Cover tape for electronic component packaging and electronic component packaging body
Patent Information
- Application Number
- MYPI2025005397
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-21
- Publication Date
- 2024-09-24
AI Technical Summary
Conventional cover tapes for electronic component packaging face issues with blocking and sticking, where the tapes tend to stick together during storage and electronic components adhere to the cover tape during transportation, making it difficult to retrieve the components.
A cover tape design with a specific surface texture characterized by a peak density (Spd) of 3×10^5 to 1×10^6/mm² and developed area ratio (Sdr) of 1×10^-3 to 5×10^-2, incorporating an inorganic particle-containing sealant layer and an intermediate polyethylene layer, which reduces contact area and prevents adhesion.
The optimized surface texture and composition effectively suppress blocking and sticking, ensuring easier unwinding and improved component retrieval, even under severe conditions like high temperatures.
Smart Images

Figure PI2025005397_DRAWING_001
Abstract
Description
Cover tape for packaging electronic components and electronic component packaging
[0001] The present invention relates to a cover tape for packaging electronic components and an electronic component package.
[0002] Electronic components such as transistors, diodes, capacitors, and piezoelectric resistors are sometimes transported in the form of "electronic component packages." These packages are housed in recesses in a carrier tape, which are formed with recesses capable of accommodating the electronic components to prevent damage, and a cover tape is heat-sealed to the carrier tape to seal the electronic components in the recesses. Electronic component packages are often imported and exported internationally by air or sea. When the packaged electronic components are to be used, the cover tape in the electronic component package is peeled off and the packaged electronic components are removed from the recesses.
[0003] The following patent documents can be cited as prior art relating to cover tapes (cover tapes for packaging electronic components) intended for use in the above-described manner.
[0004] JP 2017-171393 A International Publication No. 2012 / 079258 JP 2003-246358 A
[0005] Through research into improving conventional cover tapes, the inventors have found that conventional cover tapes still have room for improvement in the following points (i) and (ii): (i) Blocking: Cover tapes are typically long and wound up before use. At this time, the cover tapes may stick together, making them difficult to peel. (ii) Sticking of components: In electronic component packages obtained by heat-sealing a cover tape to a carrier tape, electronic components housed in recesses in the carrier tape may stick to the cover tape due to vibrations during transportation, etc. When such sticking occurs, it becomes difficult to properly remove the electronic components when peeling the cover tape from the carrier tape.
[0006] The present invention has been made in view of the above circumstances, and one of the objects of the present invention is to provide a cover tape for packaging electronic components that suppresses blocking and prevents components from sticking.
[0007] The present inventors have investigated improvements to cover tapes from various perspectives in order to solve the above-mentioned problems. Through their investigations, they have found that the condition of the surface (exposed surface) of the sealant layer in the cover tape appears to be related to blocking and adhesion of electronic components. Based on this finding, the present inventors have completed the invention provided below, which has solved the above-mentioned problems.
[0008] 1. A cover tape for packaging electronic components comprising a base layer and a sealant layer provided on one side of the base layer, wherein the surface of the sealant layer opposite to the base layer is an exposed surface, and the peak density Spd of the exposed surface as defined in ISO 25178 is 3 x 10 5 ~1 x 10 6 / mm 2 The developed area ratio Sdr of the interface defined in ISO 25178 of the exposed surface is 1 × 10 ―3 ~5 x 10 ―2 2. The cover tape according to 1., wherein the arithmetic mean height Sa of the exposed surface as defined in ISO 25178 is 0.05 to 0.5 μm. 3. The cover tape according to 1. or 2., wherein the sealant layer contains inorganic particles. 4. The cover tape according to any one of 1. to 3., wherein the sealant layer contains one or both of a styrene-based resin and a (meth)acrylic-based resin. 5. The cover tape according to any one of 1. to 4., wherein the base layer contains polyester. 6. The cover tape according to any one of 1. to 5., wherein the cover tape comprises an intermediate layer between the base layer and the sealant layer. 7. The cover tape according to 6., wherein the intermediate layer contains a polyethylene-based resin. 8. A cover tape comprising a carrier tape having electronic components housed in recesses, and a cover tape according to 1. to 7. and the cover tape according to any one of the preceding items, wherein the sealant layer is adhered to the carrier tape so as to seal the electronic component.
[0009] According to the present invention, there is provided a cover tape for packaging electronic components that is inhibited from blocking and prevents components from sticking.
[0010] 1 is a diagram showing a schematic view of an example of a layer structure of a cover tape, and FIG. 2 is a diagram showing an example of a state in which the cover tape is bonded (heat sealed) to a carrier tape.
