Separation and recovery method
Patent Information
- Application Number
- MYPI2025005352
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-04
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-04
AI Technical Summary
Current methods for recovering precious metals from waste liquids, such as solvent extraction and using activated carbon or ion exchange resins, are complex, environmentally burdensome, and inefficient, particularly due to the low selectivity and structural degradation of adsorbents during repeated adsorption and elution processes.
The use of polyarylene sulfide (PAS) resin particles as an adsorbent for selectively adsorbing and recovering metal atoms from aqueous solutions, with an alkaline solution or a chelating agent-containing eluent for efficient elution, leveraging their excellent adsorption properties and heat resistance.
This method enables efficient separation and recovery of metal atoms with improved selectivity and reduced environmental impact, as PAS resin particles maintain adsorption properties and can be effectively regenerated, simplifying the process and reducing equipment burden.
Abstract
Description
Separation and collection method
[0001] The present invention relates to a separation and recovery method in which a substance to be separated is separated from an aqueous solution containing the substance by using polyarylene sulfide (hereinafter sometimes abbreviated as PAS) resin particles as an adsorbent, and then the substance is eluted and recovered.
[0002] In recent years, from the perspective of effective utilization of valuable resources and prevention of environmental pollution toward sustainable development, efficient recovery technologies for valuable metal atoms from solutions containing these atoms have attracted attention. In particular, precious metals such as platinum group metals, gold, and silver are highly valuable, and because their production is unevenly distributed among countries, competition to recover precious metals from waste solutions such as industrial catalysts and metal plating solutions is becoming more intense.
[0003] Solvent extraction has been put to practical use as a method for recovering precious metals from wastewater, but the process is complicated, and the equipment requires large capacity. The disposal of large volumes of wastewater that does not contain precious metals presents problems. Other methods for recovering precious metals by contacting activated carbon or ion exchange resins with wastewater have also been put to practical use. However, activated carbon has low selectivity for precious metals, and high-temperature calcination is required to elute the precious metals, resulting in significant equipment and environmental impact. Ion exchange resins and chelating resins selectively adsorb precious metals using functional groups on their side chains. Repeated adsorption and elution alter the structure of the functional groups, resulting in a decline in adsorption properties. Finally, calcination is required to recover the precious metals. Therefore, further simplification of the process and reduction of the environmental impact are needed for both methods.
[0004] On the other hand, in recent years, proposals have been made to use a porous material made of PAS resin as an adsorbent, taking advantage of its excellent heat resistance and chemical resistance. For example, in Patent Document 1, a porous material made of recycled PAS resin is used as an adsorbent, taking advantage of the large specific surface area of the recycled PAS resin, particularly for ozone and NOx. 2 Furthermore, for example, Patent Document 2 discloses that the hydrogen bonding strength component δh of the three-dimensional solubility parameter is 1 to 5 (cal 1/2 cm -3/2 Polyphenylene sulfide (hereinafter referred to as PPS) has been disclosed as an adsorbent made of a microporous polymer composition which becomes a porous polymer.
[0005] Japanese Patent Application No. 8-512891 Japanese Patent Application No. 6-327970
[0006] However, there are few disclosures regarding elution in separation and recovery methods using PAS resin particles as an adsorbent. In addition, since PAS resin particles have a different adsorption mechanism and design concept from conventional adsorbents, there has been a need to develop an elution and recovery method for substances to be separated that is optimal for PAS resin particles.
[0007] Therefore, the problem that the present invention aims to solve is to provide a method for efficiently separating and recovering metal atoms, which are the substance to be separated, from an aqueous solution containing the substance to be separated, using an adsorbent that contains PAS resin particles and has excellent adsorption power in water.
[0008] As a result of various investigations, the present inventors have arrived at the following invention: The separation and recovery method of the present disclosure is a method for separating a substance to be separated from an aqueous solution containing the substance using PAS resin particles, comprising: a step (1) of contacting the aqueous solution containing the substance to be separated with PAS resin particles to selectively adsorb the substance to be separated contained in the aqueous solution onto the PAS resin particles and remove the substance from the aqueous solution; and a step (2) of contacting the PAS resin particles with an eluent to elute the substance to be separated, wherein the substance to be separated is a metal atom or a compound containing a metal atom, and the eluent is an alkaline aqueous solution or an aqueous solution in which a chelating agent containing a sulfur atom or a nitrogen atom is dissolved.
[0009] According to the present invention, a method can be provided for efficiently separating and recovering metal atoms, which are substances to be separated, from an aqueous solution containing the substances to be separated, using an adsorbent containing PAS resin particles and having excellent adsorption power in water.
[0010] While one embodiment of the present disclosure will be described in detail below, the scope of the present disclosure is not limited to the embodiment described here, and various modifications can be made without departing from the spirit of the present disclosure. Furthermore, when multiple upper and lower limit values are listed for a specific parameter, any of these upper and lower limit values can be combined to form a suitable numerical range.
[0011] The separation and recovery method according to this embodiment is a method for separating a substance to be separated from an aqueous solution containing the substance to be separated using PAS resin particles, and includes the steps of: (1) contacting the aqueous solution containing the substance to be separated with PAS resin particles to selectively adsorb the substance to be separated contained in the aqueous solution onto the PAS resin particles and remove the substance from the aqueous solution; and (2) contacting the PAS resin particles with an eluent to elute the substance to be separated, wherein the substance to be separated is a metal atom or a compound containing a metal atom, and the eluent is an alkaline aqueous solution or an aqueous solution in which a chelating agent containing a sulfur atom or a nitrogen atom is dissolved. This will be described in detail below.
