Composition for latex polymerization with excellent durability, latex for dip molding, and dip-molded article manufactured therefrom
Patent Information
- Application Number
- MYPI2025005570
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-13
- Filing Date
- 2024-02-21
- Publication Date
- 2024-09-13
AI Technical Summary
Conventional latex products, such as gloves, face durability issues when exposed to human body fluids due to degradation in mechanical properties like tensile strength and elongation, and there is a need for high-solids latex with large particle size and low viscosity for improved durability and stability in dip molding processes.
A composition for latex polymerization comprising a conjugated diene monomer, ethylenically unsaturated nitrile monomer, ethylenically unsaturated acid monomer, ionic organic compound, and ionic inorganic compound, with a specific weight ratio of ionic inorganic to ionic organic compounds, which enhances stability and mechanical properties, forming a copolymer with large particle size and low viscosity, suitable for high-solids dip molding.
The solution provides latex with excellent stability, large particle size, high solid content, and low viscosity, resulting in dip molded products with enhanced durability and resistance to degradation under actual use conditions, such as surgical gloves and medical gloves.
Abstract
Description
Durable latex polymerization composition, latex for dip molding and dip molded products manufactured therefrom
[0001] The present specification relates to a composition for polymerizing latex with excellent durability, latex for dip molding, and a dip molded product manufactured therefrom.
[0002] Traditionally, the primary raw material for gloves used for medical, agricultural, and livestock processing, or industrial purposes, has been natural rubber latex. However, when using gloves made from natural rubber latex, users frequently suffered from contact allergies due to the proteins contained in the natural rubber latex. Therefore, attempts have been made to manufacture gloves using synthetic rubber latex, such as nitrile copolymer latex, which does not contain proteins. Nitrile copolymer latex gloves offer superior mechanical strength compared to natural rubber latex gloves, and demand is growing in the medical and food industries, where contact with sharp objects is frequent.
[0003] As the use of nitrile copolymer latex increases, the need for improved quality in dip-molded products is growing. Consequently, efforts are being made to improve the durability, such as tensile strength and elongation, of dip-molded products manufactured from dip-molded latex. However, despite these attempts to improve mechanical properties, cases of dip-molded products breaking, resulting in personal injury or failure to achieve desired results continue to occur.
[0004] This is because the properties of the molded product deteriorate when it comes into contact with slightly acidic body fluids such as human skin or sweat during actual use. Conventional mechanical properties such as tensile strength and elongation are measured in air at room temperature. If these properties are excellent, the durability of the dip-molded product before use can be guaranteed, but there have been cases where the durability under actual use conditions is poor. Therefore, there is a need for technology development for manufacturing dip-molded products with excellent durability under actual use conditions.
[0005] In addition, the demand for high-solids dip molding latex that exhibits excellent quality even in small quantities is increasing. However, when the solids content of conventional dip molding latex is increased by concentrating it, there is a problem in that the viscosity increases rapidly above a certain content due to the decrease in particle stability. In addition, dip molding latex generally contains particulate polymers with an average particle size of approximately 800 Å. When this is concentrated or enlarged through chemical treatment to improve the quality of the latex, there is a problem in that the stability of the latex is rapidly reduced.
[0006] Therefore, there is a need to develop latex for dip molding and dip molded products that simultaneously satisfy the trade-offs of high solids content, large particle size, and low viscosity, while also having excellent durability for actual use.
[0007] The present specification is intended to solve the problems of the prior art described above, and one object of the present specification is to provide a latex for dip molding having excellent stability, large particle size, high solid content and low viscosity, and a polymerization composition for producing the latex.
[0008] Another object of the present specification is to provide a deep-molded product having excellent practical durability.
[0009] According to one aspect, a composition for latex polymerization is provided, which comprises a conjugated diene monomer, an ethylenically unsaturated nitrile monomer, an ethylenically unsaturated acid monomer, an ionic organic compound, and an ionic inorganic compound, wherein a weight ratio of the ionic inorganic compound to the ionic organic compound is 4.7 or more.
[0010] In one embodiment, the conjugated diene monomer may be one selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, 2-chloro-1,3-butadiene, 3-butyl-1,3-octadiene, octadiene, and combinations of two or more thereof.
[0011] In one embodiment, the ethylenically unsaturated nitrile monomer may be one selected from the group consisting of acrylonitrile, methacrylonitrile, fumaronitrile, α-chloronitrile, α-cyanoethylacrylonitrile, and combinations of two or more thereof.
[0012] In one embodiment, the ethylenically unsaturated acid monomer may be one selected from the group consisting of acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, maleic anhydride, citraconic anhydride, styrenesulfonic acid, monobutyl fumarate, monobutyl maleate, mono-2-hydroxypropyl maleate, and combinations of two or more thereof.
