Hot-dip al-zn alloy coated steel sheet and method of producing same

MYPI2025005349A0Undetermined Publication Date: 2024-10-14JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005349
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2023-11-14
Publication Date
2024-10-14

AI Technical Summary

Technical Problem

Hot-dip Al-Zn plated steel sheets face challenges in achieving stable and excellent workability and corrosion resistance, particularly due to the presence of impurities like Mg, which can lead to cracking and reduced corrosion resistance in processed parts.

Method used

A hot-dip Al-Zn plated steel sheet with a plating film composition of 45-65% Al, 1.0-3.0% Si, and ≤0.3% Mg, where the MgZn2 and Mg2Zn11 phases are minimized or eliminated, and additional elements like B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce, and Bi are added in controlled amounts to enhance stability and corrosion resistance, along with a specific heat treatment process to improve ductility and workability.

Benefits of technology

The solution provides a hot-dip Al-Zn plated steel sheet with improved workability and corrosion resistance, reducing the occurrence of cracks and maintaining high corrosion resistance even under severe processing conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005349_DRAWING_001
    Figure PI2025005349_DRAWING_001
Patent Text Reader

Abstract

Provided is a coated steel sheet having good adhesion between a chemical conversion coating and a primer coating film and excellent corrosion resistance at processed parts and cut edges. In the present disclosure, the coating has a chemical composition containing Al: 45 mass% to 65 mass% and Si: 1.0 mass% to 3.0 mass%, with the balance being Zn and inevitable impurities, the Mg content is 0.3 mass% or less with respect to the total mass of the coating, and the diffraction intensities of MgZn₂ and Mg₂Zn₁₁ in the coating measured by X-ray diffraction satisfy the following relational expressions (1) and (2): MgZn₂ (100) = 0 ...(1) Mg₂Zn₁₁ (321) = 0 ...(2).
Need to check novelty before this filing date? Find Prior Art

Description

Hot-dip Al-Zn plated steel sheet and its manufacturing method

[0001] The present invention relates to a hot-dip Al-Zn coated steel sheet having consistently excellent workability and corrosion resistance at worked portions, and a method for producing the same.

[0002] Hot-dip Al-Zn-coated steel sheets, typified by 55% Al-Zn, are known to exhibit high corrosion resistance among hot-dip galvanized steel sheets because they combine the sacrificial corrosion protection of Zn with the high corrosion resistance of Al, as disclosed in Patent Document 1, for example. Therefore, due to their excellent corrosion resistance, hot-dip Al-Zn-coated steel sheets are primarily used in the fields of building materials, such as roofs and walls, which are exposed outdoors for long periods of time, and in the fields of civil engineering and construction, such as guardrails, wiring and piping, and soundproof walls. In particular, demand for hot-dip Al-Zn-coated steel sheets has been increasing in recent years due to the growing demand for materials with excellent corrosion resistance and maintenance-free materials in more severe operating environments, such as acid rain caused by air pollution, the use of deicing agents to prevent road ice in snowy areas, and coastal area development.

[0003] The coating of hot-dip Al-Zn coated steel sheets is composed of dendritic regions (α-Al phases) where Al containing supersaturated Zn has solidified, and a Zn-Al eutectic structure present in the interdendritic spaces (interdendrites), with the α-Al phases stacked in multiple layers in the thickness direction of the coating. This unique coating structure creates a complex corrosion path from the surface, making corrosion less likely to progress. It is also known that hot-dip Al-Zn coated steel sheets offer superior corrosion resistance compared to hot-dip galvanized steel sheets with the same coating thickness.

[0004] Generally, hot-dip Al-Zn-coated steel sheets are manufactured by using thin steel sheets obtained by hot-rolling or cold-rolling slabs as the base steel sheet, and then subjecting the base steel sheet to recrystallization annealing and hot-dip coating in the annealing furnace of a continuous hot-dip coating facility. In addition to predetermined concentrations of Al and Zn, the coating bath typically contains Si to suppress excessive growth of the interfacial alloy layer formed at the interface between the base steel (base steel sheet) and the coating. This Si function allows the thickness of the interfacial alloy layer of hot-dip Al-Zn-coated steel sheets to be controlled to approximately 1 to 5 μm. Given the same coating thickness, the thinner the interfacial alloy layer, the thicker the main layer, which exhibits high corrosion resistance. Therefore, suppressing the growth of the interfacial alloy layer is known to lead to improved corrosion resistance.

[0005] It is known that when hot-dip Al-Zn-plated steel sheets are bent or otherwise processed, cracks can occur in the plating film at the processed area depending on the degree of processing (degree of processing). In hot-dip Al-Zn-plated steel sheets, the thick interfacial alloy layer serves as the crack initiation point, and the interdendrites in the plating film act as the crack propagation path. Therefore, even when the same degree of processing is performed, the cracks tend to open relatively large compared to hot-dip galvanized steel sheets with the same plating film thickness. Therefore, in applications with a high degree of processing, there are problems such as the occurrence of large cracks visible to the naked eye, which mars the appearance, and the cracked areas, where the substrate steel is exposed, have significantly reduced corrosion resistance compared to crack-free areas (decreased corrosion resistance in processed areas).

