Method for producing polyacetal copolymer
Patent Information
- Application Number
- MYPI2025005416
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-13
- Filing Date
- 2024-03-07
- Publication Date
- 2024-09-13
AI Technical Summary
The production of polyacetal copolymers using conventional boron trifluoride catalysts results in high catalyst usage, difficulty in catalyst deactivation, residual catalyst substances, low polymerization yield, and thermally unstable terminals, leading to complex and costly purification processes and potential copolymer decomposition.
Employing a protonic acid, such as heteropolyacid, as a polymerization catalyst and using a basic compound solution with a continuous mixing device to deactivate the catalyst, reducing the amount of deactivating agent and ensuring uniform dispersion, thereby minimizing discoloration and stabilizing the polyacetal copolymer.
This method allows for the production of polyacetal copolymers with excellent hue and reduced catalyst usage, achieving high yield and stability while eliminating the need for extensive purification steps and thermally unstable terminals, thus enhancing the economic and quality aspects of the process.
Abstract
Description
Method for producing polyacetal copolymer
[0001] The present invention relates to a method for producing a polyacetal copolymer.
[0002] Polyacetal copolymers have an excellent balance of mechanical properties, chemical resistance, sliding properties, etc., and are easy to process. As such, they are widely used as engineering plastics, primarily in electrical and electronic components, automotive components, and various other mechanical components.
[0003] Polyacetal copolymers are copolymers obtained by copolymerizing trioxane as the main monomer with a compound copolymerizable with trioxane as a comonomer. A known method for producing polyacetal copolymers is cationic copolymerization, in which trioxane is the main monomer and a cyclic ether and / or cyclic formal having at least one carbon-carbon bond is the comonomer. Among the cationic active catalysts used in copolymerization, boron trifluoride or a coordination compound of boron trifluoride with an organic compound, such as an ether, is the most commonly used polymerization catalyst for trioxane as the main monomer and is widely used industrially.
[0004] However, commonly used polymerization catalysts, such as boron trifluoride-based compounds, require relatively large amounts of catalyst (e.g., 40 ppm or more relative to the total monomer content) for polymerization. This makes it difficult to adequately deactivate the catalyst after polymerization. Even if deactivation is achieved, catalyst-derived substances may remain in the copolymer, accelerating copolymer decomposition and other problems. Furthermore, polymerization yields are low, with several percent to several tens of percent of unreacted monomer remaining. Therefore, catalyst deactivation is typically performed in a large amount of high-temperature aqueous solution containing a basic compound, such as triethylamine, during which unreacted monomer dissolves in the treatment solution. This process requires complex steps, such as separating and washing the copolymer from the treatment solution containing the unreacted monomer, followed by drying, which presents economic challenges.
[0005] On the other hand, the polymerization product after the deactivation as described above has thermally unstable terminals, which require purification and stabilization treatment by hydrolyzing the unstable terminals using an aqueous triethylamine solution or the like, which increases the number of steps and also leads to increased costs.
[0006] In order to solve the above problems, it has been proposed to use a heteropolyacid or an acid salt thereof as a polymerization catalyst (see Patent Document 1).
[0007] Japanese Patent Application Publication No. 1-170610
[0008] As disclosed in Patent Document 1, the above problems can be solved by producing a polyacetal copolymer using a protonic acid such as a heteropolyacid or an acid salt thereof as a polymerization catalyst, and certain results have been achieved. However, a solid deactivator is added to deactivate the polymerization catalyst, and as a result, the deactivator is not sufficiently dispersed in the polymerization catalyst. While increasing the amount of deactivator is considered to fully deactivate the polymerization catalyst, doing so can result in discoloration of the resulting polyacetal copolymer.
[0009] The present invention has been made in consideration of the above-mentioned conventional problems, and an object of the present invention is to provide a method for producing a polyacetal copolymer, which can provide a polyacetal copolymer having excellent color, even when a protonic acid is used as a polymerization catalyst to produce the polyacetal copolymer.
[0010] The present inventors have found that the use of a solution of a basic compound to deactivate a polymerization catalyst, which is a protonic acid, and the use of a specific continuous mixing device can reduce the amount of deactivator used, thereby solving the above-mentioned problems, and have completed the present invention. One aspect of the present invention that solves the above-mentioned problems is as follows.