[0013] In one embodiment, the ionic organic compound may be one selected from the group consisting of ethylenediaminetetraacetic acid (EDTA) or a sodium salt thereof, ethylene glycol tetraacetic acid (EGTA) or a sodium salt thereof, nitrilotriacetic acid (NTA) or a sodium salt thereof, iminodiacetic acid (IDA) or a sodium salt thereof, quinolinic acid (QNA) or a sodium salt thereof, and combinations of two or more thereof.
[0014] In one embodiment, the ionic inorganic compound is potassium sulfate (K2SO4), sodium carbonate (Na2CO3), sodium chloride (NaCl), potassium chloride (KCl), calcium chloride (CaCl2), magnesium chloride (MgCl2), sodium nitrate (NaNO3), potassium nitrate (KNO3), calcium nitrate (Ca(NO3)2), magnesium nitrate (Mg(NO3)2), sodium sulfate (Na2SO4), calcium sulfate (CaSO4), magnesium sulfate (MgSO4), sodium hydroxide (NaOH), potassium hydroxide (KOH), calcium hydroxide (Ca(OH)2), magnesium hydroxide (Mg(OH)2), sodium bicarbonate (NaHCO3), potassium bicarbonate (KHCO3), potassium carbonate (K2CO3), sodium bisulfite (NaHSO4), potassium bisulfite (KHSO4), sodium pyrophosphate (Na4P2O7). It may be one selected from the group consisting of potassium pyrophosphate (K4P2O7), trisodium phosphate (Na3PO4), tripotassium phosphate (K3PO4), sodium hydrogen phosphate (Na2HPO4), potassium hydrogen phosphate (K2HPO4), and a combination of two or more thereof.
[0015] In one embodiment, the composition may include 30 to 98 parts by weight of a conjugated diene monomer, 1 to 55 parts by weight of an ethylenically unsaturated nitrile monomer, and 0.001 to 20 parts by weight of an ethylenically unsaturated acid monomer.
[0016] In one embodiment, the composition may further comprise water, an emulsifier, a polymerization initiator, and a molecular weight modifier.
[0017] According to another aspect, a latex for dip molding is provided, which comprises a copolymer derived from the composition for latex polymerization.
[0018] According to another aspect, a dip-molded product manufactured from the above-described latex for dip molding is provided.
[0019] In one embodiment, the deep-molded product may be a surgical glove, a medical glove, a glove for processing agricultural and livestock products, an industrial glove, a condom, a cosmetic material, a catheter, or a healthcare-use molded product.
[0020] A latex polymerization composition according to one aspect of the present specification has high ionic conductivity, which can improve the stability of the polymer during polymerization of the latex, and accordingly, a latex for dip molding according to another aspect of the present specification can simultaneously satisfy the trade-off relationship of high solids content, large particle size, and low viscosity.
[0021] In addition, the deep-molded product according to another aspect of the present specification has excellent durability for actual use, and can be applied to various fields such as surgical gloves, medical gloves, gloves for processing agricultural and livestock products, industrial gloves, condoms, cosmetic materials, catheters, and healthcare-use molded products.
[0022] It should be understood that the effects of one aspect of this specification are not limited to the effects described above, but include all effects that can be inferred from the detailed description or claims of this specification.
[0023] Below, aspects of this specification will be described based on specific examples. However, the contents of this specification may be implemented in various different forms and are therefore not limited to the embodiments described herein.
[0024] Throughout the specification, when a part is said to be "connected" to another part, this includes not only "directly connected" but also "indirectly connected" with other elements intervening. Furthermore, when a part is said to "include" a component, this does not exclude other components, but rather implies that the other components may be included, unless otherwise specifically stated.
[0025] When a range of numerical values is stated herein, unless the specific range is otherwise specified, the values have the precision of the significant figures provided according to the standard rules in chemistry for significant figures. For example, the number 10 includes the range of 5.0 to 14.9, and the number 10.0 includes the range of 9.50 to 10.49.
[0026] Composition for latex polymerization
[0027] A latex polymerization composition according to one aspect of the present disclosure comprises a conjugated diene monomer, an ethylenically unsaturated nitrile monomer, an ethylenically unsaturated acid monomer, an ionic organic compound, and an ionic inorganic compound.
[0028] The above ionic organic compound and ionic inorganic compound can improve the stability of the latex by enhancing the ionic conductivity of the composition, and can form a large particle size copolymer of 1,000 Å or more. In addition, the latex including the copolymer derived from the composition can maintain low viscosity even at a high solid content of 50 wt% or more, thereby simultaneously satisfying the trade-off relationship of high solid content, large particle size, and low viscosity.