[0006] In order to solve these problems of workability and corrosion resistance of worked portions, for example, Patent Documents 2 and 3 disclose methods for manufacturing hot-dip Al-Zn-plated steel sheets in which the workability is improved by subjecting the hot-dip Al-Zn-plated steel sheets to a predetermined heat treatment.

[0007] Japanese Patent Publication No. 46-7161 Japanese Patent Publication No. 61-28748 Japanese Patent Application Laid-Open No. 2002-275646 Japanese Patent Application Laid-Open No. 2004-285387 Special Publication No. 2016-540885

[0008] However, even when heat treatments such as those disclosed in Patent Documents 2 and 3 are performed, the hot-dip Al-Zn-plated steel sheet does not necessarily exhibit excellent formability due to, for example, the inclusion of impurities in the plating film. Therefore, further improvements have been desired in order to stably obtain excellent formability and corrosion resistance in the processed portion.

[0009] In the production of hot-dip galvanized steel sheets, it is generally known that impurities inevitably get mixed into the plating bath, and hot-dip Al-Zn plating is no exception. Impurities that get mixed into the plating film include Fe, Cr, Ni, Cu, Co, W, Mg, and Ca, which are mixed in through impurities contained in the plating raw materials or leaching from the base steel sheet or bath-immersed equipment. These elements inevitably get mixed into the plating film. In particular, in recent years, the production volume of highly corrosion-resistant hot-dip Zn-Al-Mg-coated steel sheets and hot-dip Al-Zn-Si-Mg-coated steel sheets has increased. The widespread distribution of Zn raw materials containing high concentrations of Mg, produced by recycling dross generated during the production process, has led to the frequent inclusion of Mg as an impurity in the plating bath and, ultimately, the plating film.

[0010] As described above, unavoidable impurities in a galvanized coating can cause deterioration in the properties of hot-dip galvanized steel sheets, such as their appearance, corrosion resistance, and workability. The presence or absence of an impurity's effect is often determined by the composition and impurity concentration of the coating. In other words, even impurities of the same composition may be harmful to the properties of the galvanized steel sheet, but not harmful. Therefore, the effects of impurities on the properties of each hot-dip galvanized steel sheet have been investigated, and techniques for controlling the impurity concentration have been developed to stably obtain the required properties. For example, Patent Document 4 discloses a hot-dip galvanized steel sheet with excellent appearance, which contains, by mass, 0.10 to 0.6% Al, 0.03 to 0.3% Bi, and the remainder Zn and unavoidable impurities, with the Pb, Sn, and Cd contents each controlled to 0.002%. Furthermore, Patent Document 5 discloses a hot-dip Zn-Al-Mg coated steel sheet having excellent corrosion resistance, which contains 4.4 to 5.6% Al, 0.3 to 0.56% Mg, and the balance being Zn and unavoidable impurities, and in which the inclusion of Ni as one of the unavoidable impurities is controlled so as not to occur.

[0011] However, the techniques disclosed in Patent Documents 4 and 5 focus on improving corrosion resistance, and do not fully consider the influence of unavoidable impurities on formability and corrosion resistance of worked portions in Mg-free hot-dip Zn-Al-plated steel sheets or hot-dip Al-Zn-plated steel sheets with a high Al concentration. Therefore, there has been a demand for the development of a technique that can more reliably and stably achieve excellent formability and corrosion resistance of worked portions.

[0012] In view of the above circumstances, an object of the present invention is to provide a hot-dip Al-Zn coated steel sheet that reliably and stably has excellent workability and corrosion resistance at the worked portion, and a method for producing the same.

[0013] As a result of investigations to solve the above problems, the present inventors have noticed that it is important to control the concentration and state of existence of Mg contained as an optional component or unavoidable impurity in the hot-dip Al-Zn-plated steel sheet. In particular, it is important to keep the Mg content low and to control the MgZn2 and Mg2Zn 11 It has been discovered that by eliminating this, excellent workability and corrosion resistance of the processed part can be reliably and stably obtained.

[0014] The present invention was made based on the above findings, and its gist is as follows: 1. A hot-dip Al-Zn plated steel sheet having a plating film, wherein the plating film has a composition containing 45 to 65 mass% Al and 1.0 to 3.0 mass% Si, with the balance consisting of Zn and unavoidable impurities, the Mg content relative to the total mass of the plating film is 0.3 mass% or less, and the MgZn2 and Mg2Zn in the plating film 11 A hot-dip Al-Zn coated steel sheet characterized in that the diffraction intensity of MgZn2 (100) = 0 (1) Mg2Zn 11 (321) = 0 ... (2) MgZn2 (100): Diffraction intensity of the (100) plane of MgZn2 (plane spacing d = 0.4510 nm), Mg2Zn 11 (321): Mg2Zn 111. The hot-dip Al-Zn coated steel sheet according to item 1 above, characterized in that the plating film further contains one or more elements selected from B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce, and Bi in a total amount of 0.01 to 3.0 mass%. 2. The hot-dip Al-Zn coated steel sheet according to item 1 above, characterized in that the content of unavoidable impurities in the plating film is 5.0 mass% or less in total. 3. The hot-dip Al-Zn coated steel sheet according to item 1 or 2 above, characterized in that the content of Mg in the unavoidable impurities in the plating film is 0.3 mass% or less, relative to the total mass of the plating film.

