Hot-dip al-zn alloy coated steel sheet and method of producing same

MYPI2025005350A0Undetermined Publication Date: 2024-10-14JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005350
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2023-11-14
Publication Date
2024-10-14

AI Technical Summary

Technical Problem

Hot-dip Al-Zn plated steel sheets face issues with workability and corrosion resistance due to cracks during processing, primarily caused by the thick interfacial alloy layer and Mg-Zn compounds in the plating film, which deteriorate the appearance and corrosion resistance of processed parts.

Method used

Control the composition of the plating film by adjusting Al, Zn, and Si content, and limit Mg content to less than 0.5% by mass, with Mg-Zn compounds having a long axis less than 10 μm, and optionally include additional elements like B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, and Bi to enhance stability and corrosion resistance.

Benefits of technology

The controlled composition and size of Mg-Zn compounds in the plating film significantly improve the workability and corrosion resistance of processed parts, reducing crack formation and maintaining excellent corrosion resistance, even under harsh environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005350_DRAWING_001
    Figure PI2025005350_DRAWING_001
Patent Text Reader

Abstract

Provided is a hot-dip Al-Zn alloy coated steel sheet having stably excellent workability and corrosion resistance at processed parts. In the present disclosure, the coating has a chemical composition containing Al: 45 mass% to 65 mass% and Si: 1.0 mass% to 3.0 mass%, with the balance being Zn and inevitable impurities, and the Mg content in the inevitable impurities is less than 0.5 mass% with respect to the total mass of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Hot-dip Al-Zn plated steel sheet and its manufacturing method

[0001] The present invention relates to a hot-dip Al-Zn coated steel sheet having consistently excellent workability and corrosion resistance at worked portions, and a method for producing the same.

[0002] Hot-dip Al-Zn-coated steel sheets, typified by 55% Al-Zn, are known to exhibit high corrosion resistance among hot-dip galvanized steel sheets because they combine the sacrificial corrosion protection of Zn with the high corrosion resistance of Al, as disclosed in Patent Document 1, for example. Therefore, due to their excellent corrosion resistance, hot-dip Al-Zn-coated steel sheets are primarily used in the fields of building materials, such as roofs and walls, which are exposed outdoors for long periods of time, and in the fields of civil engineering and construction, such as guardrails, wiring and piping, and soundproof walls. In particular, demand for hot-dip Al-Zn-coated steel sheets has been increasing in recent years due to the growing demand for materials with excellent corrosion resistance and maintenance-free materials in more severe operating environments, such as acid rain caused by air pollution, the use of deicing agents to prevent road ice in snowy areas, and coastal area development.

[0003] The coating of hot-dip Al-Zn coated steel sheets is composed of dendritic regions (α-Al phases) where Al containing supersaturated Zn has solidified, and a Zn-Al eutectic structure present in the interdendritic spaces (interdendrites), with the α-Al phases stacked in multiple layers in the thickness direction of the coating. This unique coating structure creates a complex corrosion path from the surface, making corrosion less likely to progress. It is also known that hot-dip Al-Zn coated steel sheets offer superior corrosion resistance compared to hot-dip galvanized steel sheets with the same coating thickness.

[0004] Generally, hot-dip Al-Zn-coated steel sheets are manufactured by using thin steel sheets obtained by hot-rolling or cold-rolling slabs as the base steel sheet, and then subjecting the base steel sheet to recrystallization annealing and hot-dip coating in the annealing furnace of a continuous hot-dip coating facility. In addition to predetermined concentrations of Al and Zn, the coating bath typically contains Si to suppress excessive growth of the interfacial alloy layer formed at the interface between the base steel (base steel sheet) and the coating. This Si function allows the thickness of the interfacial alloy layer of hot-dip Al-Zn-coated steel sheets to be controlled to approximately 1 to 5 μm. Given the same coating thickness, the thinner the interfacial alloy layer, the thicker the main layer, which exhibits high corrosion resistance. Therefore, suppressing the growth of the interfacial alloy layer is known to lead to improved corrosion resistance.

[0005] Japanese Patent Publication No. 46-7161 Japanese Patent Laid-Open No. 2004-285387 Special Publication No. 2016-540885

[0006] However, when hot-dip Al-Zn-plated steel sheets are bent or otherwise processed, cracks can occur in the plating film at the processed area, depending on the degree of processing (deformation level). In hot-dip Al-Zn-plated steel sheets, the thick interfacial alloy layer serves as the crack initiation point, and the interdendritic gaps in the plating film serve as crack propagation paths. Therefore, even when the same degree of processing is performed, the cracks tend to be larger than those in hot-dip galvanized steel sheets with the same plating film thickness. Therefore, in applications with a high degree of processing, the appearance can be marred by the occurrence of large cracks visible to the naked eye, and the corrosion resistance of cracked areas, where the substrate steel is exposed, is significantly reduced compared to crack-free areas (decreased corrosion resistance in processed areas).