[0011] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. In all drawings, similar components are given the same reference numerals, and descriptions thereof will be omitted where appropriate. To avoid complexity, (i) when multiple identical components are present in the same drawing, only one of the components is given a reference numeral, and not all of the components are given a reference numeral, or (ii) particularly in Figure 2 and subsequent figures, components similar to those in Figure 1 are not given a reference numeral again. All drawings are for illustrative purposes only. The shapes and dimensional ratios of each component in the drawings do not necessarily correspond to actual objects.
[0012] In this specification, unless otherwise specified, the expression "X to Y" in the description of a numerical range means at least X and at most Y. For example, "1 to 5% by mass" means "at least 1% by mass and at most 5% by mass."
[0013] In this specification, the term "(meth)acrylic" represents a concept that encompasses both acrylic and methacrylic. The same applies to similar terms such as "(meth)acrylate."
[0014] <Cover Tape for Packaging Electronic Components> Fig. 1 is a schematic diagram showing an example of the layer structure of a cover tape (cover tape 10) for packaging electronic components according to this embodiment. The cover tape 10 includes a substrate layer 1 and a sealant layer 3 provided on at least one side of the substrate layer 1. The side of the sealant layer 3 opposite the substrate layer 1 is exposed (contacting air). The cover tape 10 preferably includes an intermediate layer 2 between the substrate layer 1 and the sealant layer 3.
[0015] The peak density Spd of the exposed surface of the sealant layer 3 as defined in ISO 25178 is 3×10 5 ~1 x 10 6 / mm 2, preferably 3.5×10 5 ~9 x 10 5 / mm 2 , and more preferably 3.5 × 10 5 ~8 x 10 5 / mm 2 The developed area ratio Sdr of the interface of the exposed surface of the sealant layer 3 defined in ISO 25178 is 1×10 ―3 ~5 x 10 ―2 , preferably 5 × 10 ―3 ~3 x 10 ―2 , more preferably 1 × 10 ―2 ~3 x 10 ―2 is.
[0016] The reason why blocking and component sticking are suppressed when Spd and Sdr are within appropriate numerical ranges can be explained as follows: Please note that the following explanation includes speculation, and the present invention is not limited by the following explanation.
[0017] The peak density Spd is the density of the peaks on the surface of the object to be measured. 2 This represents the number of peaks larger than a predetermined size per pixel. Unless otherwise specified, the predetermined size is set to 5% of the maximum amplitude of the contour surface. 5 / mm 2 That Spd is equal to or greater than this means that a certain density of "protrusions" is present on the exposed surface of the sealant layer 3. This is thought to reduce the contact area between the electronic component and the sealant layer 3, thereby suppressing adhesion. Furthermore, when the cover tape 10 is wound, the contact area between the base material layer 1 and the sealant layer 3 also reduces, which is thought to suppress blocking. On the other hand, if Spd is too large, problems may arise from a perspective other than the contact area. For example, the cover tape or the electronic component package may be image-inspected with a camera. In this case, if Spd is too large, there is a risk that the image inspection may be hindered. Therefore, in this embodiment, the upper limit of Spd is set to 1 x 10 6 / mm 2 It is set as follows.
[0018] The developed area ratio Sdr of the interface indicates how much the developed area (surface area) of the defined region has increased relative to the area of the defined region (projected area on the xy plane). The Sdr of a completely flat surface is 0. Although the details are unknown, it is possible that Sdr is 1 x 10 ―3 The surface of the sealant layer 3 having the above-mentioned properties has moderate irregularities or undulations, which is thought to reduce the contact area between the electronic component and the sealant layer 3 and suppress sticking. Furthermore, when the cover tape 10 is wound, the contact area between the base material layer 1 and the sealant layer 3 is also reduced, which is thought to suppress blocking. On the other hand, if Sdr is too large, the areas near the peaks of the convex portions become flat, which may make it easier for the electronic component to stick or for blocking to occur. Therefore, in this embodiment, the upper limit of Sdr is set to 5×10 ―2 It is set to.
[0019] Both Spd and Sdr are indices relating to the surface properties of the sealant layer 3. In the cover tape 10, optimizing both of these two indices reduces blocking and component sticking. As far as the inventors have investigated, optimizing one of Spd and Sdr without optimizing the other may make blocking more likely to occur and / or may not sufficiently reduce component sticking.
[0020] The cover tape 10 can be obtained using appropriate materials and by appropriate manufacturing methods and conditions. For example, by paying careful attention to the viscosity of the coating liquid used to form the sealant layer and the conditions for forming the sealant layer, a cover tape 10 with Spd and Sdr within appropriate numerical ranges can be manufactured. Specifically, by coating the surface of the intermediate layer 2 with a solvent-containing coating liquid adjusted to an appropriate viscosity, and by paying attention to drying the solvent to form the sealant layer using an appropriate device, at an appropriate temperature, and for an appropriate time, a cover tape 10 with Spd and Sdr within appropriate numerical ranges can be manufactured. The method for manufacturing the cover tape will be described in detail below.
[0021] The cover tape 10 will be described in more detail below.
