Battery separator and preparation method therefor, and secondary battery

MYPI2025005446A0Undetermined Publication Date: 2024-10-12SINOMA LITHIUM BATTERY SEPARATOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005446
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2023-07-29
Publication Date
2024-10-12

AI Technical Summary

Technical Problem

During long-term use of lithium-ion batteries, the chain segments of the polyolefin isolation film move and the pore size shrinks at high temperatures, resulting in poor permeability of lithium ions, affecting battery life, and the poor adhesion of traditional inorganic coatings leads to safety performance and capacity decrease.

Method used

By setting an inorganic coating on the battery isolation film, the contact ratio between the inorganic particles and the base film in the longitudinal section is controlled to be between 15% and 90%, and the specific air permeability relationship is met, thereby improving the peel strength and needle punch strength of the isolation film. At the same time, the air permeability of the coating is controlled to ensure high ion permeability and safety.

Benefits of technology

A battery isolation film with both high safety and high ion permeability has been realized, which extends the battery life and improves the battery capacity and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005446_DRAWING_001
    Figure PI2025005446_DRAWING_001
Patent Text Reader

Abstract

A battery separator and a preparation method therefor, and a secondary battery, relating to the technical field of battery separators. The battery separator comprises: a base film; and an inorganic coating provided on at least one surface of the base film. A contact ratio k of inorganic particles to the base film in the longitudinal section of the battery separator is 15-90%; and the relationship among the contact ratio k, air permeability A1 of the base film and air permeability A2 of the coating per unit thickness meets: A1×k≥A2. The separator is improved to a certain extent in peel strength, puncture strength and air permeability, and the battery separator with both safety and high ion permeability is provided. [FIG. 1]
Need to check novelty before this filing date? Find Prior Art

Description

Battery separator and preparation method thereof, and secondary battery Technical Field

[0001] The present invention relates to the technical field of battery separators, and in particular to a battery separator and a preparation method thereof, and a secondary battery. Background Art

[0002] With "carbon peak" and "carbon neutrality" written into the government work report, green and low-carbon development is rapidly developing in my country. New energy vehicles, essential for carbon emission reduction, have seen rapid growth in penetration over the past two years. Power batteries, a crucial component of these vehicles, are also experiencing continuous technological innovation in their constituent materials.

[0003] As we all know, the main components of lithium-ion batteries include: positive electrode, negative electrode, electrolyte, and separator. Lithium ions migrate between the positive and negative electrodes through the microporous structure of the separator, generating an electric current, thus completing the charge and discharge process. The separator's microporous structure directly affects the efficiency of lithium ion transmission, thereby affecting the battery's cycle and rate performance. At the same time, the polyolefin separator provides excellent insulation, preventing short circuits caused by direct contact between the positive and negative electrodes. However, long-term battery use inevitably generates heat. At high temperatures, the polyolefin separator's polyolefin chain segments migrate, shrinking its pore size and reducing lithium ion permeability, resulting in a shortened battery life. To address these issues, the polyolefin separator is typically coated with one or more functional coatings. Common coatings include inorganic filler coatings, polymer coatings, and hybrid coatings of inorganic fillers and polymers. Traditional inorganic coatings have a large increase in air permeability, a low lithium ion shuttle rate, and poor adhesion between the inorganic coating and the substrate. Inorganic particles fall off during battery winding and battery charging and discharging, thus affecting the safety performance and capacity of the battery.

[0004] In view of this, the present invention is proposed.

[0005] Summary of the Invention

[0006] One of the objects of the present invention is to provide a battery separator.

[0007] A second object of the present invention is to provide a method for preparing a battery separator.

[0008] A third object of the present invention is to provide a secondary battery comprising the above-mentioned battery separator.

[0009] In order to achieve the above objectives, the present invention provides a battery separator in a first aspect, comprising:

[0010] basement membrane; and

[0011] an inorganic coating disposed on at least one side of the base film;

[0012] Wherein, the contact ratio k between the inorganic particles and the base film in the longitudinal section of the battery separator is 15%-90%;

[0013] The relationship between the contact ratio k and the air permeability A1 of the base film and the air permeability A2 of the coating per unit thickness satisfies:

[0014] A1×k≥A2, wherein the unit of the air permeability A1 of the base film is s / 100cc, and the unit of the air permeability A2 per unit thickness of the coating is s / 100cc / μm.

[0015] According to an embodiment of the present invention, the battery separator has a peel strength of greater than 30 N / m, a needle puncture strength per unit thickness of the coating of greater than 6 gf / μm, and an air permeability per unit thickness of the coating of less than 20 s / 100 cc / μm.

[0016] According to an embodiment of the present invention, the contact ratio k between the inorganic particles and the base film in the longitudinal section of the battery separator is 30%-85%.

[0017] According to an embodiment of the present invention, the peel strength of the battery separator is above 50 N / m, preferably above 100 N / m, in particular above 170 N / m, or even above 190 N / m. The needle puncture strength per unit thickness of the coating is above 9 gf / μm, preferably above 12 gf / μm. The air permeability per unit thickness of the coating is below 15 s / 100 cc / μm, preferably below 10 s / 100 cc / μm.