[0029] The weight ratio of the ionic inorganic compound to the ionic organic compound may be 4.7 or greater. For example, it may be 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, a range between two of these values, or a value greater than or equal to one of these values. If the weight ratio of the ionic inorganic compound to the ionic organic compound is less than the above range, the polymerization reaction rate may decrease, resulting in a lower final conversion rate, and as the amount of residual unreacted monomer increases, the mechanical properties and practical durability of a dip-molded product manufactured therefrom may rapidly deteriorate. Meanwhile, in the present invention, the higher the weight ratio of the ionic inorganic compound to the organic compound, the more advantageous it is for the mechanical properties and practical durability of the dip-molded product. Therefore, there is no particular limitation on the upper limit, but it may be limited to 5.9 or less in consideration of the possibility of spoilage during long-term storage of latex.
[0030] The above conjugated diene monomer may be one selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, 2-chloro-1,3-butadiene, 3-butyl-1,3-octadiene, octadiene, and combinations of two or more thereof, but is not limited thereto. In the copolymer of the latex for dip molding, the structure derived from the conjugated diene monomer can impart flexibility to the dip molded product.
[0031] The above ethylenically unsaturated nitrile monomer may be one selected from the group consisting of acrylonitrile, methacrylonitrile, fumaronitrile, α-chloronitrile, α-cyanoethylacrylonitrile, and combinations of two or more thereof, but is not limited thereto. In the copolymer of the latex for dip molding, the structure derived from the ethylenically unsaturated nitrile monomer can improve the strength and chemical resistance of the dip molded product.
[0032] The above ethylenically unsaturated acid monomer may be one selected from the group consisting of acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, maleic anhydride, citraconic anhydride, styrenesulfonic acid, monobutyl fumarate, monobutyl maleate, mono-2-hydroxypropyl maleate, and a combination of two or more thereof, but is not limited thereto. In the copolymer of the latex for dip molding, the structure derived from the above ethylenically unsaturated acid monomer can form a crosslinked structure to improve the mechanical properties of the dip molded product.
[0033] The above ionic organic compound and the above ionic inorganic compound can improve the stability of the copolymer undergoing polymerization during polymerization of the latex polymerization composition, and can suppress coagulation of the latex even after polymerization.
[0034] The above ionic organic compound may be one selected from the group consisting of ethylenediaminetetraacetic acid (EDTA) or a sodium salt thereof, ethylene glycol tetraacetic acid (EGTA) or a sodium salt thereof, nitrilotriacetic acid (NTA) or a sodium salt thereof, iminodiacetic acid (IDA) or a sodium salt thereof, quinolinic acid (QNA) or a sodium salt thereof, and a combination of two or more thereof, and may be, for example, ethylenediaminetetraacetic acid (EDTA), but is not limited thereto.
[0035] The above ionic inorganic compounds are potassium sulfate (K2SO4), sodium carbonate (Na2CO3), sodium chloride (NaCl), potassium chloride (KCl), calcium chloride (CaCl2), magnesium chloride (MgCl2), sodium nitrate (NaNO3), potassium nitrate (KNO3), calcium nitrate (Ca(NO3)2), magnesium nitrate (Mg(NO3)2), sodium sulfate (Na2SO4), calcium sulfate (CaSO4), magnesium sulfate (MgSO4), sodium hydroxide (NaOH), potassium hydroxide (KOH), calcium hydroxide (Ca(OH)2), magnesium hydroxide (Mg(OH)2), sodium bicarbonate (NaHCO3), potassium bicarbonate (KHCO3), potassium carbonate (K2CO3), sodium bisulfite (NaHSO4), potassium bisulfite (KHSO4), sodium pyrophosphate (Na4P2O7), It may be one selected from the group consisting of potassium pyrophosphate (K4P2O7), trisodium phosphate (Na3PO4), tripotassium phosphate (K3PO4), sodium hydrogen phosphate (Na2HPO4), potassium hydrogen phosphate (K2HPO4), and a combination of two or more thereof, and may be, for example, a combination of potassium sulfate and sodium carbonate, but is not limited thereto.
[0036] The above composition may include, but is not limited to, 30 to 98 parts by weight of a conjugated diene monomer, 1 to 55 parts by weight of an ethylenically unsaturated nitrile monomer, and 0.001 to 20 parts by weight of an ethylenically unsaturated acid monomer.
[0037] For example, the conjugated diene monomer content of the composition may be 30 parts by weight, 32 parts by weight, 34 parts by weight, 36 parts by weight, 38 parts by weight, 40 parts by weight, 42 parts by weight, 44 parts by weight, 46 parts by weight, 48 parts by weight, 50 parts by weight, 52 parts by weight, 54 parts by weight, 56 parts by weight, 58 parts by weight, 60 parts by weight, 62 parts by weight, 64 parts by weight, 66 parts by weight, 68 parts by weight, 70 parts by weight, 72 parts by weight, 74 parts by weight, 76 parts by weight, 78 parts by weight, 80 parts by weight, 82 parts by weight, 84 parts by weight, 86 parts by weight, 88 parts by weight, 90 parts by weight, 92 parts by weight, 94 parts by weight, 96 parts by weight, 98 parts by weight, or a range between any two of these values. If the conjugated diene monomer content is below the above range, the dip-molded product may be excessively cured, resulting in poor wearing comfort. If it exceeds the above range, the durability or chemical resistance of the dip-molded product may be reduced.