[0022] [Base Material Layer] There are no particular limitations on the material that constitutes the base material layer 1. Any film can be used as long as it has the mechanical strength to withstand the external force applied to the cover tape 10 and the heat resistance to withstand the heat during heat sealing.
[0023] Specific examples of materials constituting the base material layer 1 include polyester-based resins, polyamide-based resins, polyolefin-based resins, polyacrylate-based resins, polymethacrylate-based resins, polyimide-based resins, polycarbonate-based resins, ABS resins, etc. Among these, polyester-based resins and polyolefin-based resins are preferred as materials constituting the base material layer 1, and polyester resins, particularly polyethylene terephthalate, which can improve mechanical strength, are preferred.
[0024] The film used to form the base layer 1 may be a stretched film or a uniaxially or biaxially stretched film. From the viewpoint of improving the mechanical strength of the cover tape 10, a uniaxially or biaxially stretched film is preferred.
[0025] The base layer 1 may be a single layer or may be multi-layered. The base layer 1 may contain an antistatic agent from the viewpoint of reducing the amount of static electricity generated when the carrier tape is peeled off. Furthermore, an antistatic layer may be provided as one of the base layers on the surface of the base layer 1 opposite to the surface on which the intermediate layer 2 is provided.
[0026] The thickness of the base material layer 1 is, for example, 6 to 35 μm, preferably 7 to 33 μm, and more preferably 8 to 30 μm. Because the base material layer 1 is not too thick, the rigidity of the cover tape is not too high. Even if torsional stress is applied to the carrier tape after sealing, the cover tape 10 follows the deformation of the carrier tape, reducing the possibility of peeling. Because the thickness of the base material layer 1 is not too thin, the mechanical strength of the cover tape 10 is easily optimized. Furthermore, even when the cover tape 10 is peeled off from the carrier tape at high speed, the possibility of the cover tape 10 breaking can be reduced.
[0027] [Intermediate Layer] The intermediate layer 2 is provided primarily for the purpose of improving the cushioning properties of the cover tape 10. By improving the cushioning properties of the cover tape 10, the pressure of the sealing iron during heat sealing can be more easily transmitted to the cover tape 10. This further improves the adhesion between the cover tape 10 and the carrier tape.
[0028] The material of the intermediate layer 2 is not particularly limited. Any material that can impart cushioning properties to the cover tape 10 can be used without particular limitations. Examples include one or more selected from polyacrylic acid derivatives, polyacrylic acid ester derivatives, polyvinyl acetate derivatives, styrene-based resins, olefin-based resins, and cyclic olefin resins, and copolymers thereof. Among these, polyolefin-based resins are preferred, and polyethylene-based resins are more preferred. From the viewpoint of cushioning properties, low-density polyethylene (density 880 kg / m 3 More than 930kg / m 3 Polyethylene of less than 1000 MPa is preferred.
[0029] The intermediate layer 2 may be a single layer or may be a multilayer. The thickness of the intermediate layer 2 is typically 10 to 50 μm, preferably 15 to 45 μm, from the viewpoint of further improving the adhesion between the cover tape 10 and the carrier tape during heat sealing.
[0030] [Sealant Layer] The sealant layer 3 is provided on at least one side of the substrate layer 1. When the intermediate layer 2 is present, the sealant layer 3 is provided on the side of the intermediate layer 2 opposite to the side in contact with the substrate layer 1. As already mentioned, the peak density Spd of the exposed surface of the sealant layer 3 as defined in ISO 25178 is 3×10 5 ~1 x 10 6 / mm 2 The developed area ratio Sdr of the interface of the exposed surface of the sealant layer 3 defined in ISO 25178 is 1 × 10 ―3 ~5 x 10 ―2 The sealant layer 3 comes into contact with the carrier tape when the cover tape 10 is heat-sealed to the carrier tape. The sealant layer 3 softens or melts when heated by the sealing iron, and adheres to the carrier tape.
[0031] The sealant layer 3 preferably contains a thermoplastic resin. Specifically, the sealant layer 3 contains one or more resins selected from (meth)acrylic resins, styrene resins, olefin resins, urethane resins, and ester resins. Among these, (meth)acrylic resins and styrene resins are preferred from the viewpoints of good heat sealing properties and good dispersion of inorganic particles.
[0032] Specific examples of (meth)acrylic resins include resins having structural units derived from monomers such as acrylic acid, methacrylic acid, methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate; methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, and butyl methacrylate; and acrylonitrile, methacrylonitrile, and acrylamide. The (meth)acrylic resin can contain structural units derived from one or more monomers selected from these examples. Of course, the (meth)acrylic resin may or may not further contain structural units derived from monomers other than these examples.