[0015] 5. A method for producing a hot-dip Al-Zn-plated steel sheet having a plating film, comprising: forming the plating film on a substrate steel sheet using a plating bath having a composition containing 45 to 65 mass% Al and 1.0 to 3.0 mass% Si, with the balance being Zn and unavoidable impurities, in which the Mg content relative to the total mass of the plating bath is controlled to 0.3 mass% or less; and when reheating the steel sheet on which the plating film has been formed, the maximum temperature to be reached, that is, a heating temperature T, is set to 130 to 300°C, and after heating, the average cooling rate C (°C / hr) from the heating temperature T (°C) to 100°C satisfies the following relationship (3): C≦(T-100) / 2 ... (3) 6. 6. The method for producing a hot-dip Al-Zn coated steel sheet according to item 5 above, characterized in that the coating bath further contains one or more elements selected from B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce, and Bi in a total amount of 0.01 to 3.0 mass%. 7. The hot-dip Al-Zn coated steel sheet according to item 5 or 6 above, characterized in that the content of unavoidable impurities in the coating bath is 5.0 mass% or less in total. 8. The hot-dip Al-Zn coated steel sheet according to any of items 5 to 7 above, characterized in that the content of Mg among the unavoidable impurities in the coating bath is 0.3 mass% or less, based on the total mass of the coating bath.

[0016] According to the present invention, it is possible to provide a hot-dip Al-Zn coated steel sheet having excellent workability and corrosion resistance at worked portions reliably and stably, and a method for producing the same.

[0017] 1 is an enlarged schematic view of a cross section of a hot-dip Al-Zn plated steel sheet according to an embodiment of the present invention.

[0018] (Hot-dip Al-Zn-plated steel sheet) As shown in Fig. 1, the hot-dip Al-Zn-plated steel sheet of the present invention comprises a plating film 20 on the surface of a base steel sheet 10. The plating film 20 has a main layer 21 and an interfacial alloy layer 22 formed at the interface between the main layer and the base steel sheet 10. The plating film 20 has a composition containing 45 to 65 mass% Al and 1.0 to 3.0 mass% Si, with the balance being Zn and unavoidable impurities.

[0019] The Al content in the plating film is 45 to 65 mass%, preferably 50 to 60 mass%, to balance corrosion resistance and operational efficiency. This is because an Al content of at least 45 mass% in the plating film causes dendritic solidification of Al, resulting in a plating film structure primarily composed of an α-Al phase dendritic solidification structure. The dendritic solidification structure is layered in the thickness direction of the plating film, which complicates the corrosion progression path and improves the corrosion resistance of the plating film itself. Furthermore, the more α-Al phase dendritic portions are layered, the more complex the corrosion progression path becomes, making it more difficult for corrosion to reach the substrate steel sheet, thereby improving corrosion resistance. Therefore, the Al content in the plating film is preferably 50 mass% or more. On the other hand, if the Al content in the plating film exceeds 65 mass%, most of the Zn changes to a structure in solid solution in the α-Al, making it impossible to suppress the dissolution reaction of the α-Al phase, and the corrosion resistance of the hot-dip Al-Zn plating film deteriorates. For this reason, the Al content in the plating film must be 65 mass % or less, and preferably 60 mass % or less.

[0020] The Si content in the plating film is primarily intended to suppress the growth of Fe-Al and / or Fe-Al-Si interfacial alloy layers at the interface with the substrate steel sheet, thereby preventing deterioration of the adhesion between the plating film and the steel sheet. When a steel sheet is immersed in an Al-Zn plating bath containing Si, an alloying reaction occurs between the Fe on the steel sheet surface and the Al and Si in the bath, resulting in the formation of an Fe-Al and / or Fe-Al-Si intermetallic compound layer at the interface between the substrate steel sheet and the plating film. Since the growth rate of the Fe-Al-Si alloy is slower than that of the Fe-Al alloy, a higher proportion of the Fe-Al-Si alloy suppresses the growth of the entire interfacial alloy layer. Therefore, the Si content in the plating film must be 1.0% by mass or more. On the other hand, if the Si content in the plating film exceeds 3.0% by mass, not only does the effect of suppressing the growth of the interfacial alloy layer saturate, but the presence of excess Si in the plating film also reduces workability. Therefore, the Si content is limited to 3.0% or less.

[0021] The plating film contains Zn and unavoidable impurities. Among these, the unavoidable impurities include Fe. This Fe is inevitably contained in the plating film due to dissolution of the steel sheet or bath-immersed equipment into the plating bath, and is also supplied by diffusion from the base steel sheet during the formation of the interfacial alloy layer. The Fe content in the plating film is typically approximately 0.3 to 2.0 mass%. Other unavoidable impurities include Cr, Ni, Cu, Co, W, Mg, and Ca. These elements are inevitably contained in the plating film due to dissolution into the plating bath from the base steel sheet, stainless steel bath-immersed equipment, and WC-based and Co-Cr-W-based thermal spray coatings applied to bath-immersed equipment; they are contained as impurities in the metal ingots used as raw materials for the plating bath; and they are produced using pots or bath-immersed equipment previously used to produce plated steel sheets to which these elements were intentionally added.