[0011] (1) A method for producing a polyacetal copolymer, comprising: copolymerizing trioxane as a main monomer (a) and a compound copolymerizable with trioxane as a comonomer (b) using a protonic acid as a polymerization catalyst (c) to obtain a crude polyacetal copolymer; introducing the crude polyacetal copolymer and a solution of a basic compound (d) into a continuous powder-liquid mixer configured to disperse and contact the powder in a continuously supplied liquid and obtain a uniform mixed fluid of the powder and liquid via a rotary mixer, thereby obtaining a mixture; and feeding the mixture into an extruder to melt-knead, wherein the basic compound (d) is a carbonate, hydrogencarbonate, or carboxylate of an alkali metal element or a Group 2 element (excluding Be), or a nitrogen-containing organic compound having a pH of 10 or higher in a 10 g / L aqueous solution; and wherein the solvent for the solution of the basic compound (d) is a solvent having active hydrogen.
[0012] (2) The method for producing a polyacetal copolymer according to (1) above, wherein a heteropolyacid represented by the following general formula (1) is used as the polymerization catalyst (c): m [M 1 x ・M 2 y O Z ]・nH 2 O...General formula (1) [In general formula (1), M 1 represents a central element selected from P, Si, B, and Ge. 2 represents one or more coordination elements selected from W, Mo, and V. x represents an integer of 1 or more and 10 or less, y represents an integer of 6 or more and 40 or less, z represents an integer of 10 or more and 100 or less, m represents an integer of 1 or more, and n represents an integer of 0 or more and 50 or less.
[0013] (3) The method for producing a polyacetal copolymer according to (2) above, wherein the heteropolyacid is at least one selected from the group consisting of phosphomolybdic acid, phosphotungstic acid, phosphomolybdotungstic acid, phosphomolybdovanadic acid, phosphomolybdotungstovanadic acid, phosphotungstovanadic acid, silicotungstic acid, silicomolybdic acid, silicomolybdotungstic acid, and silicomolybdotungstovanadic acid.
[0014] (4) The method for producing a polyacetal copolymer according to any one of (1) to (3), wherein the carbonate, bicarbonate or carboxylate of an alkali metal element or a Group 2 element (excluding Be), or a hydrate thereof, is a carbonate, bicarbonate or carboxylate of an alkali metal element, or a hydrate thereof.
[0015] (5) The method for producing a polyacetal copolymer according to any one of (1) to (4), wherein the comonomer (b) is at least one selected from the group consisting of 1,3-dioxolane, diethylene glycol formal, 1,4-butanediol formal, 1,3-dioxane, and ethylene oxide.
[0016] According to the present invention, a method for producing a polyacetal copolymer can be provided, which can produce a polyacetal copolymer having excellent color, even when a protonic acid is used as a polymerization catalyst to produce the polyacetal copolymer.
[0017] The method for producing a polyacetal copolymer according to this embodiment includes a step of copolymerizing trioxane as the main monomer (a) and a compound copolymerizable with trioxane as the comonomer (b) using a protonic acid as the polymerization catalyst (c) to obtain a crude polyacetal copolymer (hereinafter also referred to as "step A"); a step of introducing the crude polyacetal copolymer and a solution of a basic compound (d) into a continuous powder-liquid mixer configured to disperse the powder in a continuously supplied liquid and obtain a uniformly mixed fluid of the powder and liquid via a rotating mixer to obtain a mixture (hereinafter also referred to as "step B"); and a step of feeding the mixture into an extruder and melt-kneading the mixture (hereinafter also referred to as "step C"). The basic compound (d) is a carbonate, bicarbonate, or carboxylate of an alkali metal element or a Group 2 element (excluding Be), or a nitrogen-containing organic compound having a pH of 10 or higher in a 10 g / L aqueous solution. The solvent for the solution of the basic compound (d) is a solvent having active hydrogen.
[0018] In the production method of this embodiment, a copolymerization reaction is carried out using a protonic acid as the polymerization catalyst (c) in the step of copolymerizing trioxane as the main monomer (a) and a compound copolymerizable with trioxane as the comonomer (b). The crude polyacetal copolymer obtained by copolymerization is then mixed with a basic compound (d) in solution to deactivate the polymerization catalyst (c). By using a specific continuous mixer, the basic compound (d) is thoroughly dispersed in the crude polyacetal copolymer, fully demonstrating its deactivation ability. The resulting mixture is then introduced into an extruder for melt-kneading, thereby thoroughly deactivating the polymerization catalyst (c). Furthermore, the use of a specific continuous mixer allows for a reduced amount of deactivator to be used, resulting in pellets with excellent color. Each step is described below.