[0007] In the production of hot-dip galvanized steel sheets, it is generally known that impurities inevitably get mixed into the plating bath, and hot-dip Al-Zn plating is no exception. Impurities that get mixed into the plating film include Fe, Cr, Ni, Cu, Co, W, Mg, and Ca, which are mixed in through impurities contained in the plating raw materials or leaching from the base steel sheet or bath-immersed equipment. These elements inevitably get mixed into the plating film. In particular, in recent years, the production volume of highly corrosion-resistant hot-dip Zn-Al-Mg-coated steel sheets and hot-dip Al-Zn-Si-Mg-coated steel sheets has increased. The widespread distribution of Zn raw materials containing high concentrations of Mg, produced by recycling dross generated during the production process, has led to the frequent inclusion of Mg as an impurity in the plating bath and, ultimately, the plating film.

[0008] As described above, unavoidable impurities in a galvanized coating can degrade the appearance, corrosion resistance, workability, and other properties of hot-dip galvanized steel sheets. The impact of impurities often depends on the composition and concentration of the coating. In other words, even impurities with the same composition may be harmful or harmless to the properties of the galvanized steel sheet. Therefore, the impact of impurities on the properties of each hot-dip galvanized steel sheet has been investigated, and techniques for controlling the impurity concentration have been developed to stably obtain the required properties. For example, Patent Document 2 discloses a hot-dip galvanized steel sheet with excellent appearance, which contains, by mass, 0.10 to 0.6% Al, 0.03 to 0.3% Bi, and the remainder Zn and unavoidable impurities, with the Pb, Sn, and Cd contents each controlled to 0.002%. Furthermore, Patent Document 3 discloses a hot-dip Zn-Al-Mg coated steel sheet having excellent corrosion resistance, which contains 4.4 to 5.6% Al, 0.3 to 0.56% Mg, and the balance being Zn and unavoidable impurities, and in which the inclusion of Ni as one of the unavoidable impurities is controlled so as not to occur.

[0009] However, the techniques disclosed in Patent Documents 2 and 3 focus on improving corrosion resistance, and do not fully consider the effects of unavoidable impurities on formability and corrosion resistance of worked portions in hot-dip Zn-Al-plated steel sheets that do not contain Mg or hot-dip Al-Zn-plated steel sheets with a high Al concentration, and therefore there has been a demand for the development of a technique that can more reliably and stably achieve excellent formability and corrosion resistance of worked portions. In addition, control of impurities in the production of hot-dip plated steel sheets, not limited to hot-dip Al-Zn-plated steel sheets, is often limited to concentration control, and no technique has been established for controlling the shape, such as size, and therefore there has been a demand for the development of a technique that can more reliably achieve excellent formability and corrosion resistance of worked portions.

[0010] In view of the above circumstances, an object of the present invention is to provide a hot-dip Al-Zn coated steel sheet that reliably and stably has excellent workability and corrosion resistance at the worked portion, and a method for producing the same.

[0011] As a result of investigations aimed at solving the above-mentioned problems, the present inventors have noticed that, with respect to hot-dip Al-Zn coated steel sheets, it is important to control not only the concentrations of Al, Zn, and Si in the composition of the hot-dip Al-Zn coated film, but also the concentrations of elements contained as impurities. They have found that, among other things, proper control of the Mg content can effectively suppress deterioration of corrosion resistance, and further that proper control of the size of Mg-Zn compounds present as impurities in the coated film can more effectively suppress deterioration of formability and corrosion resistance of processed parts.

[0012] The present invention was made based on the above findings, and its gist is as follows: 1. A hot-dip Al-Zn-plated steel sheet having a plating film, wherein the plating film has a composition containing 45 to 65 mass% Al and 1.0 to 3.0 mass% Si, with the balance consisting of Zn and unavoidable impurities, and the Mg content of the unavoidable impurities is less than 0.5 mass% relative to the total mass of the plating film.

[0013] 2. The hot-dip Al-Zn plated steel sheet according to item 1 above, wherein the plated coating contains an Mg-Zn compound, and the major axis of the Mg-Zn compound is less than 10 μm.

[0014] 3. The hot-dip Al-Zn plated steel sheet according to item 1 above, wherein the plated coating does not contain any Mg-Zn compounds.