[0018] The second aspect of the present invention provides a method for preparing the battery separator according to the first aspect, comprising the following steps:

[0019] (1) providing a basement membrane;

[0020] (2) applying an inorganic coating slurry onto the surface of at least one side of the base film to obtain an inorganic coating;

[0021] (3) drying the base film and the inorganic coating to obtain a battery separator;

[0022] The method for preparing the inorganic coating slurry in step (2) comprises the following steps:

[0023] (2-1) 90-99 parts by weight of solvent is introduced into a stirring tank, the anchor paddle speed is set to 10 rpm-30 rpm, the anchor paddle speed is turned on, 1-10 parts by weight of thickener powder is added, and after the addition is completed, the dispersion disk speed is turned on, wherein the dispersion disk speed is 500 rpm-1300 rpm, and the stirring time is 80 min-120 min to obtain a thickener slurry;

[0024] 50-60 parts by weight of solvent are injected into a dual planetary agitator tank, and 32-38 parts by weight of inorganic particles are added, wherein the volume of the inorganic particles and solvent is maintained at 3 / 5-3 / 4 of the volume of the dual planetary agitator tank, and the distance between the liquid surface of the inorganic particles and solvent and the dispersion disk is 1 / 4-1 / 2 of the height of the dual planetary agitator tank; the speed of the anchor paddle in the dual planetary agitator tank is 10 rpm-30 rpm, the speed of the dispersion disk is 500 rpm-1300 rpm, and the stirring time is 10 min-20 min to obtain an inorganic particle slurry;

[0025] (2-2) 5-15 parts by weight of thickener slurry is added to the inorganic particle slurry, the anchor paddle speed in the dual planetary stirring tank is 10 rpm-30 rpm, the dispersion disk speed is 500 rpm-1300 rpm, and the stirring time is 10 min-20 min to obtain a thickening slurry;

[0026] (2-3) passing the thickening slurry through a high-speed disperser or grinder, controlling the temperature of the thickening slurry at 15°C-30°C during the process, to obtain a semi-finished slurry. After the temperature of the semi-finished slurry returns to room temperature, 2-10 parts by weight of a binder and 0.03-0.2 parts by weight of a wetting agent are added and stirred for 20-40 minutes at a stirring speed of 10 rpm-50 rpm to obtain an inorganic coating slurry;

[0027] The inorganic coating slurry has a pH of 7-11, particularly 7.8-9.8; a viscosity of 5-200 mPa·s, particularly 10-130 mPa·s; and a volume average particle size D50 浆料 0.01-2.5μm, especially 0.1-1.2μm; the average absolute value of Zeta potential is 0.025-0.3V, especially 0.035-0.1V;

[0028] In step (2), the coating process controls the tension applied to the base film per unit thickness per unit width to be 2.5-5 N / m / μm, and the difference between the coating roller speed and the coating vehicle speed during the coating process is -50-50 m / min;

[0029] In step (3), the drying process controls the drying temperature of the coating per unit thickness to be 20-50°C / μm, the oven air inlet and exhaust frequency to be 20-45Hz, and the air inlet frequency - exhaust frequency ≤ 6Hz.

[0030] The third aspect of the present invention provides a secondary battery comprising the battery separator described in the first aspect.

[0031] The technical solution of the present invention has the following beneficial effects compared with the prior art:

[0032] The battery separator provided by the present invention achieves improvements in peel strength, needle puncture strength, and air permeability by controlling the contact ratio (k) of the inorganic particles and the base film in the longitudinal cross-section of the separator to between 15% and 90%, and by controlling the relationship between k, the base film's air permeability (A1), and the coating's air permeability (A2) per unit thickness to satisfy the following equation: A1 × k ≥ A2. This results in a separator that simultaneously improves peel strength, needle puncture strength, and air permeability, providing a battery separator that combines safety with high ion permeability. This separator reduces the difficulty of secondary battery assembly, increases battery capacity, and maintains high safety.

[0033] The present invention controls the addition ratio of inorganic particles, binder, and thickener, controls the temperature of the thickening slurry in the pulping process, and controls the ratio of the distance between the liquid surface and the dispersion disk to the height of the double planetary stirring tank within a certain range. This is conducive to the thickener to build a stable steric hindrance, and also helps the binder to fully adsorb on the surface of the inorganic particles to form an electric potential, providing a stable carrier for the composite of the inorganic particles and the base film. At the same time, by controlling the tension matching during the coating process of substrates of different thicknesses, the substrate can exhibit better toughness and ductility, thereby achieving better adhesion between the inorganic particles and the substrate. By matching the oven temperature and the air intake and exhaust frequency with different coating thicknesses, the drying rate of each component in the coating is balanced, preventing the coating from cracking and excessive floating of the binder due to an excessively fast drying rate, and allowing the inorganic particles to be evenly spread on the surface of the base film. The contact ratio of inorganic particles to the base film surface is well controlled (15%-90%) through binders and thickeners, and the air permeability per unit thickness of the coating of the isolation membrane after coating is less than the product of the air permeability of the base membrane and the contact ratio. The isolation membrane is also improved to a certain extent in terms of peel strength, needle puncture strength per unit thickness of the coating, and air permeability per unit thickness of the coating.

[0034] The battery separator obtained by the present invention has a peel strength of more than 30N / m; the inorganic particles in the longitudinal section of the battery separator are in contact with the base film through the binder and the thickener at a ratio of 15-90%; the needle puncture strength per unit thickness of the coating is more than 6gf / μm; and the air permeability per unit thickness of the coating is less than 20s / 100cc / μm.

[0035] Additional aspects and advantages of the present invention will be set forth in part in the description which follows and, in part, will be obvious from the description which follows, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following detailed description, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0037] FIG1 shows an electron microscope image of a cross section in the thickness direction of a battery separator prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0038] The following describes the specific embodiments of the present invention in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention.

[0039] In a first aspect, the present invention provides a battery separator, comprising:

[0040] A base film; and an inorganic coating disposed on at least one side of the base film;

[0041] The battery separator meets the following characteristics:

[0042] The contact ratio k between the inorganic particles and the base film in the longitudinal section of the battery separator is 15%-90%, preferably 30%-85%, and more preferably 30%-65%;

[0043] The relationship between the contact ratio k and the air permeability A1 of the base film and the air permeability A2 of the coating per unit thickness satisfies:

[0044] A1×k≥A2, where the unit of the air permeability A1 of the base film is s / 100cc, and the unit of the air permeability A2 of the coating per unit thickness is s / 100cc / μm;

[0045] The peel strength of the battery separator is above 30 N / m, preferably above 50 N / m, more preferably above 100 N / m, and further preferably above 150 N / m. The needle puncture strength per unit thickness of the coating is above 6 gf / μm, preferably above 9 gf / μm, and further preferably above 12 gf / μm. The air permeability per unit thickness of the coating is below 20 s / 100 cc / μm, preferably below 15 s / 100 cc / μm, and further preferably below 10 s / 100 cc / μm.