[0033] Specific examples of styrene-based resins include polystyrene, styrene-butadiene copolymer (SB), styrene-butadiene-styrene block copolymer (SBS), styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-butadiene-butylene-styrene block copolymer (SBBS), styrene-isoprene-styrene block copolymer (SIS), styrene-ethylene-propylene-styrene block copolymer (SEPS), styrene-methyl (meth)acrylate copolymer, hydrogenated styrene block copolymer, high impact polystyrene (HIPS), general purpose polystyrene resin (GPPS), etc. Among these, from the viewpoint of the balance of various performances, styrene-ethylene-butylene-styrene block copolymer (SEBS) or styrene-butadiene-butylene-styrene block copolymer (SBBS) is preferred.
[0034] The ester resin usually comprises a structural unit derived from an alcohol component and a structural unit derived from a carboxylic acid component. Specific examples of the alcohol component include chain or branched aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2,2-dimethyl-1,3-propanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; alicyclic diols such as hydrogenated bisphenol A [2,2-bis(4-hydroxycyclohexyl)propane] and adducts of hydrogenated bisphenol A with alkylene oxides having 2 to 4 carbon atoms (average number of added moles: 2 to 12); and trihydric or higher polyhydric alcohols such as glycerin, pentaerythritol, trimethylolpropane, and sorbitol. These alcohol components may be used alone or in combination. Specific examples of the carboxylic acid component include chain or branched aliphatic dicarboxylic acids such as oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, adipic acid, sebacic acid, dodecanedioic acid, azelaic acid, dodecylsuccinic acid, dodecenylsuccinic acid, and octenylsuccinic acid, trivalent or higher polycarboxylic acids such as trimellitic acid and its anhydride, and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic aromatic dicarboxylic acids. These carboxylic acid components may be used alone or in combination.
[0035] The sealant layer 3 preferably contains inorganic particles. The use of inorganic particles adjusts the condition of the exposed surface of the sealant layer 3, making it easier to achieve desired values for Spd and Sdr, which may further reduce blocking and component sticking. The use of inorganic particles may also be expected to improve peelability from the carrier tape.
[0036] Metal-element-containing particles are one type of inorganic particle. Metal-element-containing particles have relatively high conductivity due to the metal they contain, and can therefore function as an antistatic agent. The use of metal-element-containing particles reduces static damage to the electronic components being packaged.
[0037] Specific examples of metal element-containing particles include metal oxides such as aluminum oxide, tin oxide, zinc oxide, indium oxide, and titanium oxide, and sulfides such as zinc sulfide, copper sulfide, cadmium sulfide, nickel sulfide, and palladium sulfide. Furthermore, examples of particles that do not necessarily contain metal elements but have an antistatic function include carbon fine particles. Metal oxides are preferred as metal element-containing particles because of their availability and ease of adjusting peel strength.
[0038] In particular, from the viewpoint of electrical conductivity, the metal element-containing particles may be doped with a trace element to enhance electrical conductivity. Examples of the trace element include antimony and indium. Particularly preferred antistatic agents are ITO (tin-doped indium oxide) and ATO (antimony-doped tin oxide).
[0039] The average particle size of the inorganic particles is preferably 1 to 1,000 nm, more preferably 3 to 500 nm. By selecting inorganic particles with an appropriate average particle size, it is easy to obtain improvements in other performance properties without excessively impairing the transparency of the sealant layer 3. The average particle size of the inorganic particles can be determined by averaging the circle-equivalent diameters of at least 100 inorganic particles in a microscope image.
[0040] When inorganic particles are used, the amount thereof depends on the intended use of the inorganic particles and the specific gravity of the inorganic particles, but is 40 to 80% by mass, preferably 50 to 70% by mass, of the entire sealant layer 3 (non-volatile components in the sealant layer-forming coating solution in the cover tape manufacturing method described below). Furthermore, on a volume basis, the amount of inorganic particles used is preferably 10 to 40% by volume, more preferably 15 to 35% by volume, of the entire sealant layer 3.
[0041] In addition to Spd and Sdr, it is preferable that the arithmetic mean height Sa defined in ISO 25178 on the exposed surface of the sealant layer 3 be within an appropriate range. By ensuring that Sa is within an appropriate range, further improvements in various performances can be expected. Specifically, Sa is usually 0.05 to 0.5 μm, preferably 0.1 to 0.4 μm, and more preferably 0.1 to 0.3 μm.
[0042] The thickness (dry film thickness) of the sealant layer 3 is preferably 0.05 to 5 μm, more preferably 0.1 to 3 μm, from the viewpoint of obtaining sufficient heat sealability without excessively impairing other performances.
[0043] [Total Thickness] From the viewpoint of balancing strength and ease of handling, the total thickness of the cover tape 10 is preferably 30 to 65 μm, and more preferably 35 to 60 μm.
[0044] <Method of Manufacturing Cover Tape> As described above, the cover tape 10 can be manufactured using appropriate materials and through an appropriate manufacturing process. A suitable manufacturing method and the materials used in the manufacturing method will be described in more detail below.