[0022] The total content of unavoidable impurities in the plating film is not particularly limited, but if contained in excess, various properties of the plated steel sheet may be affected, so the total content is preferably 5.0 mass% or less, and more preferably 1.0 mass% or less.

[0023] The hot-dip Al-Zn-plated steel sheet of the present invention requires that the Mg content in the plating film be 0.3 mass% or less relative to the total mass of the plating film. Since Mg contained in the plating film may deteriorate the workability and corrosion resistance of the processed portion of the hot-dip Al-Zn-plated steel sheet, the deterioration of the workability and corrosion resistance of the processed portion can be suppressed by appropriately controlling the Al, Zn, and Si contents in the plating film and then reducing the Mg content. From the same perspective, the Mg content in the plating film is preferably 0.1 mass% or less relative to the total mass of the plating film. Note that the hot-dip Al-Zn-plated steel sheet of the present invention may contain Mg as an optional component as long as the Mg content is 0.3 mass% or less relative to the total mass of the plating film. However, from the viewpoint of more reliably suppressing deterioration in the workability and corrosion resistance of the processed portion of the hot-dip Al-Zn-plated steel sheet, it is preferable that the plating film not contain Mg as an optional component. That is, the Mg content in the unavoidable impurities of the plating film is preferably 0.3 mass% or less, and more preferably 0.1 mass% relative to the total mass of the plating film. Thus, the lower the Mg content in the plating film, the better the corrosion resistance of the hot-dip Al-Zn-plated steel sheet of the present invention, so there is no particular lower limit. However, since it is technically difficult to achieve a Mg content of exactly 0.000 mass% in the plating film, the lower limit of the Mg content in the plating film is essentially about 0.001 mass%.

[0024] In the hot-dip Al-Zn coated steel sheet of the present invention, MgZn2 and Mg2Zn 11 The diffraction intensity of the MgZn2 (100) = 0 (1) Mg2Zn 11 (321) = 0 ... (2) MgZn2 (100): Diffraction intensity of the (100) plane of MgZn2 (plane spacing d = 0.4510 nm), Mg2Zn 11 (321): Mg2Zn 11 Diffraction intensity of the (321) plane (plane spacing d = 0.2290 nm)

[0025] By containing a small amount of Mg in the plating film, MgZn2 and Mg2Zn 11 may be generated, and the intermetallic compounds MgZn2 and Mg2Zn 11 Generally, these intermetallic compounds are hard and brittle. Therefore, if such intermetallic compounds are present in the plated film, they may become the starting point for cracks when subjected to severe bending or stretching, which may cause deterioration in the workability and corrosion resistance of the hot-dip Al-Zn plated steel sheet. Therefore, as described above, it is necessary to keep the Mg content in the plated film low, and to use MgZn2 and Mg2Zn as shown in the above relational expressions (1) and (2). 11 By forming a plating film free of these elements, it is possible to more reliably and stably improve the workability and the corrosion resistance of the processed portion.

[0026] Here, in the above relationships (1) and (2), MgZn 2 (100) is the diffraction intensity of the (100) plane of MgZn2 (plane spacing d = 0.4510 nm), and Mg2Zn 11 (321) is Mg2Zn 11 The diffraction intensity of the (321) plane (plane spacing d = 0.2290 nm) of MgZn 2 (100) and Mg2Zn 11 The (321) plane can be measured by mechanically scraping off a portion of the plating film, powdering it, and then subjecting it to X-ray diffraction (powder X-ray diffraction measurement). The diffraction intensity was measured using the MgZn 2 Diffraction peak intensity of Mg2Zn, corresponding to interplanar spacing d = 0.2290 nm 11 The diffraction peak intensity can be measured.

[0027] The amount of plating film required for powder X-ray diffraction measurement (amount of plating film to be scraped off) is precisely determined by the MgZn 2 (100) and Mg2Zn 11From the viewpoint of measuring (321), 0.1 g or more is sufficient, and 0.3 g or more is preferable. Furthermore, when the plating film is scraped off, steel sheet components other than the plating film may be contained in the powder, but these intermetallic compound phases are contained only in the plating film and do not affect the above-mentioned peak intensity. Furthermore, the reason for powdering the plating film and performing X-ray diffraction is that when X-ray diffraction is performed on a plating film formed on a plated steel sheet, it is affected by the plane orientation of the plating film solidification structure, making it difficult to obtain peak intensities corresponding to the amount of material present.

[0028] Here, there are no particular limitations on the method for satisfying the above-mentioned relationship (1) and relationship (2). For example, by controlling the Mg content in the plating film to be low and reducing the ratio of the Mg content to the Zn content (for example, by setting Mg / Zn to 0.008 or less, preferably 0.006 or less), MgZn2 and Mg2Zn 11 Abundance of MgZn 2 (100) and Mg2Zn 11 The diffraction intensity of (321) can be controlled to be low.

[0029] Furthermore, other than the method of controlling the Mg content in the plating film, the above relationships (1) and (2) can also be satisfied by controlling the Mg content in the plating film to a specific value and then adjusting the conditions for forming the plating film (e.g., cooling conditions after plating).

[0030] The plating film may further contain 0.01 to 3.0 mass% in total of one or more elements selected from B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce, and Bi. These elements have the effect of improving the stability of corrosion products when the plating film corrodes, thereby delaying the progression of corrosion, and the effect of stabilizing the spangle size on the plating surface, thereby improving the surface appearance.