[0046] According to the present invention, the base film can be any material known in the art that can be used as a base layer of an isolation membrane, including a polyolefin base film, a non-woven base film, an electrospinning base film, etc., preferably a polyolefin base film. There is no particular restriction on the production process of the polyolefin base film, and dry uniaxial stretching, biaxial synchronous or asynchronous stretching, and wet biaxial synchronous or asynchronous stretching can be used. Preferably, the wet biaxial synchronous or asynchronous stretching method is used for preparation. The polyolefin porous base film can be a single layer of polyethylene (PE) or polypropylene (PP), or a multilayer of polyethylene (PE) and polypropylene (PP). From the perspective of film-forming performance, polyethylene and copolymers are preferred. Polyethylene can be obtained by one-step polymerization or multi-step polymerization. The molecular weight (viscosity average molecular weight) of the polyethylene can be 500,000-4,000,000, for example, the viscosity average molecular weight of the polyethylene is 500,000, 550,000, 600,000, ... 1,000,000, 2,000,000, 3,000,000, 4,000,000. According to a specific embodiment of the present invention, the viscosity average molecular weight of the polyethylene is 600,000-3,000,000, particularly preferably 800,000-3,000,000. The volume average particle size D50 of the polyethylene is 200,000-3,000,000. 聚乙烯 ≤1000μm.

[0047] According to the present invention, the thickness of the base film can be 1-30 μm, such as 1 μm, 2 μm, 3 μm, 4 μm, 5 μm...29 μm, 30 μm. According to a specific embodiment of the present invention, the thickness of the base film is 3-20 μm.

[0048] According to the present invention, the porosity of the base film may be 10-70%, such as 10%, 12%, 15% ... 69%, 70%. According to a specific embodiment of the present invention, the porosity of the base film is 20-60%.

[0049] According to the present invention, the air permeability of the base film can be 40-350 s / 100 cc, for example, 40 s / 100 cc, 45 s / 100 cc, 50 s / 100 cc, ... 240 s / 100 cc, 300 s / 100 cc, 350 s / 100 cc. According to a specific embodiment of the present invention, the air permeability of the base film is 80-200 s / 100 cc. The air permeability can be tested according to the requirements of JIS8117-2009.

[0050] According to the present invention, there is no specific restriction on the type of the inorganic particles, as long as the electrochemical performance is stable. Based on the above reasons, inorganic particles having a dielectric constant of more than 5 and a lithium ion transfer ability are required. Examples that can be cited include oxide particles such as silicon dioxide (SiO2), aluminum oxide (Al2O3), magnesium oxide (MgO), zirconium oxide (ZrO2), titanium oxide (TiO2), calcium oxide (CaO), boehmite (ALOOH), aluminum nitride (AlN), boron nitride (BN) and other nitride particles, barium sulfate (BaSO4), barium titanate (BaTiO3), calcium fluoride (CaF2), barium fluoride (BaF2) and other insoluble ion crystalline particles. The inorganic particles can be selected from one of the above particles, or two or more particles in any proportion. Among these particles, oxide particles are preferred, considering the stability and potential in the electrolyte. In addition, the inorganic particles need to have a high thermal decomposition temperature (decomposition temperature higher than 500°C) and low water absorption. Alumina, boehmite, magnesium oxide, and silica are preferred, and alumina and boehmite are particularly preferred. Alumina and boehmite can neutralize hydrogen fluoride, a by-product formed by the reaction of electrolyte and water, inhibit voltage drop, and thus improve the battery's high-temperature charge storage capacity and room-temperature cycle capacity.

[0051] According to the present invention, there is no particular limitation on the shape of the inorganic particles, and examples thereof include plate-like, flaky, needle-like, columnar, spherical, polyhedral, massive, and rod-like shapes. A combination of multiple inorganic fillers having the above shapes may also be used. From the perspective of improving permeability, plate-like, massive, polyhedral, and columnar shapes having multiple faces are preferred.

[0052] According to the present invention, the volume average particle size D50 of the inorganic particles 无机颗粒 In the range of 0.1 μm to 3 μm, for example, 0.1 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 1 μm, ... 1.5 μm, 2 μm, 2.5 μm, 3.0 μm, according to a specific embodiment of the present invention, the inorganic particles satisfy the following conditions: 0.5 μm ≤ D50 无机颗粒 ≤1.4μm. Among them, D50 无机颗粒 The value is obtained based on the value measured by Mastersizer 3000 particle size distribution analyzer.

[0053] According to the present invention, the specific surface area of ​​the inorganic particles can be 100m 2 / g or less, preferably 50m 2 / g or less, more preferably 30m 2 / g or less, the specific surface area of ​​the inorganic particles is within the above range, which can increase the surface energy of the particles and improve the wetting performance of the electrolyte in the separator, thereby improving the cycle performance of the battery. In addition, it can also improve the cohesion between the slurry particles and the fluidity of the slurry. At the same time, the specific surface area of ​​the inorganic particles can be within 0.5m2 / g or more, preferably 3m 2 / g or above, the water content in the separator is effectively controlled, thereby inhibiting the side reaction of water in the electrolyte and improving the cycle performance of the battery.

[0054] According to the present invention, the inorganic particles may further contain particles having lithium ion transfer capability, thereby improving the conductivity of lithium ions. The particles having lithium ion transfer capability are selected from any one of the following inorganic particles or a mixture of at least two inorganic particles: lithium phosphate, lithium titanium phosphate, lithium aluminum titanium phosphate, lithium nitride, lithium carbonate, lithium chloride, lithium sulfide, and lithium hexafluorophosphate.