[0038] The content of the ethylenically unsaturated nitrile monomer of the above composition may be 1 part by weight, 2.5 parts by weight, 5 parts by weight, 7.5 parts by weight, 10 parts by weight, 12.5 parts by weight, 15 parts by weight, 17.5 parts by weight, 20 parts by weight, 22.5 parts by weight, 25 parts by weight, 27.5 parts by weight, 30 parts by weight, 32.5 parts by weight, 35 parts by weight, 37.5 parts by weight, 40 parts by weight, 42.5 parts by weight, 45 parts by weight, 47.5 parts by weight, 50 parts by weight, 52.5 parts by weight, 55 parts by weight, or a range between any two of these values. If the content of the ethylenically unsaturated nitrile monomer is less than the above range, the chemical resistance or mechanical strength of the dip-molded product may be lowered, and if it exceeds the above range, the elongation of the dip-molded product may be lowered, thereby lowering the usability.
[0039] The content of ethylenically unsaturated acid monomer of the above composition is 0.001 parts by weight, 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight, 10 parts by weight, 10.5 parts by weight, 11 parts by weight, 11.5 parts by weight, 12 parts by weight, 12.5 parts by weight, 13 parts by weight, 13.5 parts by weight, 14 parts by weight, 14.5 parts by weight, 15 parts by weight, 15.5 parts by weight, 16 parts by weight, 16.5 parts by weight, 17 parts by weight, It may be 17.5 parts by weight, 18 parts by weight, 18.5 parts by weight, 19 parts by weight, 19.5 parts by weight, 20 parts by weight, or a range between any two of these values. If the ethylenically unsaturated acid monomer content is below the above range, the tensile strength of the dip-molded product may be reduced, and if it exceeds the above range, the dip-molded product may be excessively hardened, resulting in poor wearing comfort.
[0040] The conjugated diene monomer may include isoprene. For example, the conjugated diene monomer may include isoprene and one or more conjugated diene monomers other than isoprene.
[0041] The conjugated diene monomer may include, but is not limited to, 29 to 97 parts by weight of isoprene and 1 to 50 parts by weight of a conjugated diene monomer other than isoprene. For example, the content of the isoprene may be 29 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight, 95 parts by weight, 97 parts by weight, or a range between any two of these values. If the content of the isoprene is less than the above range, the durability of a dip-molded product manufactured from the composition may be reduced.
[0042] The weight ratio of the isoprene to the ethylenically unsaturated nitrile monomer may be 1.0 to 3.5. If the weight ratio of the isoprene to the ethylenically unsaturated nitrile monomer is outside the above range, the durability of the dip-molded product manufactured from the composition may be reduced.
[0043] The weight ratio of the ethylenically unsaturated acid monomer to the ethylenically unsaturated nitrile monomer may be 0.1 to 0.4. If the weight ratio of the ethylenically unsaturated acid monomer to the ethylenically unsaturated nitrile monomer is outside the above range, the durability of a dip-molded product manufactured from the composition may be reduced.
[0044] In this specification, the “total monomers” means the sum of the conjugated diene monomer, the ethylenically unsaturated nitrile monomer, and the ethylenically unsaturated acid monomer, but the latex polymerization composition may further include a polymerizable monomer other than the conjugated diene monomer, the ethylenically unsaturated nitrile monomer, and the ethylenically unsaturated acid monomer described above, and in this case, the “total monomers” further includes the polymerizable monomer.
[0045] The total content of the ionic organic compound and the ionic inorganic compound may vary depending on the monomer composition ratio and the type of ionic compound. The total content of the ionic organic compound and the ionic inorganic compound may be 0.1 to 0.6 parts by weight based on 100 parts by weight of the total monomers. For example, 0.1 part by weight, 0.11 part by weight, 0.12 part by weight, 0.13 part by weight, 0.14 part by weight, 0.15 part by weight, 0.16 part by weight, 0.17 part by weight, 0.18 part by weight, 0.19 part by weight, 0.2 part by weight, 0.21 part by weight, 0.22 part by weight, 0.23 part by weight, 0.24 part by weight, 0.25 part by weight, 0.26 part by weight, 0.27 part by weight, 0.28 part by weight, 0.29 part by weight, 0.3 part by weight, 0.31 part by weight, 0.32 part by weight, 0.33 part by weight, 0.34 part by weight, 0.35 part by weight, 0.36 part by weight, 0.37 part by weight, 0.38 part by weight, 0.39 part by weight, 0.4 parts by weight, 0.41 parts by weight, 0.42 parts by weight, 0.43 parts by weight, 0.44 parts by weight, 0.45 parts by weight, 0.46 parts by weight, 0.47 parts by weight, 0.48 parts by weight, 0.49 parts by weight, 0.5 parts by weight, 0.51 parts by weight, 0.52 parts by weight, 0.53 parts by weight, 0.54 parts by weight, 0.55 parts by weight, 0.56 parts by weight, 0.57 parts by weight, 0.58 parts by weight, 0.59 parts by weight, 0.6 parts by weight, or a range between any two of these values. If the total content of the ionic organic compound and the ionic inorganic compound is less than the above range, the ionic conductivity of the composition may decrease or the stability of the latex may decrease, and due to the high polymerization reaction rate, the particle size of the latex may decrease and the viscosity may increase, which may make it difficult to store the product and control the heat of reaction. If the total content of ionic organic compounds and ionic inorganic compounds exceeds the above range, the polymerization reaction rate may decrease, resulting in a lower final conversion rate, and the mechanical properties and practical durability of the dip-molded product manufactured therefrom may deteriorate.