[0019] [Step A] In step A, trioxane as the main monomer (a) and a compound copolymerizable with trioxane as the comonomer (b) are copolymerized using a protonic acid as the polymerization catalyst (c) to obtain a crude polyacetal copolymer.
[0020] Trioxane as the main monomer (a) is a cyclic trimer of formaldehyde, and is generally obtained by reacting an aqueous formaldehyde solution in the presence of an acidic catalyst, and is used after being purified by a method such as distillation. The trioxane used in the polymerization is preferably one in which impurities such as water and methanol have been reduced as much as possible.
[0021] The comonomer (b) is a compound copolymerizable with trioxane. Examples of the comonomer (b) include cyclic ethers and / or cyclic formals having at least one carbon-carbon bond. Representative examples of the compound used as the comonomer (b) include 1,3-dioxolane, diethylene glycol formal, 1,4-butanediol formal, 1,3-dioxane, ethylene oxide, propylene oxide, and epichlorohydrin. Among these, in consideration of polymerization stability, at least one selected from the group consisting of 1,3-dioxolane, diethylene glycol formal, 1,4-butanediol formal, 1,3-dioxane, and ethylene oxide is preferred. Furthermore, in addition to the main monomer (a) and comonomer (b), a known modifier comonomer such as a branching agent may be added as a third comonomer component, provided that the addition does not significantly impair the performance of the resulting polyacetal copolymer.
[0022] In this embodiment, the amount of the compound selected from cyclic ethers and / or cyclic formals used as comonomer (b) is preferably 0.1 to 20 mol %, more preferably 0.2 to 10 mol %, based on the total amount of monomers (the total amount of main monomer (a) and comonomer (b)). If the amount of comonomer (b) is less than 0.1 mol %, the polyacetal copolymer produced by polymerization may have an increased number of unstable terminals, resulting in poor stability. If the amount of comonomer (b) exceeds 20 mol %, the resulting copolymer may become soft and have a lower melting point.
[0023] In the production method of this embodiment, a protonic acid is used as the polymerization catalyst (c). Examples of the protonic acid include heteropolyacids, isopolyacids, and perfluoroalkanoic acids. Among these, it is preferable to use a heteropolyacid represented by the following general formula (1):
[0024] H m [M 1 x ・M 2 y O Z ]・nH 2O ... General formula (1) [In general formula (1), M 1 represents a central element selected from P, Si, B, and Ge. 2 represents one or more coordination elements selected from W, Mo, and V. x represents an integer of 1 or more and 10 or less, y represents an integer of 6 or more and 40 or less, z represents an integer of 10 or more and 100 or less, m represents an integer of 1 or more, and n represents an integer of 0 or more and 50 or less.] Note that y is M 2 represents the number of 2 If there is only one, it represents the number of 2 When it consists of multiple elements, it represents the sum of those multiple elements.
[0025] M 1 represents a central element selected from P, Si, B and Ge, with P or Si being preferred.
[0026] The heteropolyacid represented by general formula (1) as the polymerization catalyst (c) is preferably at least one selected from the group consisting of phosphomolybdic acid, phosphotungstic acid, phosphomolybdotungstic acid, phosphomolybdovanadic acid, phosphomolybdotungstovanadic acid, phosphotungstovanadic acid, silicotungstic acid, silicomolybdic acid, silicomolybdotungstic acid, and silicomolybdotungstovanadic acid.
[0027] In this embodiment, the polymerization catalyst (c) is a heteropolyacid represented by the general formula (1) and a H m Acid salts in which a part or all of the above is replaced by various metals may also be used in combination.