[0015] 4. The hot-dip Al-Zn coated steel sheet according to any one of 1 to 3 above, wherein the plating film further contains one or more elements selected from B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce, and Bi in a total amount of 0.01 to 3.0 mass %. 5. The hot-dip Al-Zn coated steel sheet according to any one of 1 to 4 above, wherein the diffraction intensity of MgZn2 in the plating film, as measured by an X-ray diffraction method, satisfies the following relationship (1): MgZn2 (100) = 0 (1) MgZn2 (100): Diffraction intensity of the (100) plane of MgZn2 (planar spacing d = 0.4510 nm)

[0016] 6. A method for producing a hot-dip Al-Zn-plated steel sheet having a plating film, wherein forming the plating film comprises a step of forming the plating film on a base steel sheet using a plating bath having a composition containing 45 to 65 mass% Al and 1.0 to 3.0 mass% Si, with the balance consisting of Zn and unavoidable impurities, wherein the Mg content among the unavoidable impurities in the plating bath is controlled to less than 0.5 mass% with respect to the total mass of the plating bath. 7. A method for producing a hot-dip Al-Zn-plated steel sheet as set forth in 6 above, wherein the plating bath further contains 0.01 to 3.0 mass% in total of one or more elements selected from B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce, and Bi.

[0017] According to the present invention, it is possible to provide a hot-dip Al-Zn coated steel sheet having excellent workability and corrosion resistance at worked portions reliably and stably, and a method for producing the same.

[0018] 1 is an enlarged schematic view of a cross section of a hot-dip Al-Zn plated steel sheet according to an embodiment of the present invention.

[0019] (Hot-dip Al-Zn-plated steel sheet) As shown in Fig. 1, the hot-dip Al-Zn-plated steel sheet of the present invention has a plating film 20 on the surface of a base steel sheet 10. The plating film 20 has a composition containing 45 to 65 mass% Al, 1.0 to 3.0 mass% Si, and the balance being Zn and unavoidable impurities.

[0020] The Al content in the plating film is 45 to 65 mass%, preferably 50 to 60 mass%, to balance corrosion resistance and operational efficiency. This is because an Al content of at least 45 mass% in the plating film causes dendritic solidification of Al, resulting in a plating film structure primarily composed of an α-Al phase dendritic solidification structure. The dendritic solidification structure is layered in the thickness direction of the plating film, which complicates the corrosion progression path and improves the corrosion resistance of the plating film itself. Furthermore, the more α-Al phase dendritic portions are layered, the more complex the corrosion progression path becomes, making it more difficult for corrosion to reach the substrate steel sheet, thereby improving corrosion resistance. Therefore, the Al content in the plating film is preferably 50 mass% or more. On the other hand, if the Al content in the plating film exceeds 65 mass%, most of the Zn changes to a structure in solid solution in the α-Al, making it impossible to suppress the dissolution reaction of the α-Al phase, and the corrosion resistance of the hot-dip Al-Zn plating film deteriorates. For this reason, the Al content in the plating film must be 65 mass % or less, and preferably 60 mass % or less.

[0021] The Si content in the plating film is primarily intended to suppress the growth of Fe-Al and / or Fe-Al-Si interfacial alloy layers at the interface with the substrate steel sheet, thereby preventing deterioration of the adhesion between the plating film and the steel sheet. When a steel sheet is immersed in an Al-Zn plating bath containing Si, an alloying reaction occurs between the Fe on the steel sheet surface and the Al and Si in the bath, resulting in the formation of an Fe-Al and / or Fe-Al-Si intermetallic compound layer at the interface between the substrate steel sheet and the plating film. Since the growth rate of the Fe-Al-Si alloy is slower than that of the Fe-Al alloy, a higher proportion of the Fe-Al-Si alloy suppresses the growth of the entire interfacial alloy layer. Therefore, the Si content in the plating film must be 1.0% by mass or more. On the other hand, if the Si content in the plating film exceeds 3.0% by mass, not only does the effect of suppressing the growth of the interfacial alloy layer saturate, but the presence of excess Si in the plating film also reduces workability. Therefore, the Si content is limited to 3.0% or less.

[0022] The plating film contains Zn and unavoidable impurities. Among these, the unavoidable impurities include Fe. This Fe is inevitably contained in the plating film due to dissolution of the steel sheet or bath-immersed equipment into the plating bath, and is also supplied by diffusion from the base steel sheet during the formation of the interfacial alloy layer. The Fe content in the plating film is typically approximately 0.3 to 2.0 mass%. Other unavoidable impurities include Cr, Ni, Cu, Co, W, Mg, and Ca. These elements are inevitably contained in the plating film due to dissolution into the plating bath from the base steel sheet, stainless steel bath-immersed equipment, and WC-based and Co-Cr-W-based thermal spray coatings applied to bath-immersed equipment; they are contained as impurities in the metal ingots used as raw materials for the plating bath; and they are produced using pots or bath-immersed equipment previously used to produce plated steel sheets to which these elements were intentionally added.