[0031] In addition, the coating weight of the plating film is set to 45 to 120 g / m per side from the viewpoint of satisfying various characteristics. 2 It is preferable that the coating weight of the plating film is 45 g / m 2In the above cases, sufficient corrosion resistance can be obtained for applications requiring long-term corrosion resistance, such as building materials, and the coating weight of the plating film is 120 g / m 2 This is because, in the following cases, it is possible to achieve excellent corrosion resistance while suppressing the occurrence of plating cracks during processing. From the same viewpoint, the coating weight of the plating film is 45 to 100 g / m 2 It is more preferable that:

[0032] The coating weight of the plating film can be determined, for example, by a method described in JIS H 0401:2013, in which a specific area of ​​the plating film is dissolved and stripped using a mixture of hydrochloric acid and hexamethylenetetramine, and the weight of the steel sheet is calculated from the difference between before and after stripping. To determine the coating weight per side using this method, the plating surface on the non-target side can be sealed with tape to prevent exposure, and then the dissolution process described above can be performed. Similarly to the coating weight described above, the composition of the plating film can be determined by immersing the plating film in a hydrochloric acid solution or the like to dissolve it, and then analyzing the resulting solution using ICP emission spectroscopy, atomic absorption spectroscopy, or the like. This method is merely an example, and any method that can accurately quantify the composition of the plating film may be used, and is not particularly limited.

[0033] The coating film on the hot-dip Al-Zn coated steel sheet obtained according to the present invention has a composition generally equivalent to that of the coating bath, and therefore the composition of the coating film can be controlled with high precision by controlling the composition of the coating bath.

[0034] Furthermore, the base steel sheet constituting the hot-dip Al-Zn-plated steel sheet of the present invention is not particularly limited, and cold-rolled steel sheets, hot-rolled steel sheets, etc. can be used as appropriate depending on the required performance and specifications. Furthermore, the method for obtaining the base steel sheet is also not particularly limited. For example, in the case of the hot-rolled steel sheet, a steel sheet that has been subjected to a hot-rolling process and a pickling process can be used, and in the case of the cold-rolled steel sheet, a steel sheet can be produced by further adding a cold-rolling process. Furthermore, in order to obtain the desired steel sheet properties, a recrystallization annealing process or the like can also be performed before the hot-dip plating process.

[0035] As shown in FIG. 1 , the hot-dip Al-Zn-plated steel sheet of the present invention has a plating film 20 formed on a base steel sheet 10. If necessary, an intermediate layer or a coating film can be further formed on the plating film. The type of coating film and the method for forming the coating film are not particularly limited and can be appropriately selected depending on the required performance. Examples of methods include roll coating, curtain flow coating, and spray coating. A coating film can be formed by applying an organic resin-containing paint and then heating and drying it using means such as hot air drying, infrared heating, and induction heating. The intermediate layer is not particularly limited as long as it is formed between the plating film of the hot-dip Al-Zn-plated steel sheet and the coating film. Examples include a chemical conversion coating and a primer such as an adhesive layer. The chemical conversion coating can be formed, for example, by a chromate treatment or a chromium-free chemical conversion treatment, in which a chromate treatment solution or a chromium-free chemical conversion treatment solution is applied, followed by drying at a steel sheet temperature of 80 to 300°C without rinsing with water. These chemical conversion coatings may be single-layer or multi-layer, and in the case of multi-layer, multiple chemical conversion treatments may be carried out in sequence.

[0036] (Method for producing hot-dip Al-Zn plated steel sheet) The method for producing a hot-dip Al-Zn plated steel sheet of the present invention is a method for producing a hot-dip Al-Zn plated steel sheet having a plating film.

[0037] The method for producing a hot-dip Al-Zn-plated steel sheet of the present invention includes a step of forming the plating film on a substrate steel sheet using a plating bath having a composition containing 45 to 65 mass% Al, 1.0 to 3.0 mass% Si, with the balance being Zn and unavoidable impurities, in which the Mg content relative to the total mass of the plating bath is controlled to 0.3 mass% or less.

[0038] The step of forming the plating film is not particularly limited except for the conditions of the plating bath, which will be described later. For example, the steel sheet can be produced by cleaning, heating, and immersing the base steel sheet in a plating bath using continuous hot-dip plating equipment. In the steel sheet heating step, recrystallization annealing or the like is performed to control the structure of the base steel sheet itself, and heating in a reducing atmosphere, such as a nitrogen-hydrogen atmosphere, is effective in preventing oxidation of the steel sheet and reducing the trace oxide film present on the surface.

[0039] The plating bath used in the step of forming the plating film contains 45 to 65 mass % Al, 1.0 to 3.0 mass % Si, and the remainder Zn and unavoidable impurities, because, as described above, the composition of the plating film as a whole is approximately the same as the composition of the plating bath.

[0040] The method for producing a hot-dip Al-Zn-plated steel sheet according to the present invention is characterized in that the Mg content relative to the total mass of the coating bath is controlled to 0.3 mass% or less. As described above, Mg contained in the coating film may deteriorate the workability and corrosion resistance of the processed portion of the hot-dip Al-Zn-plated steel sheet. Therefore, by appropriately controlling the contents of Al, Zn, and Si in the coating bath and then reducing the Mg content, deterioration of the workability and corrosion resistance of the processed portion can be suppressed.

