Film adhesive, dicing / die bonding integrated film, and semiconductor device and method for producing same
Patent Information
- Application Number
- MYPI2025005479
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-03-14
- Publication Date
- 2024-09-15
AI Technical Summary
In the manufacturing of stacked Multi Chip Packages (MCPs), existing film adhesives used in dicing/die bonding integrated films face challenges in providing sufficient breaking strength and processability for thin film formation while preventing chip cracks, which occur due to the thinning and brittleness of semiconductor chips during wire bonding.
A film adhesive with a thermosetting resin component and elastomer, containing 18% or more elastomer by mass and up to 25% inorganic filler by mass, cured at 140°C for 30 minutes, achieving a storage modulus of 80 MPa or more at 150°C and 2000 MPa or less at 30°C, ensuring improved processability and crack suppression.
The film adhesive enhances the breaking strength and processability of thin films, effectively preventing chip cracks and warping of semiconductor devices, while maintaining suitable flexibility and adhesive strength.
Smart Images

Figure PI2025005479_DRAWING_001 
Figure PI2025005479_DRAWING_002 
Figure PI2025005479_DRAWING_003
Abstract
Description
Film-like adhesive, dicing / die bonding integrated film, semiconductor device, and manufacturing method thereof
[0001] The present disclosure relates to a film adhesive, a dicing and die bonding integrated film, a semiconductor device, and a method for manufacturing the same.
[0002] In recent years, stacked MCPs (Multi Chip Packages), in which semiconductor chips are stacked in multiple stages, have become widespread and are installed as memory semiconductor packages for mobile phones, mobile audio devices, etc. Furthermore, as mobile phones and other devices become more multifunctional, semiconductor packages are being made faster, denser, and more highly integrated.
[0003] A commonly used method for manufacturing a semiconductor device is to attach a dicing / die-bonding integrated film having an adhesive layer and a pressure-sensitive adhesive layer to the backside of a semiconductor wafer, and then cut the semiconductor wafer, adhesive layer, and part of the pressure-sensitive adhesive layer to separate the wafer (semiconductor wafer backside attachment method). For example, Patent Documents 1 and 2 disclose film-like adhesives used in the adhesive layer in such a method.
[0004] International Publication No. WO 2013 / 133275 International Publication No. WO 2020 / 013250
[0005] In a stacked MCP, semiconductor chips are stacked in multiple stages, and therefore the film adhesive used in the dicing / die bonding integrated film is required to have sufficient breaking strength even when a thin film (for example, a thickness of 15 μm or less) is formed. When a film adhesive has sufficient breaking strength, it tends to have excellent processability (for example, film cuttability for cutting into a predetermined shape) when a thin film is formed.
[0006] In addition, in recent semiconductor packages, semiconductor chips composed of a circuit layer and a semiconductor layer tend to have thicker circuit layers and thinner semiconductor layers. In such semiconductor packages, chip cracks may occur, for example, during wire bonding, which connects the circuit layer of the semiconductor chip to an electrode on the substrate with a bonding wire. It is believed that such chip cracks occur when the semiconductor layer becomes thin and brittle, resulting from vibrations during wire bonding. Therefore, film-like adhesives used in dicing and die bonding integrated films are also required to be able to suppress the occurrence of chip cracks.
[0007] Therefore, a main object of the present disclosure is to provide a film-like adhesive that has excellent processability when formed into a thin film and is capable of suppressing the occurrence of chip cracks.
[0008] The inventors conducted extensive research to solve the above-mentioned problems and discovered that by ensuring that the elastomer content in the film adhesive is above a predetermined range, that the inorganic filler content in the film adhesive is below a predetermined range, and that the storage modulus of the film adhesive after curing is above a predetermined range, it is possible to improve the processability when a thin film is formed and further to suppress the occurrence of chip cracks, which led to the completion of the invention of the present disclosure.
[0009] The present disclosure provides the film-like adhesives described in [1] to [8], the dicing-die bonding integrated film described in [9], the semiconductor devices described in
[10] and
[11] , and the semiconductor devices described in
[12] and
[13] . [1] A film-like adhesive containing a thermosetting resin component and an elastomer and optionally further containing an inorganic filler, wherein the content of the elastomer is 18% by mass or more based on the total amount of the film-like adhesive, the content of the inorganic filler is 0 to 25% by mass based on the total amount of the film-like adhesive, and when the film-like adhesive is cured under conditions of 140°C and 30 minutes, the cured product has a storage modulus at 150°C of 80 MPa or more and a thickness of the film-like adhesive of 15 μm or less. [2] The film-like adhesive described in [1], wherein the content of the elastomer is 18 to 35% by mass based on the total amount of the film-like adhesive. [3] The film-like adhesive according to [1] or [2], wherein the content of the inorganic filler is 0 to 3 mass % based on the total amount of the film-like adhesive. [4] The film-like adhesive according to any one of [1] to [3], wherein the storage modulus at 30°C of the cured product when the film-like adhesive is cured under conditions of 140°C and 30 minutes is 2000 MPa or less. [5] The film-like adhesive according to any one of [1] to [4], wherein the thermosetting resin component comprises an epoxy resin and a phenolic resin. [6] The film-like adhesive according to any one of [1] to [5], wherein the glass transition temperature of the elastomer is 0 to 30°C. [7] The film-like adhesive according to any one of [1] to [6], which is used in a manufacturing process of a semiconductor device comprising a plurality of stacked semiconductor chips. [8] The film-like adhesive according to [7], wherein the semiconductor device is a three-dimensional NAND memory. [9] An integrated dicing and die bonding film comprising, in this order: a base layer, a pressure-sensitive adhesive layer, and an adhesive layer made of the film-like adhesive according to any one of [1] to [6].
[10] A semiconductor device comprising: a first semiconductor chip; a support member on which the first semiconductor chip is mounted; and a cured film adhesive according to any one of [1] to [6], which is provided between the first semiconductor chip and the support member and bonds the first semiconductor chip to the support member.
[11] The semiconductor device according to
[10] , further comprising a second semiconductor chip different from the first semiconductor chip, stacked on a surface of the first semiconductor chip.
[12] A method for manufacturing a semiconductor device, comprising the steps of: attaching the adhesive layer of the dicing and die bonding integrated film according to [9] to a semiconductor wafer; cutting the semiconductor wafer with the adhesive layer attached to produce a plurality of individual adhesive piece-attached semiconductor chips; and bonding the first adhesive piece-attached semiconductor chip, which has the first semiconductor chip and the first adhesive piece, to a support member via the adhesive piece.
[13] The method for manufacturing a semiconductor device according to
[12] , further comprising the step of attaching a second adhesive piece-attached semiconductor chip, which has a second semiconductor chip and a second adhesive piece, to the surface of the first semiconductor chip in the first adhesive piece-attached semiconductor chip adhered to the support member via the second adhesive piece.
[0010] According to the present disclosure, a film-like adhesive is provided that exhibits excellent processability when a thin film is formed and is capable of suppressing the occurrence of chip cracks. Some embodiments of the film-like adhesive can also suppress warpage of a semiconductor device (semiconductor package). The present disclosure also provides an integrated dicing and die bonding film using such a film-like adhesive, as well as a semiconductor device and a method for manufacturing the same. The present disclosure also provides a method for manufacturing a semiconductor device using such a dicing and die bonding integrated film.
[0011] Fig. 1 is a schematic cross-sectional view showing one embodiment of a film-like adhesive. Fig. 2 is a schematic cross-sectional view showing one embodiment of a dicing / die bonding integrated film. Fig. 3 is a schematic cross-sectional view showing one embodiment of a semiconductor device. Fig. 4 is a schematic cross-sectional view showing another embodiment of a semiconductor device. Fig. 5 is a schematic cross-sectional view showing another embodiment of a semiconductor device. Fig. 6 is a diagram showing the shape of a test piece used to measure breaking strength.
