Powder coating composition, coating film, and coated body
Patent Information
- Application Number
- MYPI2025005541
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2023-09-28
- Publication Date
- 2024-09-30
AI Technical Summary
Conventional powder coatings with fluororesin, non-fluororesin, and pigments face issues such as separation between resin and pigment particles during electrostatic coating, leading to deteriorated coating design, color tone changes, and difficulties in recycling due to solvent compatibility problems with specific binders.
A powder coating composition using resin-containing powder particles, bright pigments, and a binder with specific Hansen solubility parameters, allowing for solvent selection that dissolves the binder without dissolving the resin, ensuring a glossy and reusable coating film with improved workability and recyclability.
The solution forms a glossy coating film with excellent glitter properties and enhances the recovery and reusability of powder coatings by preventing resin-pigment separation and maintaining coating film appearance, while allowing for versatile application across various resin types.
Smart Images

Figure PI2025005541_DRAWING_001 
Figure PI2025005541_DRAWING_002 
Figure PI2025005541_DRAWING_003
Abstract
Description
Powder coating composition, coating film and coated body
[0001] The present invention relates to a powder coating composition, a coating film, and a coated body.
[0002] Conventionally, thermosetting powder coatings containing fluororesin, non-fluororesin, and pigments have been known as powder coatings that have weather resistance and adhesion to substrates. When a luster pigment is used as the pigment in these powder coatings, a coating film with luster can be formed (see, for example, Patent Document 1). For example, electrostatic powder coating is used as a method for forming the coating film.
[0003] Generally, the resin powder and the luster pigment (e.g., metallic pigment) that make up a powder coating material have significantly different electrostatic charges. Therefore, when electrostatic powder coating is performed using a powder coating material containing a resin powder and a luster pigment, separation between the resin powder and the luster pigment is likely to occur during coating. This separation can lead to a problem in that the design of the resulting coating film is likely to be impaired. Furthermore, this separation can easily cause a change in the pigment content of the powder coating material before and after application. This change in pigment content can easily lead to a change in color tone between the coating film obtained using the recovered and reused powder coating material and the coating film obtained using the original powder coating material, making it difficult to recycle (recover and reuse) the powder coating material.
[0004] In response to this, various proposals have been made. For example, Patent Documents 2 and 3 disclose a method (bonding method) in which the surface of the thermosetting resin powder and the luster pigment are adhered to each other with an adhesive binder in order to avoid separation between the thermosetting resin powder and the metal pigment. Furthermore, the examples of Patent Documents 2 and 3 disclose the use of a terpene resin as the binder.
[0005] Furthermore, Patent Document 4 discloses a bonding method for resin powder, particularly fluororesin powder. Specifically, Patent Document 4 discloses a powder coating containing resin powders including fluororesin and non-fluororesin, a luster pigment, and a binder, and a method for adhering the luster pigment to the surface of a thermosetting resin powder using a binder made of a surfactant having a melting point of 25° C. or higher. An example of Patent Document 4 discloses the use of a fluoro-based halogen-containing solvent as a solvent for the binder.
[0006] Japanese Patent Application Laid-Open No. 2011-12119 Japanese Patent Application Laid-Open No. 2004-175813 Japanese Patent No. 3926270 Japanese Patent No. 6841235
[0007] When the terpene resin used in the examples of Patent Documents 2 and 3 is used as an adhesive binder, it is necessary to dissolve the terpene resin in a low-polarity solvent such as n-heptane. However, these low-polarity solvents generally also dissolve fluororesins, and therefore problems are likely to occur when they are used with thermosetting resin powder particles containing fluororesins. Specifically, when such low-polarity solvents are used with thermosetting resin powder particles containing fluororesins, some of the fluororesin dissolves, causing the thermosetting resin powder particles to bond together, which can increase the particle size of the thermosetting resin powder, reduce coating workability, and degrade the appearance of the coating film.
[0008] Furthermore, the fluoro-based halogen-containing solvent used in the examples of Patent Document 4 generally dissolves fluororesin. Therefore, when the above-mentioned fluoro-based halogen-containing solvent is used for thermosetting resin powder particles containing fluororesin, there is a risk that the particle size of the thermosetting resin powder will increase, coating workability will decrease, and the appearance of the coating film will deteriorate, as in the cases where the low-polarity solvents of Patent Documents 2 and 3 are used.
[0009] In addition, when the powder coating material contains a resin having a carboxyl group, there is also a problem that the gloss of the appearance of the coating film is likely to decrease when the binders disclosed in Patent Documents 2 to 4 are used.
[0010] Powder coating compositions containing resin-containing powder particles, a luster pigment, and a binder for use in bonding methods are desired to contain a solvent that dissolves the binder but does not dissolve the resin of the resin-containing powder particles. In contrast, the powder coating compositions disclosed in Patent Documents 2 to 4 can only be used in bonding methods when they involve a combination of a specific resin and a specific binder. In view of the degree of freedom in designing powder coating compositions, a bonding method that can be widely applied to various types of resin-containing powder particles is desired in the industry.
[0011] The present invention has been made in view of the above problems, and has an object to provide a powder coating composition that is capable of forming a coating film that is glossy and has excellent brilliance, and that is also highly recyclable. Another object of the present invention is to provide a coating film and a coated body formed using the powder coating composition.
[0012] The present inventors have investigated the Hansen solubility parameter (HSP) (δ) of a powder coating composition containing resin-containing powder particles, a luster pigment, and a binder. d , δ p , δ h ) to form a specific Hansen melting sphere, and the binder is attached to the specific Hansen melting sphere by an interaction distance R a The present inventors have succeeded in developing a powder coating composition that is capable of forming a glossy coating film having excellent brilliance when the resin is soluble or dispersible in 20 or more solvents, and that is also highly recyclable and reusable, thereby completing the present invention.
[0013] (1) The powder coating composition according to the present invention is a powder coating composition containing resin-containing powder particles (A), a luster pigment (B) and a binder (C), and the binder (C) has a central coordinate (δ ) in the Hansen Solubility Sphere (HSS) that determines the solubility of the binder with a solvent to be mixed. d , δ p , δ h ) is (19.0, 7.0, 5.0), the interaction distance R a The resin is characterized in that it is soluble or dispersible in a solvent (D) having a Tg of 20 or more, a Tg of 30° C. or more, and a weight average molecular weight of 1,000 to 100,000.
[0014] (2) The binder (C) has the interaction distance R a It is preferable that the resin is soluble or dispersible in the solvent (D) having a molecular weight of 30 or more.
[0015] (3) The binder (C) preferably has a Tg of 40° C. or higher.
[0016] (4) The resin (A1) constituting the resin-containing powder particles (A) is preferably a resin obtained by reacting one or more binder resins (A11) selected from the group consisting of fluororesins, polyester resins, and acrylic resins with one or more curing agents (A12) selected from the group consisting of compounds having an epoxy group or polymers thereof, amide compounds, and isocyanate compounds.
[0017] (5) The solvent (D) is preferably one or more solvents selected from the group consisting of water, ethylene glycol, and methanol.
[0018] (6) The solvent (D) is preferably a mixed solvent of water and a water-soluble organic solvent.
[0019] (7) The bright pigment (B) is preferably aluminum flakes.
[0020] (8) The coating film according to the present invention is formed using the powder coating composition.
[0021] (9) The coated body according to the present invention comprises a substrate and a coating film formed on the surface of the substrate using the powder coating composition.
[0022] According to the present invention, it is possible to provide a powder coating composition that is capable of forming a coating film that is glossy and has excellent brilliance, and that is also highly recyclable. Furthermore, according to the present invention, it is possible to provide a coating film formed using the powder coating composition, and a coated article having this coating film.
