but changed the paper substrate to a sized one, had high air permeability. In addition to high-temperature oil resistance, it also had poor oil resistance (kit) and long-term oil resistance.
[0072] According to the present invention, it is possible to provide a low-air-permeability greaseproof paper and packaging material that are excellent in high-temperature oil resistance, and a package using this packaging material.
Claims
1. A grease-resistant paper having a paper base material whose main component is pulp, and an grease-resistant composition containing hydrophobized starch adhered to the paper base material, in which at least a portion of the grease-resistant composition has impregnated the paper base material, the total content of a crosslinking agent, a fatty acid, a fatty acid salt and a modified fatty acid being 0.8 mass% or less relative to the mass of the grease-resistant paper, and the air permeability being 30,000 seconds or less.
2. The greaseproof paper according to claim 1, wherein the paper base material does not contain a sizing agent.
3. An oil-resistant paper as described in claim 1 or 2, wherein the content of the crosslinking agent is 0.70 mass% or less relative to the mass of the oil-resistant paper.
4. An grease-resistant paper as described in claim 1 or 2, wherein the total content of the fatty acid, the fatty acid salt and the modified fatty acid is 0.30 mass% or less relative to the mass of the grease-resistant paper.
5. The amount of the oil-resistant composition adhered to the oil-resistant paper is 2 The weight of the hydrophobized starch per unit area is 1 to 20 g / m 2 The greaseproof paper according to claim 1 or 2, 6. Basis weight: 20-400g / m 2 The greaseproof paper according to claim 1 or 2, 7. The greaseproof paper according to claim 1 or 2, wherein the pulp obtained by disintegrating the greaseproof paper has a Canadian standard freeness of 150 to 500 ml / L.
8. The grease-resistant paper according to claim 1 or 2, wherein either or both of the paper substrate and the grease-resistant composition contain the crosslinking agent.
9. The grease-resistant paper according to claim 8, wherein the crosslinking agent comprises an epichlorohydrin-based crosslinking agent.
10. A packaging material comprising the greaseproof paper according to claim 1 or 2.
11. A package in which an article is packaged with the packaging material according to claim 10.