[0045] First, an intermediate layer 2 is formed on at least one surface of a substrate layer 1. The substrate layer 1 is preferably a film formed from an ester-based resin, an olefin-based resin, or the like. The intermediate layer 2 can be formed, for example, by extrusion lamination or dry lamination. To prevent peeling between the substrate layer 1 and the intermediate layer 2, a layer of, for example, an anchor coating agent may be present between the substrate layer 1 and the intermediate layer 2.
[0046] Next, a coating liquid for forming a sealant layer is applied to the surface of the intermediate layer 2 opposite to the substrate layer 1, and then dried. As a coating method, for example, a gravure coating method can be used.
[0047] The sealant layer-forming coating liquid can typically be prepared by thoroughly mixing a resin (preferably a thermoplastic resin such as the aforementioned (meth)acrylic resin or styrene-based resin), an organic solvent, and, if necessary, additives such as inorganic particles and antistatic components. From the viewpoint of coatability and achieving a desired film thickness, the viscosity of the sealant layer-forming coating liquid is preferably 2 to 10 mPa·s at 28°C when measured using a vibration viscometer in accordance with JIS Z 8803. The viscosity can be adjusted by adjusting the amount of solvent or by using an appropriate organic solvent. The organic solvent that can be used to prepare the sealant layer-forming coating liquid is not particularly limited, but is preferably selected from esters such as ethyl acetate and butyl acetate; ketones such as methyl ethyl ketone, acetone, cyclohexanone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene and xylene; and aliphatic or alicyclic alcohols such as methanol, ethanol, n-propanol, isopropanol, and cyclohexanol.
[0048] In this embodiment, in addition to using a coating liquid with an appropriate viscosity, it is possible to manufacture a cover tape 10 having Spd and Sdr values within appropriate numerical ranges by optimizing the drying conditions of the coating liquid applied to the surface of the intermediate layer 2 opposite the substrate layer 1. Specifically, the sealant layer-forming coating liquid, adjusted to the above-described viscosity, is applied to the intermediate layer to form a coated body, which is then transported through an 8-12 m long drying oven with an oven temperature set to 70-100°C to dry the solvent. The transport speed is set to 140-200 m / min. While the details are unclear, it is believed that the drying of the solvent is uneven and subject to fluctuations. Therefore, by appropriately controlling the viscosity of the coating liquid (particularly related to spreading), as well as the drying rate of the solvent and other drying conditions, unevenness is created on the surface of the sealant layer 3, and the exposed surface of the sealant layer 3 after drying is likely to have surface properties that are favorable for preventing blocking and component sticking. Furthermore, when the sealant layer-forming coating solution contains particles (e.g., particles containing a metal element), it is presumed that the values of Spd and Sdr can be adjusted not only by the viscosity of the coating solution, which is closely related to the ease with which the particles settle, but also by controlling the drying rate of the solvent so that the particles are fixed in an appropriately sunk state (or an appropriately floating state) in the final sealant layer 3.
[0049] <Electronic Component Packaging> An electronic component packaging can be obtained from the cover tape 10 described above and a carrier tape having electronic components housed in recesses. This will be described with reference to FIG.
[0050] 2, the cover tape 10 for packaging electronic components is used as a lid for a strip-shaped carrier tape 20 having a continuous series of recessed pockets 21 formed to fit the shapes of the electronic components. Specifically, the cover tape 10 for packaging electronic components is adhered (usually by heat sealing) to the surface of the carrier tape 20 so as to cover the entire openings of the pockets 21 of the carrier tape 20. Hereinafter, the structure obtained by adhering the cover tape 10 for packaging electronic components and the carrier tape 20 together will be referred to as an electronic component package 100.
[0051] The electronic component packaging body 100 can be produced, for example, by the following procedure. First, electronic components are placed in the pockets 21 of the carrier tape 20. Next, the cover tape 10 for packaging electronic components is adhered to the surface of the carrier tape 20 by a heat sealing method so as to cover the entire opening of the pocket 21 of the carrier tape 20. At this time, the sealant layer 3 of the cover tape 10 for packaging electronic components is in contact with the carrier tape 20 (i.e., the heat sealing is performed so that the "back surface" of the cover tape 10 for packaging electronic components in FIG. 2 becomes the sealant layer 3). The specific method and conditions for heat sealing are not particularly limited as long as the cover tape 10 for packaging electronic components is sufficiently strongly adhered to the carrier tape 20. Typically, a known heat sealing machine is used, and heat sealing can be performed at a temperature of 100 to 240°C, a load of 0.1 to 10 kgf, and a time of 0.0001 to 1 second.