[0023] HSP(δ d , δ p , δ h ) on the Hansen 3D graph, a specific center coordinate and a specific interaction radius R 01 is a diagram for explaining a method for creating a Hansen melting sphere having a specific resin (virtual resin X) used in forming the Hansen melting sphere, and a solvent group that does not dissolve the resin (virtual resin X). 2 is a diagram showing a solvent group that dissolves the resin (virtual resin X) used in forming the Hansen melting sphere, and a solvent group that does not dissolve the resin (virtual resin X), and ... from the center coordinate (CC) of the specific Hansen melting sphere at an interaction distance R a and a solvent located at .
[0024] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Note that the shapes and sizes of the drawings have been appropriately changed for the convenience of explanation. Therefore, the present invention is not limited to the shapes of the drawings.
[0025] [Powder Coating Composition] The powder coating composition according to the present invention contains resin-containing powder particles (A), a luster pigment (B), and a binder (C).
[0026] (Resin-containing powder particles (A)) The resin-containing powder particles (A) contain at least a resin (A1). The resin (A1) contains at least a binder resin (A11) and may contain a curing agent (A12) as needed. Here, the curing agent (A12) is a compound or polymer that reacts with the binder resin (A11). It is preferable that the curing agent (A12) does not react during the preparation of the resin-containing powder particles (A), but reacts when a film is formed using the powder coating composition.
[0027] The resin-containing powder particles (A) are prepared by, for example, melting and kneading a mixture containing at least a binder resin (A11) and, optionally, a curing agent (A12), followed by cooling and pulverization, so as to contain the resin (A1). The mixture may further contain additives (A2) such as a surface conditioner and a lubricant, and color pigments (A3), as required.
[0028] When the mixture further contains an additive (A2), the resulting resin-containing powder particles (A) contain the resin (A1) and a component derived from the additive (A2). Here, the "component derived from the additive (A2)" means the additive (A2) itself or a reaction product of the additive (A2) with another component.
[0029] When the mixture further contains a color pigment (A3), the resulting resin-containing powder particles (A) contain the resin (A1) and the color pigment (A3).
[0030] Furthermore, when the additive (A2) and the color pigment (A3) are further contained, the resulting resin-containing powder particles (A) contain the resin (A1), a component derived from the additive (A2), and the color pigment (A3).
[0031] <Binder Resin (A11)> As the binder resin (A11), for example, one or more types selected from the group consisting of fluororesins, polyester resins, and acrylic resins are used, and a combination of multiple types of binders may also be used.
[0032] The fluororesin used in the binder resin (A11) is a fluorocopolymer obtained by polymerizing or copolymerizing a fluorine-containing monomer.
[0033] The fluororesin is, for example, a resin that is solid at room temperature and has a softening point of 50 to 150°C.
[0034] Examples of fluorine-containing monomers that can be used include vinyl fluoride, vinylidene fluoride, trifluoroethylene, tetrafluoroethylene, bromotrifluoroethylene, chlorotrifluoroethylene, pentafluoropropylene, hexafluoropropylene, and (per)fluoroalkyltrifluorovinyl ethers (the (per)fluoroalkyl group has 1 to 18 carbon atoms).
[0035] The fluororesin may be a copolymer of a fluorine-containing monomer and a polymerizable monomer other than the fluorine-containing monomer, such as vinyl ethers, olefins, allyl ethers, vinyl esters, allyl esters, (meth)acrylic esters, or crotonates.
[0036] Examples of polymerizable monomers include alkyl vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, butyl vinyl ether, isobutyl vinyl ether, cyclohexyl vinyl ether, and chloroethyl vinyl ether; olefins such as ethylene, propylene, 1-butene, isobutylene, cyclohexene, vinyl chloride, and vinylidene chloride; styrene-based monomers such as styrene and α-methylstyrene; alkyl allyl ethers such as methyl allyl ether, ethyl allyl ether, butyl allyl ether, and cyclohexyl allyl ether; fatty acid vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, vinyl valerate, vinyl hexanoate, vinyl octanoate, and vinyl versatate; fatty acid allyl esters such as allyl propionate and allyl acetate; (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and cyclohexyl (meth)acrylate; Polymerizable monomers that can be used include (meth)acrylic acid amides such as (meth)acrylic acid amide; cyano group-containing monomers such as acrylonitrile and 2,4-dicyanobutene-1; and dienes such as isoprene and butadiene.
[0037] The fluororesin may have a reactive site that reacts with a curing agent, etc. The fluororesin may also be a copolymer of one or more of the above-mentioned fluorine-containing monomers and polymerizable monomers with a reactive group-containing monomer.
[0038] The reactive group-containing monomer may be a monomer containing a functional group such as a hydroxyl group, a carboxyl group, an amide group, an amino group, a nitrile group, a glycidyl group, an isocyanate group, etc. Examples of the reactive group-containing monomer include a hydroxyl group-containing monomer, a carboxyl group-containing monomer, an amino group-containing monomer, an amide group-containing monomer, a nitrile group-containing monomer, a glycidyl group-containing monomer, an isocyanate group-containing monomer, etc.
[0039] Examples of the hydroxyl group-containing monomer that can be used include allyl alcohol; hydroxyalkyl vinyl ethers such as 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, and 4-hydroxycyclohexyl vinyl ether; hydroxyalkyl allyl ethers such as 2-hydroxyethyl allyl ether, 3-hydroxypropyl allyl ether, 4-hydroxybutyl allyl ether, and 4-hydroxycyclohexyl allyl ether; hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate; esters of hydroxyalkyl carboxylic acids with vinyl alcohol such as vinyl hydroxyacetate, vinyl hydroxyisobutyrate, vinyl hydroxypropionate, vinyl hydroxybutyrate, vinyl hydroxyvalerate, and vinyl hydroxycyclohexylcarboxylate; and hydroxyalkyl allyl esters such as hydroxyethyl allyl ester, hydroxypropyl allyl ester, hydroxybutyl allyl ester, and hydroxyisobutyl allyl ester.
[0040] Furthermore, (meth)acrylic acid, carboxyalkyl allyl ester, etc. are used as carboxyl group-containing monomers. Aminoalkyl vinyl ethers, aminoalkyl allyl ethers are used as amino group-containing monomers. (Meth)acrylamide, N-methyl(meth)acrylamide, etc. are used as amide group-containing monomers. (Meth)acrylonitrile is used as nitrile group-containing monomers. Glycidyl allyl ether, glycidyl (meth)acrylate, etc. are used as glycidyl group-containing monomers. Vinyl isocyanate, isocyanate ethyl acrylate, etc. are used as isocyanate group-containing monomers.
[0041] The fluorine content of the fluororesin used in the present invention is preferably 10 to 70% by mass.
[0042] When a curing agent that reacts with a hydroxyl group is used as the curing agent component (A12), the hydroxyl value of the fluororesin is preferably 10 to 100 mgKOH / g, and more preferably 30 to 70 mgKOH / g.
[0043] When a curing agent that reacts with a carboxyl group is used as the curing agent component (A12), the acid value of the fluororesin is preferably 1 to 80 mgKOH / g, and more preferably 10 to 60 mgKOH / g.
[0044] The polyester resin used for the binder resin (A11) is a resin that is solid at room temperature and is obtained by reacting a carboxylic acid with a polyhydric alcohol by a known method. The softening point of the polyester resin is preferably 100 to 150°C.
[0045] Examples of the carboxylic acid component that contains a carboxylic acid include polycarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,2-octadecanedicarboxylic acid, maleic acid, fumaric acid, cyclohexanedicarboxylic acid, hexahydrophthalic acid, tetrahydrophthalic acid, trimellitic acid, and pyromellitic acid; lower alkyl esters of these polycarboxylic acids and anhydrides thereof; and hydroxycarboxylic acids such as malic acid, tartaric acid, 1,2-hydroxystearic acid, and parahydroxybenzoic acid.