[0046] The ionic conductivity of the above composition may be 250 μs / cm or more. For example, 250 ㎲ / cm, 255 ㎲ / cm, 260 ㎲ / cm, 265 ㎲ / cm, 270 ㎲ / cm, 275 ㎲ / cm, 280 ㎲ / cm, 285 ㎲ / cm, 290 ㎲ / cm, 295 ㎲ / cm, 300 ㎲ / cm, 305 ㎲ / cm, 310 ㎲ / cm, 315 ㎲ / cm, 320 ㎲ / cm, 325 ㎲ / cm, 330 ㎲ / cm, 335 ㎲ / cm, 340 ㎲ / cm, 345 ㎲ / cm, 350 ㎲ / cm, 355 ㎲ / cm, 360 ㎲ / cm, 365 ㎲ / cm, 370 ㎲ / cm, 375 ㎲ / cm, 380 ㎲ / cm, 385 ㎲ / cm, 390 ㎲ / cm, 395 ㎲ / cm, 400 ㎲ / cm, a range between two of these values, or a value greater than or equal to one of these values. If the ionic conductivity of the composition is less than the above range, the stability of the polymerized latex may be reduced, and the viscosity may rapidly increase when the solid content is concentrated.
[0047] The ionic conductivity of the above composition may be, but is not limited to, 10 ms / cm or less, 5 ms / cm or less, or 1 ms / cm or less. If the ionic conductivity of the above composition is excessively high, components unnecessary for polymerization may increase, thereby reducing the stability of the latex.
[0048] The composition may further include water, an emulsifier, a polymerization initiator, and a molecular weight regulator.
[0049] The content of the water is 75 to 150 parts by weight based on 100 parts by weight of the total monomer, for example, 75 parts by weight, 77.5 parts by weight, 80 parts by weight, 82.5 parts by weight, 85 parts by weight, 87.5 parts by weight, 90 parts by weight, 92.5 parts by weight, 95 parts by weight, 97.5 parts by weight, 100 parts by weight, 102.5 parts by weight, 105 parts by weight, 107.5 parts by weight, 110 parts by weight, 112.5 parts by weight, 115 parts by weight, 117.5 parts by weight, 120 parts by weight, 122.5 parts by weight, 125 parts by weight, 127.5 parts by weight, 130 parts by weight, 132.5 parts by weight, 135 parts by weight, 137.5 parts by weight, 140 parts by weight, The water content may be 142.5 parts by weight, 145 parts by weight, 147.5 parts by weight, 150 parts by weight, or a range between any two of these values. If the water content is less than the above range, the viscosity may increase excessively during polymerization, making it difficult to manufacture a molded product, and if it exceeds the above range, the solids content may decrease excessively. The water may have an ionic conductivity of 5 μS / cm or less, 2.5 μS / cm or less, or 1 μS / cm or less. For example, the water may be ion-exchanged water, ultrapure water, or purified water. If water with high ionic conductivity is used, impurities that adversely affect the polymerization stability or the stability of the latex may be included.
[0050] The above emulsifier may be an anionic surfactant, a nonionic surfactant, a cationic surfactant, or an amphoteric surfactant. For example, as the anionic surfactant, one or more selected from the group consisting of alkylbenzene sulfonates, aliphatic sulfonates, sulfuric acid esters of higher alcohols, α-olefin sulfonates, and alkyl ether sulfuric acid esters may be used, but is not limited thereto. The above emulsifier may be used in an amount of 0.8 to 8 parts by weight based on 100 parts by weight of the total monomer.
[0051] The polymerization initiator may be a radical initiator. The radical initiator may be, for example, an inorganic peroxide selected from the group consisting of sodium persulfate, potassium persulfate, ammonium persulfate, potassium perphosphate, and hydrogen peroxide; an organic peroxide selected from the group consisting of t-butyl peroxide, cumene hydroperoxide, p-menthane hydroperoxide, di-t-butyl peroxide, t-butylcumyl peroxide, acetyl peroxide, isobutyl peroxide, octanoyl peroxide, dibenzoyl peroxide, 3,5,5-trimethylhexanol peroxide, and t-butylperoxyisobutyrate; It may be at least one azo-based initiator selected from the group consisting of azobisisobutyronitrile, azobis-2,4-dimethylvaleronitrile, azobiscyclohexanecarbonitrile, and azobisisobutyrate(methylbutyrate), but is not limited thereto. The polymerization initiator may be used in an amount of 0.01 to 1.5 parts by weight based on 100 parts by weight of the total monomers.