[0012] PAS Resin Particles In the separation and recovery method according to this embodiment, PAS resin particles are used as an adsorbent. The PAS resin particles refer to particles essentially made of PAS resin, or particulate PAS resin. The PAS resin used in this embodiment has a resin structure with a repeating unit in which an aromatic ring and a sulfur atom are bonded, and specifically, a PAS resin having a structure represented by the following formula (1):
[0013] (In the formula, R 1 and R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a nitro group, an amino group, a phenyl group, a methoxy group, or an ethoxy group, and, if necessary, a structural portion represented by the following general formula (2):
[0014] The trifunctional structural moiety represented by formula (2) is preferably present in an amount of 0.001 to 3 mol %, particularly preferably 0.01 to 1 mol %, based on the total number of moles of the trifunctional structural moiety and other structural moieties.
[0015] Here, the structural moiety represented by the general formula (1) is particularly R 1 and R 2 is preferably a hydrogen atom from the viewpoint of the mechanical strength of the PAS resin, and in that case, examples include those bonded at the para position represented by the following formula (3) and those bonded at the meta position represented by the following formula (4).
[0016] Among these, a structure in which the bond between the sulfur atom and the aromatic ring in the repeating unit is at the para position represented by the general formula (3) is particularly preferred in terms of adsorption properties for the substance to be separated.
[0017] The PAS resin may contain not only the structural moieties represented by the general formula (1) or (2) but also the structural moieties represented by the following structural formulae (5) to (8):
[0018] The structural moieties represented by the general formula (1) and the general formula (2) may be contained in an amount of 30 mol % or less of the total of the structural moieties represented by the general formula (1) and the general formula (2). In particular, in the present disclosure, it is preferable that the structural moieties represented by the general formulas (5) to (8) be 10 mol % or less from the viewpoint of the heat resistance and mechanical strength of the PAS resin. When the structural moieties represented by the general formulas (5) to (8) are contained in the PAS resin, the bonding mode thereof may be either a random copolymer or a block copolymer.
[0019] The PAS resin may also have naphthyl sulfide bonds or the like in its molecular structure, but the amount of such bonds is preferably 3 mol % or less, and particularly preferably 1 mol % or less, relative to the total number of moles including other structural moieties.
[0020] The polymerization method for the PAS resin is not particularly limited as long as it is a known method, but examples thereof include (polymerization method 1) a method in which a dihalogenoaromatic compound is polymerized in the presence of sulfur and sodium carbonate, and if necessary, a polyhalogenoaromatic compound or other copolymerization component is added; (polymerization method 2) a method in which a dihalogenoaromatic compound is polymerized in a polar solvent in the presence of a sulfidizing agent or the like, and if necessary, a polyhalogenoaromatic compound or other copolymerization component is added; (polymerization method 3) a method in which p-chlorothiophenol is added, and if necessary, other copolymerization components are added, and then self-condensed; and (production method 4) a method in which a diiodoaromatic compound and elemental sulfur are melt-polymerized under reduced pressure in the presence of a polymerization inhibitor. Among these polymerization methods, (polymerization method 2) is preferred because it is versatile. During the reaction, an alkali metal salt of a carboxylic acid or sulfonic acid or an alkali hydroxide may be added to adjust the degree of polymerization. Among the above (polymerization method 2) methods, there is a method for producing a PAS resin by introducing a water-containing sulfidizing agent into a mixture containing a heated organic polar solvent and a dihalogeno aromatic compound at a rate at which water can be removed from the reaction mixture, and then adding the dihalogeno aromatic compound and the sulfidizing agent, and optionally a polyhalogeno aromatic compound, in the organic polar solvent to react with each other, and controlling the amount of water in the reaction system to be in the range of 0.02 to 0.5 mol per mol of the organic polar solvent (see JP-A-07-228699). In particular, a method is preferred in which a dihalogenoaromatic compound and, if necessary, a polyhalogenoaromatic compound or other copolymerization component are added in the presence of an alkali metal sulfide of the above form and an aprotic polar organic solvent, and the alkali metal hydrosulfide and the alkali metal salt of an organic acid are reacted while controlling the amount of the alkali metal salt of an organic acid in an amount of 0.01 to 0.9 moles per mole of the sulfur source and the amount of water in the reaction system to be 0.02 moles per mole of the aprotic polar organic solvent (see WO 2010 / 058713 pamphlet).
[0021] Specific examples of the dihalogeno aromatic compound include p-dihalobenzene, m-dihalobenzene, o-dihalobenzene, 2,5-dihalotoluene, 1,4-dihalonaphthalene, 1-methoxy-2,5-dihalobenzene, 4,4'-dihalobiphenyl, 3,5-dihalobenzoic acid, 2,4-dihalobenzoic acid, 2,5-dihalonitrobenzene, 2,4-dihalonitrobenzene, 2,4-dihaloanisole, p,p'-dihalodiphenyl ether, 4,4'-dihalobenzophenone, 4,4'-dihalo Examples of the polyhalogenoaromatic compounds include 1,2,3-trihalobenzene, 1,2,4-trihalobenzene, 1,3,5-trihalobenzene, 1,2,3,5-tetrahalobenzene, 1,2,4,5-tetrahalobenzene, 1,4,6-trihalonaphthalene, etc. The halogen atoms contained in the above compounds are preferably chlorine atoms or bromine atoms.