[0052] As a result of the above, a structure (electronic component packaging 100) in which an electronic component is hermetically housed is obtained. This structure (electronic component packaging 100) is, for example, wound on a reel and stored until the electronic component is to be used. Alternatively, the reel on which the electronic component packaging 100 is wound may be transported to a remote location by sea or air. The reel may be made of metal, paper, plastic, or the like.
[0053] When using the electronic components, the cover tape 10 for packaging electronic components is peeled off from the carrier tape 20, and the housed electronic components are removed. There are no particular limitations on the electronic components housed in the electronic component packaging body 100. Examples include general components used in the manufacture of electrical and electronic devices, such as semiconductor chips, transistors, diodes, capacitors, piezoelectric elements, optical elements, LED-related components, connectors, and electrodes.
[0054] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention.
[0055] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. However, it should be noted that the present invention is not limited to the Examples.
[0056] Example 1 A cover tape was manufactured using the following procedure. (1) A 25 μm-thick biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) was prepared as the substrate layer. A low-density polyethylene ("Sumikathene L705" manufactured by Sumitomo Chemical Co., Ltd.) was extrusion-laminated to one side at an extrusion temperature of 300°C to form a 20 μm-thick film of low-density polyethylene to form an intermediate layer. A laminated film was thus obtained. (2) As non-volatile components, a coating liquid was prepared by uniformly dispersing or dissolving 60% by weight of antimony-doped tin oxide ("T-1" manufactured by Mitsubishi Materials Corporation, average particle size approximately 20 nm) and 40% by weight of poly(meth)acrylic acid derivative ("A450A" manufactured by DIC Corporation) in toluene. The amount of solvent used was adjusted so that the viscosity at 28°C was 6 mPa·s. (3) The coating liquid was gravure-coated onto the side of the laminated film on which the intermediate layer was formed to obtain a coated body. The temperature of the coating liquid immediately before coating was 28°C. The coated body was then transported through a drying oven approximately 10 m long, with the temperature inside the oven set at 85°C, to dry off the solvent. The transport speed was set at 180 m / min (i.e., the coated body was heated in the drying oven for 10 m / (180 m / min) = 1 / 18 min = approximately 3.3 seconds while being transported). The amount of coating liquid applied was adjusted so that the dry film thickness of the sealant layer would be 0.5 μm.
[0057] Example 2 A cover tape was manufactured according to the following procedure. (1) A 25 μm-thick biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) was prepared as a substrate layer. A low-density polyethylene ("Sumikathen L705" manufactured by Sumitomo Chemical Co., Ltd.) was extrusion laminated on one side of the substrate layer to a thickness of 20 μm at an extrusion temperature of 300° C. to form an intermediate layer. A laminated film was thus obtained. (2) A coating liquid was prepared by uniformly dispersing or dissolving the following non-volatile components in toluene: antistatic agent: 60% by mass of antimony-doped tin oxide ("T-1" manufactured by Mitsubishi Materials Corporation), poly(meth)acrylic acid derivative: 24% by mass of "A450A" manufactured by DIC Corporation, and styrene-butadiene copolymer: 16% by mass of "Tuftec H1517" manufactured by Asahi Kasei Corporation (styrene content (PS ratio): 43%, MFR (230°C, 2.16 kg): 3 g / 10 min). The amount of solvent used was adjusted so that the viscosity at 28°C was 4 mPa·s. (3) The coating liquid was coated onto the side of the laminate film on which the intermediate layer was formed by gravure coating to obtain a coated body. The temperature of the coating liquid immediately before coating was 28°C. The coated body was then transported through a drying oven approximately 10 m long, with the oven temperature set at 85°C, to dry the solvent. The conveying speed was set to 180 m / min (i.e., the coated body was heated in the drying oven for 10 m / (180 m / min) = 1 / 18 min = approximately 3.3 seconds while being conveyed.) The amount of coating liquid applied was adjusted so that the dry thickness of the sealant layer would be 0.2 μm.
[0058] Example 3 A cover tape was manufactured according to the following procedure. (1) A 25 μm-thick biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) was prepared as a substrate layer. A low-density polyethylene ("Sumikathen L705" manufactured by Sumitomo Chemical Co., Ltd.) was extrusion laminated on one side of the substrate layer to a thickness of 20 μm at an extrusion temperature of 300° C. to form an intermediate layer. A laminated film was thus obtained. (2) A coating liquid was prepared by uniformly dispersing or dissolving the following non-volatile components in toluene: antistatic agent: 60% by mass of antimony-doped tin oxide ("T-1" manufactured by Mitsubishi Materials Corporation), poly(meth)acrylic acid derivative: 24% by mass of "A450A" manufactured by DIC Corporation, and styrene-butadiene copolymer: 16% by mass of "Tuftec H1517" manufactured by Asahi Kasei Corporation (styrene content (PS ratio): 43%, MFR (230°C, 2.16 kg): 3 g / 10 min). The amount of solvent used was adjusted to a viscosity of 2.5 mPa·s at 28°C. (3) The coating liquid was coated onto the side of the laminate film on which the intermediate layer was formed by gravure coating to obtain a coated body. The temperature of the coating liquid immediately before coating was 28°C. The coated body was then transported through a drying oven approximately 10 m long, with the oven temperature set at 85°C, to dry the solvent. The conveying speed was set to 180 m / min (i.e., the coated body was heated in the drying oven for 10 m / (180 m / min) = 1 / 18 min = approximately 3.3 seconds while being conveyed.) The amount of coating liquid applied was adjusted so that the dry thickness of the sealant layer would be 0.2 μm.