[0046] Examples of polyhydric alcohols that can be used include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, spiroglycol, 1,4-cyclohexanedimethanol, trimethylolethane, trimethylolpropane, glycerin, and pentaerythritol.
[0047] The polyester resin can be produced using the above-mentioned carboxylic acid component and polyhydric alcohol as raw materials by a conventional method for producing polyester resins for powder coatings. For example, the above-mentioned raw materials are used in an appropriate combination and blending ratio, and an esterification or transesterification reaction is carried out at 200 to 280°C according to a conventional method, followed by a polycondensation reaction at 230 to 290°C using a catalyst under reduced pressure, followed by a depolymerization reaction with an alcohol component to produce the polyester resin.
[0048] It is preferable from the viewpoint of controlling the melt viscosity that the polyester resin has a number average molecular weight of 8,000 or less and a weight average molecular weight of 10,000 to 20,000.
[0049] When a curing agent that reacts with a hydroxyl group is used as the curing agent component (A12), the hydroxyl value of the polyester resin is preferably 20 to 100 mgKOH / g, more preferably 30 to 80 mgKOH / g.
[0050] When a curing agent that reacts with a carboxyl group is used as the curing agent component (A12), the acid value of the polyester resin is preferably 1 to 80 mgKOH / g, more preferably 10 to 60 mgKOH / g.
[0051] Furthermore, for powder coatings containing a fluororesin and a polyester resin, if the melt viscosity of the polyester resin used is 3.5 Pa s (190°C) or less, and the slope of an Arrhenius plot of temperature and viscosity at 100-120°C measured with a rheometer at a cooling rate of 10°C / min from 200°C is 15,000 or more, the fluororesin component is likely to be unevenly distributed on the surface of the coating film during coating film formation. When the fluororesin component is unevenly distributed on the surface of the coating film in this way, the weather resistance of the coating film improves.
[0052] The slope is calculated, for example, by the following method. First, using an ARES rheometer manufactured by TA Instruments, the viscosity is measured under the measurement conditions of parallel plates with a diameter of 40 mm, a gap width of 1.0 mm, a frequency of 9.42 rad / s, and a strain of 1.0%. Next, using the obtained measurement results, the reciprocal 1 / T of temperature T (K) is plotted on the horizontal axis and the logarithm lnV of viscosity V is plotted on the vertical axis (Arrhenius plot). The slope of the obtained straight line from 100 to 120°C is then determined, and this value is defined as the slope.
[0053] The above gradient is more preferably 16,000 to 20,000 from the viewpoint of facilitating layer separation of the coating film.
[0054] The acrylic resin used in the binder resin (A11) is a solid resin at room temperature and is a polymer of acrylic acid esters or methacrylic acid esters. Examples of the acrylic resin include polymers obtained by polymerizing one or more acrylic components selected from acrylic acid, methacrylic acid, and their esters, amides, and nitriles. Examples of the acrylic resin include polymers obtained by polymerizing an acrylic component with a non-acrylic component such as styrene. From the perspective of controlling melt viscosity, it is preferable for the acrylic resin to have a softening point of 100 to 150°C, a number average molecular weight of 8,000 or less, and a weight average molecular weight of 10,000 to 20,000.
[0055] Examples of the acrylic component include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, Examples of the monomers that can be used include (meth)acrylate monomers such as 2-hydroxyethyl (meth)acrylate, benzyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, and ethoxypropyl (meth)acrylate; and functional group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl acrylate, 2-aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, 3-aminopropyl (meth)acrylate, 2-butylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, and allyl glycidyl ether.Examples of the acrylic component that can be used include acrylic acid and methacrylic acid; amide monomers such as acrylic acid amide and methacrylic acid amide; and alkoxysilyl group-containing monomers such as γ-(meth)acryloxypropyltrimethoxysilane, γ-(meth)acryloxypropyltriethoxysilane, β-(meth)acryloxyethyltrimethoxysilane, β-(meth)acryloxyethyltriethoxysilane, γ-(meth)acryloxypropylmethyldimethoxysilane, γ-(meth)acryloxypropylmethyldiethoxysilane, γ-(meth)acryloxypropylmethyldipropoxysilane, γ-(meth)acryloxybutylphenyldimethoxysilane, γ-(meth)acryloxypropyldimethylmethoxysilane, and γ-(meth)acryloxypropyldiethylmethoxysilane.
[0056] The proportion of the acrylic component relative to the total components constituting the acrylic resin is, for example, 40 to 100% by mass.
[0057] Examples of non-acrylic components that can be used include carboxyl group-containing monomers such as fumaric acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, crotonic acid, and vinyl versatic acid; aromatic monomers such as styrene, methylstyrene, chlorostyrene, methoxystyrene, and vinyltoluene; olefin monomers such as ethylene and propylene; vinyl monomers such as vinyl acetate and vinyl chloride; amide monomers such as maleic acid amide; alkoxysilyl group-containing monomers such as vinyltrimethoxysilane, vinyltriethoxysilane, vinylmethyldimethoxysilane, and vinylmethyldiethoxysilane; dialkyl fumarate, allyl alcohol, vinylpyridine, and butadiene.
[0058] When a curing agent that reacts with a hydroxyl group is used as the curing agent component (A12), the hydroxyl value of the acrylic resin is preferably 20 to 100 mgKOH / g, more preferably 30 to 80 mgKOH / g.
[0059] When a curing agent that reacts with a carboxyl group is used as the curing agent component (A12), the acid value of the acrylic resin is preferably 1 to 80 mgKOH / g, more preferably 10 to 60 mgKOH / g.
[0060] <Curing Agent (A12)> As the curing agent (A12), one or more compounds selected from the group consisting of a compound having an epoxy group or a polymer thereof, an amide compound, and an isocyanate compound are used.
[0061] The compound having an epoxy group is preferably a compound having a plurality of epoxy groups in the molecule, and a representative example thereof is triglycidyl isocyanurate.The polymer having an epoxy group (hereinafter also referred to as epoxy resin) includes bisphenol type epoxy resins such as bisphenol A type epoxy resins and bisphenol F type epoxy resins, naphthalene type epoxy resins, biphenyl type epoxy resins, novolac type epoxy resins, cycloaliphatic epoxy resins, glycidylamine type resins, heterocyclic epoxy resins, polyfunctional type epoxy resins, etc.These can be used alone or in combination.
[0062] Examples of the epoxy resin that can be used include a solid epoxy resin synthesized from bisphenol A and an epihalohydrin such as epichlorohydrin, and a solid epoxy resin obtained by an elongation reaction between bisphenol A and an epoxy resin derived from bisphenol A, a dihydric phenol, and an epihalohydrin.
[0063] Examples of epoxy resins available on the market include jER1004, jER1004F, jER1007, and jER4005P manufactured by Mitsubishi Chemical Corporation, EPICLON3050 and EPICLON4050 manufactured by DIC Corporation, Epotohto YD014D manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and EPONANYAMPES-904 manufactured by Nan-A Plastics Co., Ltd.
[0064] The softening point of the epoxy resin is not particularly limited, but is preferably 60 to 150° C. The epoxy equivalent of the epoxy resin is also not particularly limited, but is preferably 400 to 3,000.
[0065] As the epoxy resin, a mixture of multiple epoxy resins with different epoxy equivalents can be used. When a mixture of multiple epoxy resins is used, it is preferable to combine an epoxy resin with an epoxy equivalent of 1000 or less with an epoxy resin with an epoxy equivalent of 1000 or more.