[0023] The hot-dip Al-Zn-plated steel sheet of the present invention is characterized in that the Mg content among the unavoidable impurities is less than 0.5 mass% relative to the total mass of the plated film. Since Mg contained in the plated film may deteriorate the workability and corrosion resistance of the processed portion of the hot-dip Al-Zn-plated steel sheet, by appropriately controlling the Al, Zn, and Si contents in the plated film and further reducing the Mg content as an unavoidable impurity, deterioration of the workability and corrosion resistance of the processed portion can be suppressed. From the same perspective, the Mg content among the unavoidable impurities is preferably 0.3 mass% or less, more preferably 0.1 mass% or less, relative to the total mass of the plated film. Thus, the lower the Mg content in the plated film, the better the corrosion resistance of the hot-dip Al-Zn-plated steel sheet of the present invention, so there is no particular lower limit. However, because it is technically difficult to achieve a Mg content of exactly 0.000 mass% in the plated film, the lower limit of the Mg content in the plated film is essentially about 0.001 mass%.

[0024] When Mg is contained in the inevitable impurities, Mg-Zn compounds may be contained as impurities in the coating film of the hot-dip Al-Zn coated steel sheet. In most cases, the Mg-Zn compounds are MgZn2, but other compounds such as Mg2Zn 11 Binary intermetallic compounds such as Mg 21 (Al, Zn) 17 and Mg 32 (Al, Zn) 49 However, the present invention is not particularly limited to ternary intermetallic compounds such as those listed above. From the viewpoint of achieving better workability and corrosion resistance of worked portions, it is preferable that the plating film does not contain these Mg-Zn compounds.

[0025] The presence of Mg-Zn-based compounds in the plating film can be confirmed, for example, by using a scanning electron microscope to observe the plating film from the surface or cross section using secondary electron images or backscattered electron images, followed by analysis using energy dispersive X-ray spectroscopy (EDS). For example, approximately 5 to 10 locations on a 100 μm plating cross section can be arbitrarily selected, and observation and elemental mapping analysis can be performed at an accelerating voltage of 5 kV or less. Further point analysis can be performed on the areas where Mg is detected to confirm the composition of the Mg-Zn-based inclusions. This method is merely an example, and any method that can confirm the presence of Mg-Zn-based compounds can be used, and is not particularly limited.

[0026] Furthermore, when the plating film contains Mg-Zn-based compounds, it is preferable to reduce the major axis of the Mg-Zn-based compounds. Because the Mg-Zn-based compounds present in the plating film are hard and brittle, they can become crack initiation sites during severe bending or stretching, potentially causing deterioration in workability and corrosion resistance in the processed area. In particular, the presence of coarse Mg-Zn-based compounds in the plating film may significantly reduce the workability and corrosion resistance of the processed area of ​​the hot-dip Al-Zn-plated steel sheet. Therefore, in order to obtain a hot-dip Al-Zn-plated steel sheet with improved workability and corrosion resistance in the processed area, it is effective to reduce the size of the Mg-Zn-based compounds contained as impurities in the plating film. Specifically, it is preferable to reduce the major axis of the Mg-Zn-based compounds to less than 10 μm. From the same perspective, it is preferable that the major axis of the Mg-Zn-based compounds be as small as possible. The major axis of the Mg-Zn-based compounds can be measured, for example, by using a scanning electron microscope to observe a backscattered electron image of the cross section of the plating film, confirming that the compounds are Mg-Zn-based compounds by EDS, and then observing a backscattered electron image with an enlarged observation field that includes the Mg-Zn-based compounds. Note that the major axis of the Mg-Zn-based compounds in the present invention refers to the average of the five largest major axis values ​​measured for all Mg-Zn-based compounds identified in a continuous cross section of the plating film having a length of 5 mm in a direction parallel to the surface of the substrate steel sheet.

[0027] In the hot-dip Al-Zn coated steel sheet of the present invention, the diffraction intensity of MgZn2 in the coating film as determined by X-ray diffraction preferably satisfies the following relationship (1): MgZn2 (100) = 0 (1) MgZn2 (100): Diffraction intensity of the (100) plane of MgZn2 (planar spacing d = 0.4510 nm),

[0028] As described above, in order to stabilize the workability and corrosion resistance of hot-dip Al-Zn-plated steel sheets, it is important to suppress the content of Mg as an unavoidable impurity and to minimize the formation of Mg-Zn compounds in the coating film. In particular, by minimizing the amount of MgZn2, which is thermodynamically stable and easily formed in hot-dip Al-Zn-plated films (i.e., by reducing the diffraction intensity of MgZn2 (100) to zero), the workability and corrosion resistance of the processed parts can be further stabilized.

[0029] Here, in the above-mentioned relationship (1), MgZn2(100) is the diffraction intensity of the (100) plane of MgZn2 (planar spacing d = 0.4510 nm). The method for measuring MgZn2(100) by X-ray diffraction is to mechanically scrape off a part of the plating film, powder it, and then perform X-ray diffraction on it (powder X-ray diffraction measurement method). For the measurement of the diffraction intensity, the MgZn2 (100) corresponding to the planar spacing d = 0.4510 nm is used. 2 The diffraction peak intensity can be measured.