[0055] The inorganic coating includes inorganic particles, a binder, a thickener, a wetting agent and other ingredients. The inorganic particles are in contact with the base film through the binder.

[0056] According to the present invention, the thickness of the inorganic coating may be 0.5-10 μm, such as 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, ... 9 μm, 10 μm. According to a specific embodiment of the present invention, the thickness of the inorganic coating is 2-5 μm.

[0057] According to the present invention, the battery separator of the present invention satisfies the following characteristics:

[0058] 1. The contact ratio k between the inorganic particles and the base film in the longitudinal section of the battery separator is 15-90%. For example, the contact ratio between the inorganic particles and the base film in the longitudinal section of the battery separator can be 15%, 16%...30%, 40%, 50%, 60%, 70%, 80%, 90%, 95%.

[0059] The contact ratio (k) refers to the length of the contact between the inorganic particles and the base film in the thickness direction section / the total length of the contact surface between the base film and the coating.

[0060] The test method for the contact ratio k between the inorganic particles and the base film in the longitudinal section can be:

[0061] Take a 10cm×10cm isolation film and take a longitudinal cross-section electron microscope photo. Mark the contact interface between the inorganic particles and the base film k1, k2, k3…k on the photo. n . Measure the contact interface k1, k2, k3…k n The lengths l1, l2, l3…l n , and the total length L of the contact surface between the coating and the base film in the picture. l1, l2, l3…l n The ratio of the sum to L is the contact ratio between the inorganic particles and the base film in the longitudinal section.

[0062] Controlling the contact ratio k can ensure strong adhesion between the inorganic particles and the base film, and significantly improve the peel strength of the isolation film after coating. On the other hand, the permeability of the coating per unit thickness after coating is effectively controlled, reducing the internal resistance of the battery and improving the battery's cycle performance.

[0063] 2. The air permeability of the base film A1×k ≥ the air permeability of the coating per unit thickness A2.

[0064] "Air permeability per unit coating thickness" is the value obtained by dividing the difference between the air permeability of the separator and the air permeability of the base film by the thickness of the inorganic coating (separator thickness - base film thickness). The unit of air permeability is "s / 100cc", and the unit of inorganic coating thickness is "μm".

[0065] Controlling the relationship between k and A1 and A2 can greatly reduce the permeability of the coated separator, improve the lithium ion transmission capacity, and improve the battery's cycle performance; at the same time, it can also improve the coating's peel strength and needle puncture strength, thereby improving battery safety performance.

[0066] 3. The battery separator has a peel strength of 30 N / m or greater, for example, 30 N / m, 31 N / m, 79 N / m, 80 N / m, 90 N / m, 100 N / m, 110 N / m, 120 N / m, 150 N / m, 160 N / m, 170 N / m, 180 N / m, 190 N / m, 200 N / m, 220 N / m, etc.;

[0067] The coating has a needle puncture strength per unit thickness of not less than 6 gf / μm. For example, the coating may have a needle puncture strength per unit thickness of 6 gf / μm, 7 gf / μm, ..., 9 gf / μm, 12 gf / μm, 16 gf / μm, ...;

[0068] "Needle puncture strength per unit coating thickness" is the difference between the needle puncture strength of the separator and the base film, divided by the thickness of the inorganic coating (separator thickness - base film thickness). The unit of needle puncture strength is "gf", and the unit of inorganic coating thickness is "μm".

[0069] The air permeability per unit thickness of the coating is below 20s / 100cc / μm, for example, the air permeability per unit thickness of the coating can be 20s / 100cc / μm, 19s / 100cc / μm...2s / 100cc / μm, 1s / 100cc / μm.

[0070] In a second aspect, the present invention provides a method for preparing the battery separator according to the first aspect, the method comprising the following steps:

[0071] (1) providing a basement membrane;

[0072] (2) applying an inorganic coating slurry onto the surface of at least one side of the base film to obtain an inorganic coating;

[0073] (3) drying the base film and the inorganic coating to obtain a battery separator;

[0074] The method for preparing the inorganic coating slurry in step (2) comprises the following steps:

[0075] (2-1) 90-99 parts by weight of solvent is introduced into a stirring tank, the anchor paddle speed is set to 10 rpm-30 rpm, the anchor paddle speed is turned on, and 1-10 parts by weight of thickener powder is slowly added. After the addition is completed, the dispersion disk is turned on, the dispersion disk speed is set to 500 rpm-1300 rpm, and the stirring time is 80 min-120 min to obtain a thickener slurry;

[0076] 50-60 parts by weight of solvent are injected into a dual planetary agitator tank, and 32-38 parts by weight of inorganic particles are slowly added, wherein the volume of the inorganic particles and solvent is maintained at 3 / 5-3 / 4 of the volume of the dual planetary agitator tank, and the distance between the liquid surface of the inorganic particles and solvent and the dispersion disk is 1 / 4-1 / 2 of the height of the dual planetary agitator tank; the speed of the anchor paddle in the dual planetary agitator tank is 10 rpm-30 rpm, the speed of the dispersion disk is 500 rpm-1300 rpm, and the stirring time is 10 min-20 min to obtain an inorganic particle slurry;

[0077] (2-2) 5-15 parts by weight of thickener slurry is added to the inorganic particle slurry, the anchor paddle speed in the dual planetary stirring tank is 10 rpm-30 rpm, the dispersion disk speed is 500 rpm-1300 rpm, and the stirring time is 10 min-20 min to obtain a thickening slurry;

[0078] (2-3) passing the thickening slurry through a high-speed disperser or grinder, strictly controlling the temperature of the thickening slurry at 15°C-30°C during the process, to obtain a semi-finished slurry. After the temperature of the semi-finished slurry returns to room temperature, 2-10 parts by weight of a binder and 0.03-0.2 parts by weight of a wetting agent are added and stirred for 20-40 minutes at a stirring speed of 10 rpm-50 rpm to obtain an inorganic coating slurry;