[0022] The crude reaction mixture containing the PAS resin obtained by the polymerization step may be subjected to post-treatment. In this case, the post-treatment method is not particularly limited. For example, (post-treatment 1) after the completion of the polymerization reaction, the solvent is first distilled off under reduced pressure or normal pressure, either as is or after adding an acid or base, and then the solid remaining after solvent distillation is washed once or twice or more times with a solvent such as water, the reaction solvent (or an organic solvent having a similar solubility to the low-molecular-weight polymer), acetone, methyl ethyl ketone, or alcohols, followed by neutralization, washing with water, filtration, and drying; (post-treatment 2) after the completion of the polymerization reaction, a solvent such as water, acetone, methyl ethyl ketone, alcohols, ethyls, halogenated hydrocarbons, aromatic hydrocarbons, or aliphatic hydrocarbons (a solvent that is soluble in the polymerization solvent used and is a poor solvent for at least PAS) is added to the reaction mixture as a precipitant to precipitate solid products such as PAS and inorganic salts, which are then filtered off, washed, and dried; (post-treatment 3) after the completion of the polymerization reaction, the reaction mixture is washed with the reaction solvent (or an organic solvent having a similar solubility to the low-molecular-weight polymer) once or twice or more times, followed by neutralization, washing with water, filtration, and drying; (an organic solvent having a solubility equivalent to that of the crude PAS) is added to the reaction mixture after stirring, followed by filtration to remove the low-molecular-weight polymer, followed by washing once or twice or more times with a solvent such as water, acetone, methyl ethyl ketone, or an alcohol, followed by neutralization, washing with water, filtration, and drying; (post-treatment 4) a method in which, after the polymerization reaction is completed, water is added to the reaction mixture, followed by washing with water, filtration, and if necessary, an acid is added during the water washing to perform an acid treatment, and then drying; or (post-treatment 5) a method in which, after the polymerization reaction is completed, the reaction mixture is filtered, and if necessary, washed once or twice or more times with the reaction solvent, followed by further washing with water, filtration, and drying; or (post-treatment 6) a method in which, after the polymerization reaction is completed, a part of the reaction mixture is desolvated to obtain a slurry containing the crude PAS, and the slurry containing the crude PAS is brought into contact with water and an oxygen atom-containing solvent having 1 to 3 carbon atoms to convert the crude PAS into porous particles, and the obtained porous particles are washed with carbonated water and filtration.
[0023] Examples of oxygen-containing solvents having 1 to 3 carbon atoms that can be used in the post-treatment method exemplified above in (Post-treatment 6) include at least one selected from the group consisting of alcohols and ketones. Examples of alcohols (also referred to as alcohol-based solvents or alcohol solvents) include alcohols having 10 or fewer carbon atoms, such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, t-butyl alcohol, ethylene glycol, propylene glycol, trimethylolpropane, and benzyl alcohol; alcohols having 10 or fewer carbon atoms and containing an ether bond, such as 2-methoxyethyl alcohol, 2-ethoxyethyl alcohol, 1-methoxy-2-propyl alcohol, 1-ethoxy-2-propyl alcohol, 3-methoxy-1-butyl alcohol, and 2-isopropoxyethyl alcohol; alcohols having 10 or fewer carbon atoms and containing a ketone group, such as 3-hydroxy-2-butanone; and alcohols having 10 or fewer carbon atoms and containing an ester group, such as methyl hydroxyisobutyrate. Examples of ketones (also referred to as ketone-based solvents or ketone solvents) include acetone, methyl ethyl ketone, cyclohexanone, γ-butyrolactone, and N-methylpyrrolidinone. In the present disclosure, it is preferable to use a monohydric alcohol having 10 or less carbon atoms because it can efficiently remove the residual carboxyalkylamino group-containing compound, and more preferably a monohydric alcohol having 3 or less carbon atoms.
[0024] In the post-treatment methods exemplified above as (Post-treatment 1) to (Post-treatment 6), the PAS resin may be dried in a vacuum, in air, or in an inert gas atmosphere such as nitrogen.
[0025] The PAS resin constituting the PAS resin particles used in this embodiment can be a resin newly polymerized by the above method, or a recycled PAS resin. For example, a PAS resin recovered from a PAS resin composition or a PAS resin molded product can be used. Specifically, a PAS resin obtained by heating a PAS resin composition or a PAS resin molded product in an organic polar solvent to dissolve the PAS resin contained therein and then performing the above-mentioned post-treatment on the resulting solution can be used.
[0026] (Melt Viscosity) The melt viscosity of the PAS resin constituting the PAS resin particles used in this embodiment is not particularly limited, but the melt viscosity (V6) measured at 300°C is preferably 1 to 800 Pa s, more preferably 3 to 500 Pa s, and even more preferably 5 to 200 Pa s. The melt viscosity (V6) is measured using a flow tester, CFT-500D, manufactured by Shimadzu Corporation, at 300°C and a load of 1.96 × 10 6 The melt viscosity is measured after holding the sample at a temperature of 10 Pa and L / D=10 (mm) / 1 (mm) for 6 minutes.
[0027] (Non-Newtonian Index) The non-Newtonian index of the PAS resin constituting the PAS resin particles used in this embodiment is not particularly limited, but is preferably 0.90 to 1.25, and more preferably 0.95 to 1.20. However, in the present disclosure, the non-Newtonian index (N value) is a value calculated using the following formula after measuring the shear rate (SR) and shear stress (SS) using a capillary rheometer under conditions of a melting point of +20°C and an orifice length (L) to orifice diameter (D) ratio of L / D = 40. The closer the non-Newtonian index (N value) is to 1, the more linear the structure is, and the higher the non-Newtonian index (N value), the more branched the structure is.
[0028] [where SR is the shear rate (sec -1 ), SS is the shear stress (dyne / cm 2 ), and K denotes a constant.
[0029] (Zeta Potential) The PAS resin constituting the PAS resin particles used in this embodiment is not particularly limited as long as it does not impair the effects of the present invention. However, the zeta potential measured by the streaming potential method under conditions of pH 7.8 to 8.2 is preferably -50 mV or higher, and more preferably -30 mV or higher. The zeta potential of the PAS resin refers to the average value measured three times by packing approximately 100 mg of PAS resin particles into a cylindrical cell and measuring the zeta potential of the resin particle surface using a SurPASS3 (Anton Paar) in an electrolyte of 1 mmol / L KCl aqueous solution at a measurement temperature of 22 to 26°C. Note that, in order to stabilize the measured value, it is preferable to sieve the PAS resin and select and use PAS resin with a particle diameter of 0.05 to 1.0 mm.
[0030] (Specific Surface Area) The specific surface area of the PAS resin constituting the PAS resin particles used in this embodiment is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 1 to 300 m 2 / g, more preferably 10 to 250 m 2 / g, more preferably 50 to 200m 2 / g, particularly preferably 50 to 150 m 2 / g. The specific surface area of the PAS resin particles can be measured by the method described in the Examples. The specific surface area of the PAS resin is a BET specific surface area measured using a "Tristar II3020" manufactured by Shimadzu Corporation after pretreating the PAS resin particles under vacuum at 60°C for 4 hours.