[0066] In addition, the difference in epoxy equivalent between the epoxy resin having the minimum epoxy equivalent (A-min) and the epoxy resin having the maximum epoxy equivalent (A-max) is usually 300 or more, preferably 500 or more, and more preferably 800 or more.
[0067] As the amide compound, for example, β-hydroxyalkylamide is used. From the viewpoint of low-temperature curing ability and water resistance of the coating film obtained by application, the β-hydroxyalkylamide is preferably a β-hydroxyalkylamide having two or more functional groups per molecule. From the viewpoint of low-temperature curing ability and water resistance of the coating film obtained by application, the β-hydroxyalkylamide is more preferably N,N-di(β-hydroxyethyl)acetamide, bis(β-hydroxyethyl)adipamide, bis(β-hydroxypropyl)adipamide, bis[N,N-di(β-hydroxyethyl)]adipamide, or bis[N,N-di(β-hydroxypropyl)]adipamide. In the β-hydroxyalkylamide, the equivalent of the hydroxyl amide group relative to the carboxyl group in the resin is preferably 0.5 to 1.5 equivalents.
[0068] The isocyanate compound may be, for example, a blocked isocyanate compound, and is preferably a solid at room temperature.
[0069] Blocked isocyanate compounds can be produced easily, for example, by reacting an aliphatic, aromatic, or araliphatic diisocyanate with a low-molecular-weight compound having active hydrogen to obtain a polyisocyanate, and then reacting the resulting polyisocyanate with a blocking agent to perform masking.
[0070] Examples of diisocyanates that can be used include tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate, hexamethylene diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methylcyclohexane diisocyanate, bis(isocyanatomethyl)cyclohexane, isophorone diisocyanate, dimer acid diisocyanate, and lysine diisocyanate.
[0071] Examples of low molecular weight compounds having active hydrogen include water, ethylene glycol, propylene glycol, trimethylolpropane, glycerin, sorbitol, ethylenediamine, ethanolamine, diethanolamine, and hexamethylenediamine, as well as isocyanurate, uretidione, low molecular weight polyesters containing hydroxyl groups, and polycaprolactone.
[0072] Examples of blocking agents that can be used include alcohols such as methanol, ethanol, and benzyl alcohol; phenols such as phenol and cresone; lactams such as caprolactam and butyrolactam; and oximes such as cyclohexanone, oxime, and methyl ethyl ketoxime.
[0073] For example, specific examples of blocked isocyanates include isophorone diisocyanate blocked with ε-caprolactam (Vestagon B1530 manufactured by Evonik, Crelan UI manufactured by Bayer), etc.
[0074] The softening point of the isocyanate compound is preferably 10 to 120° C., more preferably 40 to 100° C. If the softening point is less than 10° C., the powder coating composition may harden at room temperature or may form granular lumps. On the other hand, if the softening point exceeds 120° C., it becomes difficult to uniformly disperse the isocyanate compound in the powder coating composition when producing the powder coating composition by melt kneading, and the performance of the resulting coating film, such as smoothness, strength, and moisture resistance, may be impaired.
[0075] The isocyanate compound preferably has an equivalent weight of isocyanate groups relative to hydroxyl groups in the resin of 0.05 to 1.5 equivalents, more preferably 0.8 to 1.2 equivalents. If the isocyanate group equivalent is less than 0.05 equivalents, the degree of cure of the powder coating composition may be insufficient, and coating film performance such as adhesion, coating film hardness, and chemical resistance may be reduced. If the isocyanate group equivalent is more than 1.5 equivalents, the coating film may become brittle and may exhibit poor heat resistance, chemical resistance, moisture resistance, and the like. Furthermore, because blocked isocyanates are expensive, using an excessive amount of blocked isocyanates is likely to increase costs.
[0076] The resin (A1) constituting the resin-containing powder particles (A) preferably contains one or more binder resins (A11) selected from the group consisting of fluororesins, polyester resins, and acrylic resins, and one or more curing agents (A12) selected from the group consisting of compounds having an epoxy group or polymers thereof, amide compounds, and isocyanate compounds.
[0077] The resin (A1) constituting the resin-containing powder particles (A) more preferably contains one or more binder resins (A11) selected from the group consisting of fluororesins and polyester resins, and a curing agent (A12) consisting of an isocyanate compound.
[0078] The resin (A1) constituting the resin-containing powder particles (A) more preferably contains a binder resin (A11) made of a polyester resin and a curing agent (A12) made of a compound having an epoxy group or a polymer thereof.
[0079] The resin (A1) constituting the resin-containing powder particles (A) more preferably contains a binder resin (A11) made of a polyester resin and a curing agent (A12) made of an amide compound.
[0080] <Additive (A3)> Examples of the additive (A3) that can be used include general paint additives such as plasticizers, curing accelerators, crosslinking accelerator catalysts, surface conditioners, ultraviolet absorbers, light stabilizers, antioxidants, flowability adjusters, anti-sagging agents, and antifoaming agents.
[0081] <Color Pigment (A4)> Examples of the color pigment (A4) that can be used include inorganic pigments such as titanium oxide, yellow iron oxide, titanium yellow, red iron oxide (red iron oxide), lithopone, and antimony oxide, and organic pigments such as Hansa Yellow 5G, Permanent Yellow FGL, Phthalocyanine Blue, Indanthrene Blue RS, Permanent Red F5RK, and Brilliant Fast Scarlet G.
[0082] As described above, the resin-containing powder particles (A) are prepared so as to contain the resin (A1), for example, by melting and kneading a mixture containing at least the binder resin (A11) and the curing agent (A12), followed by cooling and pulverizing the mixture.
[0083] The resin-containing powder particles (A) may further contain, in addition to the resin (A1), a component derived from the additive (A2), a color pigment (A3), and the like, as needed.
[0084] The resin-containing powder particles (A) have a 50% volume average particle size of, for example, 15 to 100 μm, preferably 20 to 70 μm, and more preferably 30 to 50 μm.
[0085] (Brightening pigment (B)) Examples of the brightening pigment (B) that can be used include aluminum powder pigments, nickel powder pigments, stainless steel powder pigments, copper powder, bronze powder, gold powder, silver powder, mica pigments, graphite pigments, glass flake pigments, flaked plastic pigments, and scaly iron oxide pigments. Examples of the aluminum powder pigment that can be used include flaky aluminum flakes. When the brightening pigment (B) is flaky aluminum flakes, it is preferred because of its high brightness.
[0086] The bright pigment (B) has a 50% volume average particle size of, for example, 3 to 100 μm, preferably 5 to 80 μm, and more preferably 15 to 60 μm.
[0087] The bright pigment (B) has an aspect ratio of, for example, 2 to 60, preferably 3 to 40, and more preferably 5 to 25.
[0088] (Binder (C)) The binder (C) is a resin that bonds the resin-containing powder particles (A) and the luster pigment (B). The binder (C) is used by dissolving or dispersing in the solvent (D) so as to have fluidity when bonding the resin-containing powder particles (A) and the luster pigment (B).
[0089] The binder (C) constituting the powder coating composition of the present invention is used together with a solvent (D) that does not dissolve the resin (A1) constituting the resin-containing powder particles (A) but dissolves or disperses the binder (C) when bonding the resin-containing powder particles (A) and the luster pigment (B).
[0090] Specifically, the binder (C) is a binder having a specific center coordinate (δ) of the Hansen melting sphere on the Hansen 3D graph. d , δ p , δ h ) = (19.0, 7.0, 5.0) a The resin is soluble or dispersible in a solvent (D) having a specific range of Tg and weight average molecular weight, and the Tg and weight average molecular weight are also within specific ranges.