[0012] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings as appropriate. However, the present disclosure is not limited to the following embodiments. In the following embodiments, components (including steps, etc.) are not essential unless specifically stated. The sizes of the components in each figure are conceptual, and the relative size relationships between the components are not limited to those shown in each figure.
[0013] The same applies to numerical values and ranges in the present disclosure and do not limit the present disclosure. In this specification, numerical ranges indicated using "to" indicate ranges that include the numerical values before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this specification, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in numerical ranges described in this specification, the upper or lower limit value of that numerical range may be replaced with a value shown in the examples. In addition, the upper and lower limits described individually can be arbitrarily combined. In addition, "A or B" may include either A or B, or may include both. In addition, unless otherwise specified, the materials exemplified below may be used alone or in combination of two or more. When multiple substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified.
[0014] In this specification, (meth)acrylate means acrylate or its corresponding methacrylate, and the same applies to other similar expressions such as (meth)acryloyl group, (meth)acrylic copolymer, etc.
[0015] [Film-like adhesive] Fig. 1 is a schematic cross-sectional view showing one embodiment of a film-like adhesive. The film-like adhesive 1 shown in Fig. 1 may be thermosetting, and may be capable of passing through a semi-cured (B-stage) state and then becoming fully cured (C-stage) after a curing treatment.
[0016] The film adhesive 1 satisfies the following conditions: - The storage modulus at 150°C after curing under conditions of 140°C and 30 minutes is 80 MPa or more; - The thickness is 15 μm or less.
[0017] The storage modulus of the film-like adhesive 1 at 150°C after curing at 140°C for 30 minutes is 80 MPa or more, and may be 85 MPa or more, 90 MPa or more, 95 MPa or more, 100 MPa or more, 105 MPa or more, 110 MPa or more, 115 MPa or more, 120 MPa or more, 125 MPa or more, or 130 MPa or more. A storage modulus of 80 MPa or more can compensate for the brittleness of semiconductor chips due to thinning, and as a result, it is possible to suppress the occurrence of chip cracks. The upper limit of the storage modulus is not particularly limited, but may be, for example, 500 MPa or less, 300 MPa or less, 250 MPa or less, or 200 MPa or less.
[0018] The storage modulus of the film-like adhesive 1 at 30°C after curing at 140°C for 30 minutes may be 2000 MPa or less, or may be 1800 MPa or less, 1600 MPa or less, 1400 MPa or less, or 1200 MPa or less. If the storage modulus is 2000 MPa or less, the film-like adhesive can be more easily thinned, and the cured film-like adhesive tends to be more sufficiently prevented from becoming too hard. The lower limit of the storage modulus is not particularly limited, but may be, for example, 600 MPa or more, 700 MPa or more, 800 MPa or more, 900 MPa or more, or 1000 MPa or more.
[0019] In this specification, the storage modulus at 150°C after curing of a film-like adhesive can be measured, for example, by the following method. A measurement sample is prepared by laminating multiple 5 μm-thick film-like adhesives to a thickness of 100 μm or more, and then cutting this into a size of 4 mm wide x 20 mm long or more. The prepared sample is cured at 140°C for 30 minutes, and then the cured sample is placed in a dynamic viscoelasticity measuring device (e.g., Rheogel E-4000, manufactured by UBM Corporation). Dynamic viscoelasticity is measured in a temperature dependence measurement mode, applying a tensile load and measuring from room temperature (25°C) to 300°C under conditions of a chuck distance of 20 mm, a frequency of 10 Hz, and a heating rate of 3°C / min. The storage modulus values at 30°C and 150°C are then read, and the respective values are taken as the storage modulus at 30°C and 150°C.
[0020] The thickness of the film adhesive 1 is 15 μm or less, and may be 12 μm or less, 10 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, or 5 μm or less. The lower limit of the thickness of the film adhesive is not particularly limited, but may be, for example, 1 μm or more.
[0021] The film-like adhesive 1 contains a thermosetting resin component (hereinafter sometimes referred to as "component (A)") and an elastomer (hereinafter sometimes referred to as "component (B)"), and may further contain an inorganic filler (hereinafter sometimes referred to as "component (C)"). Component (A) may contain, for example, an epoxy resin (hereinafter sometimes referred to as "component (A1)") and a phenolic resin (hereinafter sometimes referred to as "component (A2)"). The content of component (B) is 18 mass% or more based on the total amount of the film-like adhesive. The content of component (C) is 0 to 25 mass% based on the total amount of the film-like adhesive. In addition to components (A), (B), and (C), the film-like adhesive 1 may further contain a coupling agent (hereinafter sometimes referred to as "component (D)"), a curing accelerator (hereinafter sometimes referred to as "component (E)"), other components, and the like. By employing such constituent components, it tends to be easier to prepare a film-like adhesive that satisfies the above conditions of storage modulus after curing and thickness.
[0022] Component (A): Thermosetting Resin Component Component (A1): Epoxy Resin Component (A1) can be any resin having an epoxy group in the molecule without any particular limitations. Examples of component (A1) include bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, bisphenol A novolac epoxy resins, bisphenol F novolac epoxy resins, stilbene epoxy resins, triazine skeleton-containing epoxy resins, fluorene skeleton-containing epoxy resins, triphenolmethane epoxy resins, biphenyl epoxy resins, xylylene epoxy resins, biphenyl aralkyl epoxy resins, naphthalene epoxy resins, and diglycidyl ether compounds of polyfunctional phenols and polycyclic aromatics such as anthracene. Among these, component (A1) may contain cresol novolac epoxy resins, bisphenol F epoxy resins, bisphenol A epoxy resins, or naphthalene epoxy resins from the viewpoint of film tackiness, flexibility, and the like. Bisphenol F type epoxy resins have a relatively low softening point, and many of them have a softening point of 40° C. or less.
[0023] The component (A1) may contain an epoxy resin having a softening point of 40°C or lower (or an epoxy resin that is liquid at 30°C, hereinafter sometimes referred to as "component (A1a)"). The component (A1) may be a combination of component (A1a) and an epoxy resin having a softening point of more than 40°C (or an epoxy resin that is solid at 30°C, hereinafter sometimes referred to as "component (A1b)"). When component (A1) contains component (A1a), the storage modulus after curing tends to be more easily improved. Furthermore, when component (A1) is a combination of component (A1a) and component (A1b), thinning of the film tends to be even more easily achieved. The component (A1a) may contain, for example, a bisphenol F epoxy resin.
[0024] In this specification, the softening point refers to a value measured by the ring and ball method in accordance with JIS K7234:1986.
[0025] Examples of commercially available products of component (A1a) include EXA-830CRP (trade name, manufactured by DIC Corporation, liquid at 30°C), YDF-8170C (trade name, manufactured by Nippon Steel Chemical & Material Co., Ltd., liquid at 30°C), and EP-4088S (trade name, manufactured by ADEKA Corporation, liquid at 30°C).
[0026] When the component (A1) is a combination of the components (A1a) and (A1b), the content of the component (A1a) may be 5% by mass or more, 10% by mass or more, or 15% by mass or more, and may be 70% by mass or less, 60% by mass or less, or 50% by mass or less, based on the total amount of the component (A1). Note that the content of the component (A1a) in the component (A1) in the adhesive composition when forming the film-like adhesive may be the same as the above range.