[0079] The inorganic coating slurry has a pH of 7-11, particularly 7.8-9.8; a viscosity of 5-200 mPa·s, particularly 10-130 mPa·s, such as 60-80 mPa·s; and a volume average particle size D50 浆料 0.01-2.5μm, especially 0.1-1.2μm, such as 0.8-1μm; the average absolute value of the Zeta potential is 0.025-0.3V, especially 0.035-0.1V, such as 0.07-0.1V;

[0080] In step (2), the coating process controls the tension applied to the base film per unit thickness per unit width to be 2.5-5 N / m / μm, and the difference between the coating roller speed and the coating vehicle speed during the coating process is -50-50 m / min;

[0081] In step (3), the drying process controls the drying temperature of the coating per unit thickness to be 20-50°C / μm, the oven air inlet and exhaust frequency to be 20-45Hz, and the air inlet frequency - exhaust frequency ≤ 6Hz.

[0082] Inorganic coating slurry and preparation:

[0083] The pH of the inorganic coating slurry is 7-11. When the pH of the slurry is within this range, the charge distribution in the slurry is balanced, and the spatial stable structure formed between the particles is not easily broken; the viscosity of the slurry is 5-200 mPa·s, and the flowability of the slurry is significantly improved, thereby reducing the difficulty of coating processing; the volume average particle size D50 of the slurry is 100-200 mPa·s. 浆料 The volume average particle size of the slurry is within the range of 0.01-2.5 μm, which can ensure the uniformity of the coating after coating; the average absolute value of the Zeta potential of the prepared slurry is between 0.025-0.3 V. The larger the absolute value of the Zeta potential, the more balanced the charge distribution of the prepared slurry, and the better the stability and shelf life of the slurry.

[0084] The pH value was measured using a pH meter. Viscosity was measured using a Brookfield viscometer at 25°C and 40 rpm. The volume average particle size was measured using a Mastersizer 3000 particle size distribution analyzer. The zeta potential was the average of the absolute values ​​measured using a Stabino zeta potential analyzer.

[0085] According to the present invention, the solvent can be any of water and organic solvents. Examples of organic solvents include: aliphatic hydrocarbons such as cyclopropane and cyclohexane; ketones such as ethyl methyl ketone and cyclohexanone; aromatic hydrocarbons such as benzene and toluene; nitriles such as acetonitrile and propionitrile; esters such as ethyl acetate and butyl acetate; alcohols such as methanol, ethanol, isopropanol, and ethylene glycol; ethers such as tetrahydrofuran and ethylene glycol diethyl ether; and amides such as N-methylpyrrolidone and N,N-dimethylformamide. These solvents can be used alone or in combination. Among them, water is preferably used as the solvent for preparing the slurry.

[0086] According to the present invention, there is no specific limitation on the type of the binder. It can be any polymer that can be used as an inorganic particle binder in the art. Examples include acrylate, polyvinylidene fluoride, styrene-butadiene rubber, polyacrylonitrile, polyvinyl alcohol, vinyl acetate, etc.

[0087] According to the present invention, the binder may be an acrylate polymer, which may be selected from water-soluble acrylic polymers, emulsion-type acrylic polymers, or a mixture thereof in any proportion, preferably an emulsion-type acrylic polymer.

[0088] According to the present invention, the emulsion-type acrylate polymer refers to a water-emulsion type, that is, an acrylate polymer having a milky white or bluish appearance, and the main monomer is a monomer containing a carboxylic acid or ester functional group, for example, it can be at least one of acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, octyl acrylate, lauryl acrylate, stearic acrylate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, butyl methacrylate, isobutyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl acrylate, n-octyl methacrylate, n-hexyl acrylate, dodecyl methacrylate, n-decyl methacrylate, 2-ethylhexyl acrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, and trimethylolpropane triacrylate.

[0089] As thickeners, polysaccharides are preferred. Examples include natural polymer compounds and cellulose semi-synthetic polymer compounds. A single thickener may be used alone, or two or more may be combined in any proportion. To improve the dispersibility of the inorganic particles, cellulose semi-synthetic compounds such as carboxymethyl cellulose, sodium carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose are preferred.

[0090] The etherification degree of the cellulose semisynthetic polymer is preferably 0.5 or higher, more preferably 0.7 or higher, and preferably 1.2 or lower, more preferably 1.0 or lower. The etherification degree refers to the degree of substitution of the three hydroxyl groups of each anhydroglucose unit in the cellulose with substituents such as carboxymethyl groups. An etherification degree between 0 and 3 ensures the compatibility of the cellulose with the solvent while also forming a stable steric structure, improving the dispersibility of the inorganic particles in the solvent and extending the storage life of the slurry.

[0091] The average degree of polymerization of the cellulose semisynthetic polymer compound is preferably 500 or more, more preferably 1000 or more, preferably 2500 or less, more preferably 2000 or less, and particularly preferably 1500 or less. The average degree of polymerization of the thickener forms a certain steric hindrance through the interaction with the solvent, promoting the fluidity of the slurry, thereby improving the stability of the slurry and the coating effect. By controlling the average degree of polymerization of the thickener within the above range, the stability of the slurry, storage aging, and uniformity of the coating during coating are improved.

[0092] The wetting agent is mainly an alkyl surfactant, a silicon surfactant, a fluorine surfactant, an ether surfactant, etc. The amount of the wetting agent is preferably less than 0.5% of the coating weight, more preferably less than 0.2%, preferably more than 0.01%, and more preferably more than 0.03%. Controlling the amount of surfactant added within the above range can reduce the surface tension of the slurry on the porous membrane and improve the wetting or spreading effect of the slurry. If the amount of surfactant added is more than 5% of the slurry weight, the wetting agent will penetrate into the pores of the substrate, affecting the transmission of lithium ions and the adhesion of inorganic particles to the substrate, resulting in the separation membrane shedding during the battery winding process, increasing the internal resistance of the battery, and reducing the capacity.