[0091] More specifically, the binder (C) has the central coordinates (δ) of the Hansen dissolving sphere, which determines the solubility of the binder (C) in the solvent to be mixed. d , δ p , δ h ) is (19.0, 7.0, 5.0), the interaction distance R a The resin is dissolved or dispersed in a solvent (D) having a Tg of 20 or more, and has a Tg of 30° C. or more and a weight average molecular weight of 1,000 to 100,000.
[0092] The above Hansen 3D graph, Hansen melting sphere, center coordinate (δ d , δ p , δ h ), and the interaction distance R a is HSP(δ d , δ p , δ h These concepts will be explained below with reference to the drawings.
[0093] <Hansen Solubility Parameter (HSP)> Figure 1 shows the HSP (δ d , δ p , δ h ) on the Hansen 3D graph, a specific center coordinate and a specific interaction radius R 0 1 is a diagram for explaining a method for creating a Hansen melting sphere having a shape.
[0094] Hansen HSP (δ d , δ p , δ h ) is a parameter defined by the following equation (1).
[0095] (δ: Hildebrand solubility parameter (SP) of substance X [KJ / cm 3 ] 1/2 , ΔE V : Molar evaporation energy of substance X [KJ / mol], V: Molar volume of substance X [cm 3 / mol], ΔE d V : Molar evaporation energy of dispersion force term of substance X [KJ / mol], ΔE p V : Molar evaporation energy of dipole-dipole force term of substance X [KJ / mol], ΔE h V : Molar evaporation energy of hydrogen bonding term of substance X [KJ / mol], δ d : Dispersion force term of HSP of substance X, δ p : Dipole-dipole force term of HSP of substance X, δ h : hydrogen bond term of HSP of substance X)
[0096] In the present invention, the substance X is defined as a virtual resin X that can be applied to many resins (A1) constituting the resin-containing powder particles (A). Specifically, in the present invention, the virtual resin X is defined as a specific central coordinate (δ d , δ p , δ h ) = (19.0, 7.0, 5.0). In the present invention, the center coordinates of the Hansen dissolving sphere are set to specific center coordinates (δ d , δ p , δh ) = (19.0, 7.0, 5.0), it becomes possible to bond the bright pigment to various types of resin-containing powder particles.
[0097] As shown in Figure 1, HSP(δ d , δ p , δ h ) is δ d axis, δ p axis and δ h The HSP (δ) is expressed on the Hansen 3D graph G, which has three axes. d , δ p , δ h ) is represented at point XC in FIG.
[0098] In the present invention, the point XC(δ d , δ p , δ h ) of the virtual resin X as described above. d , δ p , δ h ) = (19.0, 7.0, 5.0), and this (δ d , δ p , δ h ) = (19.0, 7.0, 5.0) is set as the center coordinate CC of the Hansen melting sphere HSS.
[0099] In the present invention, the (δ d , δ p , δ h The Hansen Dissolution Sphere HSS is created with the center coordinates CC at (19.0, 7.0, 5.0). The Hansen Dissolution Sphere HSS is the smallest sphere that contains only a solvent that dissolves the virtual resin X. The smallest sphere is calculated as the smallest sphere that contains only a solvent that dissolves the virtual resin X when testing or simulating whether the virtual resin X dissolves in various solvents.
[0100] The radius of the Hansen melting sphere HSS is the interaction radius R 0 The interaction radius R is defined as 0 is the interaction distance R, which is the distance from the center coordinate CC on the Hansen 3D graph G, defined by the following formula (2): aThe Hansen Dissolving Sphere HSS is the radius of the smallest sphere that contains only the solvent that dissolves the virtual resin X. In the following formula (2), component 1 is the virtual resin X, and component 2 is the solvent. In the present invention, the interaction radius R of the virtual resin X is calculated from the results of the aforementioned "tests or simulations on whether the virtual resin X dissolves in various solvents." 0 It has been found that it is possible to set the value to less than 20 (but excluding 0).
[0101] (R a : interaction distance, δ d,1 : dispersion force term of HSP of component 1 (virtual resin X), δ d,2 : dispersion force term of HSP of component 2 (solvent), δ p,1 : Dipole-dipole force term of HSP of component 1 (virtual resin X), δ p,2 : Dipole-dipole force term of HSP of component 2 (solvent), δ h,1 : Hydrogen bonding term of HSP of component 1 (virtual resin X), δ h,2 : hydrogen bond term of HSP of component 2 (solvent)
[0102] Generally, Δδ defined by the following formula (3), that is, the solubility parameter HSP (δ) of component 1 (hypothetical resin X) on the Hansen 3D graph G, d,1 , δ p,1 , δ h,1 ) and component 2 (solvent) on Hansen's 3D graph G. d,2 , δ p,2 , δ h,2 The distance Δδ between component 1 (virtual resin X) and component 2 (solvent) is an index showing the solubility of component 1 (virtual resin X) and component 2 (solvent). The smaller Δδ, the more easily the two components dissolve, and the larger Δδ, the more difficult it is to dissolve the two components.
[0103] (Δδ: Solubility parameter HSP (δ) of component 1 (hypothetical resin X) on Hansen's 3D graph G d,1 , δ p,1 , δ h,1 ) and component 2 (solvent) on Hansen's 3D graph G. d,2 , δ p,2 , δ h,2 ) and the distance δ d,1: dispersion force term of HSP of component 1 (virtual resin X), δ d,2 : dispersion force term of HSP of component 2 (solvent), δ p,1 : Dipole-dipole force term of HSP of component 1 (virtual resin X), δ p,2 : Dipole-dipole force term of HSP of component 2 (solvent), δ h,1 : Hydrogen bonding term of HSP of component 1 (virtual resin X), δ h,2 : hydrogen bond term of HSP of component 2 (solvent)
[0104] FIG. 2 is a diagram showing a group of solvents that dissolve a resin (hypothetical resin X) used to form a specific Hansen dissolving sphere, and a group of solvents that do not dissolve the resin (hypothetical resin X).
[0105] In FIG. 2, the solvents plotted as "○ (open circle)" have the central coordinates CC and the interaction radius R 0 The solvents plotted as "□ (open square)" are outside the Hansen melting sphere HSS and do not dissolve the hypothetical resin X.
[0106] FIG. 3 shows a group of solvents that dissolve a resin (virtual resin X) used to form a specific Hansen melting sphere, a group of solvents that do not dissolve the resin (virtual resin X), and a group of solvents that dissolve the resin (virtual resin X) at an interaction distance R from the center coordinate CC of the specific Hansen melting sphere. a and a solvent located at
[0107] In FIG. 3, the solvents indicated by the plot ○ have the central coordinates CC and the interaction radius R 0 The solvents in the plot □ are outside the Hansen sphere HSS and dissolve the hypothetical resin X. The solvents in the plot □ are outside the Hansen sphere HSS and do not dissolve the hypothetical resin X. Furthermore, the solvents in the plot DD are outside the Hansen sphere HSS and have an interaction distance R a is the interaction radius R 0 Since the difference is considerably larger than the difference, it can be said that the hypothetical resin X is not dissolved.
[0108] The binder (C) has an interaction distance R aThe resin is soluble or dispersible in a solvent (D) having a molecular weight of 20 or more, preferably a solvent (D) having a molecular weight of 25 or more, and more preferably a solvent (D) having a molecular weight of 30 or more. The solvent (D) will be described later.
[0109] The binder (C) has a Tg of 30° C. or higher, preferably 40° C. or higher, and more preferably 45° C. or higher. If the Tg is lower than 30° C., the binder will remain tacky even after the solvent has evaporated, making it impossible to obtain sufficient binding between the resin-containing powder particles and the bright pigment. Furthermore, the binder remaining on the powder particle surfaces will bind the resin-containing powder particles (A) together, increasing the particle size of the resin-containing powder particles (A).