[0028] When the polymerization catalyst (c) is in the form of a solution, preferred examples of the solvent include, but are not limited to, esters obtained by condensation of a low-molecular-weight carboxylic acid having 1 to 10 carbon atoms, such as formic acid, acetic acid, propionic acid, or butyric acid, with a low-molecular-weight alcohol having 1 to 10 carbon atoms, such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 3-methyl-1-butanol, or 1-hexanol; and low-molecular-weight ketones having 1 to 10 carbon atoms, such as acetone, 2-butanone, 2-pentanone, 3-pentanone, 2-hexanone, 3-hexanone, methyl isobutyl ketone, or methyl t-butyl ketone. Taking into consideration industrial availability and other factors, methyl formate, ethyl formate, methyl acetate, ethyl acetate, butyl acetate, acetone, 2-butanone, or methyl isobutyl ketone is most preferred. The polymerization catalyst (c) is dissolved in the inert solvent preferably at a concentration of 0.1 to 30% by mass / mass, but is not limited thereto.
[0029] In the production method of this embodiment, a copolymer can be obtained in high yield even when the amount of polymerization catalyst (c) used is small. Specifically, the amount of polymerization catalyst (c) used relative to the total amount of main monomer (a) and comonomer (b) can be 1.0 to 20.0 ppm by mass, and preferably 1.5 to 10.0 ppm by mass. The fact that copolymerization is possible even with such a small amount of polymerization catalyst (c) minimizes undesirable reactions such as main chain decomposition and depolymerization of the polymer caused by the polymerization catalyst, and prevents unstable formate end groups (—O—CH═O) and hemiacetal end groups (—O—CH 2 This is effective in suppressing the generation of —OH) and is also economically advantageous.
[0030] In step A, the main monomer (a), the comonomer (b), and the polymerization catalyst (c) are introduced into a polymerization reactor to carry out a copolymerization reaction. In this process, the main monomer (a) and the comonomer (b) are mixed together, followed by the addition of the polymerization catalyst (c), or the main monomer (a) or the comonomer (b) are mixed with the polymerization catalyst (c), followed by the addition of the comonomer (b) or the main monomer (a). The polymerization reaction is preferably carried out by bulk polymerization using the main monomer (a) as a melt, typically initiated at a temperature between 65°C and 114°C. Since the polyacetal copolymer is insoluble in the main monomer (a), it precipitates. However, high-speed, powerful stirring is performed to prevent the reaction product from forming a blocky mass, and the reaction product is pulverized. While maintaining a temperature above 65°C is necessary to ensure a sustained reaction, maintaining a temperature below 130°C is preferred to prevent depolymerization. A temperature between 70°C and 125°C is more preferred.
[0031] The polymerization time depends on the concentration of the polymerization catalyst, the concentration of the comonomer, and the reaction temperature, and cannot be particularly limited, but generally, a polymerization time of 0.5 to 10 minutes is selected.
[0032] By carrying out the copolymerization reaction as described above, a crude polyacetal copolymer can be obtained in high yield. This crude polyacetal copolymer contains almost no unreacted monomers, eliminating the need for a removal step of washing with hot water. Furthermore, since the crude polyacetal copolymer is used in the next step, step B, in a powdered state, it is preferable that the crude polyacetal copolymer obtained in step A is in the form of a powder. Therefore, if there are coarse lumps, the crude polyacetal copolymer may be pulverized using a pulverizer, as necessary.
[0033] In the method for producing a polyacetal copolymer of this embodiment, a molecular weight modifier may be used in step A, if necessary. A linear formal compound can be used as the molecular weight modifier. Examples of the linear formal compound include methylal, ethylal, dibutoxymethane, bis(methoxymethyl) ether, bis(ethoxymethyl) ether, and bis(butoxymethyl) ether. Among these, one or more compounds selected from the group consisting of methylal, ethylal, and dibutoxymethane are preferred.
[0034] Furthermore, in the method for producing the polyacetal copolymer of the present embodiment, an antioxidant may be added in step A, if necessary.
[0035] [Step B] In step B, the crude polyacetal copolymer and the solution of the basic compound (d) are introduced into a continuous mixer for powder and liquid (hereinafter also simply referred to as a "continuous mixer") configured to disperse and contact the powder in a continuously supplied liquid and to obtain a uniform mixed fluid of the powder and liquid via a rotary mixer, thereby obtaining a mixture.