[0052] The above molecular weight regulator may be, but is not limited to, mercaptans such as α-methylstyrene dimer, t-dodecyl mercaptan, n-dodecyl mercaptan, and octyl mercaptan; halogenated hydrocarbons such as carbon tetrachloride, methylene chloride, and methylene bromide; and sulfur-containing compounds such as tetraethylthiuram disulfide, dipentamethylenethiuram disulfide, and diisopropylxantogen disulfide. The content of the above molecular weight regulator may be 0.1 to 1 part by weight based on 100 parts by weight of the total monomer. For example, it may be 0.1 parts by weight, 0.15 parts by weight, 0.2 parts by weight, 0.25 parts by weight, 0.3 parts by weight, 0.35 parts by weight, 0.4 parts by weight, 0.45 parts by weight, 0.5 parts by weight, 0.55 parts by weight, 0.6 parts by weight, 0.65 parts by weight, 0.7 parts by weight, 0.75 parts by weight, 0.8 parts by weight, 0.85 parts by weight, 0.9 parts by weight, 0.95 parts by weight, 1 part by weight, or a range between any two of these values. If the content of the molecular weight modifier is less than the above range, a gel may be formed, which may lower the latex stability, and if it exceeds the above range, the tensile strength may be poor, the stress retention rate may be lowered, and the durability for actual use may also be lowered.
[0053] Latex for deep molding
[0054] According to another aspect of the present disclosure, a latex for dip molding may comprise a copolymer derived from the aforementioned latex polymerization composition.
[0055] The average particle diameter of the above copolymer may be 1,000 to 3,000 Å. For example, 1,000 Å, 1,050 Å, 1,100 Å, 1,150 Å, 1,200 Å, 1,250 Å, 1,300 Å, 1,350 Å, 1,400 Å, 1,450 Å, 1,500 Å, 1,550 Å, 1,600 Å, 1,650 Å, 1,700 Å, 1,750 Å, 1,800 Å, 1,850 Å, 1,900 Å, 1,950 Å, 2,000 Å, 2,050 Å, 2,100 Å, 2,150 Å, 2,200 Å, 2,250 Å, 2,300 Å, 2,350 Å, 2,400 Å, 2,450 Å, 2,500 Å, 2,550 Å, 2,600 Å, 2,650 Å, 2,700 Å, 2,750 Å, 2,800 Å, 2,850 Å, 2,900 Å, 2,950 Å, 3,000 Å, or a range between any two of these values. The latex for dip molding can be manufactured by polymerizing a composition including an ionic organic compound and an ionic inorganic compound, thereby minimizing a decrease in stability and increasing the particle size of the copolymer. In addition, the latex can have a low oligomer content and thus have better stability.
[0056] The magnitude (absolute value) of the zeta potential of the latex for the above-mentioned dip molding may be 60 mV or more, 62.5 mV or more, 65 mV or more, 67.5 mV or more, or 70 mV or more. The latex satisfying these conditions has excellent stability and can suppress viscosity increase even when concentrated to a high solids content of 50 wt% or more.
[0057] The viscosity of the latex for dip molding at 25°C is 50 to 2,500 cps, for example, 50 cps, 75 cps, 100 cps, 125 cps, 150 cps, 175 cps, 200 cps, 225 cps, 250 cps, 275 cps, 300 cps, 325 cps, 350 cps. cps, 375 cps, 400 cps, 425 cps, 450 cps, 475 cps, 500 cps, 525 cps, 550 cps, 575 cps, 600 cps, 625 cps, 650 cps, 675 cps, 700 cps, 725 cps, 750 cps, 775 cps, 800 cps, 825 cps, 850 cps, 875 cps, 900 cps, 925 cps, 950 cps, 975 cps, 1,000 cps, 1,100 cps, 1,200 cps, 1,300 cps, 1,400 cps, 1,500 cps, 1,600 cps, 1,700 cps, 1,800 cps, 1,900 cps, 2,000 cps, 2,100 cps, 2,200 cps, 2,300 cps, 2,400 cps, 2,500 cps, or a range between any two of these values. Latexes having a viscosity outside the above range may be practically impossible to manufacture or may be difficult to dip mold.
[0058] The solids content of the latex for the above-mentioned dip molding may be in the range of 50 to 65 wt%, for example, 50 wt%, 52.5 wt%, 55 wt%, 57.5 wt%, 60 wt%, 62.5 wt%, 65 wt%, or a range between any two of these values. If the solids content is outside the above range, the effect of the stability improvement described above may be unnecessary, or coagulation of the latex may occur.