[0031] (Particle diameter) The PAS resin constituting the PAS resin particles used in this embodiment is preferably a particle. The particle diameter of the PAS resin is not particularly limited as long as it does not impair the effects of the present invention. However, from the viewpoint of excellent adsorption characteristics, the upper limit is preferably about 2 mm, more preferably about 500 μm, and even more preferably about 300 μm. On the other hand, from the viewpoint of excellent handleability and liquid transferability when packed into a column, the lower limit is preferably about 10 μm, more preferably about 20 μm, and even more preferably about 30 μm. The average particle diameter of the PAS resin is the average particle diameter (D 50 )
[0032] The PAS resin particles are preferably in a wet state containing water, from the viewpoint of excellent adsorption speed at the start of use. The water content of the PAS resin particles is not particularly limited, but from the viewpoint of the balance between adsorption ability and transportation costs, it is preferably 1 to 500 parts by mass, more preferably 10 to 250 parts by mass, and even more preferably 10 to 150 parts by mass, per 100 parts by mass of the PAS resin particles. It may also be 0 part by mass (dry product).
[0033] The PAS resin particles used in this embodiment may be recycled PAS resin particles that have been used as an adsorbent. The PAS resin particles can be recycled, for example, by the method described below.
[0034] The PAS resin particles used in this embodiment preferably do not contain any external additives (components present outside the PAS resin particles, mainly components present at the interface between the PAS resin particles and the liquid) other than the PAS resin particles (excluding unavoidable components derived from the polymerization reaction of the PAS resin and water), such as known and commonly used additives such as surfactants (dispersants), colorants, antistatic agents, antioxidants, heat stabilizers, UV stabilizers, UV absorbers, foaming agents, flame retardants, flame retardant assistants, rust inhibitors, mold release agents, and coupling agents. The absence of any other components other than the PAS resin particles as components constituting the PAS resin particles means that the PAS resin content in the particles, excluding the unavoidable components and water, is preferably 95% by mass or more, more preferably 99% by mass or more, and even more preferably 99.9% by mass or more. The upper limit of this content is not particularly limited, but it is generally 100% by mass or less.
[0035] Furthermore, the PAS resin particles preferably do not contain, as internal additives (components present inside the PAS resin particles due to melt-kneading) constituting the particles, any other components than the PAS resin (excluding unavoidable components derived from the polymerization reaction of the PAS resin), such as known and commonly used additives such as surfactants (dispersants), colorants, antistatic agents, antioxidants, heat stabilizers, UV stabilizers, UV absorbers, foaming agents, flame retardants, flame retardant assistants, rust inhibitors, mold release agents, and coupling agents. The absence of any other components than the PAS resin as components constituting the particles means that the content of the PAS resin in the PAS resin particles, excluding the unavoidable components, is preferably 95% by mass or more, more preferably 99% by mass or more, and even more preferably 99.9% by mass or more. The upper limit of this content is not particularly limited, but it means that it is in the range of 100% by mass or less.
[0036] The inevitable components resulting from the polymerization reaction of the PAS resin include unreacted raw materials and by-products used in the polymerization reaction, particularly metal atom-containing components thereof, such as sulfidizing agents (alkali metal sulfides or alkali metal hydrosulfides) and alkali metal halides, and compounds represented by the following general formula (1):
[0037] (wherein n is 0 to 2, and Y 1 represents a halogen atom, Y 2 represents a hydrogen atom or a halogen atom, R 1 represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a cyclohexyl group; R 2 represents an alkylene group having 3 to 5 carbon atoms, and X represents an alkali metal atom.
[0038] When the PAS resin particles contain the above-mentioned external additives or internal additives, the proportion of sulfur components on the particle surface that contribute to the adsorption capacity may decrease, or the affinity of the particles for the solution may decrease, resulting in a decrease in adsorption characteristics.
[0039] In this embodiment, the aqueous solution to be brought into contact with the PAS resin particles is an aqueous solution containing the substance to be separated and water as essential components (hereinafter, simply referred to as "aqueous solution"). The aqueous solution does not substantially contain a surfactant.
[0040] The aqueous solution may contain a weak acid such as acetic acid, formic acid, carbonic acid, oxalic acid, phosphoric acid, etc., or a strong acid such as hydrochloric acid, sulfuric acid, nitric acid, aqua regia, etc. Furthermore, in the separation and recovery method according to this embodiment, there is no limitation on the pH of the aqueous solution containing the substance to be separated, and for example, the substance to be separated can be adsorbed from the aqueous solution containing the substance to be separated using PAS resin particles under strongly acidic conditions.
[0041] - Substances to be separated
[0042] Examples of substances to be separated that can be applied to this embodiment include metal atoms or compounds containing metal atoms (however, sodium atoms and lithium atoms are excluded as metal atoms). Examples of the metal atoms include at least one selected from the group consisting of alkali metal atoms, alkaline earth metal atoms, transition metal atoms, lanthanoid atoms, and actinoid atoms. These may exist as metal atoms alone or may be bonded with other atoms to form compounds or alloys. Among these, transition metals are preferred, and metal atoms classified as soft acids under the HSAB rule are even more preferred. This is thought to be because the PAS resin used as the adsorbent is primarily composed of sulfur atoms, which are classified as soft bases under the HSAB rule.