[0030] The amount of plating film required for powder X-ray diffraction measurement (amount of plating film scraped off) is 0.1 g or more, preferably 0.3 g or more, from the viewpoint of accurately measuring MgZn2 (100). Furthermore, when the plating film is scraped off, steel sheet components other than the plating film may be contained in the powder. However, these intermetallic compound phases are contained only in the plating film and do not affect the peak intensity described above. Furthermore, the reason for powdering the plating film and performing X-ray diffraction is that when X-ray diffraction is performed on a plating film formed on a plated steel sheet, it is affected by the plane orientation of the plating film solidification structure, making it difficult to evaluate the amount of a substance present from the diffraction intensity of a specific interplanar spacing.

[0031] Here, the method for satisfying the above-mentioned relationship (1) is not particularly limited. For example, by controlling the Mg content in the plating film to a low level and reducing the ratio of the Mg content to the Zn content (for example, by setting the Mg / Zn ratio to 0.008 or less, preferably 0.006 or less), MgZn2 and Mg2Zn 11 Abundance of MgZn 2 (100) and Mg2Zn 11 Furthermore, in addition to the method of controlling the Mg content in the plating film, the Mg content in the plating film can be controlled to a specific value, and then the conditions for forming the plating film (for example, the cooling conditions after plating) can be adjusted to satisfy the relationship (1).

[0032] Furthermore, as for unavoidable impurities in the plating film, the Mg content relative to the Fe content (Mg / Fe) is preferably 1.0 or less. This reduces the amount of Mg dissolved in the Fe-Al and / or Fe-Al-Si interfacial alloy layer, suppressing the increase in hardness of the interfacial alloy layer due to solid solution strengthening, thereby achieving better workability and corrosion resistance of the processed part. From the same perspective, the Mg / Fe ratio is more preferably 0.6 or less.

[0033] The plating film may further contain 0.01 to 3.0 mass% in total of one or more elements selected from B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce, and Bi. These elements have the effect of improving the stability of corrosion products when the plating film corrodes, thereby delaying the progression of corrosion, and the effect of stabilizing the spangle size on the plating surface, thereby improving the surface appearance.

[0034] In addition, the coating weight of the plating film is set to 45 to 120 g / m per side from the viewpoint of satisfying various characteristics. 2 It is preferable that the coating weight of the plating film is 45 g / m 2 In the above cases, sufficient corrosion resistance can be obtained for applications requiring long-term corrosion resistance, such as building materials, and the coating weight of the plating film is 120 g / m 2This is because, in the following cases, it is possible to achieve excellent corrosion resistance while suppressing the occurrence of plating cracks during processing. From the same viewpoint, the coating weight of the plating film is 45 to 100 g / m 2 It is more preferable that:

[0035] The coating weight of the plating film can be determined, for example, by a method described in JIS H 0401:2013, in which a specific area of ​​the plating film is dissolved and stripped using a mixture of hydrochloric acid and hexamethylenetetramine, and the weight of the steel sheet is calculated from the difference between before and after stripping. To determine the coating weight per side using this method, the plating surface on the non-target side can be sealed with tape to prevent exposure, and then the dissolution process described above can be performed. Similarly to the coating weight described above, the composition of the plating film can be determined by immersing the plating film in a hydrochloric acid solution or the like to dissolve it, and then analyzing the resulting solution using ICP emission spectroscopy, atomic absorption spectroscopy, or the like. This method is merely an example, and any method that can accurately quantify the composition of the plating film may be used, and is not particularly limited.

[0036] The coating film on the hot-dip Al-Zn coated steel sheet obtained according to the present invention has a composition generally equivalent to that of the coating bath, and therefore the composition of the coating film can be controlled with high precision by controlling the composition of the coating bath.

[0037] Furthermore, the base steel sheet constituting the hot-dip Al-Zn-plated steel sheet of the present invention is not particularly limited, and cold-rolled steel sheets, hot-rolled steel sheets, etc. can be used as appropriate depending on the required performance and specifications. Furthermore, the method for obtaining the base steel sheet is also not particularly limited. For example, in the case of the hot-rolled steel sheet, a steel sheet that has been subjected to a hot-rolling process and a pickling process can be used, and in the case of the cold-rolled steel sheet, a steel sheet can be produced by further adding a cold-rolling process. Furthermore, in order to obtain the desired steel sheet properties, a recrystallization annealing process or the like can also be performed before the hot-dip plating process.

[0038] As shown in FIG. 1 , the hot-dip Al-Zn-plated steel sheet of the present invention has a plating film 20 formed on a base steel sheet 10. If necessary, an intermediate layer or a coating film can be further formed on the plating film. The type of coating film and the method for forming the coating film are not particularly limited and can be appropriately selected depending on the required performance. Examples of methods include roll coating, curtain flow coating, and spray coating. A coating film can be formed by applying an organic resin-containing paint and then heating and drying it using means such as hot air drying, infrared heating, and induction heating. The intermediate layer is not particularly limited as long as it is formed between the plating film of the hot-dip Al-Zn-plated steel sheet and the coating film. Examples include a chemical conversion coating and a primer such as an adhesive layer. The chemical conversion coating can be formed, for example, by a chromate treatment or a chromium-free chemical conversion treatment, in which a chromate treatment solution or a chromium-free chemical conversion treatment solution is applied, followed by drying at a steel sheet temperature of 80 to 300°C without rinsing with water. These chemical conversion coatings may be single-layer or multi-layer, and in the case of multi-layer, multiple chemical conversion treatments may be carried out in sequence.