[0027] When the component (A1) is a combination of the components (A1a) and (A1b), the content of the component (A1b) may be 30% by mass or more, 40% by mass or more, or 50% by mass or more, and may be 95% by mass or less, 90% by mass or less, or 85% by mass or less, based on the total amount of the component (A1). Note that the content of the component (A1b) in the component (A1) in the adhesive composition when forming the film-like adhesive may be the same as the above range.
[0028] The epoxy equivalent of component (A1) is not particularly limited, but may be 90 to 300 g / eq or 110 to 290 g / eq. When the epoxy equivalent of component (A1) is within this range, it tends to be easier to ensure the fluidity of the adhesive composition when forming the film adhesive while maintaining the bulk strength of the film adhesive.
[0029] Component (A2): Phenolic Resin The component (A2) acts as a curing agent for the component (A1), i.e., it can be a curing agent for the epoxy resin. By including the component (A2) in the film-like adhesive, the film-like adhesive becomes highly crosslinked, and the storage modulus after curing can be improved.
[0030] The component (A2) can be used without any particular limitation as long as it has a phenolic hydroxyl group in the molecule. The component (A2) is not particularly limited as long as it has a phenolic hydroxyl group in the molecule. Examples of the component (A2) include novolak-type phenolic resins obtained by condensing or co-condensing phenols such as phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol and / or naphthols such as α-naphthol, β-naphthol, and dihydroxynaphthalene with a compound having an aldehyde group such as formaldehyde under an acidic catalyst; phenol aralkyl resins synthesized from phenols such as allylated bisphenol A, allylated bisphenol F, allylated naphthalenediol, phenol novolak, and / or naphthols with dimethoxyparaxylene or bis(methoxymethyl)biphenyl; naphthol aralkyl resins; biphenyl aralkyl-type phenolic resins; and phenyl aralkyl-type phenolic resins. Among these, the phenolic resin may include a novolac type phenolic resin or a phenylaralkyl type phenolic resin.
[0031] The hydroxyl equivalent of component (A2) may be 70 g / eq or more, or 70 to 300 g / eq. When the hydroxyl equivalent of component (A2) is 70 g / eq or more, the storage modulus tends to be further improved, and when it is 300 g / eq or less, problems such as foaming and outgassing can be prevented.
[0032] There are no particular limitations on the softening point of component (A2), but it may be, for example, at least 90° C., at least 100° C., or at least 110° C. The upper limit of the softening point of component (A2) may be, for example, at most 200° C.
[0033] Examples of commercially available products of component (A2) include PSM-4326 (trade name, manufactured by Gun-ei Chemical Industry Co., Ltd., softening point: 120°C), J-DPP-140 (trade name, manufactured by JFE Chemical Corporation, softening point: 140°C), and GPH-103 (trade name, manufactured by Nippon Kayaku Co., Ltd., softening point: 99 to 106°C).
[0034] From the viewpoint of curability, the ratio of the epoxy equivalent of component (A1) to the hydroxyl equivalent of component (A2) (epoxy equivalent of component (A1) / hydroxyl equivalent of component (A2)) may be 0.30 / 0.70 to 0.70 / 0.30, 0.35 / 0.65 to 0.65 / 0.35, 0.40 / 0.60 to 0.60 / 0.40, or 0.45 / 0.55 to 0.55 / 0.45. When the equivalent ratio is 0.30 / 0.70 or more, more sufficient curability tends to be obtained. When the equivalent ratio is 0.70 / 0.30 or less, excessive viscosity increase can be prevented, and more sufficient fluidity can be obtained.
[0035] The content of the component (A1) (the sum of the components (A1a) and (A1b)) may be 20% by mass or more, or may be 25% by mass or more, 30% by mass or more, 35% by mass or more, 40% by mass or more, or 45% by mass or more, based on the total amount of the film-like adhesive. When the content of the component (A1) is within this range, the storage modulus after curing tends to be more easily improved. From the viewpoint of handleability, the content of the component (A1) may be 70% by mass or less, 65% by mass or less, 60% by mass or less, or 55% by mass or less, based on the total amount of the film-like adhesive. Note that the content of the component (A1) (the sum of the components (A1a) and (A1b)) in the adhesive composition when forming the film-like adhesive may be the same as the above range.
[0036] The content of component (A2) may be 10% by mass or more, or may be 12% by mass or more, 15% by mass or more, 18% by mass or more, 20% by mass or more, or 22% by mass or more, based on the total amount of the film-like adhesive. When the content of component (A2) is within this range, the storage modulus after curing tends to be more easily improved. From the viewpoint of handleability, the content of component (A2) may be 35% by mass or less, 32% by mass or less, or 30% by mass or less, based on the total amount of the film-like adhesive. Note that the content of component (A2) in the adhesive composition when forming the film-like adhesive may be the same as the above range.
[0037] The content of component (A) (the sum of components (A1) and (A2)) may be 40% by mass or more, 45% by mass or more, 50% by mass or more, 55% by mass or more, 60% by mass or more, 65% by mass or more, or 70% by mass or more, based on the total amount of the film-like adhesive. When the content of component (A) is within this range, there is a tendency for the storage modulus after curing to be more easily improved. From the viewpoint of handleability, the content of component (A) may be 90% by mass or less, 85% by mass or less, or 80% by mass or less, based on the total amount of the film-like adhesive. Note that the content of component (A) (the sum of components (A1) and (A2)) in the adhesive composition when forming the film-like adhesive may be the same as the above range.
[0038] Component (B): Elastomer Examples of component (B) include acrylic resins, polyester resins, polyamide resins, polyimide resins, silicone resins, butadiene resins, and modified versions of these resins. Other examples of component (B) include polymers having organopolysiloxanes in their side chains. Among these, component (B) may be an acrylic resin (acrylic rubber) primarily composed of structural units derived from (meth)acrylic esters, because it contains fewer ionic impurities, has better heat resistance, facilitates ensuring the connection reliability of semiconductor devices, and has better fluidity. The content of structural units derived from (meth)acrylic esters in component (B) may be, for example, 70% by mass or more, 80% by mass or more, or 90% by mass or more, based on the total amount of structural units. The acrylic resin (acrylic rubber) may contain structural units derived from (meth)acrylic esters having crosslinkable functional groups such as epoxy groups, alcoholic or phenolic hydroxyl groups, and carboxyl groups.
[0039] The glass transition temperature (Tg) of component (B) may be 0 to 30°C. When the Tg of component (B) is 0°C or higher, the adhesive strength of the film-like adhesive can be further improved, and the flexibility of the film-like adhesive tends to be prevented from becoming too high. When the Tg of component (B) is 30°C or lower, the decrease in flexibility of the film-like adhesive can be suppressed, and when a thin film is formed, the adhesive tends to have excellent breaking strength and processability. The glass transition temperature (Tg) of component (B) may be 5°C or higher or 10°C or higher, and may be 25°C or lower or 20°C or lower. Here, Tg refers to a value measured using a DSC (differential scanning calorimeter) (e.g., Thermo Plus 2, manufactured by Rigaku Corporation). The Tg of component (B) can be adjusted to a desired range by adjusting the type and content of the structural units constituting component (B) (when component (B) is an acrylic resin (acrylic rubber), structural units derived from (meth)acrylic acid esters).
[0040] The weight average molecular weight (Mw) of component (B) may be 100,000 or more, 300,000 or more, or 500,000 or more, and may be 3,000,000 or less, 2,000,000 or less, or 1,000,000 or less. When the Mw of component (B) is within this range, film formability, film strength, flexibility, tackiness, etc. can be appropriately controlled, and excellent reflowability and embeddability can be achieved. Here, Mw refers to a value measured by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene. When multiple peaks are observed in GPC, the weight average molecular weight corresponding to the peak with the highest peak intensity is defined as the weight average molecular weight in this specification.