[0036] In step B, the crude polyacetal copolymer obtained in step A is mixed with a solution of a basic compound (d) to obtain a mixture. The basic compound (d) functions as a basic deactivator for the polymerization catalyst (c), and the polymerization catalyst (c) can be deactivated by the basic compound (d). To obtain a mixture of the crude polyacetal copolymer and the solution of the basic compound (d), a continuous powder-liquid mixer is used, which is configured to disperse and contact powder with a continuously supplied liquid and to obtain a uniform mixed fluid of the powder and liquid via a rotating mixer. That is, the continuously supplied liquid is used as a solution of the basic compound (d), and the powder is mixed as the crude polyacetal copolymer. Such continuous mixers are described in detail, for example, in JP-A-2002-248330 and JP-A-2004-168055.
[0037] In this embodiment, by using a continuous mixer, the crude polyacetal copolymer powder and the liquid solution of the basic compound (d) are made into a uniform mixed fluid, and the solution of the basic compound (d) is uniformly dispersed in the crude polyacetal copolymer. As a result, even if the amount of the basic compound (d) used is reduced, the polymerization catalyst (c) is sufficiently deactivated in the subsequent step C. Furthermore, because the amount of the basic compound (d) used is small, discoloration of the polyacetal copolymer can be prevented after melt-kneading.
[0038] The advantage of using a continuous mixer is that, as described above, the solution of the basic compound (d) is uniformly dispersed throughout the crude polyacetal copolymer. There are other advantages as well. For example, while it is preferable to use as little basic compound (d) solution as possible, using a continuous mixer allows the amount of basic compound (d) solution used to be kept to a minimum. Specifically, when the basic compound (d) solution is to be approximately 0.1 to 0.2 mass% relative to the crude polyacetal copolymer powder, only a continuous mixer can achieve this at present. Note that even when a continuous mixer is used and a small amount of basic compound (d) solution is used, this does not mean that the deactivation effect of the polymerization catalyst (c) by the basic compound (d) solution is inferior.
[0039] When mixing using a continuous mixer, it is preferable to set the peripheral speed of the rotating mixer to 0.1 to 20.0 m / s.
[0040] In step B, the basic compound (d) used is a carbonate, bicarbonate, or carboxylate of an alkali metal or Group 2 element, or a hydrate thereof, or a nitrogen-containing organic compound having a pH of 10 or higher in a 10 g / L aqueous solution. Examples of carbonate, bicarbonate, or carboxylate of an alkali metal or Group 2 element, or a hydrate thereof, include sodium carbonate, sodium bicarbonate, potassium carbonate, calcium carbonate, calcium bicarbonate, sodium formate, sodium acetate, disodium succinate, sodium laurate, sodium palmitate, sodium stearate, calcium stearate, sodium hydroxide, and potassium hydroxide. Examples of nitrogen-containing organic compounds having a pH of 10 or higher in a 10 g / L aqueous solution include amine compounds such as triethylamine, choline hydroxide, trimethylamine, and ethanolamine. Among these, carbonate, bicarbonate, or carboxylate of an alkali metal element, or a hydrate thereof, is preferred. The pH of a nitrogen-containing organic compound having a pH of 10 or higher in a 10 g / L aqueous solution is the pH at 25°C.
[0041] On the other hand, a solvent having active hydrogen is used as the solvent for the solution of basic compound (d). Examples of solvents having active hydrogen include water, alcohols having 1 to 5 carbon atoms, and formic acid. Examples of alcohols having 1 to 5 carbon atoms include methanol, ethanol, n-propanol, isopropanol, and n-butanol. Of these, water is preferred.
[0042] Furthermore, when the basic compound (d) is used, the amount of formaldehyde generated in the final composition is particularly low, which is more preferable.
[0043] In this embodiment, the basic compound (d) may be one type, or two or more types may be used in combination, and may be in the form of a hydrate, a mixture, a double salt, or the like.
[0044] In this embodiment, as described above, the amount of the polymerization catalyst (c) used is small, and therefore the amount of the basic compound (d) used as a deactivator for the polymerization catalyst (c) can also be small, specifically, 1 to 100 ppm relative to the polymerization product.
[0045] After the polymerization and deactivation treatment, if necessary, the unreacted monomers may be separated and recovered, dried, etc. by a conventionally known method.
[0046] [Step C] In step C, a mixture of the crude polyacetal copolymer and the solution of the basic compound (d) is fed into an extruder and melt-kneaded. In step B, the basic compound (d) is in a uniformly dispersed state, and in step C, the mixture is melt-kneaded in this state, so that the polymerization catalyst (c) can be sufficiently deactivated.