[0110] The binder (C) has a weight-average molecular weight of 1,000 to 100,000, preferably 2,000 to 70,000, and more preferably 2,000 to 50,000. If the weight-average molecular weight of the binder (C) is less than 1,000, it is difficult to obtain sufficient binding between the resin-containing powder particles and the luster pigment. If the weight-average molecular weight of the binder (C) exceeds 100,000, the solubility or dispersibility in the solvent tends to deteriorate. Note that the dispersibility of the binder can be improved by further using an emulsifier, dispersant, or the like, but in this case, the binding between the resin-containing powder particles and the luster pigment tends to decrease.
[0111] (Solvent (D)) The solvent (D) is a solvent that dissolves or disperses the binder (C). As the solvent (D), for example, one or more solvents selected from the group consisting of water, ethylene glycol, and methanol are used. If the solvent (D) is a mixed solvent of water and a water-soluble organic solvent, it is preferable because the binder can easily wet the surfaces of the resin-containing powder particles while maintaining sufficient insolubility in the resin-containing powder particles.
[0112] (Function) In the powder coating composition of the present invention, a solution or dispersion is prepared in advance by dissolving or dispersing the binder (C) in the solvent (D), and then the resulting solution or dispersion is added to the resin-containing powder particles (A) and mixed thoroughly. Thereafter, the solvent (D) is completely evaporated, thereby binding (bonding) the resin-containing powder particles (A) and the luster pigment (B) with the binder (C).
[0113] Here, examples of the "method of adding a solution or dispersion in which a binder (C) is dissolved or dispersed in a solvent (D) to the resin-containing powder particles (A) and thoroughly mixing" include a method of "dropping a solution or dispersion in which a binder (C) is dissolved or dispersed in a solvent (D) little by little at a specific speed while stirring the resin-containing powder particles (A)" and a method of "spraying a mist of a solution or dispersion in which a binder (C) is dissolved or dispersed in a solvent (D) using a spray nozzle or the like while stirring the resin-containing powder particles (A)".
[0114] A method using vacuum suction is preferred as a method for completely volatilizing the solvent (D). The temperature at which the solvent is volatilized is preferably 0 to 80° C. When the temperature is within the range of 0 to 80° C., a powder coating composition in a good bonding state is easily obtained.
[0115] The solvent (D) dissolves or disperses the binder (C), but does not dissolve the resin-containing powder particles (A) or the resin (A1) that constitutes them. Therefore, even if the solvent (D) is added, there is no risk that the resin-containing powder particles (A) will be bound together, resulting in an increase in the particle size of the resin-containing powder particles (A), a decrease in coating workability, or a deterioration in the appearance of the coating film.
[0116] Therefore, the powder coating composition according to the present invention is capable of forming a coating film that is glossy and has excellent brilliance, and is also highly recyclable.
[0117] In addition, in the powder coating composition according to the present invention, a specific virtual resin X is set as a resin applicable to many resins (A1) constituting the resin-containing powder particles (A), and specific center coordinates CC (δ d , δ p , δ h ) = (19.0, 7.0, 5.0). Therefore, by using the solvent (D) present outside this specific Hansen melting sphere as the solvent for the binder (C), it is possible to dissolve or disperse the binder (C) without dissolving the large amount of resin (A1) present inside the Hansen melting sphere. Therefore, in the present invention, it is possible to bond the bright pigment to various types of resin-containing powder particles.
[0118] (Effects) The powder coating composition according to the present invention can provide a powder coating composition that can form a coating film having high brightness and gloss and that is excellent in terms of recyclability.
[0119] [Coating Film] The coating film according to the present invention is formed using the powder coating composition according to the present invention. Examples of methods for forming the coating film include electrostatic powder coating, corona charging, and tribocharging powder coating.
[0120] The thickness of the coating film is not particularly limited, but is preferably 20 to 1000 μm, more preferably 20 to 500 μm, and even more preferably 20 to 300 μm. When the coating film is a coating film for components for high-rise buildings such as aluminum curtain walls, the thickness of the coating film is preferably 20 to 90 μm. When the coating film is a coating film for components that require high weather resistance, such as outdoor units of air conditioners installed along the coast, traffic light poles, and signs, the thickness of the coating film is preferably 100 to 200 μm.
[0121] The method for forming the coating film is not particularly limited, and examples of the method for forming the coating film include applying the powder coating composition of the present invention to a substrate to form a molten film made of a melt of the powder coating composition, and then cooling the molten film to form the coating film.
[0122] The molten film made of the melt of the powder coating composition can be obtained, for example, by a method in which it is formed simultaneously with the application of the powder coating composition to a substrate, or by a method in which the powder coating composition is attached to a substrate and then heated and melted on the substrate to form the film.
[0123] In addition, when the powder coating composition contains a curing agent, the curing reaction of the reactive components in the composition may start almost simultaneously when the powder coating composition is heated and melted. In this case, the method for forming the coating film is preferably a method in which the powder coating composition is heated and melted and then attached to the substrate almost simultaneously, or a method in which the powder coating composition is attached to the substrate and then heated and melted.
[0124] The heating temperature (hereinafter also referred to as the "baking temperature") and heating maintenance time (hereinafter also referred to as the "baking time") for heating and melting the powder coating composition and for maintaining this heated and melted state for a predetermined period of time are set appropriately depending on the type and composition of the raw material components of the powder coating composition, the desired thickness of the coating film, etc.
[0125] When the powder coating composition does not contain a curing agent, the baking temperature is preferably 160 to 300°C. When the powder coating composition contains a curing agent, the baking temperature is preferably set according to the reaction temperature of the curing agent. When a curing agent is used, the baking temperature is preferably 120 to 240°C.
[0126] The reaction temperature of the curing agent can be determined by measuring the change in the elastic modulus of the powder coating composition, which can be measured using a rheometer such as the ARES rheometer manufactured by TA Instruments Japan, Inc.
[0127] The baking time is preferably 2 to 60 minutes. When the powder coating composition does not contain a curing agent, the baking time is more preferably 5 to 60 minutes, and even more preferably 10 to 50 minutes. When the powder coating composition contains a curing agent, the baking time is more preferably 2 to 50 minutes, and even more preferably 5 to 40 minutes.
[0128] Coating methods used to form coating films include electrostatic coating, electrostatic spraying, electrostatic immersion, atomization, fluidized bed immersion, spraying, spraying, thermal spraying, and plasma spraying. Of these, electrostatic coating using a powder coating gun is preferred because it produces excellent surface smoothness of the molten film. As the powder coating gun, a corona-charged coating gun, a tribo-charged coating gun, and the like are used. Here, a corona-charged coating gun refers to a gun that sprays a powder coating composition after corona discharge treatment. Also, a tribo-charged coating gun refers to a gun that sprays a powder coating composition after tribo-charging treatment.
[0129] The cooling temperature of the molten film is preferably 20 to 25°C. When the powder coating composition according to the present invention contains a curing agent, the coating film formed is a cured film. The cooling after baking may be rapid or slow, with slow cooling being preferred since it prevents the coating film from peeling off from the substrate.
[0130] (Effects) According to the coating film of the present invention, a coating film having high brightness and gloss can be formed using a powder coating composition that is excellent in recyclability.
[0131] [Coated Body] The coated body according to the present invention comprises a substrate and a coating film formed on the surface of the substrate using the powder coating composition according to the present invention.