[0041] Commercially available products of component (B) include SG-P3 and SG-80H (both manufactured by Nagase ChemteX Corporation), and KH-CT-865 (manufactured by Resonac Corporation).
[0042] The content of the (B) component is 18% by mass or more, and may be 18 to 35% by mass, based on the total amount of the film-like adhesive. The content of the (B) component may be 20% by mass or more, 22% by mass or more, or 24% by mass or more, based on the total amount of the film-like adhesive. When the content of the (B) component is 18% by mass or more, based on the total amount of the film-like adhesive, the resulting thin film tends to have excellent breaking strength and processability, and warpage of the semiconductor device (semiconductor package) tends to be suppressed. Furthermore, when the content of the (B) component is 18% by mass or more, based on the total amount of the film-like adhesive, the storage modulus at 30°C after curing tends to be suppressed from becoming too high. The content of the (B) component may be 35% by mass or less, 33% by mass or less, 30% by mass or less, or 28% by mass or less, based on the total amount of the film-like adhesive. When the content of the (B) component is 35% by mass or less, based on the total amount of the film-like adhesive, the storage modulus after curing tends to be more easily improved. The content of component (B) in the adhesive composition when forming the film adhesive may be in the same range as above.
[0043] Component (C): Inorganic Filler The film adhesive 1 may further contain component (C). That is, the film adhesive 1 may contain component (C) or may be substantially free of component (C).
[0044] Examples of component (C) include fillers such as aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whisker, boron nitride, and silica. Among these, component (C) may be a silica filler from the viewpoint of adjusting the melt viscosity. The shape of component (C) is not particularly limited, but may be spherical.
[0045] From the viewpoint of fluidity and storage modulus, the average particle size of component (C) may be 0.7 μm or less, or may be 0.6 μm or less, 0.5 μm or less, 0.4 μm or less, or 0.3 μm or less. The average particle size of component (C) may be, for example, 0.01 μm or more. Here, the average particle size refers to the particle size at a cumulative frequency of 50% in the particle size distribution determined by laser diffraction / scattering. The average particle size of component (C) can also be determined by using a film-like adhesive containing component (C). In this case, the film-like adhesive is heated to decompose the resin component, and the resulting residue is dispersed in a solvent to prepare a dispersion. The average particle size of component (C) can be determined from the particle size distribution obtained by applying laser diffraction / scattering to this dispersion.
[0046] The content of component (C) is 0 to 25% by mass, based on the total amount of the film-like adhesive, and may be 0 to 22% by mass, 0 to 20% by mass, 0 to 17% by mass, 0 to 15% by mass, 0 to 12% by mass, 0 to 10% by mass, 0 to 7% by mass, 0 to 5% by mass, 0 to 4% by mass, 0 to 3% by mass, 0 to 2% by mass, 0 to 1% by mass, 0 to 0.5% by mass, or 0 to 0.1% by mass. When the content of component (C) is within this range, thinner films tend to be more readily formed. Furthermore, when the content of component (C) is 25% by mass or less, based on the total amount of the film-like adhesive, the resulting thin film tends to have excellent breaking strength and processability, and warpage of the semiconductor device (semiconductor package) tends to be suppressed. In one embodiment, the content of the (C) component may be 22% by mass or less, 20% by mass or less, 17% by mass or less, 15% by mass or less, 12% by mass or less, 10% by mass or less, 7% by mass or less, 5% by mass or less, 4% by mass or less, 3% by mass or less, 2% by mass or less, 1% by mass or less, 0.5% by mass or less, or 0.1% by mass or less, based on the total amount of the film-like adhesive. In one embodiment, the content of the (C) component may be 0% by mass, based on the total amount of the film-like adhesive. That is, in one embodiment, the film-like adhesive does not need to contain the (C) component. In one embodiment, the lower limit of the content of the (C) component may be 0% by mass or more, more than 0% by mass, 1% by mass or more, 3% by mass or more, or 5% by mass or more, based on the total amount of the film-like adhesive. The content of the (C) component in the adhesive composition when forming the film-like adhesive may be the same as the above range.
[0047] The (A) component and the (B) component, or the (A), (B), and (C) component may be the main components of the film-like adhesive of this embodiment. The total content of the (A) component and the (B) component, or the total content of the (A), (B), and (C) component may be, for example, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 96% by mass or more, 97% by mass or more, 98% by mass or more, 99% by mass or more, 99.5% by mass or more, 99.7% by mass or more, or 99.9% by mass or more. The total content of the (A) component and the (B) component, or the total content of the (A), (B), and (C) component may be, for example, 100% by mass or less, 99.9% by mass or less, 99.7% by mass or less, or 99.5% by mass or less.
[0048] Component (D): Coupling Agent Component (D) may be a silane coupling agent. Examples of the silane coupling agent include γ-ureidopropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane.
[0049] Component (E): Curing Accelerator Examples of the component (E) include imidazoles and derivatives thereof, organic phosphorus compounds, secondary amines, tertiary amines, quaternary ammonium salts, etc. Among these, from the viewpoint of reactivity, the component (E) may be imidazoles and derivatives thereof.
[0050] Examples of imidazoles include 2-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-methylimidazole.
[0051] The component (E) may contain 2-phenylimidazole, which facilitates curing at low temperatures.
[0052] The film adhesive may further contain other components, such as pigments, ion scavengers, and antioxidants.
[0053] The total content of component (D), component (E), and other components may be 0 mass% or more, 0.1 mass% or more, 0.3 mass% or more, or 0.5 mass% or more, and may be 30 mass% or less, 20 mass% or less, 10 mass% or less, 5 mass% or less, 4 mass% or less, 3 mass% or less, 2 mass% or less, or 1 mass% or less, based on the total amount of the film-like adhesive. The total content of component (D), component (E), and other components in the adhesive composition when forming the film-like adhesive may be in the same range as above.
[0054] The film-like adhesive 1 shown in FIG. 1 is obtained by forming an adhesive composition containing components (A) and (B), and, if necessary, component (C) and additional components, into a film. Such a film-like adhesive 1 can be formed by applying the adhesive composition to a support film. A varnish (adhesive varnish) containing the adhesive composition and a solvent may be used to form the film-like adhesive 1. When using an adhesive varnish, the components (A) and (B), and, if necessary, component (C) and additional components, are mixed or kneaded in a solvent to prepare the adhesive varnish, and the resulting adhesive varnish is applied to a support film, and the solvent is removed by heating and drying, thereby obtaining the film-like adhesive 1.
[0055] The support film is not particularly limited as long as it can withstand the above-mentioned heat drying, and may be, for example, a polyester film, a polypropylene film, a polyethylene terephthalate film, a polyimide film, a polyetherimide film, a polyethylene naphthalate film, a polymethylpentene film, etc. The support film may be a multilayer film made by combining two or more types of film, and may have a surface treated with a silicone-based, silica-based, or other mold release agent. The thickness of the support film may be, for example, 10 to 200 μm or 20 to 170 μm.
[0056] The mixing or kneading can be carried out using a dispersing machine such as a conventional stirrer, a mortar and pestle, a three-roll mill, or a ball mill, and by appropriately combining these.
[0057] The solvent used in preparing the adhesive varnish is not limited as long as it can uniformly dissolve, knead, or disperse each component, and conventionally known solvents can be used. Examples of such solvents include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, as well as dimethylformamide, dimethylacetamide, N-methylpyrrolidone, toluene, and xylene. From the viewpoints of drying speed and cost, the solvent may be methyl ethyl ketone or cyclohexanone.