[0047] Step C can be, for example, (1) a method in which the mixture obtained in step B is directly melt-kneaded and deactivation-stabilized to obtain a polyacetal copolymer, or (2) a method in which other additives are added to the mixture obtained in step B and melt-kneaded to obtain a resin composition by deactivation-stabilization. In (2), the additives may be added together with the mixture to the main feed section of the extruder, or may be added alone through a side feed section of the extruder. In both of the above (1) and (2), the polyacetal copolymer or resin composition discharged from the extruder outlet can be pelletized by a known method, such as cutting the cooled resin discharged from the extruder outlet with a strand cutter.
[0048] In step C, since deactivation is carried out in a homogeneous molten resin, the polymerization catalyst (c) can be deactivated without the need for the conventional method of immersing a powder obtained by pulverizing a crude polyacetal copolymer in an aqueous solution of a deactivator and treating it in a heterogeneous solid-liquid state for a long time. Therefore, the steps of immersion in an aqueous solution of a deactivator followed by drying, which have been performed to deactivate a polymerization catalyst in the past, can be omitted. Furthermore, since the generation of thermally unstable terminals, which are generated by long-term immersion in an aqueous solution of a deactivator, can be suppressed, stabilization treatment is not required. Thermally unstable terminals include -CH 2 CH 2 O-(CH 2 O) n -CH 2 OH or -CH 2 CH 2 O-(CH 2 O) n -CH 2 Examples of such unstable terminal groups include O-CHO. In the group representing the unstable terminal, n represents zero or any positive integer. Furthermore, it is now possible to recover unreacted monomers that would have been extracted into an aqueous solution when the catalyst in the crude polyacetal copolymer was deactivated by immersion in a basic solution, thereby suppressing loss of monomers.
[0049] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to the following examples.
[0050] Examples 1 to 11, Comparative Examples 1 and 2 (Step A) A continuous twin-screw polymerization reactor was used as the polymerization reactor. This polymerization reactor was equipped with an external jacket for passing a heating or cooling medium, and two rotating shafts equipped with numerous paddles for stirring, propulsion, and grinding were installed longitudinally inside the polymerization reactor. While the two rotating shafts of the polymerization reactor were rotated at a constant speed so that the peripheral speed of the paddle tips was 0.5 m / s, the main monomer (a) (trioxane) and the comonomer (b) shown in Table 1 were added and mixed in the proportions shown in Table 1. To the resulting mixture, the polymerization catalyst (c) shown in Table 1 (5 ppm relative to the total monomers in a 2 g / L methyl formate solution) was further added. In Table 1, the amounts of additives (polymerization catalyst (c) and basic compound (d)) added are expressed as a percentage relative to the total amount of the main monomer (a) and comonomer (b). Next, methylal was added as a molecular weight modifier so that the melt flow rate of the resulting copolymer was 9 g / 10 min. Bulk polymerization was carried out under the above conditions, and a powdery crude polyacetal copolymer was obtained which was pulverized and discharged from the polymerization reactor. In Table 1, the comonomers are indicated by abbreviations, and the specific abbreviations are as follows: DO: 1,3-dioxolane BDF: 1,4-butanediol formal Furthermore, in Table 1, catalysts C1 and C2 are as follows: Catalyst C1: phosphotungstic acid (H 3 P.W. 12 O 40 Catalyst C2: Phosphomolybdic acid (H 3 PMo 12 O 40 )
[0051] (Step B) Next, the powdered crude polyacetal copolymer powder continuously discharged from the polymerization reactor and a 1 g / L aqueous solution of the basic compound (d) shown in Table 1 were introduced into a continuous mixer (Flow Jet Mixer, Continuous Injection Mixer, Model 100, manufactured by Funken Powtex Co., Ltd.) at a flow rate such that the amount of basic compound (d) added was in the ratio shown in Table 1, to obtain a mixture of basic compound (d) and crude polyacetal copolymer. The flow jet mixer system was operated so that the peripheral speed of the rotating mixer plate was 2.5 m / s. However, in Comparative Examples 1 and 2, the basic compound was not converted into an aqueous solution but was used as a solid. In Table 1, basic compounds D1 to D8 are as follows: Basic compound D1: Sodium carbonate Basic compound D2: Potassium carbonate Basic compound D3: Sodium hydrogen carbonate Basic compound D4: Sodium oleate Basic compound D5: Sodium acetate Basic compound D6: Sodium formate Basic compound D7: Triethylamine Basic compound D8: Sodium stearate
[0052] (Step C) Thereafter, 0.3 mass % of Irganox 1010 manufactured by BASF Japan Ltd. was added as an antioxidant to the mixture of the crude polyacetal copolymer obtained in Step B and the basic compound (d), and the mixture was fed into a twin-screw extruder and melt-kneaded (cylinder temperature: 200°C) to deactivate the polymerization catalyst (c), thereby obtaining pellets of the polyacetal copolymer.