[0041] Furthermore, the Mg content in the coating bath needs to be controlled to 0.3 mass% or less, preferably 0.1 mass% or less, based on the total mass of the coating bath. If the Mg content in the coating bath is 0.3 mass% or less, the resulting hot-dip Al-Zn-plated steel sheet can have sufficiently excellent formability and corrosion resistance in the processed area. If the Mg content in the coating bath is 0.1 mass% or less, even better formability and corrosion resistance in the processed area can be achieved. Thus, the lower the Mg content in the coating bath, the better the corrosion resistance of the hot-dip Al-Zn-plated steel sheet. Therefore, there is no particular lower limit for the Mg content. However, because it is technically difficult to achieve a Mg content of exactly 0.000 mass% in the coating bath, the lower limit for the Mg content in the coating is essentially about 0.001 mass%.

[0042] The means for reducing the Mg content in the coating bath is not particularly limited. For example, it is effective to not intentionally add Mg to the coating bath, or not to use pots or bath-immersed equipment used in the production of coated steel sheets, such as Zn-Al-Mg-coated steel sheets or Al-Zn-Si-Mg-coated steel sheets, to which Mg is intentionally added, in the production of hot-dip Al-Zn-coated steel sheets. This is because it is possible to prevent Mg-containing metal chunks adhering to the pot or bath-immersed equipment from dissolving and being mixed into the coating bath. Another means for reducing the Mg content in the coating bath is to preferably use metal chunks with a low Mg content among impurities as a raw material for the coating bath.

[0043] The bath temperature of the coating bath is not particularly limited, but is preferably in the range of (melting point + 20°C) to 650°C. The reason why the lower limit of the bath temperature is set to melting point + 20°C is that the bath temperature needs to be at or above the solidification point in order to perform hot-dip coating, and setting the temperature to melting point + 20°C prevents solidification due to a local drop in the bath temperature of the coating bath. On the other hand, the reason why the upper limit of the bath temperature is set to 650°C is that if the temperature exceeds 650°C, it becomes difficult to rapidly cool the coating film, and there is a risk that the interfacial alloy layer formed between the coating film and the steel sheet will become thick.

[0044] Furthermore, the temperature of the base steel sheet immersed in the coating bath (immersion sheet temperature) is not particularly limited, but from the viewpoint of ensuring coating characteristics in the continuous hot dip coating operation and preventing changes in bath temperature, it is preferable to control it to within ±20°C of the coating bath temperature.

[0045] Furthermore, the immersion time of the substrate steel sheet in the coating bath is preferably 0.5 seconds or more. This is because if it is less than 0.5 seconds, there is a risk that a sufficient coating film will not be formed on the surface of the substrate steel sheet. There is no particular upper limit to the immersion time, but if the immersion time is longer, there is a risk that the interfacial alloy layer formed between the coating film and the steel sheet will become thick, so it is more preferable to keep it within 8 seconds.

[0046] Furthermore, the manufacturing method of the hot-dip Al-Zn-plated steel sheet of the present invention is characterized in that when the steel sheet on which the plating film is formed is reheated, the heating temperature T, which is the maximum temperature to be reached, is set to 130 to 300°C, and after heating, the average cooling rate C (°C / hr) from the heating temperature T (°C) to 100°C satisfies the following relationship (3): C≦(T−100) / 2 (3) This is because applying a heat treatment that satisfies the above condition softens the plating film and improves its ductility, thereby making it possible to impart excellent workability to the hot-dip Al-Zn-plated steel sheet.

[0047] Generally, solidification of the coating during the production of hot-dip Al-Zn-coated steel sheets proceeds in a non-equilibrium state with a high cooling rate. As a result, the α-Al phase in the coating is supersaturated with Zn, resulting in a hard, low-ductility hot-dip Al-Zn-coated coating. By subjecting the hot-dip Al-Zn-coated coating in this state to the heat treatment (heating), the strain accumulated in the coating at the time of solidification is released, solid-state diffusion occurs within the coating, and the two-phase separation of Al and Zn progresses. In other words, the solid content of Zn in the α-Al phase of the heat-treated hot-dip Al-Zn-coated steel sheet is reduced, resulting in a softer coating and higher ductility, thereby imparting excellent formability and corrosion resistance to the processed parts.

[0048] In the heating step, the heating temperature T is 130 to 300°C. If the heating temperature T is less than 130°C, the rate of solid diffusion is low, so that two-phase separation does not proceed sufficiently, and the softening of the plating film does not occur sufficiently. On the other hand, if the heating temperature T exceeds 300°C, the growth of the alloy phase at the interface between the base steel sheet and the plating film is promoted, which actually has a negative effect on workability. Therefore, the heating temperature T is set to a range of 130 to 300°C. From the same viewpoint, the heating temperature T is preferably 130 to 200°C.

[0049] Furthermore, after the heating step, cooling is performed so that the average cooling rate C (°C / hr) from the heating temperature T (°C) to 100°C satisfies the relationship (3) above in order to promote the two-phase separation of Al and Zn. Because solid-state diffusion of Al and Zn continues during the cooling process, ensuring a sufficient cooling time to satisfy relationship (3) effectively promotes the two-phase separation of Al and Zn. On the other hand, if the average cooling rate C (°C / hr) is greater than (T-100) / 2, the two-phase separation of Al and Zn is insufficient, resulting in insufficient softening of the plating film and insufficient workability and corrosion resistance of the processed part.