[0058] The adhesive varnish can be applied to the support film by any known method, such as knife coating, roll coating, spray coating, gravure coating, bar coating, curtain coating, etc. The heat drying conditions are not particularly limited as long as the solvent used is sufficiently evaporated, but may be 50 to 150°C for 1 to 30 minutes.
[0059] Since the film adhesive 1 can be thinned, it can be suitably used in the manufacturing process of a semiconductor device in which multiple semiconductor chips are stacked. In this case, the semiconductor device may be a stacked MCP or a three-dimensional NAND memory.
[0060] [Dicing and die bonding integrated film] Figure 2 is a schematic cross-sectional view showing one embodiment of a dicing and die bonding integrated film. The dicing and die bonding integrated film 10 shown in Figure 2 comprises, in this order, a base layer 2, a pressure-sensitive adhesive layer 3, and an adhesive layer 1A made of the above-mentioned film-like adhesive 1. A laminate made of the base layer 2 and the pressure-sensitive adhesive layer 3 is sometimes called a dicing film 4 (dicing tape). Use of such a dicing and die bonding integrated film 10 reduces the lamination process to a single step on a semiconductor wafer, thereby improving work efficiency. The dicing and die bonding integrated film may be in the form of a film, sheet, tape, or the like.
[0061] The dicing film 4 includes a base layer 2 and a pressure-sensitive adhesive layer 3 provided on the base layer 2 .
[0062] Examples of the substrate layer 2 include plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, and polyimide film. These substrate layers 2 may be subjected to surface treatment such as primer coating, UV treatment, corona discharge treatment, polishing treatment, and etching treatment, as needed.
[0063] The adhesive layer 3 is a layer made of an adhesive. There are no particular limitations on the adhesive, so long as it has sufficient adhesive strength to prevent the semiconductor chips from scattering during the dicing process and low adhesive strength to prevent damage to the semiconductor chips during the subsequent semiconductor chip pick-up process, and any adhesive conventionally known in the field of dicing films can be used. The adhesive may be either a radiation-curable or non-radiation-curable adhesive. The radiation may be, for example, ultraviolet light. A non-radiation-curable adhesive is an adhesive that exhibits a certain level of adhesiveness when pressure is applied for a short period of time. On the other hand, a radiation-curable adhesive is an adhesive that has the property of decreasing adhesiveness upon irradiation with radiation (e.g., ultraviolet light).
[0064] The thickness of the dicing film 4 (base layer 2 and adhesive layer 3) may be 60 to 150 μm or 70 to 130 μm from the viewpoints of economy and film handling.
[0065] The dicing and die bonding integrated film 10 can be obtained, for example, by preparing a film adhesive 1 and a dicing film 4, and bonding the film adhesive 1 to the pressure-sensitive adhesive layer 3 of the dicing film 4. The dicing and die bonding integrated film 10 can also be obtained, for example, by preparing a dicing film 4, and applying an adhesive composition (adhesive varnish) onto the pressure-sensitive adhesive layer 3 of the dicing film 4, in the same manner as in the method of forming the film adhesive 1 described above.
[0066] When the film-like adhesive 1 and the pressure-sensitive adhesive layer 3 of the dicing film 4 are bonded together, the dicing / die bonding integrated film 10 can be formed by laminating the film-like adhesive 1 onto the dicing film 4 under predetermined conditions (for example, room temperature (25°C) or in a heated state) using a roll laminator, vacuum laminator, or the like. The dicing / die bonding integrated film 10 can be produced continuously and is highly efficient, so it may be formed in a heated state using a roll laminator.
[0067] The film-like adhesive and dicing / die bonding integrated film may be used in a manufacturing process for a semiconductor device, or may be used in a manufacturing process for a semiconductor device comprising stacked semiconductor chips. The film-like adhesive and dicing / die bonding integrated film may be used in a manufacturing process for a semiconductor device including a step of laminating an adhesive layer of the film-like adhesive or dicing / die bonding integrated film to a semiconductor wafer or an already-diced semiconductor chip, and cutting it with a rotary blade, a laser, or stretching to obtain a semiconductor chip with an adhesive piece attached, and a step of adhering the semiconductor chip with the adhesive piece attached to a support member or a semiconductor chip via the adhesive piece.
[0068] The film adhesive is also suitable for use as an adhesive for bonding semiconductor chips together in a stacked MCP (for example, a three-dimensional NAND memory), which is a semiconductor device formed by stacking multiple semiconductor chips.
[0069] The film adhesive can also be used, for example, as a protective sheet for protecting the back surface of a semiconductor chip in a flip-chip type semiconductor device, or as a sealing sheet for sealing the gap between the surface of the semiconductor chip in a flip-chip type semiconductor device and an adherend.
[0070] A semiconductor device manufactured using the film adhesive and the dicing / die bonding integrated film will be specifically described below with reference to the drawings. Note that, in recent years, semiconductor devices with various structures have been proposed, and the use of the film adhesive and dicing / die bonding integrated film of this embodiment is not limited to semiconductor devices with the structures described below.
[0071] [Semiconductor Device] Fig. 3 is a schematic cross-sectional view showing one embodiment of a semiconductor device. The semiconductor device 100 shown in Fig. 3 includes a semiconductor chip 11 (first semiconductor chip), a support member 12 on which the semiconductor chip 11 is mounted, and an adhesive member 15. The adhesive member 15 is provided between the semiconductor chip 11 and the support member 12 and bonds the semiconductor chip 11 to the support member 12. The adhesive member 15 is a cured product of an adhesive composition (a cured product of a film-like adhesive). Connection terminals (not shown) of the semiconductor chip 11 are electrically connected to external connection terminals (not shown) via bonding wires 13 and are sealed with a sealing material 14.
[0072] FIG. 4 is a schematic cross-sectional view showing another embodiment of a semiconductor device. In the semiconductor device 110 shown in FIG. 4, a first-tier semiconductor chip 11a (first semiconductor chip) is adhered to a support member 12 on which terminals 16 are formed by an adhesive member 15a (a cured product of an adhesive composition (a cured product of a film-like adhesive)). A second-tier semiconductor chip 11b (second semiconductor chip) is further adhered to the first-tier semiconductor chip 11a by an adhesive member 15b (a cured product of an adhesive composition (a cured product of a film-like adhesive)). Connection terminals (not shown) of the first-tier semiconductor chip 11a and the second-tier semiconductor chip 11b are electrically connected to external connection terminals via bonding wires 13 and are sealed with a sealing material 14. The semiconductor device 110 shown in FIG. 4 can also be said to be the semiconductor device 100 shown in FIG. 3, further including another semiconductor chip (11b) stacked on the surface of the semiconductor chip (11a).
[0073] FIG. 5 is a schematic cross-sectional view showing another embodiment of a semiconductor device. The semiconductor device 120 shown in FIG. 5 includes a support member 12 and semiconductor chips 11a (first semiconductor chip), 11b (second semiconductor chip), 11c (third semiconductor chip), and 11d (fourth semiconductor chip) stacked on the support member 12. The four semiconductor chips 11a, 11b, 11c, and 11d are stacked at positions shifted from one another in the horizontal direction (a direction perpendicular to the stacking direction) for connection to connection terminals (not shown) formed on the surface of the support member 12 (see FIG. 5). The semiconductor chip 11a is adhered to the support member 12 by an adhesive member 15a (a cured product of an adhesive composition (a cured product of a film-like adhesive)), and adhesive members 15b, 15c, and 15d (cured products of an adhesive composition (a cured product of a film-like adhesive)) are also interposed between the three semiconductor chips 11b, 11c, and 11d, respectively. The semiconductor device 120 shown in Figure 5 can also be said to be the semiconductor device 100 shown in Figure 3, further comprising other semiconductor chips (11b, 11c, 11d) stacked on the surface of the semiconductor chip (11a).