[0132] (Substrate) As the substrate, for example, a substrate made of metal (iron, stainless steel, aluminum, copper, titanium, brass, aluminum alloy, etc.), steel, cast iron, etc. As the steel, alloy steel, special steel, or carbon steel is used.
[0133] Specific examples of substrates made of aluminum alloys include architectural sashes and architectural panels, etc. Specific examples of substrates made of carbon steel include railway bridges, road bridges, gas tanks, oil tanks, steel towers, springs, etc.
[0134] The coated body according to the present invention can be obtained by using the powder coating composition according to the present invention and carrying out the method for forming the coating film described in the section on the coating film according to the present invention.
[0135] (Effects) According to the coated body of the present invention, it is possible to form a coating film that is glossy and has excellent brilliance, and furthermore, it can be formed using a powder coating composition that is also highly recyclable and reusable.
[0136] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the descriptions of the examples and comparative examples, "parts" and "%" are based on mass.
[0137] In the examples and comparative examples shown below, the following raw materials were used.
[0138] <1. Raw materials for powder coating composition> (1) Raw materials for resin-containing powder particles (A) (1-1) Binder resin (A11) Fluororesin 1: Lumiflon LF710F, a hydroxyl-containing fluororesin (hydroxyl value: 46 mg KOH / g, manufactured by AGC Inc.) Polyester resin 1: U-Picacoat GV560, a hydroxyl-containing polyester resin (hydroxyl value: 50 mg KOH / g, acid value: 5 mg KOH / g, softening point: 125°C, manufactured by Japan U-Pica Co., Ltd.) Polyester resin 2: Krylcoat 1683-0, a carboxylic acid-containing polyester resin (acid value: 50 mg KOH / g, manufactured by Daicel-Allnex Corporation) Polyester resin 3: Krylcoat 2630-2, a carboxylic acid-containing polyester resin (acid value: 33 mg KOH / g, manufactured by Daicel-Allnex Corporation)
[0139] (1-2) Curing Agent (A12) Curing agent 1: ε-caprolactam blocked isocyanate (manufactured by Evonik Degussa Co., Ltd., trade name: VESTAGON B1530) Curing agent 2: Bis-A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, trade name: jER (registered trademark) 1004) Curing agent 3: β-hydroxyl alkylamide (manufactured by M-Chemie Co., Ltd., trade name: Primid XL-552)
[0140] (1-3) Additives (A3) Additive 1: Silica-based surface conditioner (manufactured by BYK-Chemie Co., Ltd., trade name: BYK360P) Lubricant 1: Amorphous silicon dioxide (manufactured by Fuji Silysia Corporation, trade name: SYLYSIA 358)
[0141] (2) Luster pigment (B) Aluminum flake 1: PCF7620A (manufactured by Toyo Aluminum Co., Ltd.)
[0142] (3) Binder (C) Binder 1: Joncryl JDX-C3000 (manufactured by BASF, acrylic resin, active ingredient 100% by mass, Tg 57°C, weight average molecular weight 10,000) Binder 2: Pluscoat Z-730 (manufactured by GOO Chemical Industry Co., Ltd., polyester resin aqueous solution, active ingredient 25% by mass, Tg 46°C, weight average molecular weight 3,000) Binder 3: BURNOCK WD-551P (manufactured by DIC Corporation, aqueous hydroxyl group-containing acrylic resin dispersion, active ingredient 40% by mass, Tg 40°C, weight average molecular weight 28,000) Binder 4: WATERSOL EFD-5580 (manufactured by DIC Corporation, aqueous acrylic resin dispersion, active ingredient 40% by mass, Tg 15°C, weight average molecular weight 70,000) Binder 5: JER 1001 (manufactured by Mitsubishi Chemical Corporation, epoxy resin, active ingredient 100% by mass, Tg 64°C, weight average molecular weight 3000) Binder 6: HA 3509 (manufactured by Resonac Holdings Inc., acrylic resin solution, active ingredient 55% by mass, Tg 50°C, weight average molecular weight 7500) Binder 7: YS Polystar TH130 (manufactured by Yasuhara Chemical Co., Ltd., terpene phenol resin, active ingredient 100% by mass, Tg 130°C, weight average molecular weight 1500)
[0143] (4) Solvent (D) Solvent 1: Ion-exchanged water Solvent 2: A mixture of 75 wt% ion-exchanged water and 25 wt% methanol (manufactured by Kanto Chemical Co., Ltd.) Solvent 3: A mixture of 50 wt% ion-exchanged water and 50 wt% methanol (manufactured by Kanto Chemical Co., Ltd.) Solvent 4: A mixture of 25 wt% ion-exchanged water and 75 wt% methanol (manufactured by Kanto Chemical Co., Ltd.) Solvent 5: Methanol (manufactured by Kanto Chemical Co., Ltd.) Solvent 6: Ethylene glycol (manufactured by Kanto Chemical Co., Ltd.) Solvent 7: Xylene (manufactured by Kanto Chemical Co., Ltd.) Solvent 8: n-Heptane (manufactured by Kanto Chemical Co., Ltd.) Solvent 9: Perfluoromethylcyclohexane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0144] Table 2 shows the NV (%), which is the ratio of the mass of the binder (C) in the paint after drying to the mass of the paint before drying, the glass transition temperature Tg (°C), and the weight average molecular weight Mw.
[0145] [Test Example 1] Using Hansen's solubility parameter calculation software "Hansen Solubility Parameters in Practice (HSPiP)", the HSP (δ d , δ p , δ h The HSP of the solvent (D) was calculated using the (δ d,2 , δ p,2 , δ h,2 ), but in the test examples and the following examples and comparative examples, it is simply referred to as (δ d , δ p , δ h ) on the 3D graph G. d , δ p , δ h ) = (19.0, 7.0, 5.0) a was calculated. d , δ p , δ h ) and the interaction distance R a are shown in Table 2.
[0146]
[0147]
[0148] [Test Example 2] (Solubility Evaluation Test) Each of Binders 1, 2, and 5-7 was adjusted to 100% solids in a reduced-pressure environment of 25°C and 760 mmHg (gauge pressure), and 0.01 g was then measured out. Next, the measured Binders 1, 2, and 5-7 were mixed with 10 ml of each of Solvents 1-9 and stirred at 25°C for 30 minutes. After stirring, the mixture was left for 24 hours, and the state of the resulting mixture was visually evaluated. The evaluation results are shown in Table 3. The evaluation criteria are as follows. Note that Binders 3 and 4 are in a state where the resin component is dispersed in water (solvent 1). If the solids content were 100%, a film would form, making it impossible to determine the solubility of the resin itself. Therefore, 0.04 g (solids content 0.01 g) of Binder 3 was measured out, and then methanol was added so that the water / methanol mixture ratio was equivalent to that of Solvents 2 and 3, and the dispersion state was evaluated. For binder 4, 0.018 g (solid content: 0.01 g) was measured out, and then methanol was added so that the water / methanol mixture ratio was the same as in solvents 2 and 3, and the dispersion state was evaluated.
[0149] <Evaluation> Evaluation was made as follows: ◎ (Excellent): A transparent liquid, dissolved. ○ (Good): A cloudy liquid, dispersed (no precipitate formed). × (Poor): Precipitate formed from the time of stirring. -: Dispersion evaluation not performed.