[0059] The characteristics of the latex for dip molding may be measured at a pH of 8.0 to 10.0, for example, pH 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9.0, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9, 10.0. When the pH of the latex is adjusted using an additive, the solids content and average particle size may change, but the latex for dip molding can simultaneously satisfy the above-mentioned average particle size, solids content and viscosity requirements in the above pH range.
[0060] The above-mentioned latex for dip molding may further include one or more additives selected from the group consisting of a chelating agent, a dispersing agent, a pH regulator, a deoxidizing agent, a particle size regulator, an anti-aging agent, and an oxygen scavenger. These additives may be any composition known in the art, and may be added before or after the polymerization of the copolymer.
[0061] The above-mentioned latex for dip molding satisfies low viscosity, high solids content, and large particle size simultaneously, thereby ensuring excellent latex stability. Therefore, it can prevent quality degradation of dip molded products even when subjected to external impact or during long-term storage.
[0062] Method for manufacturing latex for deep molding
[0063] A method for producing latex for dip molding according to another aspect of the present specification may include the steps of (a) preparing a monomer mixture including a conjugated diene monomer, an ethylenically unsaturated nitrile monomer, and an ethylenically unsaturated acid monomer; (b) adding an ionic organic compound, an ionic inorganic compound, an emulsifier, and water to the monomer mixture; and (c) adding a polymerization initiator to produce latex for dip molding.
[0064] The weight ratio of the ionic inorganic compound to the ionic organic compound introduced in the above step (b) may be 4.7 or more.
[0065] The above step (a) is a step of preparing a monomer mixture including a conjugated diene monomer, an ethylenically unsaturated nitrile monomer, and an ethylenically unsaturated acid monomer, which are monomers constituting a carboxylic acid-modified nitrile copolymer, and can be performed under a nitrogen atmosphere.
[0066] The above step (b) is a step of preparing the aforementioned latex polymerization composition by introducing an ionic compound. A molecular weight modifier may be further introduced in the above step (b).
[0067] The polymerization in step (c) above can be performed at 10 to 90°C, for example, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C or a temperature between any two of these temperatures, but is not limited thereto, and the polymerization temperature can be adjusted according to the target conversion rate.
[0068] The polymerization in step (c) above can be performed for 2 to 24 hours, for example, but not limited to, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, or a time period between any two of these.
[0069] The above step (c) may further include a step of stopping polymerization by introducing a polymerization terminator.
[0070] The polymerization terminator may be one selected from the group consisting of hydroxyl amine, hydroxyl amine sulfate, diethyl hydroxyl amine, hydroxyl amine sulfonic acid and alkali metal ions thereof, sodium dimethyldithiocarbamate, hydroquinone derivatives, aromatic hydroxyl dithiocarboxylic acids such as hydroxyl diethyl benzene dithiocarboxylic acid and hydroxyl dibutyl benzene dithiocarboxylic acid, and combinations of two or more thereof. The content of the polymerization terminator may be 0.02 to 1.5 parts by weight based on 100 parts by weight of the monomer mixture.
[0071] In the above step (c), the final conversion rate of the polymerization reaction may be 92% or higher. For example, it may be 92% or higher, 93% or higher, 94% or higher, 95% or higher, 96% or higher, 97% or higher, or 98% or higher, but is not limited thereto. If the conversion rate is lower than the above range, the amount of residual unreacted monomer increases, which may deteriorate the mechanical properties and practical durability of the dip-molded product manufactured therefrom.
[0072] Other raw materials, contents, etc. used in the above manufacturing method are as described above.
[0073] Deep molded products
[0074] According to another aspect of the present disclosure, a dip molded article may be manufactured from the aforementioned dip molding latex.
[0075] The above-mentioned dip-molded product may be manufactured by adding 1 to 2 parts by weight of sulfur, 0.1 to 1 part by weight of zinc oxide, and 0.3 to 1.5 parts by weight of a vulcanization accelerator to 100 parts by weight of the above-mentioned dip-molding latex, and then performing dip-molding, but is not limited thereto.
[0076] The sulfur can react with a structure derived from the conjugated diene monomer to form a crosslinking structure. When the ionic organic compound and the ionic inorganic compound are added in the above-mentioned weight ratio range, shrinkage of the molded product due to syneresis during vulcanization can be suppressed. The content of the sulfur can be, for example, 1 part by weight, 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, 1.6 parts by weight, 1.7 parts by weight, 1.8 parts by weight, 1.9 parts by weight, 2 parts by weight, or a range between any two of these values. If the content of sulfur is less than the above range, mechanical properties such as tensile strength and durability in actual use may deteriorate, and if it exceeds the above range, it may cause an allergic reaction in the user.