[0074] Although the semiconductor device (semiconductor package) according to the embodiment of the present disclosure has been described in detail above, the present disclosure is not limited to the above embodiment. For example, while Fig. 5 illustrates a semiconductor device in which four semiconductor chips are stacked, the number of stacked semiconductor chips is not limited to this. Furthermore, Fig. 5 illustrates a semiconductor device in which the semiconductor chips are stacked in positions offset from each other in the horizontal direction (a direction perpendicular to the stacking direction), the semiconductor device may also be one in which the semiconductor chips are stacked in positions not offset from each other in the horizontal direction (a direction perpendicular to the stacking direction).
[0075] 3, 4, and 5 can be obtained by a method including a step of interposing the above-mentioned film-like adhesive between a semiconductor chip (first semiconductor chip) and a support member, or between the semiconductor chip (first semiconductor chip) and the semiconductor chip (second semiconductor chip), and bonding the semiconductor chip (first semiconductor chip) and the support member, or between the semiconductor chip (first semiconductor chip) and the semiconductor chip (second semiconductor chip). More specifically, the semiconductor device can be obtained by interposing the above-mentioned film-like adhesive between the semiconductor chip and the support member, or between the semiconductor chip (first semiconductor chip) and the semiconductor chip (second semiconductor chip), bonding them together by heat and pressure, and then, as necessary, undergoing a thermosetting step, a wire bonding step, a sealing step using a sealing material, a heat-melting step including solder reflow, and the like.
[0076] A method for interposing a film-like adhesive between a semiconductor chip (first semiconductor chip) and a support member, or between a semiconductor chip (first semiconductor chip) and a semiconductor chip (second semiconductor chip), may be a method in which a semiconductor chip with an adhesive piece is prepared in advance and then attached to a support member or another semiconductor chip, as described below.
[0077] Next, an embodiment of a method for manufacturing a semiconductor device using the dicing and die bonding integrated film shown in Fig. 2 will be described. Note that the method for manufacturing a semiconductor device using the dicing and die bonding integrated film is not limited to the method for manufacturing a semiconductor device described below.
[0078] The semiconductor device can be obtained, for example, by a method comprising the steps of: attaching a semiconductor wafer to the adhesive layer of the above-mentioned dicing / die bonding integrated film (laminating step); cutting the semiconductor wafer with the adhesive layer attached to produce a plurality of individual adhesive piece-attached semiconductor chips (dicing step); and adhering the first adhesive piece-attached semiconductor chip, which has a first semiconductor chip and a first adhesive piece, to a support member via the first adhesive piece (step of adhering the adhesive piece-attached semiconductor chip to a support member via the adhesive piece) (first adhering step). The method for manufacturing a semiconductor device may further include a step of adhering a second semiconductor chip with adhesive piece, which has a second semiconductor chip and a second adhesive piece, to the surface of the first semiconductor chip in the first semiconductor chip with adhesive piece adhered to a support member via the second adhesive piece (a step of adhering another semiconductor chip with adhesive piece to the surface of the semiconductor chip adhered to a support member via an adhesive piece possessed by the other semiconductor chip with adhesive piece) (second adhering step).
[0079] The laminating step is a step of pressing a semiconductor wafer onto the adhesive layer 1A of the dicing and die bonding integrated film 10, adhesively holding and attaching the semiconductor wafer. This step may be performed while pressing with a pressing means such as a pressing roll.
[0080] Examples of semiconductor wafers include single crystal silicon, polycrystalline silicon, various ceramics, and compound semiconductors such as gallium arsenide.
[0081] The dicing process is a process of dicing a semiconductor wafer. This allows the semiconductor wafer to be cut to a predetermined size, producing multiple individual semiconductor chips with adhesive. Dicing can be performed, for example, from the circuit side of the semiconductor wafer according to a conventional method. This process can also employ a method known as a full cut, in which a cut is made all the way to the dicing film; a method in which a half cut is made in the semiconductor wafer and the wafer is separated by cooling and pulling; or a method in which the wafer is separated by a laser. The dicing device used in this process is not particularly limited, and conventionally known devices can be used.
[0082] A semiconductor chip is composed of, for example, a circuit layer and a semiconductor layer (for example, single crystal silicon, polycrystalline silicon, various ceramics, compound semiconductors such as gallium arsenide, etc.). Examples of semiconductor chips include integrated circuits (ICs). Examples of support members include lead frames such as 42 alloy lead frames and copper lead frames; plastic films such as polyimide resin and epoxy resin; modified plastic films obtained by impregnating and curing a substrate such as glass nonwoven fabric with a plastic such as polyimide resin or epoxy resin; and ceramics such as alumina.
[0083] The method for manufacturing a semiconductor device may include a pick-up step, if necessary. The pick-up step is a step of picking up the semiconductor chips with adhesive pieces attached thereto in order to peel off the semiconductor chips with adhesive pieces attached thereto that have been adhesively fixed to the dicing-die bonding integrated film. The pick-up method is not particularly limited, and various conventionally known methods can be used. Examples of such methods include a method in which individual semiconductor chips with adhesive pieces are pushed up from the dicing-die bonding integrated film side by a needle, and the pushed-up semiconductor chips with adhesive pieces attached thereto are then picked up by a pick-up device.
[0084] Here, if the adhesive layer is a radiation-curable (e.g., ultraviolet) adhesive layer, the pickup can be performed after irradiating the adhesive layer with radiation. This reduces the adhesive strength of the adhesive layer to the adhesive piece, making it easier to peel off the semiconductor chip with the adhesive piece. As a result, the semiconductor chip with the adhesive piece can be picked up without damaging it.
[0085] The first bonding step is a step of bonding a semiconductor chip with a first adhesive piece formed by dicing to a support member for mounting the semiconductor chip via the first adhesive piece. The semiconductor device manufacturing method may optionally include a step (second bonding step) of bonding a semiconductor chip with a second adhesive piece to the surface of the semiconductor chip bonded to the support member via the second adhesive piece. Both bonding steps can be performed by pressure bonding. The pressure bonding conditions are not particularly limited and can be set appropriately as needed. The pressure bonding conditions may be, for example, a temperature of 80 to 160°C, a load of 5 to 15 N, and a time of 1 to 10 seconds. The support member may be the same as the support member described above.
[0086] The method for manufacturing a semiconductor device may, if necessary, include a step of further thermally curing the adhesive pieces (the first adhesive pieces in the semiconductor chip with the first adhesive pieces, and the second adhesive pieces in the semiconductor chip with the second adhesive pieces) or the film-like adhesive (thermal curing step). Further thermally curing the adhesive pieces (the first adhesive pieces in the semiconductor chip with the first adhesive pieces, and the second adhesive pieces in the semiconductor chip with the second adhesive pieces) bonding the semiconductor chip (first semiconductor chip) and the support member, and the semiconductor chip (first semiconductor chip) and the semiconductor chip (second semiconductor chip), enables more firmly bonded and fixed. When thermal curing is performed, pressure may be applied simultaneously to harden the adhesive pieces. The heating temperature in this step can be appropriately changed depending on the constituent components of the adhesive pieces. The heating temperature may be, for example, 60 to 200°C or 100 to 180°C. The temperature or pressure may be changed stepwise. The heating time may be, for example, 1 to 120 minutes or 15 to 60 minutes.