[0053] Comparative Example 3 A crude polyacetal copolymer was obtained by the same procedure as in Example 2, and then a basic compound (d) shown in Table 1 was added to the obtained crude polyacetal copolymer, and the mixture was charged into a twin-screw extruder and melt-kneaded (cylinder temperature: 200°C) to obtain pellets of the polyacetal copolymer.
[0054] <Evaluation> [Evaluation of hue of pellets] Using a color difference meter SE-2000 (manufactured by Nippon Denshoku Industries Co., Ltd.), a predetermined amount of pellets was placed in a cell (round cell) for measuring pellets, which was then placed on a sample stage and covered with a cover. The b value displayed during measurement was read. The results are shown in Table 1.
[0055]
[0056] From Table 1, it can be seen that the b value in the hue evaluation was a negative value, indicating no yellowing, in all of Examples 1 to 11. In contrast, in Comparative Examples 1 and 2, in which the basic compound (d) was used as a solid and mixed with the crude polyacetal copolymer, and in Comparative Example 3, in which no continuous mixer was used, the b value in the hue evaluation was a positive value, indicating yellowing.
Claims
1. A method for producing a polyacetal copolymer, comprising the steps of: copolymerizing trioxane as a main monomer (a) and a compound copolymerizable with trioxane as a comonomer (b) by using a protonic acid as a polymerization catalyst (c) to obtain a crude polyacetal copolymer; introducing and mixing the crude polyacetal copolymer and a solution of a basic compound (d) into a continuous powder and liquid mixer configured to disperse and contact the powder with a continuously supplied liquid and obtain a uniform mixed fluid of the powder and liquid via a rotating mixer to obtain a mixture; and feeding the mixture into an extruder to perform melt kneading, wherein the basic compound (d) is a carbonate, hydrogencarbonate or carboxylate of an alkali metal element or a Group 2 element (excluding Be), or a nitrogen-containing organic compound having a pH of 10 or more in a 10 g / L aqueous solution, and the solvent of the solution of the basic compound (d) is a solvent having active hydrogen.
2. The method for producing a polyacetal copolymer according to claim 1, wherein a heteropolyacid represented by the following general formula (1) is used as the polymerization catalyst (c). m [M 1 x M 2 y O Z ]·nH 2 O...General formula (1) [In general formula (1), M 1 represents a central element selected from P, Si, B and Ge. 2 represents one or more coordination elements selected from W, Mo, and V. x represents an integer of 1 or more and 10 or less, y represents an integer of 6 or more and 40 or less, z represents an integer of 10 or more and 100 or less, m represents an integer of 1 or more, and n represents an integer of 0 or more and 50 or less.
3. The method for producing a polyacetal copolymer according to claim 2, wherein the heteropolyacid is at least one selected from the group consisting of phosphomolybdic acid, phosphotungstic acid, phosphomolybdotungstic acid, phosphomolybdovanadic acid, phosphomolybdotungstovanadic acid, phosphotungstovanadic acid, silicotungstic acid, silicomolybdic acid, silicomolybdotungstic acid, and silicomolybdotungstovanadic acid.
4. A method for producing a polyacetal copolymer according to claim 1 or 2, wherein the carbonate, hydrogencarbonate or carboxylate of an alkali metal element or a Group 2 element (excluding Be), or a hydrate thereof, is a carbonate, hydrogencarbonate or carboxylate of an alkali metal element, or a hydrate thereof.
5. The method for producing a polyacetal copolymer according to claim 1 or 2, wherein the comonomer (b) is at least one selected from the group consisting of 1,3-dioxolane, diethylene glycol formal, 1,4-butanediol formal, 1,3-dioxane, and ethylene oxide.