[0150]
[0151] Examples 1 to 36, Comparative Examples 1 to 15 (1. Preparation of Powder Coating Compositions) <1-1: Preparation of Resin-Containing Powder Particles (A)> (1) 1-1-1: Preparation of Powder Particles Containing Fluorine Resin and Polyester Resin Using the raw materials shown in Tables 1 and 2, the components were mixed to the blending ratios shown in Tables 4 and 5 to obtain powder particles (A) containing fluororesin and polyester resin. Specifically, the fluororesin, polyester resin, curing agent (blocked isocyanate), additives, and lubricant were placed in a high-speed mixer and mixed for 1 minute. The mixture was then kneaded using a single-screw kneader (manufactured by BUSS) adjusted to a temperature of 120°C, and the discharged mixture was cold-rolled with a cooling roll. The mixture was then pulverized using a pin mill and classified using a 150-mesh screen to obtain powder particles (A) (50% volume average particle diameter: approximately 35 μm) that served as the raw materials for the powder coating compositions (Coatings 1 to 17).
[0152] (2) 1-1-2: Preparation of Powder Particles Containing Polyester Resin and Epoxy Resin Using the raw materials shown in Tables 1 and 2, the components were mixed to the blending ratios shown in Tables 6 and 7 to obtain powder particles (A) containing polyester resin and epoxy resin. Specifically, the polyester resin, epoxy resin, and additives were placed in a high-speed mixer and mixed for 1 minute. The mixture was then kneaded using a single-screw kneader (manufactured by BUSS Co., Ltd.) adjusted to 120°C, and the discharged mixture was cold-rolled with a cooling roll. The mixture was then pulverized using a pin mill, classified using a 150-mesh screen, and a lubricant was added to obtain powder particles (A) (50% volume average particle diameter: approximately 35 μm) that served as the raw materials for the powder coating compositions (Coatings 18 to 34).
[0153] (3) 1-1-3: Preparation of Powder Particles Containing a Polyester Resin and an Amide Compound Using the raw materials shown in Tables 1 and 2, the components were mixed to the blending ratios shown in Tables 8 and 9 to obtain powder particles (A) containing a polyester resin and an amide compound. Specifically, the polyester resin, amide compound, additives, and lubricant were placed in a high-speed mixer and mixed for 1 minute. The mixture was then kneaded using a single-screw kneader (manufactured by BUSS Co., Ltd.) adjusted to 120°C, and the discharged mixture was cold-rolled with a cooling roll. The mixture was then pulverized using a pin mill and classified using a 150-mesh screen to obtain powder particles (A) (50% volume average particle diameter: approximately 35 μm) that served as the raw materials for the powder coating compositions (Coatings 35 to 51).
[0154] <1-2: Preparation of binder liquid> Binders and binder solvents were mixed to the blending ratios shown in Tables 4 to 9 to prepare binder liquids to be used in producing powder coating compositions (Coatings 1 to 51).
[0155] <1-3: Preparation of Powder Coating Compositions (Coatings 1 to 51)> A luster pigment (PCF7620A, average particle size 21 μm, resin-coated aluminum powder, manufactured by Toyo Aluminum K.K.) was added to the powder particles (A) obtained by the above-mentioned method in the blending ratios shown in Tables 4 to 9, and mixed uniformly with a spoon. Next, the binder liquid obtained by the above-mentioned method was added, and the mixture was allowed to dry naturally for 1 hour while kneading. The mixture was filled into a 1-liter measuring flask and vacuum-dried at room temperature for 20 minutes using an evaporator, with rotational mixing for 30 minutes. The powder obtained in this way was classified using a mesh with 100 μm openings to obtain powder coating compositions (Coatings 1 to 51).
[0156] (2. Property Evaluation) The properties of the obtained powder coating compositions (Coatings 1 to 51) were evaluated. The results of each evaluation test are shown in Tables 4 to 9. In the evaluation tests for brilliance and surface smoothness, test pieces prepared as follows were used.
[0157] <2-1: Method of preparing test pieces> Each powder coating material was electrostatically coated on one side of a chromate-treated aluminum plate (substrate) using an electrostatic coating machine (manufactured by Onoda Cement Co., Ltd., product name: GX3600C) equipped with a powder coating gun, and the coated aluminum plate was then held for 20 minutes in an atmosphere at 200° C. The coated aluminum plate was then left to cool to room temperature, yielding an aluminum plate (test piece) with a coating film (cured film) having a thickness of 55 to 65 μm.
[0158] <2-2: Evaluation> Layer separation, brightness, surface smoothness, and recyclability were measured and evaluated as follows.
[0159] (1) Layer Separability The cross sections of the coating films of Examples 1 to 12 and Comparative Examples 1 to 5 were observed using a microscope (Keyence Corporation) to evaluate whether the coating film was separated into upper and lower layers inside. The cross sections of the coating films were also observed using a scanning electron microscope (Hitachi High-Technologies Corporation Ultra-High Resolution Analytical Scanning Electron Microscope SU-70) to confirm the distribution of elemental fluorine (fluororesin) in the cross sections of the coating film by elemental analysis.
[0160] The evaluation was made as follows: ◯ (good): Fluorine element was unevenly distributed on the surface layer of the coating film. × (poor): No uneven distribution of fluorine element on the surface layer of the coating film was observed.
[0161] (2) Glossiness Evaluation was made as follows: For each test piece, color unevenness of the coating film was visually evaluated according to the following criteria: ○ (Good): Color unevenness occurred in 20% or less of the total area of the test piece. × (Poor): Color unevenness occurred in more than 20% of the total area of the test piece.
[0162] (3) Surface smoothness Evaluation was made as follows. After the test panel was prepared, the condition of the coating surface was visually evaluated. ⊚ (Excellent): No abnormalities ∘ (Good): Yuzu skin ∘ (Poor): Rough skin
[0163] (4) Recovery and Reusability Evaluation was made as follows. Paint that did not adhere during the first coating was repainted, and each test piece was visually inspected for color unevenness in the coating film and evaluated according to the following criteria: ○ (Good): Color unevenness occurred in 20% or less of the total area of the test piece. × (Poor): Color unevenness occurred in more than 20% of the total area of the test piece.
[0164] The results are shown in Tables 4 to 9.
[0165]
[0166]
[0167]
[0168]
[0169]
[0170]
[0171] From the examples and comparative examples, it was found that the powder coating compositions of the examples were excellent in all respects of brightness, surface smoothness, and recoverability and reusability.
[0172] CC Center coordinates G Hansen's 3D graph HSS Hansen's melting ball R 0 interaction radius R a interaction distance
Claims
1. A powder coating composition comprising resin-containing powder particles (A), a luster pigment (B) and a binder (C), wherein the binder (C) has a central coordinate (δ) of the Hansen dissolution sphere, which determines the solubility of the binder with a solvent to be mixed. d , δ p , δ h ) is (19.0, 7.0, 5.0), the interaction distance R a 20 or more, and is a resin having a Tg of 30° C. or more and a weight average molecular weight of 1,000 to 100,000.
2. The binder (C) has an interaction distance R a 2. The powder coating composition according to claim 1, wherein the resin is soluble or dispersible in a solvent (D) having a molecular weight of 30 or more.
3. The powder coating composition according to claim 1, wherein the binder (C) has a Tg of 40° C. or higher.
4. The powder coating composition according to claim 1, characterized in that the resin (A1) constituting the resin-containing powder particles (A) is a resin obtained by reacting one or more binder resins (A11) selected from the group consisting of fluororesins, polyester resins, and acrylic resins with one or more curing agents (A12) selected from the group consisting of compounds having an epoxy group or their polymers, amide compounds, and isocyanate compounds.
5. The powder coating composition according to claim 1, wherein the solvent (D) is one or more solvents selected from the group consisting of water, ethylene glycol, and methanol.
6. The powder coating composition according to claim 1, wherein the solvent (D) is a mixed solvent of water and a water-soluble organic solvent.
7. The powder coating composition according to claim 1, wherein the luster pigment (B) is a flake-like aluminum piece.
8. A coating film formed by using the powder coating composition according to any one of claims 1 to 7.