[0087] The method for manufacturing a semiconductor device may optionally include a step of electrically connecting the first semiconductor chip and the second semiconductor chip to a support member with bonding wires, more specifically, a step of electrically connecting electrode pads on the semiconductor chip to the tips of terminal portions (inner leads) of the support member with bonding wires (wire bonding step). Examples of bonding wires that can be used include gold wires, aluminum wires, copper wires, etc. The temperature during wire bonding may be within a range of 80 to 250°C or 80 to 220°C. The heating time may be several seconds to several minutes. Wire bonding may be performed by combining ultrasonic vibration energy and compression energy due to applied pressure while the substrate is heated within the above temperature range.
[0088] The method for manufacturing a semiconductor device may optionally include a step of encapsulating the semiconductor chip with an encapsulant (encapsulation step). This step is performed to protect the semiconductor chip or bonding wires mounted on the support member. This step can be performed by molding the encapsulating resin (encapsulation resin) in a mold. The encapsulation resin may be, for example, an epoxy-based resin. The heat and pressure during encapsulation bury the support member and residue, preventing peeling due to air bubbles at the adhesive interface.
[0089] The method for manufacturing a semiconductor device may, if necessary, include a step (post-curing step) of completely curing the encapsulating resin that is insufficiently cured in the encapsulating step. Even if the adhesive piece is not thermally cured in the encapsulating step, in this step, the adhesive piece can be thermally cured along with the curing of the encapsulating resin, thereby enabling adhesive fixation. The heating temperature in this step can be appropriately set depending on the type of encapsulating resin, and may be, for example, in the range of 165 to 185°C, and the heating time may be approximately 0.5 to 8 hours.
[0090] The method for manufacturing a semiconductor device may, as necessary, include a step of heating the semiconductor chip bonded to the support member or the semiconductor chip using a reflow furnace (heat melting step). In this step, the resin-encapsulated semiconductor device may be surface-mounted on the support member. Examples of surface mounting methods include reflow soldering, in which solder is first supplied onto a printed wiring board, and then heated and melted using hot air or the like to perform soldering. Examples of heating methods include hot air reflow and infrared reflow. The heating method may be either a method of heating the entire device or a method of heating a localized area. The heating temperature may be, for example, within a range of 240 to 280°C.
[0091] The present disclosure will be specifically described below based on examples, but the present disclosure is not limited to these examples.
[0092] [Preparation of Film-Like Adhesive] (Examples 1 to 5 and Comparative Examples 1 to 4) <Preparation of Adhesive Varnish> Cyclohexanone was added to a mixture of component (A) (component (A1) and component (A2)) and component (C) in the components and amounts (unit: parts by mass) shown in Table 1, and the mixture was stirred and mixed. Component (B) was added to this in the components and amounts (unit: parts by mass) shown in Table 1, and the mixture was stirred. Component (D) and component (E) were then added and the mixture was stirred until the components were uniform, thereby preparing an adhesive varnish. The components shown in Table 1 have the following meanings, and the numerical values shown in Table 1 refer to the parts by mass of the components (solid content) excluding solvents and the like.
[0093] Component (A): Thermosetting Resin Component Component (A1): Epoxy Resin (A1a-1) EXA830-CRP (trade name, manufactured by DIC Corporation, bisphenol F type epoxy resin, epoxy equivalent: 155 to 163 g / eq, softening point: 40°C or less, liquid at 30°C) (A1b-1) N-500P-10 (trade name, manufactured by DIC Corporation, o-cresol novolac type epoxy resin, epoxy equivalent: 204 g / eq, softening point: 75 to 85°C, solid at 30°C) (A1b-2) HP-4710 (trade name, manufactured by DIC Corporation, naphthalene type epoxy resin, epoxy equivalent: 170 g / eq, softening point: 95°C, solid at 30°C)
[0094] Component (A2): Phenolic resin (A2-1) PSM-4326 (trade name, manufactured by Gunei Chemical Industry Co., Ltd., novolac type phenolic resin, hydroxyl group equivalent: 105 g / eq, softening point: 120°C)
[0095] Component (B): Elastomer (B-1) SG-P3 (trade name, manufactured by Nagase ChemteX Corporation, acrylic rubber, weight average molecular weight: 800,000, Tg: 12°C)
[0096] Component (C): Inorganic filler (C-1) Silica filler dispersion (manufactured by CIK Nanotech Co., Ltd., silica filler, average particle size: 0.10 μm) (C-2) SC2050-HLG (trade name, manufactured by Admatechs Co., Ltd., silica filler dispersion, average particle size: 0.50 μm)
[0097] Component (D): Coupling agent (D-1) Z-6119 (trade name, manufactured by Dow Toray Industries, Inc., γ-ureidopropyltriethoxysilane) (D-2) A-189 (trade name, manufactured by Nippon Unicar Co., Ltd., γ-mercaptopropyltrimethoxysilane)
[0098] Component (E): Curing accelerator (E-1) 2PZ (trade name, manufactured by Shikoku Chemicals Corporation, 2-phenylimidazole) (E-2) 2PZ-CN (trade name, manufactured by Shikoku Chemicals Corporation, 1-cyanoethyl-2-phenylimidazole)
[0099] <Preparation of Film-Like Adhesive> The prepared adhesive varnish was filtered through a 100-mesh filter and vacuum degassed. A 38 μm-thick polyethylene terephthalate (PET) film that had been subjected to a release treatment was prepared as a support film, and the vacuum degassed adhesive varnish was applied to the PET film. The applied adhesive varnish was dried by heating at 90°C for 5 minutes and then at 140°C for 5 minutes, yielding film-like adhesives of Examples 1 to 5 and Comparative Examples 1 to 4 in a B-stage state. In the film-like adhesives of Examples 1 to 5 and Comparative Examples 1 to 4, the thickness of the film-like adhesive was adjusted to 5 μm by adjusting the amount of adhesive varnish applied.
[0100] [Evaluation of Film-Like Adhesives] <Measurement of Storage Modulus> The storage modulus after curing was measured using the film-like adhesives of Examples 1 to 5 and Comparative Examples 1 to 4. The storage modulus after curing was measured using the following method. Specifically, a measurement sample was prepared by laminating multiple 5 μm-thick film-like adhesives to a thickness of 100 μm or more, and then cutting this into a size of 4 mm wide x 20 mm long or more. The prepared sample was cured at 140°C for 30 minutes, and then the cured sample was placed in a dynamic viscoelasticity measuring device (Rheogel E-4000, manufactured by UBM Corporation). A tensile load was applied to the cured sample, and dynamic viscoelasticity was measured in a temperature dependency measurement mode measuring from room temperature (25°C) to 300°C under conditions of a chuck distance of 20 mm, a frequency of 10 Hz, and a heating rate of 3°C / min. The storage modulus values at 30°C and 150°C were read, and these values were recorded as the storage modulus at 30°C and 150°C. The results are shown in Table 1. The larger the storage modulus at 150°C (e.g., 80 MPa or more), the more it can compensate for the brittleness of the semiconductor chip due to thinning, and as a result, it becomes possible to suppress the occurrence of chip cracks.The smaller the storage modulus at 30°C (e.g., 2000 MPa or less), the more easily it becomes possible to thin the film adhesive, and it becomes possible to more sufficiently suppress the cured film adhesive from becoming too hard.