[0043] The metal atom or compound containing a metal atom (metal salt) of the substance to be separated is not particularly limited, but examples thereof include alkali metal atoms such as potassium, rubidium, cesium, and francium; alkaline earth metal atoms such as calcium, strontium, barium, and radium; transition metal atoms such as scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, yttrium, zirconium, niobium, molybdenum, technetium, ruthenium, rhodium, palladium, silver, cadmium, lanthanoids, hafnium, tantalum, tungsten, rhenium, osmium, iridium, platinum, gold, and mercury; and base metal atoms such as aluminum, zinc, gallium, germanium, indium, tin, antimony, mercury, thallium, lead, bismuth, and polonium, as well as salts containing them. Examples of lanthanoids include lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium. Examples of actinoids include actinium, thorium, protactinium, uranium, neptunium, plutonium, americium, curium, berkelium, californium, einsteinium, fermium, mendelevium, nobelium, and lawrencium. Among these, metal atoms classified as soft acids according to the HSAB rule or compounds containing such metal atoms are preferred because they are easily adsorbed by PAS resin. For example, ruthenium, rhodium, palladium, silver, cadmium, osmium, iridium, platinum, gold, mercury, thallium, and lead, as well as metal salts thereof, are preferred, and palladium and metal salts containing palladium are particularly preferred.
[0044] The metal atom of the substance to be separated may be a metal complex coordinated with a ligand such as an acid, a base, or an organic substance. The three-dimensional structure is not particularly limited as long as it does not impair the effects of the present invention, and examples include a tetrahedral, square planar, triangular bipyramidal, square pyramidal, and regular octahedral structure, with a square planar structure being particularly preferred. The coordination number is also not particularly limited, but from the viewpoint of stability, 4 to 7 coordinations are preferred. The molecular weight of the metal complex is not particularly limited, but from the viewpoint of adsorption, a molecular weight of 2000 or less is preferred. When a metal complex is used as the substance to be separated, a complex with a fast ligand exchange rate is preferred, and a metal complex containing palladium(II) is more preferred.
[0045] In this embodiment, the amount of the substance to be separated contained in the aqueous solution brought into contact with the PAS resin particles is not particularly limited, but the metal concentration of the substance to be separated in the liquid is preferably 1000 ppm or less, more preferably 200 ppm or less, even more preferably 20 ppm or less, and particularly preferably 10 ppm or less. Within this range, the substance to be separated can be efficiently adsorbed onto the PAS resin particles.
[0046] Eluent: In this embodiment, the eluent brought into contact with the PAS resin particles is an alkaline aqueous solution or an aqueous solution containing a sulfur- or nitrogen-containing chelating agent. In this disclosure, elution refers to the process in which a substance to be separated that has been adsorbed on the PAS resin particles is desorbed from the PAS resin particles and dissolved in the aqueous solution.
[0047] The alkaline aqueous solution applicable to this embodiment is not particularly limited as long as it does not impair the effects of the present invention, and may be any solution having a pH of 7 or higher at room temperature (23°C), such as an aqueous solution of alkaline hydroxide, such as an aqueous solution of sodium hydroxide or an aqueous solution of potassium hydroxide, with an aqueous solution of sodium hydroxide being particularly preferred from the viewpoint of elution rate. The concentration of the alkaline aqueous solution is not particularly limited, but is preferably 0.5 mol / L or higher and 2 mol / L or lower from the viewpoint of efficiently eluting the substance to be separated.
[0048] The sulfur- or nitrogen-atom-containing chelating agent applicable to this embodiment is not particularly limited as long as it does not impair the effects of the present invention. Examples include thiourea, potassium thiocyanate, and thiosulfuric acid, as well as ammonium salts such as ammonium chloride, ammonium nitrate, ammonium thiocyanate, ammonium acetate, ammonium carbonate, ammonium sulfate, ammonium thiosulfate, ammonium sulfide, and ammonium phosphate; ammonia; and amines such as diethylamine, dimethylethanolamine, triethylamine, ethylenediamine, hexanediamine, and melamine. Thiourea, ammonium thiocyanate, ethylenediamine, and dimethylethanolamine are preferred because of their excellent elution properties for the target substance adsorbed to the PAS resin particles. These chelating agents may be dissolved in water or in an acidic or basic aqueous solution such as hydrochloric acid or sodium hydroxide. The concentration of the chelating agent in the aqueous solution is not particularly limited, but is preferably 0.5% by mass or more and 5% by mass or less from the viewpoint of efficient elution of the target substance.
[0049] Step (1) The separation and recovery method according to this embodiment includes step (1) of contacting an aqueous liquid containing a substance to be separated with PAS resin particles, selectively adsorbing the substance to be separated contained in the organic solvent onto the PAS resin particles, and removing it from the aqueous solution.
[0050] In this step, the contact between the aqueous solution and the PAS resin particles can be achieved, for example, by adding the PAS resin particles to the aqueous solution, so that the substances to be separated contained in the aqueous solution are selectively adsorbed onto the PAS resin particles and removed from the aqueous solution. At this time, in order to suppress aggregation of the PAS resin particles, mechanical shear force such as stirring, vibration, or ultrasonic irradiation can be applied.
[0051] The proportion of the PAS resin particles used in relation to the aqueous solution containing the substance to be separated is not particularly limited. However, after measuring the concentration of the substance to be separated in advance, if the substance to be separated is a metal, the PAS resin particles can be used in a mass ratio preferably in the range of 1 to 1000 times, more preferably 5 to 500 times, and even more preferably 10 to 100 times the substance to be separated.
[0052] Furthermore, the separation and recovery method according to this embodiment may include a solid-liquid separation step of the PAS resin particles and the aqueous solution. Examples of solid-liquid separation include sedimentation, flotation, sand filtration, centrifugation, micromembrane filtration, and ultrafiltration. This allows the PAS resin particles to be efficiently contacted with the eluent in the subsequent step (2), making it easy to recover the substance to be separated.