[0059] Comparative Example 1 A cover tape was manufactured according to the following procedure. (1) A biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) with a thickness of 25 μm was prepared as a substrate layer. A low-density polyethylene ("Sumikathen L705" manufactured by Sumitomo Chemical Co., Ltd.) was extrusion laminated on one side of the substrate layer to a thickness of 20 μm at an extrusion temperature of 300° C. to form an intermediate layer. A laminated film was thus obtained. (2) A coating liquid was prepared by uniformly dispersing or dissolving the following non-volatile components in toluene: antistatic agent: 60% by mass of antimony-doped tin oxide ("T-1" manufactured by Mitsubishi Materials Corporation), poly(meth)acrylic acid derivative: 24% by mass of "A450A" manufactured by DIC Corporation, and styrene-butadiene copolymer: 16% by mass of "Tuftec H1517" manufactured by Asahi Kasei Corporation (styrene content (PS ratio): 43%, MFR (230°C, 2.16 kg): 3 g / 10 min). The amount of solvent used was adjusted so that the viscosity at 28°C was 1.5 mPa·s. (3) The coating liquid was coated onto the side of the laminate film on which the intermediate layer was formed by gravure coating to obtain a coated body. The temperature of the coating liquid immediately before coating was 28°C. The coated body was then transported through a drying oven approximately 10 m long, with the oven temperature set at 85°C, to dry the solvent. The conveying speed was set to 180 m / min (i.e., the coated body was heated in the drying oven for 10 m / (180 m / min) = 1 / 18 min = approximately 3.3 seconds while being conveyed.) The amount of coating liquid applied was adjusted so that the dry thickness of the sealant layer would be 0.2 μm.
[0060] Comparative Example 2 A cover tape was manufactured using the following procedure. (1) A 25 μm-thick biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) was prepared as the substrate layer. A low-density polyethylene ("Sumikathene L705" manufactured by Sumitomo Chemical Co., Ltd.) was extruded onto one side of the substrate layer at an extrusion temperature of 300°C to form a 20 μm-thick intermediate layer. A laminated film was thus obtained. (2) A molten mixture of 90% by weight of ethylene-vinyl acetate copolymer ("Ultrathene 537" manufactured by Tosoh Corporation, vinyl acetate group content: 6% by weight) and 10% by weight of tackifier ("Arcon P-100" manufactured by Arakawa Chemical Industries, Ltd.) was extruded onto the surface of the intermediate layer at an extrusion temperature of 280°C to form a 10 μm-thick film. Immediately thereafter, the sealant layer surface was roughened by rotating the rolls at a pressure of 0.2 MPa between a cooling roll with protrusions having a surface roughness of 5.5 μm on the sealant layer side and a silicone rubber mat roll on the base layer side. The temperature of the cooling roll was set to 20° C.
[0061] Comparative Example 3 A cover tape was manufactured using the following procedure. (1) A 25 μm-thick biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) was prepared as the substrate layer. A low-density polyethylene ("Sumikathene L705" manufactured by Sumitomo Chemical Co., Ltd.) was extruded onto one side of the substrate layer at an extrusion temperature of 300°C to form a 20 μm-thick intermediate layer. (2) A molten mixture of 90% by weight of ethylene-vinyl acetate copolymer ("Ultrathene 537" manufactured by Tosoh Corporation, vinyl acetate group content: 6% by weight) and 10% by weight of tackifier ("Arcon P-100" manufactured by Arakawa Chemical Industries, Ltd.) was extruded onto the surface of the intermediate layer at an extrusion temperature of 280°C to form a 10 μm-thick film. Immediately thereafter, the sealant layer surface was roughened by rotating the rolls at a pressure of 0.2 MPa, with the sealant layer side being sandwiched between a cooling roll with protrusions having a surface roughness of 7.0 μm and the base layer side being sandwiched between a silicone rubber mat roll. The temperature of the cooling roll was set to 20° C.