[0101] <Measurement of Breaking Strength> The breaking strength of the film-like adhesives of Examples 1 to 5 and Comparative Examples 1 to 4 was measured at 25°C using a tensile tester (RTF-1250-HS-PL, A&D Co., Ltd.). More specifically, test specimens having the shape shown in Figure 6 were prepared using film-like adhesives in a B-stage state. A tensile test was conducted by gripping both ends of the prepared test specimen with the tester. The tensile test was conducted in an environment of 25°C, and the tensile speed was 100 mm / min. The breaking strength was calculated using the following formula from the average thickness (0.005 mm (5 μm)) and width (10 mm) of the test specimen before the test and the maximum load (N) until the test specimen broke. The results are shown in Table 1. The values shown in Table 1 are values converted to the load when the average thickness of the test specimen before the test was 5 μm (unit: N / 10 mm). A larger breaking strength value (for example, 0.7 N / 10 mm or more) means that the processability when a thin film is formed is better. Breaking strength (MPa) = maximum load (N) until the test piece breaks / (average thickness (mm) x width (mm) of the test piece)
[0102] <Evaluation of Warpage of Semiconductor Device (Semiconductor Package)> (Preparation of Dicing and Die Bonding Integrated Film) A dicing film (product name 6363-45, manufactured by Resonac Co., Ltd.) having a substrate and an adhesive layer was prepared, and the adhesive layer of the dicing film was attached to each of the film-like adhesives of Examples 1 to 5 and Comparative Examples 1 to 4 using a rubber roll to prepare the dicing and die bonding integrated films of Examples 1 to 5 and Comparative Examples 1 to 4 each having a substrate, adhesive layer, and adhesive layer (film-like adhesive) in this order.
[0103] (Preparation of Evaluation Samples) Evaluation samples were prepared using the dicing and die bonding integrated films of Examples 1 to 5 and Comparative Examples 1 to 4. Evaluation samples for evaluating warpage were prepared as follows. A semiconductor wafer with a thickness of 40 μm was prepared, and the film-like adhesive side of the dicing and die bonding integrated film was laminated to the semiconductor wafer at a stage temperature of 70°C to prepare a dicing sample. The obtained dicing sample was cut using a fully automatic dicer DFD-6362 (manufactured by Disco Corporation). Cutting was performed using a single-cut method using a single blade, and a ZH05-SD4000-N1-70-EE (manufactured by Disco Corporation) was used. The cutting conditions were a blade rotation speed of 40,000 rpm, a cutting speed of 50 mm / sec, and a chip size of 10 mm x 6 mm. The cutting was performed so as to make an incision of approximately 20 μm in the dicing film. Next, the adhesive layer made of an ultraviolet-curable adhesive was irradiated with ultraviolet light to harden the adhesive layer, and the semiconductor chip with the adhesive piece was picked up. The adhesive piece of the semiconductor chip with the adhesive piece was then pressure-bonded to a 90 μm thick, 240 mm wide, and 74 mm long organic substrate with solder resist at a temperature of 130°C, a load of 10 N, and a time of 1 second, to produce evaluation samples for Examples 1 to 5 and Comparative Examples 1 to 4. In the evaluation samples, 60 first-tier semiconductor chips were arranged side-by-side in 15 rows and 4 columns, and then 60 second-tier semiconductor chips were arranged on each surface of the first-tier semiconductor chips.
[0104] (Evaluation of Warpage of Semiconductor Devices (Semiconductor Packages)) The warpage of semiconductor devices (semiconductor packages) was evaluated using the evaluation samples of Examples 1 to 5 and Comparative Examples 1 to 4. Each evaluation sample was placed in an oven, heated from 35°C to 140°C at a heating rate of 3°C / min, and heated at 140°C for 30 minutes. The heat-treated evaluation sample was removed from the pressure oven, and the amount of warpage of the semiconductor device (semiconductor package) was measured. More specifically, the heat-treated evaluation sample was placed on a flat surface with the semiconductor chip side facing downwards, and a Digimatic Indicator ID-H0530 (manufactured by Mitutoyo Corporation) was used to measure five points on the heat-treated evaluation sample placed on the flat surface: the upper left, upper right, center, lower left, and lower right. The difference between the maximum and minimum values of the measurement results was calculated as the amount of warpage. A warpage of 3.0 mm or less was evaluated as "A," indicating that the amount of warpage was sufficiently suppressed, and a warpage of more than 3.0 mm was evaluated as "B." The results are shown in Table 1.
[0105]
[0106] As shown in Table 1, the film-like adhesives of Examples 1 to 5 were excellent in both storage modulus and breaking strength at 150° C., whereas the film-like adhesives of Comparative Examples 1 to 4 were insufficient in at least one of storage modulus and breaking strength at 150° C. These results confirmed that the film-like adhesives of the present disclosure have excellent processability when formed into thin films, and are also capable of suppressing the occurrence of chip cracks.
[0107] 1...film-like adhesive, 1A...adhesive layer, 2...base material layer, 3...pressure-sensitive adhesive layer, 4...dicing film, 10...dicing / die bonding integrated film, 11, 11a, 11b, 11c, 11d...semiconductor chip, 12...support member, 13...bonding wire, 14...sealing material, 15, 15a, 15b, 15c, 15d...adhesive member, 16...terminal, 100, 110, 120...semiconductor device.
Claims
1. A film-like adhesive comprising a thermosetting resin component and an elastomer, and optionally further comprising an inorganic filler, wherein the content of the elastomer is 18% by mass or more, based on the total amount of the film-like adhesive, and the content of the inorganic filler is 0-25% by mass, based on the total amount of the film-like adhesive, and when the film-like adhesive is cured under conditions of 140°C and 30 minutes, the cured product has a storage modulus at 150°C of 80 MPa or more, and the thickness of the film-like adhesive is 15 μm or less.
2. The film-like adhesive according to claim 1, wherein the content of the elastomer is 18 to 35 mass % based on the total amount of the film-like adhesive.
3. The film-like adhesive according to claim 1, wherein the content of the inorganic filler is 0 to 3 mass % based on the total amount of the film-like adhesive.
4. A film-like adhesive according to any one of claims 1 to 3, wherein when the film-like adhesive is cured under conditions of 140°C for 30 minutes, the cured product has a storage modulus at 30°C of 2000 MPa or less.
5. The film-like adhesive according to any one of claims 1 to 3, wherein the thermosetting resin component comprises an epoxy resin and a phenolic resin.
6. The film-like adhesive according to any one of claims 1 to 3, wherein the elastomer has a glass transition temperature of 0 to 30°C.
7. The film-like adhesive according to any one of claims 1 to 3, which is used in the manufacturing process of a semiconductor device comprising a plurality of stacked semiconductor chips.
8. The film adhesive according to claim 7, wherein the semiconductor device is a three-dimensional NAND type memory.
9. A dicing and die bonding integrated film comprising, in this order, a base layer, a pressure-sensitive adhesive layer, and an adhesive layer made of the film-like adhesive according to any one of claims 1 to 3.
10. A semiconductor device comprising: a first semiconductor chip; a support member on which the first semiconductor chip is mounted; and a cured film-like adhesive according to claim 1 or 2, which is provided between the first semiconductor chip and the support member and bonds the first semiconductor chip to the support member.
11. The semiconductor device according to claim 10, further comprising a second semiconductor chip different from the first semiconductor chip, stacked on a surface of the first semiconductor chip.
12. A method for manufacturing a semiconductor device, comprising the steps of: attaching the adhesive layer of the dicing and die bonding integrated film described in claim 9 to a semiconductor wafer; cutting the semiconductor wafer to which the adhesive layer has been attached, thereby producing a plurality of individual adhesive piece-attached semiconductor chips; and adhering, as the adhesive piece-attached semiconductor chips, a first adhesive piece-attached semiconductor chip having a first semiconductor chip and a first adhesive piece to a support member via the adhesive piece.
13. The method for manufacturing a semiconductor device according to claim 12, further comprising a step of adhering, as the semiconductor chip with adhesive piece, a second semiconductor chip with a second adhesive piece having a second semiconductor chip and a second adhesive piece, to a surface of the first semiconductor chip in the first semiconductor chip with adhesive piece adhered to the support member via the second adhesive piece.