[0093] According to the present invention, the anchor paddle speed is 10rpm-30rpm, for example, it can be 10rpm, 15rpm...30rpm, the dispersion disk speed is 500rpm-1300rpm, for example, it can be 500rpm, 600rpm...1200rpm, 1300rpm, and the stirring time is 80-120min, for example, it can be 80min, 90min...100min, 120min.

[0094] According to the present invention, the volume of the inorganic particles and the solvent is maintained between 3 / 5-3 / 4 of the volume of the double planetary stirring tank, for example, it can be 3 / 5, 5 / 8...29 / 40, 3 / 4, and the distance between the liquid surface of the inorganic particles and the solvent and the dispersion disk is 1 / 4-1 / 2 of the height of the double planetary stirring tank, for example, it can be 1 / 4, 7 / 24...11 / 24, 1 / 2. The volume ratio and the distance between the liquid surface and the dispersion disk are controlled within this range. During the stirring process, the inorganic particles can be evenly dispersed in the solvent, thereby improving the stability of the slurry.

[0095] According to the present invention, the thickening slurry is passed through a high-speed disperser or grinder, and the temperature of the thickening slurry is strictly controlled at 15°C-30°C during the process, for example, 15°C, 16°C...29°C, 30°C. When the temperature is below 5°C, the colloid particles coagulate to form micelles, which is not conducive to dispersion in the subsequent process, and the film surface forms leaks during the coating process. When the temperature is above 30°C, the steric hindrance formed by the colloid particles is destroyed, the slurry is olefinized, and the stability is reduced; after the temperature of the half-layer slurry returns to room temperature, the binder and wetting agent are added and stirred, and the anchor paddle stirring speed is controlled at 10rpm-50 rpm, for example it can be 10rpm, 11rpm...49rpm, 50rpm. When the stirring speed is lower than 10rpm, the binder and wetting agent cannot be evenly dispersed in the slurry, resulting in uneven coating of the isolation membrane after coating, and the contact ratio between the inorganic particles and the base membrane in the longitudinal section of the isolation membrane is reduced, thereby affecting the peel strength of the isolation membrane; when the stirring speed is greater than 50rpm, the binder is sheared into a film and a crust is formed, resulting in an increase in large particles in the slurry, poor coating consistency, and poor heat resistance of the isolation membrane. At the same time, there is a large amount of foam in the slurry, the slurry utilization rate is reduced, and the cost increases.

[0096] In addition to the aforementioned components, the inorganic coating slurry may also contain other optional components. Examples include dispersants and electrolyte dispersion inhibitors. These components are not particularly limited as long as they do not adversely affect the lithium battery. The optional components may be one, two, or more, but their addition ratio must not exceed 5% of the slurry weight.

[0097] By controlling the addition amount of each component, the stirring speed during the slurry preparation, the material temperature during the dispersion process and other formula design and process control, the inorganic particles in the prepared slurry are evenly dispersed, and the volume average particle size D50 浆料 0.01-2.5μm, the inorganic particles in the slurry are suspended in the solvent, and the average absolute value of the Zeta potential is 0.025-0.3V.

[0098] Coating and drying process:

[0099] According to the present invention, the tension applied to the base film during the coating process can be controlled to be 2.5N / m / μm, 1.5N / m / μm...4.5N / m / μm, 5N / m / μm; by setting the coating tension corresponding to base films of different thicknesses and widths, the extension of the base film during high-speed coating can be reduced, and at the same time, the speed difference between the coating roller and the coating speed can be controlled during the process, and the difference can be controlled within -50 / min-50m / min, ensuring that the slurry is better spread on the base film, preventing the slurry from demulsifying under high-speed shearing, and at the same time, it can Ensure the adhesion between inorganic particles and the contact area ratio between the inorganic particles and the base film surface; the temperature during the drying process of the unit coating thickness is 20-50℃ / μm, the oven air intake and exhaust frequency is 20-45Hz, and the air intake frequency-exhaust frequency ≤6Hz. Setting the oven temperature and air intake and exhaust frequency within this range can control the rate of the slurry in the drying process, avoid coating cracking caused by too fast a rate, and allow the adhesive and thickener to be fully cured to form a certain contact area, thereby improving the peel strength of the isolation film.

[0100] According to the present invention, there is no particular limitation on the coating method of the slurry, and methods such as coating method and dipping method can be selected for coating. As coating methods, methods such as scraper method, reverse roller method, direct roller method, micro gravure roller method, extrusion method, spraying method, and spot coating method can be cited. Considering the uniformity of the thickness of the porous film, the micro gravure roller method is preferably used for coating.

[0101] According to the present invention, there is no particular limitation on the drying method, and drying methods such as hot air, low-humidity air, vacuum drying, spray drying, and freeze drying can be selected.

[0102] According to a third aspect of the present invention, a secondary battery is provided, comprising the battery separator according to the first aspect.

[0103] According to the present invention, the secondary battery may include a lithium ion battery or a sodium ion battery.

[0104] The isolation membrane and the secondary battery prepared by the method for preparing the isolation membrane have the same advantages as the above isolation membrane, and will not be described in detail here.

[0105] The present invention will be described below with reference to specific examples. It should be noted that these examples are merely illustrative and do not limit the present invention in any way. Unless otherwise specified, the raw materials, reagents, methods, etc. adopted in the examples are all conventional raw materials, reagents, methods in this area.

[0106] Peel strength test method:

[0107] Use a 2.5cm x 30cm mold to cut the specimen and affix it evenly to a short steel ruler covered with double-sided tape. Roll the specimen back and forth three times with a roller. Manually peel off 1cm of the specimen and clamp it to a tensile testing machine for a 180° test at a tensile speed of 50mm / min. Take the average of the three measurements.