[0062] <Measurement of Surface Properties of Sealant Layer> Using a laser microscope VK-X3000 manufactured by Keyence Corporation, the following indices were measured for the sealant layer (exposed) of each of the above Examples and Comparative Examples. The analysis software used was that included with the device. - Arithmetic mean height Sa defined in ISO 25178 - Peak density Spd defined in ISO 25178 - Developed surface area ratio Sdr defined in ISO 25178
[0063] <Evaluation: Blocking> The cover tape of each example and comparative example was cut to a width of 5.4 mm and a length of 500 m. The cut cover tape was then wound tightly around a reel. The cover tape wound on the reel was left in an environment of 65°C for 24 hours. After leaving it, the reel on which the cover tape was wound was vertically rotated slowly in the opposite direction to the direction in which the cover tape was wound. At this time, the strength of adhesion between the front and back of the cover tape (degree of blocking) was evaluated by examining whether the wound cover tape could be unwound under its own weight, and if it could not be unwound under its own weight, how much force was required to unwind it. Specifically, the evaluation was based on the following criteria. - The cover tape could be unwound under its own weight: Very good - Some adhesion between the cover tapes was observed, and the cover tape could not be unwound under its own weight, but the adhesion could be broken off by gently shaking the cover tape with a hand and the tape could be unwound: Good - The cover tapes adhered relatively strongly to each other, and the adhesion did not break off even when the cover tape was gently shaken with a hand, and the tape could not be unwound: Poor
[0064] <Evaluation: Sticking of Components> The sticking of components was evaluated by carrying out the following adhesion test using metal pieces simulating electronic components.
[0065] (1) The cover tapes obtained in the Examples and Comparative Examples were cut to an appropriate size and attached to a glass slide with the sealant layer facing upward. Test specimens were prepared by placing 20 metal pieces (0.4 mm long x 0.8 mm wide x 0.4 mm thick) on the sealant layer. The metal pieces were obtained by cutting nickel with a precision cutting machine. (2) The obtained test specimens were left standing for 24 hours under conditions of 60°C and 95% RH, and then for another 24 hours at room temperature and humidity. (3) After (2) above, the test specimens were fixed with double-sided tape in an inverted position on a vortex mixer. The vortex mixer was then set to 1,500 rpm and subjected to vibration for 20 seconds. (Because there was no dedicated equipment for applying vibration, a vortex mixer, which is normally used to stir liquids, was used to apply vibration to the test piece.) (4) After completing the above (3), the adhesion rate was calculated from the number of metal pieces adhering to the surface of the sealant layer.
[0066] The above measurement results and evaluation results are summarized in the table below.
[0067]
[0068] As shown in the table above, the peak density Spd of the exposed surface of the sealant layer is 3 × 10 5 ~1 x 10 6 / mm 2 and the developed area ratio Sdr of the interface of the exposed surface of the sealant layer is 1×10 ―3 ~5 x 10 ―2 In the evaluation of the cover tapes of Examples 1, 2 and 3, blocking was suppressed and component sticking was also suppressed. 5 Comparative Examples 1 and 2, Spd is 3 × 10 5 is smaller than 5×10 ―2 In Comparative Example 3, in which the thickness was larger than 1 / 2 mm, the evaluation result of blocking was poor and sticking of parts occurred.
[0069] Incidentally, in the above-mentioned blocking evaluation, blocking was suppressed even under the severe evaluation conditions of leaving the sealant at 65°C for 24 hours. Such good results were achieved by focusing on the indicators Spd and Sdr of the sealant layer and optimizing these indicators.
[0070] This application claims priority based on Japanese Patent Application No. 2023-048721, filed March 24, 2023, the disclosure of which is incorporated herein by reference in its entirety.
[0071] REFERENCE SIGNS LIST 1 base layer 2 intermediate layer 3 sealant layer 10 cover tape 20 carrier tape 21 pocket 100 electronic component package
Claims
1. A cover tape for packaging electronic components comprising a base layer and a sealant layer provided on one side of the base layer, the surface of the sealant layer opposite to the base layer being an exposed surface, and the peak density Spd of the exposed surface as defined in ISO 25178 is 3×10 5 ~1×10 6 / mm 2 The exposed surface has an interface development area ratio Sdr defined in ISO 25178 of 1×10 ―3 ~5×10 ―2 That is the cover tape.
2. The cover tape according to claim 1, wherein the exposed surface has an arithmetic mean height Sa, as defined by ISO 25178, of 0.05 to 0.5 μm.
3. The cover tape according to claim 1 or 2, wherein the sealant layer contains inorganic particles.
4. A cover tape according to claim 1 or 2, wherein the sealant layer contains one or both of a styrene-based resin and a (meth)acrylic-based resin.
5. The cover tape according to claim 1 or 2, wherein the base layer comprises polyester.
6. A cover tape according to claim 1 or 2, comprising an intermediate layer between the base layer and the sealant layer.
7. The cover tape according to claim 6, wherein the intermediate layer comprises a polyethylene resin.
8. An electronic component package comprising a carrier tape having an electronic component housed in a recess and the cover tape according to claim 1 or 2, wherein the sealant layer is adhered to the carrier tape so as to seal the electronic component.