[0039] (Method for producing hot-dip Al-Zn plated steel sheet) The method for producing a hot-dip Al-Zn plated steel sheet of the present invention is a method for producing a hot-dip Al-Zn plated steel sheet having a plating film.

[0040] The method for producing a hot-dip Al-Zn-plated steel sheet of the present invention includes a step of forming the plating film on a substrate steel sheet using a plating bath having a composition containing 45 to 65 mass % Al, 1.0 to 3.0 mass % Si, and the balance consisting of Zn and unavoidable impurities.

[0041] The step of forming the plating film is not particularly limited except for the conditions of the plating bath, which will be described later. For example, the steel sheet can be produced by cleaning, heating, and immersing the base steel sheet in a plating bath using continuous hot-dip plating equipment. In the steel sheet heating step, recrystallization annealing or the like is performed to control the structure of the base steel sheet itself, and heating in a reducing atmosphere, such as a nitrogen-hydrogen atmosphere, is effective in preventing oxidation of the steel sheet and reducing the trace oxide film present on the surface.

[0042] The plating bath used in the step of forming the plating film contains 45 to 65 mass % Al, 1.0 to 3.0 mass % Si, and the remainder Zn and unavoidable impurities, because, as described above, the composition of the plating film as a whole is approximately the same as the composition of the plating bath.

[0043] The method for producing a hot-dip Al-Zn-plated steel sheet according to the present invention is characterized in that the Mg content among unavoidable impurities in the coating bath is controlled to less than 0.5 mass% relative to the total mass of the coating bath. As described above, Mg contained in the coating film may deteriorate the workability and corrosion resistance of the processed portion of the hot-dip Al-Zn-plated steel sheet. Therefore, by appropriately controlling the contents of Al, Zn, and Si in the coating bath and further reducing the Mg content as an unavoidable impurity, deterioration of the workability and corrosion resistance of the processed portion can be suppressed.

[0044] Furthermore, the content of Mg as an unavoidable impurity in the coating bath needs to be controlled to 0.5% by mass or less, preferably 0.2% by mass or less, relative to the total mass of the coating bath. If the Mg content in the coating bath is less than 0.5% by mass, the resulting hot-dip Al-Zn-plated steel sheet can have sufficiently excellent formability and corrosion resistance in the processed area. If the Mg content is 0.2% by mass or less, even better formability and corrosion resistance in the processed area can be achieved. Thus, the lower the Mg content in the coating bath, the better the corrosion resistance of the hot-dip Al-Zn-plated steel sheet. Therefore, there is no particular lower limit for the Mg content. However, because it is technically difficult to achieve a Mg content of exactly 0.000% by mass in the coating bath, the lower limit for the Mg content in the coating is essentially about 0.001% by mass.

[0045] The means for reducing the Mg content in the coating bath is not particularly limited. For example, it is effective to not intentionally add Mg to the coating bath, or not to use pots or bath-immersed equipment used in the production of coated steel sheets, such as Zn-Al-Mg-coated steel sheets or Al-Zn-Si-Mg-coated steel sheets, to which Mg is intentionally added, in the production of hot-dip Al-Zn-coated steel sheets. This is because it is possible to prevent Mg-containing metal chunks adhering to the pot or bath-immersed equipment from dissolving and being mixed into the coating bath. Another means for reducing the Mg content in the coating bath is to preferably use metal chunks with a low Mg content among impurities as a raw material for the coating bath.

[0046] The bath temperature of the coating bath is not particularly limited, but is preferably in the range of (melting point + 20°C) to 650°C. The reason why the lower limit of the bath temperature is set to melting point + 20°C is that the bath temperature needs to be at or above the solidification point in order to perform hot-dip coating, and setting the temperature to melting point + 20°C prevents solidification due to a local drop in the bath temperature of the coating bath. On the other hand, the reason why the upper limit of the bath temperature is set to 650°C is that if the temperature exceeds 650°C, it becomes difficult to rapidly cool the coating film, and there is a risk that the interfacial alloy layer formed between the coating film and the steel sheet will become thick.

[0047] Furthermore, the temperature of the base steel sheet immersed in the coating bath (immersion sheet temperature) is not particularly limited, but from the viewpoint of ensuring coating characteristics in the continuous hot dip coating operation and preventing changes in bath temperature, it is preferable to control it to within ±20°C of the coating bath temperature.