[0050] The heat treatment for providing the silencing heating and the subsequent heat retention can be performed using a heating or heat retention device installed inside or outside the continuous hot-dip plating equipment. Continuous heating can be performed in-line using a heating mechanism (e.g., induction heater, hot air stove, etc.) installed inside the continuous hot-dip plating equipment, or batch heating can be performed offline after coiling. Continuous heating can also be performed using a heating mechanism (e.g., induction heater, hot air stove, etc.) in continuous processing equipment outside the plating line. Furthermore, the plated steel sheet continuously heated in the plating line or the continuous processing equipment can be appropriately heat-retained or heated after coiling. Furthermore, a heat retention device can be installed to retain the heat and slowly cool the plated film during the cooling process after solidification of the hot-dip plated metal. However, there are no particular limitations on the type, shape, size, etc. of the heating or heat retention device, as long as it can impart the above-mentioned thermal history to the plated film.

[0051] In the method for producing a hot-dip Al-Zn-plated steel sheet of the present invention, in addition to the above-mentioned plating film formation step and the temperature-raising, heating, and cooling steps after plating film formation, it is possible to appropriately carry out steps that are employed in the production of ordinary plated steel sheets.

[0052] [Samples 1 to 37] A cold-rolled steel sheet having a thickness of 0.8 mm, produced by a conventional method, was used as a base steel sheet, and annealing and plating were performed using a hot-dip galvanizing simulator manufactured by Rhesca Corporation, to produce hot-dip galvanized steel sheet samples 1 to 37 under the conditions shown in Table 1. The composition of the coating bath used in producing the hot-dip galvanized steel sheets was varied within the ranges of Al: 0.2 to 70 mass%, Si: 0.0 to 3.2 mass%, B: 0.00 to 0.02 mass%, Ca: 0.0 to 1.0 mass%, Ti: 0.0 to 0.1 mass%, V: 0.1 to 0.1 mass%, Cr: 0.0 to 0.2 mass%, Mn: 0.0 to 0.1 mass%, Sr: 0.0 to 0.1 mass%, Mo: 0.0 to 0.1 mass%, In: 0.0 to 0.5 mass%, Sn: 0.0 to 0.1 mass%, Sb: 0.0 to 0.1 mass%, Ce: 0.0 to 1.0 mass%, and Bi: 0.00 to 0.05 mass% so as to obtain the composition of the coating of each sample shown in Table 1. The bath temperature of the coating was controlled to 460°C when the Al content was 0.2 to 5% by mass, 600°C when the Al content was 35 to 55% by mass, and 660°C when the Al content was over 60% by mass, so that the temperature of the substrate steel sheet entering the coating was the same as the coating bath temperature. Furthermore, when the Al content was 35 to 70% by mass, the coating was carried out under the condition that the sheet was cooled to a temperature range of 520 to 500°C in 3 seconds. The coating weight of the coating was 85±5 g / m per side for Samples 1 to 34. 2 , and sample 35: 50±5 g / m per side 2 , and sample 36: 100±5 g / m per side 2 , and sample 37 is 125±5 g / m per side 2 Furthermore, after the above plating treatment, samples 1 to 37, except for sample 16, were subjected to a predetermined thermal history (heating, heating, and cooling) in a heating furnace. The thermal history conditions are shown in Table 1.

[0053] [Evaluation] Each sample of the obtained hot-dip plated steel sheet was evaluated as follows. The evaluation results are shown in Table 1.

[0054] (1) Plating film (composition, coating amount, MgZn2 and Mg2Zn 11(X-ray diffraction intensity of 100 mm diameter) For each sample of the prepared plated steel sheet, a 100 mm diameter cut was punched out, and the non-measurement surface was sealed with tape. The plating was then dissolved and stripped using a mixture of hydrochloric acid and hexamethylenetetramine as specified in JIS H 0401:2013. The coating mass was calculated from the mass difference between the sample before and after stripping. The resulting coating mass is shown in Table 1. The stripping solution was then filtered, and the filtrate and solids were analyzed separately. Specifically, the filtrate was subjected to ICP atomic emission spectroscopy to quantify components other than insoluble silicon. The solids were dried and incinerated in a heating furnace at 650°C, and then melted by adding sodium carbonate and sodium tetraborate. The melt was then dissolved in hydrochloric acid, and the solution was subjected to ICP atomic emission spectroscopy to quantify insoluble silicon. The silicon concentration in the plating film was calculated by adding the soluble silicon concentration obtained from the filtrate analysis to the insoluble silicon concentration obtained from the solids analysis. The compositions of the resulting plating films are shown in Table 1. Each sample was sheared to a size of 100 mm x 100 mm, and the plating film on the surface to be evaluated was mechanically scraped off until the steel substrate was exposed. The resulting powder was thoroughly mixed, and 0.3 g of the powder was then subjected to qualitative analysis using an X-ray diffraction apparatus (Rigaku Corporation, "SmartLab") under the following conditions: Cu-Kα X-ray (wavelength = 1.54178 Å), Kβ ray removal: Ni filter, tube voltage: 40 kV, tube current: 30 mA, scanning speed: 4° / min, sampling interval: 0.020°, divergence slit: 2 / 3°, Soller slit: 5°, and detector: high-speed one-dimensional detector (D / teX Ultra). The intensity obtained by subtracting the base intensity from each peak intensity was taken as the diffraction intensity (kcps). 11 The diffraction intensity of the (321) plane (plane spacing d = 0.2290 nm) was measured. The measurement results are shown in Table 1.