[0053] In addition, the contact between the PAS resin particles and the aqueous solution in this step can be carried out, for example, by immobilizing the PAS resin particles by filling a column or supporting them on fibers or a membrane, and then supplying the aqueous solution thereto, thereby selectively adsorbing the substances to be separated contained in the aqueous solution onto the PAS resin particles and removing them from the aqueous solution. In this case, when performing separation treatment using a batch system, a method of supplying the aqueous solution to a container in which the PAS resin particles are immobilized can be exemplified. When performing separation treatment using a continuous system, a method of immobilizing the PAS resin particles in a flow path can be exemplified, and the aqueous solution can be supplied into the flow path. For immobilization, any known method can be used as long as it allows separation from the aqueous solution by partitioning the PAS resin particles with a wall having pores of a size that allows the liquid to pass through but not the PAS resin particles. By fixing the PAS resin particles, solid-liquid separation of the PAS resin particles and the aqueous solution can be easily performed. However, there is a possibility that PAS resin particles with small particle sizes may be mixed into the aqueous solution after solid-liquid separation. If it is necessary to avoid this, a separate solid-liquid separation process such as sedimentation, flotation, sand filtration, centrifugation, precision membrane filtration, or ultramembrane filtration can also be performed.
[0054] Furthermore, when performing separation treatment in a continuous manner as described above, from the viewpoint of the adsorption efficiency of the substance to be separated, the space velocity (SV) of the aqueous solution in the flow path is preferably 200 or less, more preferably 100 or less, and even more preferably 20 or less. Within this range, the adsorbent is excellent in the efficiency of separating the substance to be separated from the aqueous solution. Note that the space velocity (SV) in the present disclosure is determined by the volume (m 3 ) how many times the amount of solution (m 3 ) is passed through.
[0055] The PAS resin particles of the present disclosure are brought into contact with the aqueous solution containing the substance to be separated in the absence of a surfactant, that is, in an environment where no surfactant is present.
[0056] Step (2) The separation and recovery method according to this embodiment includes step (2) of bringing the PAS resin particles into contact with an eluent to elute the substance to be separated.
[0057] In this step, the PAS resin particles are brought into contact with the eluent by, for example, adding the PAS resin particles to the eluent, thereby desorbing the substances to be separated that have been adsorbed onto the PAS resin particles and dissolving them in the eluent. At this time, in order to suppress aggregation of the PAS resin particles, mechanical shear force such as stirring, vibration, or ultrasonic irradiation can be applied.
[0058] The ratio of the PAS resin particles to the eluent used is not particularly limited as long as it does not impair the effects of the present invention, but the eluent can be used in a mass ratio of preferably 1 to 1000 times, more preferably 5 to 500 times, and even more preferably 10 to 100 times, the PAS resin particles.
[0059] Furthermore, the separation and recovery method according to this embodiment may include a solid-liquid separation step of the PAS resin particles and the eluent. Examples of solid-liquid separation include sedimentation, flotation, sand filtration, centrifugation, precision membrane filtration, and ultrafiltration. This makes it easy to remove the PAS resin particles from which the substances to be separated have been desorbed and reuse them after the solid-liquid separation.
[0060] In addition, the contact between the PAS resin particles and the eluent in this process can be carried out, for example, by immobilizing the PAS resin particles by filling them into a column or supporting them on fibers or a membrane, and then supplying the eluent thereto, thereby dissolving the separation target substance adsorbed on the PAS resin particles in the eluent and desorbing it from the adsorbent. In this case, in the case of a batch recovery process, a method in which the eluent is supplied to a container in which the PAS resin particles are immobilized can be exemplified, and in the case of a continuous separation process, a method in which the PAS resin particles are immobilized in a flow path can be exemplified, and the like. The immobilization method is the same as described above.
[0061] Furthermore, when performing the elution treatment in a continuous manner as described above, from the viewpoint of the concentration of the substance to be separated, the space velocity (SV) in the flow path of the eluent is preferably 30 or less, and more preferably 10 or less. This range is preferable because the concentration of the substance to be separated increases and the load on the subsequent process of recovering the substance to be separated from the eluent is reduced. Note that, in the present disclosure, the concentration is the ratio of the concentration of the substance to be separated in the aqueous solution containing the substance to be separated before contact in step (1) to the concentration of the substance to be separated in the eluent recovered after elution in step (2).
[0062] The PAS resin particles separated by solid-liquid separation in this process can be regenerated by washing or the like and reused as an adsorbent in a new separation and recovery process. The regeneration method is not particularly limited, but examples include washing the PAS resin particles after solid-liquid separation of the eluent with preferably 2 parts by mass or more of water, more preferably 5 parts by mass or more of water. When the PAS resin particles are immobilized in a container or flow path as described above, water can be supplied and contacted after use. The temperature when washing with water is not particularly limited, but using water at 23°C or higher is preferred from the perspective of washing efficiency. Furthermore, a step of washing the adsorbent with an acidic aqueous solution such as hydrochloric acid to further remove impurities may be included before, after, or during the water washing. When used as a regenerated product, it is preferable from the perspective of adsorption performance that 95% or more of the adsorbed separation target substance is eluted, i.e., an elution rate of 95% or more.
[0063] The reason why PAS resin particles can be sufficiently regenerated by simply washing with water is thought to be because they have high selectivity for the substances to be separated during adsorption and adsorption of impurities is low. However, the above mechanism is merely speculative, and even if the effect is achieved for other reasons, it is still within the technical scope of the present invention.
[0064] Furthermore, the reasons why the separation and recovery method according to this embodiment is excellent in the separation and recovery of the target substance and in the recyclability of the adsorbent are not entirely clear, but are presumed to be due to the following reasons. That is, first, while conventional ion exchange resins and chelating resins have a mechanism of action in which polar functional groups in the side chains ion-exchange or coordinate with the target substance to be separated, the PAS resin used as the adsorbent in this embodiment is thought to have a mechanism of action in which sulfur atoms in the main chain coordinate with the target substance to be separated. Therefore, it is presumed that this difference in mechanism results in excellent separation and recovery capabilities and recyclability, and therefore even hydroxide ions with weak chelating power can be eluted. Note that the above mechanism is merely presumed, and even cases in which the effects of the present invention are achieved for other reasons are within the technical scope of the present invention.