[0048] Furthermore, the immersion time of the substrate steel sheet in the coating bath is preferably 0.5 seconds or more. This is because if it is less than 0.5 seconds, there is a risk that a sufficient coating film will not be formed on the surface of the substrate steel sheet. There is no particular upper limit to the immersion time, but if the immersion time is longer, there is a risk that the interfacial alloy layer formed between the coating film and the steel sheet will become thick, so it is more preferable to keep it within 8 seconds.

[0049] In the method for producing a hot-dip Al-Zn-plated steel sheet of the present invention, in addition to the above-mentioned plating film formation step and the temperature-raising, heating, and cooling steps after plating film formation, it is possible to appropriately carry out steps that are employed in the production of ordinary plated steel sheets.

[0050] [Samples 1 to 32] A cold-rolled steel sheet having a thickness of 0.8 mm, produced by a conventional method, was used as a base steel sheet, and annealing and plating were performed using a hot-dip galvanizing simulator manufactured by Rhesca Corporation, to produce hot-dip galvanized steel sheet samples 1 to 32 under the conditions shown in Table 1. The composition of the coating bath used in producing the hot-dip galvanized steel sheets was varied within the ranges of Al: 0.2 to 70 mass%, Si: 0.0 to 3.2 mass%, B: 0.00 to 0.02 mass%, Ca: 0.0 to 1.0 mass%, Ti: 0.0 to 0.1 mass%, V: 0.1 to 0.1 mass%, Cr: 0.0 to 0.2 mass%, Mn: 0.0 to 0.1 mass%, Sr: 0.0 to 0.1 mass%, Mo: 0.0 to 0.1 mass%, In: 0.0 to 0.5 mass%, Sn: 0.0 to 0.5 mass%, Sb: 0.0 to 0.1 mass%, Ce: 0.0 to 1.0 mass%, and Bi: 0.00 to 0.05 mass% so as to obtain the composition of the coating of each sample shown in Table 1. The bath temperature of the coating was controlled to 460°C for Al: 0.2-5% by mass, 600°C for Al: 35-55% by mass, and 660°C for Al: over 60% by mass, so that the temperature of the substrate steel sheet entering the coating was the same as the coating bath temperature. Furthermore, for Al: 35-65% by mass, the coating was performed under the condition that the sheet was cooled to a temperature range of 520-500°C in 3 seconds. The coating weight of the coating was 85±5 g / m per side for Samples 1-29. 2 , and sample 30 is 50±5 g / m per side 2 , and sample 31 is 100±5 g / m per side 2 , and sample 32 has a thickness of 125±5 g / m per side. 2 It was controlled so that

[0051] [Evaluation] Each sample of the obtained hot-dip plated steel sheet was evaluated as follows. The evaluation results are shown in Table 1.

[0052] (1) Plating Film (Composition, Coating Weight, Mg-Based Compounds) A 100 mm diameter cutout was punched from each of the prepared plated steel sheets, and the non-measurement surface was sealed with tape. The plating was dissolved and stripped using a mixture of hydrochloric acid and hexamethylenetetramine as specified in JIS H 0401:2013. The coating weight of the plating film was calculated from the mass difference between the sample before and after stripping. The calculated coating weights of the plating film are shown in Table 1. The stripping solution was then filtered, and the filtrate and solid content were analyzed separately. Specifically, the filtrate was subjected to ICP atomic emission spectroscopy to quantify components other than insoluble silicon. The solid content was then dried and ashed in a heating furnace at 650°C, and then melted by adding sodium carbonate and sodium tetraborate. The melt was then dissolved in hydrochloric acid, and the solution was subjected to ICP atomic emission spectroscopy to quantify insoluble silicon. The Si concentration in the plating film was calculated by adding the soluble Si concentration obtained by filtrate analysis to the insoluble Si concentration obtained by solids analysis. The composition of the resulting plating film is shown in Table 1. Furthermore, each sample was sheared to a size of 15 mm x 15 mm, embedded in conductive resin so that the cross-section of the steel sheet could be observed, and mechanically polished. Using a scanning electron microscope (ULTRA55, manufactured by Carl Zeiss), backscattered electron images of 100 μm wide sections of the plating film, each 5 mm long and parallel to the surface of the base steel sheet, were sequentially captured at an accelerating voltage of 3 kV. Furthermore, elemental mapping analysis (Al, Zn, Si, Fe, and Mg) of each section was performed using an energy-dispersive X-ray spectrometer (Ultim Extreme, manufactured by Oxford Instruments) at an accelerating voltage of 3 kV. For areas where high Mg intensity was detected in this analysis, point analysis was performed using the same spectrometer at an accelerating voltage of 3 kV, and the substance was identified from the presence or absence of Mg-based compounds and the semi-quantitative values ​​of the obtained components. The major axis of all Mg-based compounds confirmed in the observation field was measured, and the average of the values ​​for the top five points was taken as the major axis. The calculated major axis values ​​are shown in Table 1.Each sample was then sheared to a 100mm x 100mm size, and the plating film on the target surface was mechanically removed until the steel substrate was visible. The resulting powder was thoroughly mixed and 0.3g of the removed powder was analyzed using an X-ray diffraction spectrometer (Rigaku Corporation, "SmartLab") under the following conditions: Cu-Kα (wavelength = 1.54178Å), Kβ (removal of Kβ) with a Ni filter, tube voltage = 40kV, tube current = 30mA, scanning speed = 4° / min, sampling interval = 0.020°, divergence slit = 2 / 3°, solar slit = 5°, and a high-speed one-dimensional detector (D / teX Ultra). The diffraction intensity (kcps) of the MgZn2 (100) plane (planar spacing d = 0.4510nm) was measured using the intensity obtained by subtracting the base intensity from each peak intensity. The measurement results of the diffraction intensity are shown in Table 1.