[0108] Thickness test method:

[0109] Cut a 20cm x 10ncm coating width strip, where n is a natural number greater than 2. Use a Mahr thickness gauge to measure the thickness of the base film and coating film at points every 10cm. The difference between the two is the coating thickness. The average of all coating thicknesses is recorded as the average coating thickness.

[0110] Air permeability test method:

[0111] The test was carried out with reference to the requirements of JIS8117-2009.

[0112] When the coated mother roll is cut along the TD direction and the width is ≥5cm, and the TD width of the coated finished product sample is less than 5cm, a small measuring head is used for detection. A Wangyan air permeability meter is used with the test time set to 3S to measure the air permeability of the base film and the coating film. The difference between the two is the coating air permeability. The average of all coating air permeabilities is recorded as the average coating air permeability, and the ratio of the average coating air permeability to the average coating thickness is recorded as the coating unit thickness air permeability.

[0113] Acupuncture strength test method:

[0114] Refer to ASTM D4833-00e1 or GB / T 10004-2008 for testing.

[0115] A sample approximately 50mm wide was cut from the film roll along its TD and placed in a fixture on the sample stage for testing. The needle tip was a 1.0mm hemisphere at a speed of 1mm / s. The needle puncture strength of the base film and the coating was measured. The difference between the two was the coating puncture strength. The average of all coating puncture strengths was recorded as the average coating puncture strength, and the ratio of the average coating puncture strength to the average coating thickness was recorded as the coating puncture strength per unit thickness.

[0116] Test method for the contact ratio between inorganic particles and base film in longitudinal section:

[0117] Take a 10cm×10cm smooth inorganic coating film and take a longitudinal cross-section electron microscope photo. Mark the contact interface k1, k2, k3…k between the inorganic particles and the base film on the photo. n , measure the contact interface k1, k2, k3…k n The lengths l1, l2, l3…l n , and the total length L of the contact surface between the coating and the base film in the picture, l1, l2, l3…ln The ratio of the sum to L is the contact ratio between the inorganic particles and the base film in the longitudinal section.

[0118] Example 1

[0119] Preparation of inorganic coating slurry:

[0120] (1) Preparation of thickener stock: 95 kg of ultrapure water was introduced into a stirring tank, the speed of the anchor paddle was set to 20 rpm, and the anchor paddle speed was turned on. 5 kg of thickener sodium carboxymethyl cellulose (Dacel, 1220) powder was slowly added. After the addition was completed, the dispersion plate was turned on, the dispersion plate speed was 1200 rpm, and the stirring time was 100 min to obtain 100 kg of thickener stock;

[0121] (2) Preparation of alumina slurry: 52.9 kg of ultrapure water was poured into a double planetary mixing tank, and 35 kg of volume average particle size D50 was slowly added. 无机颗粒 The aluminum oxide is 0.912 μm in diameter; the volume of the aluminum oxide and ultrapure water is maintained at 72.04% of the volume of the dual planetary mixing tank, and the distance between the upper liquid surface of the aluminum oxide and ultrapure water and the dispersion disk is 32.34% of the height of the dual planetary mixing tank; the anchor paddle speed is 20 rpm, the dispersion disk speed is 1000 rpm, and the stirring time is 15 minutes, to obtain 87.9 kg of aluminum oxide slurry;

[0122] (3) adding 7.5 kg of thickener slurry to the above 87.9 kg of alumina slurry, and using the double planetary stirring anchor propeller speed, dispersion disk speed, and stirring time in step (2) to obtain a thickening slurry;

[0123] (4) The thickening slurry was passed through a high-speed dispersing grinder, and the temperature of the thickening slurry was controlled at 17°C during the process to obtain a semi-finished slurry. After the temperature of the semi-finished slurry returned to room temperature, 4.3 kg of adhesive acrylate (Ruiong; 900B) and 0.05 kg of wetting agent (Guangdong Guoyuanxing TEGO202E) were added and stirred for 30 minutes. The stirring speed was controlled at 20 rpm to obtain a finished slurry. The pH of the finished slurry was 8.39, the viscosity was 64.1 mPa·s, and the volume average particle size D50 of the slurry was 8.39. 浆料 At 0.897 μm; the average Zeta potential of the slurry is -0.0871 V.

[0124] Preparation of isolation film:

[0125] A polyethylene base film with a thickness of 5 μm (produced by China National Materials Lithium Membrane Co., Ltd., with an air permeability of 126s / 100cc) was used; a coating tension of 5 N / m / μm was used, and the coating machine speed and coating roller speed during the coating process were 120 m / min and 100 m / min, respectively. The prepared finished slurry was coated on one side of the base film, and the prepared coated isolation film was dried in an oven at a drying temperature of 22°C / μm. The oven inlet and exhaust frequencies were 27 Hz and 30 Hz, respectively, to obtain a coating film, and its cross-sectional electron microscope image in the thickness direction is shown in Figure 1.

[0126] It was determined that the contact ratio k between the inorganic particles and the base film in the longitudinal section of the coated isolation film was 50.37%;

[0127] The peel strength is 204N / m, the coating thickness is 2.9μm, the needle puncture strength per unit thickness of the coating is 12.2gf / μm, the air permeability of the isolation film is 157s / 100cc, and the air permeability per unit thickness of the coating is 10.7s / 100cc / μm.

[0128] Examples 2-6, Comparative Examples 1-4

[0129] The specific raw materials, preparation parameters, and isolation membrane parameters and properties of the remaining embodiments and comparative examples are shown in Tables 1 and 2 below (the unlisted parts are the same as those of Example 1).