[0065] The present invention will be specifically described below with reference to examples. These examples are illustrative and not limiting. Unless otherwise specified, "%" and "parts" are based on mass.
[0066] Synthesis Example 1 (PAS resin polymerization process) 33.222 kg (226 mol) of p-dichlorobenzene (hereinafter abbreviated as DCB), 2.280 kg (23 mol) of NMP, 27.300 kg (230 mol) of 47.23% by mass sodium hydrosulfide, and 18.533 kg (228 mol) of 49.21% by mass caustic soda were charged into a 150 L autoclave equipped with a pressure gauge, a thermometer, a condenser, a decanter, and a rectification column, and the temperature was raised to 173 ° C. over 5 hours under a nitrogen atmosphere with stirring. 27.3 kg of water was distilled off, and the kettle was then sealed. The DCB distilled by azeotropy during dehydration was separated using a decanter and returned to the kettle as needed. After completion of dehydration, the anhydrous sodium sulfide composition was dispersed in the DCB in the kettle. The internal temperature was then cooled to 160°C, and 47.492 kg (479 mol) of NMP was charged, followed by heating to 185°C. When the pressure reached 0.00 MPa, the valve connected to the distillation column was opened, and the internal temperature was raised to 200°C over 1 hour. During this time, the cooling and valve opening were controlled so that the outlet temperature of the distillation column would be 110°C or lower. The distilled mixed vapor of DCB and water was condensed in a condenser and separated in a decanter, and the DCB was returned to the kettle. The amount of distilled water was 179 g. Next, the internal temperature was raised from 200°C to 230°C over 3 hours, and stirred for 1 hour. After that, the temperature was raised to 250°C and stirred for 1 hour. After the reaction was completed, the internal temperature of the autoclave was cooled from 250°C to 235°C. After reaching this temperature, the bottom valve of the autoclave was opened and the contents were flushed into a 150-liter vacuum agitation dryer equipped with an agitator (desolventizer jacket temperature: 120°C) while still under reduced pressure to remove N-methyl-2-pyrrolidone. The contents were then cooled to room temperature and sampled, resulting in a PPS mixture with an N.V. of 55%.
[0067] (PAS Resin Purification Process) 400 g of the PPS mixture obtained in Synthesis Example 1 and 317 g of methanol were placed in a flask and stirred and mixed at 40°C for 30 minutes. The resulting slurry was vacuum filtered using a Kiriyama funnel, compacted from above, and then 634 g of methanol was poured in several portions from above and filtered. The filtered cake was then transferred to a beaker and crushed into powder using a medicine spoon. 634 g of 70°C water was poured into the cake and stirred and mixed for 30 minutes. The slurry was vacuum filtered using a Kiriyama funnel, compacted from above, and then 845 g of 70°C water was poured in several portions from above and filtered. The cake was transferred to a beaker, and 636 g of carbonated water was poured into the cake and stirred and mixed for 1 hour. The slurry was vacuum filtered using a Kiriyama funnel, compacted from above, and then 848 g of carbonated water was poured in several portions from above and filtered to obtain a wet cake (PPS particles). The moisture content of the PPS particles calculated from the loss on drying was 45 wt%.
[0068] <Production Example 1> (Preparation of Aqueous Solution Containing Substance to be Separated) Kanto Chemical Co., Inc.'s "Palladium Standard Stock Solution Pd1000" was dissolved in a 0.1 mol / L aqueous hydrochloric acid solution so that the palladium concentration was 10 mg / L (ppm) or 100 mg / L (ppm), to prepare a 10 ppm palladium standard solution and a 100 ppm palladium standard solution.
[0069] Examples 1 to 16, Comparative Examples 1 to 3 Step (1) 9.1 g of the PPS particles produced in Synthesis Example 1 (5.0 g as PPS resin) and 1 L of the 100 ppm palladium standard solution produced in Production Example 1 were placed in a 2 L beaker and stirred for 3 hours, after which the PPS resin was recovered by solid-liquid separation through suction filtration. The palladium concentration in the filtrate was measured with an atomic absorption spectrophotometer, and the amount of palladium adsorption to PPS was calculated to be 20.0 mg / g.
[0070] Step (2): The palladium-adsorbed PPS particles obtained in step (1) were dispensed into 30 mL test tubes so that the PPS resin content was 0.05 g (1 mg of adsorbed palladium). 5 mL of eluent having the composition shown in Tables 1 to 3 was added to each tube. The mixture was then shaken horizontally at 200 rpm for 3 hours using a shaker ("SA300" manufactured by Yamato Scientific Co., Ltd.) at a liquid temperature of 30°C. This treatment allowed the elution state to reach equilibrium. The liquid phase component was then recovered by solid-liquid separation using suction filtration. The elution rate (%) was calculated from the palladium concentration (ppm) of the liquid phase component at equilibrium using the following formula. The results are shown in Tables 1 to 3. Elution rate (%) = Amount of palladium in liquid phase component (mg) / 1 mg × 100. Note that 1 mg in this formula represents the amount of palladium when 0.05 g of 20.0 mg / g palladium-adsorbed PPS particles was used.