[0053] (2) Workability Evaluation Each sample of the obtained hot-dip galvanized steel sheet was sheared to a size of 70 mm x 150 mm, and then n sheets (n = 8, 10, 12, 14, 16) of the same thickness were sandwiched inside each other, and each sample was bent 180° (nT bend) to obtain a 150 mm apex. After bending, Cellotape (registered trademark) was firmly attached to the outer surface of the bent portion and then peeled off. The outer surface (apex) of the bent portion was observed with a scanning electron microscope (ULTRA55 manufactured by Carl Zeiss) at an accelerating voltage of 5 kV to confirm the occurrence of cracks, and the workability was evaluated according to the following criteria. The evaluation results are shown in Table 1. ◯: No large cracks with an opening width of 20 μm or more were observed. ×: Large cracks with an opening width of 20 μm or more were observed.

[0054] (3) Evaluation of corrosion resistance of processed parts Each sample of hot-dip galvanized steel sheet obtained was sheared to a size of 70 mm x 150 mm, and then each edge was sealed with tape. 14 or 16 sheets of the same thickness were sandwiched inside, and 14T and 16T bendings were performed to obtain a 150 mm apex. Each sample prepared as described above was subjected to the Japanese Automotive Standards Combined Cycle Test (JASO-CCT). The accelerated corrosion test started from wet conditions and continued for 60 cycles. After that, the appearance of the outer surface (apex) of the bent part of each sample was visually inspected and judged according to the following criteria. The inspection results and judgment results are shown in Table 1. ◯: No red rust or white rust was observed in the 16T bent sample. ×: Red rust or white rust was observed in the 16T bent sample.

[0055]

[0056] The results in Table 1 show that the samples of the invention have a good balance of workability and corrosion resistance of the worked portion compared to the samples of the comparative examples.

[0057] According to the present invention, it is possible to provide a hot-dip Al-Zn coated steel sheet having excellent workability and corrosion resistance at worked portions reliably and stably, and a method for producing the same.

[0058] REFERENCE SIGNS LIST 10 Base steel sheet 20 Plating film 21 Main layer 22 Interface alloy layer 211 Dendrite 212 Interdendrite

Claims

1. A hot-dip Al-Zn plated steel sheet having a plating film, the plating film having a composition containing 45-65 mass% Al, 1.0-3.0 mass% Si, with the balance being Zn and unavoidable impurities, and the Mg content of the unavoidable impurities is less than 0.5 mass% with respect to the total mass of the plating film.

2. The hot-dip Al-Zn plated steel sheet according to claim 1, characterized in that the plated film contains Mg-Zn compounds, the major axis of which is less than 10 μm.

3. The hot-dip Al-Zn plated steel sheet according to claim 1, characterized in that the plated coating does not contain any Mg-Zn compounds.

4. The hot-dip Al-Zn plated steel sheet according to any one of claims 1 to 3, characterized in that the plating film further contains 0.01 to 3.0 mass% in total of one or more elements selected from B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce and Bi.

5. The hot-dip Al-Zn plated steel sheet according to any one of claims 1 to 4, characterized in that the diffraction intensity of MgZn2 in the plated film by X-ray diffraction method satisfies the following relationship (1): MgZn2 (100) = 0 ... (1) MgZn2 (100): Diffraction intensity of the (100) plane (plane spacing d = 0.4510 nm) of MgZn2 6. A method for producing a hot-dip Al-Zn plated steel sheet having a plating film, comprising the steps of forming the plating film on a base steel sheet using a plating bath containing 45-65 mass% Al and 1.0-3.0 mass% Si, with the balance being Zn and unavoidable impurities, and controlling the Mg content in the unavoidable impurities of the plating bath to less than 0.5 mass% with respect to the total mass of the plating bath.

7. The method for producing a hot-dip Al-Zn coated steel sheet according to claim 6, characterized in that the coating bath further contains 0.01 to 3.0 mass % in total of one or more elements selected from B, Ca, Ti, V, Cr, Mn, Sr, Mo, In, Sn, Sb, Ce, and Bi.