[0130] Table 1

[0131] Table 2

[0132] Analysis: As can be seen from the table above, in Examples 1-6, by controlling the content of each component in the slurry, the percentage of the non-conductive particle slurry in the tank volume, the non-conductive particle slurry interface liquid level and the dispersion plate spacing as a percentage of the tank height, the dispersion material temperature, and the coating process, k was consistently between 15% and 90%, and A1×k≥A2. The resulting separators exhibited excellent peel strength, high needle punch strength value-added, and low air permeability value-added. In contrast, in Comparative Examples 1-4, k was not between 15% and 90%, or A1×k<A2, due to adjustments to the dispersion material temperature, the non-conductive particle slurry interface liquid level and the dispersion plate spacing as a percentage of the tank height, and the coating process. The separators produced failed to achieve a balance between the three properties.

[0133] Although the embodiments of the present invention have been shown and described above, it will be understood that the above embodiments are illustrative and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A battery separator, characterized in that: include: Basement membrane; as well as An inorganic coating disposed on at least one side of the base film; Wherein, the contact ratio k between the inorganic particles and the base film in the longitudinal section of the battery separator is 15%-90%; The relationship between the contact ratio k and the air permeability A1 of the base film and the air permeability A2 of the coating per unit thickness satisfies: A1×k≥A2, wherein the unit of the air permeability A1 of the base film is s / 100cc, and the unit of the air permeability A2 of the coating per unit thickness is s / 100cc / μm.

2. The battery separator according to claim 1, characterized in that: The battery separator has a peel strength of more than 30 N / m, a needle puncture strength per unit thickness of the coating layer of more than 6 gf / μm, and an air permeability per unit thickness of the coating layer of less than 20 s / 100 cc / μm.

3. The battery separator according to claim 1, characterized in that: The contact ratio k between the inorganic particles and the base film in the longitudinal section of the battery separator is 30%-85%; and / or The battery separator has a peel strength of more than 50 N / m, a coating layer having a unit thickness needle puncture strength value-added of more than 9 gf / μm, and a coating layer having a unit thickness air permeability value-added of less than 15 s / 100 cc / μm.

4. The battery separator according to claim 1, characterized in that: The thickness of the base film is 1-30 μm; and / or The air permeability of the base film is 40-350s / 100cc.

5. The battery separator according to claim 1, characterized in that: The inorganic particles are selected from one or more of silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide, calcium oxide, boehmite, aluminum nitride, boron nitride, barium sulfate, calcium fluoride, and barium fluoride; and / or The volume average particle size D50 of the inorganic particles 无机颗粒 0.1μm-3μm.

6. The battery separator according to claim 1, characterized in that: The thickness of the inorganic coating is 0.5-10 μm.

7. The method for preparing a battery separator according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) providing a basement membrane; (2) applying an inorganic coating slurry onto at least one side of the base film to obtain an inorganic coating; (3) drying the base film and the inorganic coating to obtain a battery separator; The method for preparing the inorganic coating slurry in step (2) comprises the following steps: (2-1) 90-99 parts by weight of solvent is introduced into a stirring tank, the speed of the anchor paddle is set to 10 rpm-30 rpm, the anchor paddle speed is turned on, 1-10 parts by weight of thickener powder is added, and after the addition is completed, the speed of the dispersion disk is turned on, wherein the speed of the dispersion disk is 500 rpm-1300 rpm, and the stirring time is 80 min-120 min to obtain a thickener slurry; 50-60 parts by weight of solvent are injected into a double planetary stirring tank, and 32-38 parts by weight of inorganic particles are added, wherein the volume of the inorganic particles and the solvent is maintained at 3 / 5-3 / 4 of the volume of the double planetary stirring tank, and the distance between the liquid surface of the inorganic particles and the solvent and the dispersion disk is 1 / 4-1 / 2 of the height of the double planetary stirring tank; the speed of the anchor paddle in the double planetary stirring tank is 10rpm-30rpm, the speed of the dispersion disk is 500rpm-1300rpm, and the stirring time is 10min-20min to obtain an inorganic particle slurry; (2-2) 5-15 parts by weight of thickener slurry is added to the inorganic particle slurry, the anchor paddle speed in the double planetary stirring tank is 10 rpm-30 rpm, the dispersion disk speed is 500 rpm-1300 rpm, and the stirring time is 10 min-20 min to obtain a thickening slurry; (2-3) passing the thickening slurry through a high-speed disperser or grinder, controlling the temperature of the thickening slurry at 15° C.-30° C. during the process, to obtain a semi-finished slurry, and after the temperature of the semi-layer slurry returns to room temperature, adding 2-10 parts by weight of a binder and 0.03-0.2 parts by weight of a wetting agent, stirring for 20-40 minutes at a stirring speed of 10 rpm-50 rpm, to obtain an inorganic coating slurry; In step (2), the tension applied to the base film per unit thickness per unit width is controlled to be 2.5-5 N / m / μm, and the difference between the coating roller speed and the coating vehicle speed during the coating process is -50-50 m / min; In step (3), the drying process controls the drying temperature of the coating per unit thickness to be 20-50°C / μm, the oven air inlet and exhaust frequency to be 20-45Hz, and the air inlet frequency - exhaust frequency ≤ 6Hz.

8. The preparation method according to claim 7, characterized in that: The parameters of the inorganic coating slurry in step (2) are as follows: pH 7-11; viscosity 5-200 mPa·s; volume average particle size D50 浆料 0.01-2.5μm; the average absolute value of Zeta potential is 0.025-0.3V.

9. The preparation method according to claim 7, characterized in that: The thickener is selected from one or more of carboxymethyl cellulose, sodium carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose; and / or The binder is one or more selected from acrylate, polyvinylidene fluoride, styrene-butadiene rubber, polyacrylonitrile, polyvinyl alcohol, and vinyl acetate; and / or The wetting agent is selected from one or more of an alkyl surfactant, a silicon surfactant, a fluorine surfactant, and an ether-based surfactant.

10. A secondary battery, characterized in that: The invention comprises the battery separator according to any one of claims 1 to 6.