[0071]
[0072]
[0073]
[0074] Example 17 - Step (1) A glass cylindrical column with an inner diameter of 9 mm and a height of 100 mm was packed with 6.4 ml (1.8 g as PPS resin) of the PPS particles obtained in Synthesis Example 1, and the 10 ppm palladium standard solution prepared in Production Example 1 was passed through the column at 10 ml / min (SV = 10). The aqueous solution discharged from the column outlet was then collected in 10 600 mL portions. The palladium concentrations of the resulting aqueous solutions were measured, and the average values were below 10 ppb, the measurement limit of the atomic absorption spectrophotometer. The solution was then passed through the column until the adsorption capacity of the adsorbent was saturated and the palladium concentration in the discharged solution became constant at 10 ppm. Then, to remove unadsorbed palladium, 64 mL of a 0.1 mol / L aqueous hydrochloric acid solution was passed through the column, followed by 64 mL of ultrapure water. At this time, the amount of palladium adsorbed on the column was 59.9 g, and the amount of palladium adsorbed on the PPS resin was 33.3 mg / g. Amount of palladium (mg) = Amount of palladium (mg) in liquid phase component - Amount of palladium (mg) in discharged liquid
[0075] Step (2): A 1 mol / L aqueous sodium hydroxide solution was passed through the column that had undergone step (1) as the eluent at SV = 10. First, 32 mL (5 times the column volume) of eluent was passed through, and the concentration was calculated from the metal content of the recovered solution using the following formula. Note that 10 ppm is the concentration of the aqueous solution containing the substance to be separated used in step (1). Concentration (times) = palladium concentration in the recovered solution (ppm) / 10 (ppm). Next, an additional 64 mL of eluent was passed through, and the elution rate was calculated from the metal content of the 96 mL recovered solution, combined with the previously recovered solution, using the following formula. Note that 59.9 mg is the amount of palladium adsorbed on the column, calculated in step (1). The results are shown in Table 4. Elution rate (%) = amount of palladium in the recovered solution (mg) / 59.9 mg x 100
[0076] Example 18 The same procedure as in Example 17 was carried out, except that the space velocity (SV) of the eluent in step (2) was set to 30. The results are shown in Table 4.
[0077] Example 19 The same procedure as in Example 17 was carried out, except that the space velocity (SV) of the eluent in step (2) was 100. The results are shown in Table 4.
[0078] Comparative Example 4 The same procedure as in Example 17 was carried out, except that the eluent in step (2) was changed from 1 mol / L aqueous sodium hydroxide solution to ultrapure water. The results are shown in Table 4.
[0079] Comparative Example 5 The same procedure as in Example 17 was carried out, except that the eluent in step (2) was changed from a 1 mol / L aqueous sodium hydroxide solution to a 0.1 mol / L aqueous hydrochloric acid solution. The results are shown in Table 4.
[0080]
[0081] Example 20: An additional 64 ml of ultrapure water was passed through the column that had undergone steps (1) and (2) in Example 17 to wash and regenerate the PPS particles. Using this column, steps (1) and (2) similar to those in Example 17 and the regeneration by water washing were repeated 10 times. The adsorption rate and elution rate for each run are shown in Table 5. Adsorption rate (%) = Amount of palladium adsorbed for each run (mg) / Amount of palladium adsorbed in Example 17 (mg) × 100 Elution rate (%) = Amount of palladium eluted for each run (mg) / Amount of palladium adsorbed for each run (mg) × 100
[0082]
[0083] <Evaluation>
[0084] (1) Evaluation of Metal Content of Solution The palladium concentration and amount of the solution in each example and comparative example were measured by the furnace method using a Shimadzu Corporation atomic absorption spectrophotometer "GFA-7000A." For the calibration curve, solutions were used in which "Palladium Standard Stock Solution (Pd 1000)," a palladium standard solution for atomic absorption spectrometry manufactured by Kanto Chemical Co., Ltd., was diluted with 0.5% by volume of nitric acid aqueous solution to 0, 50, 100, 150, 200, and 250 ppb. The measurement solution was also diluted with 0.5% by volume of nitric acid aqueous solution to fall within the calibration curve range of 0 to 250 ppb.
[0085] Comparing Examples 1 to 16 with Comparative Examples 1 to 3 from Tables 1 to 3, it was found that the elution rate was excellent when the eluent used was an alkaline aqueous solution or an aqueous solution containing a sulfur atom- or nitrogen atom-containing chelating agent, demonstrating that the method of the present disclosure is a method for efficiently separating and recovering metal atoms, which are the target substances to be separated. Table 4 suggests that, as another embodiment, even when PPS particles are supported on a column, the separation and recovery method of the present disclosure, which utilizes a specific eluent, has an excellent elution rate. Furthermore, it was confirmed that the excellent elution rate also results in a high concentration. Table 5 suggests that the separation and recovery method of the present disclosure can maintain its performance even when repeatedly performed.
Claims
1. A separation and recovery method for separating and recovering a substance to be separated from an aqueous solution containing the substance using polyarylene sulfide resin particles, comprising: a step (1) of contacting the aqueous solution containing the substance to be separated with polyarylene sulfide resin particles, selectively adsorbing the substance to be separated contained in the aqueous solution onto the polyarylene sulfide resin particles, and removing the substance from the aqueous solution; and a step (2) of contacting the polyarylene sulfide resin particles with an eluent to elute the substance to be separated, wherein the substance to be separated is a metal atom or a compound containing a metal atom (however, sodium atoms and lithium atoms are excluded as metal atoms), and the eluent is an alkaline aqueous solution or an aqueous solution in which a chelating agent containing sulfur atoms or nitrogen atoms is dissolved.
2. The separation and recovery method according to claim 1, wherein the aqueous solution containing the substance to be separated and the polyarylene sulfide resin particles are contacted in the absence of a surfactant.
3. A separation and recovery method according to claim 1 or 2, wherein the polyarylene sulfide resin particles used in step (1) are regenerated products, that is, regenerated polyarylene sulfide resin particles that have been regenerated by adsorbing the substance to be separated, contacting the eluent, and then washing with water.
4. The separation and recovery method according to claim 3, wherein the elution rate of the recycled polyarylene sulfide resin particles is 95% or more.
5. A separation and recovery method as described in claim 1 or 2, wherein the method of contacting the polyarylene sulfide resin particles with the aqueous solution containing the substance to be separated and the eluent in steps (1) and (2) comprises supplying an aqueous solution containing the substance to be separated and an eluent, respectively, to the polyarylene sulfide resin particles fixed in the flow path to bring them into contact with each other.
6. The separation and recovery method according to claim 5, wherein the aqueous solution containing the substance to be separated has a space velocity (SV) of 100 or less in the flow path.
7. The separation and recovery method according to claim 5 or 6, wherein the space velocity (SV) of the eluent in the flow path is 30 or less.