[0055] (2) Workability Evaluation Each sample of the obtained hot-dip galvanized steel sheet was sheared to a size of 70 mm x 150 mm, and then n sheets (n = 4, 5, 6, 7, 8) of the same thickness were sandwiched inside each other, and each sample was bent 180° (nT bend) to obtain a 150 mm apex. Cellotape (registered trademark) was firmly attached to the outer surface of the bent portion after bending and then peeled off. The outer surface (apex) of the bent portion was observed with a scanning electron microscope (ULTRA55 manufactured by Carl Zeiss) at an accelerating voltage of 5 kV to confirm the form of cracks, and the workability was evaluated according to the following criteria. The evaluation results are shown in Table 1. ◯: No large cracks with an opening width of 20 μm or more were observed. ×: Large cracks with an opening width of 20 μm or more were observed.

[0056] (3) Evaluation of corrosion resistance of processed parts Each sample of the obtained hot-dip galvanized steel sheet was sheared to a size of 70 mm x 150 mm, and then each edge was sealed with tape. Six or eight sheets of the same thickness were sandwiched inside, and 6T and 8T bending was performed to obtain a 150 mm apex. Each sample prepared as described above was subjected to the Japanese Automotive Standards Combined Cycle Test (JASO-CCT). The accelerated corrosion test started from wet conditions and continued for 60 cycles. After that, the appearance of the outer surface (apex) of the bent part of each sample was visually inspected and evaluated according to the following criteria. The evaluation results are shown in Table 1. ◯: No red rust or white rust was observed in the 8T bent sample. ×: Red rust or white rust was observed in the 8T bent sample.

[0057]

[0058] The results in Table 1 show that the samples of the invention have a good balance of workability and corrosion resistance of the worked portion compared to the samples of the comparative examples.

[0059] According to the present invention, it is possible to provide a hot-dip Al-Zn coated steel sheet having excellent workability and corrosion resistance at worked portions reliably and stably, and a method for producing the same.

[0060] REFERENCE SIGNS LIST 10 Base steel sheet 20 Plating film 21 Main layer 22 Interface alloy layer 211 Dendrite 212 Interdendrite

Claims

1. A hot-dip Al-Zn plated steel sheet having a plating film, wherein the plating film contains 45-65 mass% Al and 1.0-3.0 mass% Si, with the balance being Zn and unavoidable impurities, the Mg content relative to the total mass of the plating film is 0.3 mass% or less, and the MgZn2 and Mg2Zn 11 The diffraction intensity of the above-mentioned hot-dip Al-Zn-coated steel sheet as measured by the X-ray diffraction method satisfies the following relationships (1) and (2). 11 (321)=0 ・・・(2) MgZn2 (100): Diffraction intensity of the (100) plane of MgZn2 (plane spacing d=0.4510 nm), Mg2Zn 11 (321): Mg2Zn 11 Diffraction intensity of the (321) plane (plane spacing d = 0.2290 nm) 2. The hot-dip Al-Zn plated steel sheet according to claim 1, characterized in that the plating film further contains 0.01 to 3.0 mass% in total of one or more elements selected from B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce, and Bi.

3. The hot-dip Al-Zn plated steel sheet according to claim 1 or 2, characterized in that the content of unavoidable impurities in the plated film is 5.0 mass% or less in total.

4. The hot-dip Al-Zn plated steel sheet according to any one of claims 1 to 3, characterized in that the Mg content in unavoidable impurities in the plating film is 0.3 mass% or less relative to the total mass of the plating film.

5. A method for producing a hot-dip Al-Zn plated steel sheet having a plating film, comprising forming the plating film on a base steel sheet using a plating bath containing 45-65 mass% Al and 1.0-3.0 mass% Si, with the balance being Zn and unavoidable impurities, and in which the Mg content relative to the total mass of the plating bath is controlled to 0.3 mass% or less, the heating temperature T, which is the maximum temperature reached when reheating the steel sheet on which the plating film has been formed, is set to 130-300°C, and the average cooling rate C (°C / hr) from the heating temperature T (°C) to 100°C after heating satisfies the following relationship (3): C≦(T-100) / 2 ... (3) 6. The method for producing a hot-dip Al-Zn coated steel sheet according to claim 5, characterized in that the coating bath further contains 0.01 to 3.0 mass% in total of one or more elements selected from B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce, and Bi.

7. A method for producing hot-dip Al-Zn plated steel sheet as described in claim 5 or 6, characterized in that the content of unavoidable impurities in the plating bath is 5.0 mass% or less in total.

8. A method for producing hot-dip Al-Zn plated steel sheet according to any one of claims 5 to 7, characterized in that the Mg content in the unavoidable impurities in the plating bath is 0.3 mass% or less based on the total mass of the plating bath.