[0077] The zinc oxide can form an ionic bond with a structure derived from the ethylenic unsaturated acid to form a cross-linked structure. In addition, by adding an ionic organic compound and an ionic inorganic compound in the weight ratio range described above, the ionic bond strength can be improved, thereby enhancing durability. The content of the zinc oxide can be, for example, 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, or a range between any two of these values. If the content of the zinc oxide is less than the above range, the durability in actual use may be reduced, and if it exceeds the above range, the tensile strength may be reduced.
[0078] The above-mentioned dip-molded product may be a product that has been dip-molded by adjusting the solid content by adding an aqueous potassium hydroxide solution to the dip-molding latex, but is not limited thereto.
[0079] The tensile strength of the above-mentioned deep-molded product may be, but is not limited to, 3 MPa or more, 5 MPa or more, 7 MPa or more, 9 MPa or more, 11 MPa or more, 13 MPa or more, 15 MPa or more, 20 MPa or more, 25 MPa or more, 30 MPa or more, or 35 MPa or more. The higher the tensile strength, the better the durability during storage, but other mechanical properties such as elongation may decrease.
[0080] The elongation of the above-mentioned deep-molded product may be, but is not limited to, 600% or more, 650% or more, 700% or more, 750% or more, 800% or more, 850% or more, or 900% or more. A higher elongation improves wearability, but may be a trade-off with other mechanical properties.
[0081] The durability test results of the above-mentioned dip-molded product according to the durability test method below can be 60 minutes or more, indicating high quality with excellent durability for actual use. For example, the durability test results of the above-mentioned dip-molded product can be 60 minutes or more, 90 minutes or more, 120 minutes or more, 150 minutes or more, 180 minutes or more, 210 minutes or more, or 240 minutes or more.
[0082] [Durability Test Method]
[0083] A dip-molded product having a width of 30 mm, a length of 135 mm, and a thickness of 0.06 to 0.08 mm was immersed in a pH 4.0 to 4.3 solution at 35°C, stretched by 20% in the longitudinal direction, and the molded product was stretched to a longitudinal elongation of 50% for 10 seconds, fixed for 2 seconds, and then relaxed to a longitudinal elongation of 20% for 10 seconds. This process was repeated, and the time until the molded product broke was measured.
[0084] The above durability test method checks whether a specimen is damaged by repeating stretching and relaxation in a solution of 35°C and pH 4.0 to 4.3, which is similar to the skin and body fluids that are likely to come into contact with the dip-molded product during actual use. For example, if the above-mentioned molded product is a glove, the durability of the dip-molded product under actual use conditions can be measured by simulating a situation in which the molded product repeats stretching and relaxation according to the movement of the fingers.
[0085] The above-mentioned deep-molded product may be, but is not limited to, surgical gloves, medical gloves, gloves for agricultural and livestock processing, industrial gloves, condoms, cosmetic materials, catheters, or healthcare-use molded products. For example, the above-mentioned deep-molded product may be surgical gloves, other medical gloves, industrial gloves such as gloves for handling chemicals, or cosmetic materials such as puffs.
[0086] Hereinafter, the embodiments of this specification will be described in more detail. However, the experimental results below represent only representative experimental results among the above embodiments, and the scope and content of this specification cannot be interpreted as being reduced or limited by the embodiments, etc. The effects of each of the various implementation examples of this specification that are not explicitly presented below will be specifically described in the relevant sections.
[0087] Examples and Comparative Examples
[0088] A 1 L high-pressure reactor equipped with a stirrer, a thermometer, a cooler, and a nitrogen gas inlet, and configured to continuously input each component such as a monomer, an emulsifier, and a polymerization initiator, was prepared. Ion-exchanged water having a conductivity of 1 μS / cm or less was prepared. After the reactor was replaced with nitrogen, a monomer mixture containing 40 wt% of isoprene (IP), 25 wt% of 1,3-butadiene (BD), 30 wt% of acrylonitrile (AN), and 5 wt% of methacrylic acid (MAA) based on the total weight of the monomer mixture was input. Thereafter, for 100 parts by weight of the monomer mixture, ethylenediaminetetraacetic acid (EDTA) as an ionic organic compound, potassium sulfate (K2SO4) and sodium carbonate (Na2CO3) as ionic inorganic compounds, 0.5 parts by weight of t-dodecyl mercaptan (TDDM) as a molecular weight regulator, 2 parts by weight of sodium alkylbenzenesulfonate as an emulsifier, and 120 parts by weight of ion-exchanged water were introduced into the reactor to prepare a composition for latex polymerization. After the temperature of the reactor was raised to about 40°C, 0.3 parts by weight of potassium persulfate as a polymerization initiator was introduced. After polymerization for 12 hours, 0.9 parts by weight of sodium hydroxide was introduced to stop the polymerization reaction. Afterwards, unreacted monomers, etc. were removed through a deodorizing process, and ammonia water, antioxidant, antifoaming agent, etc. were added to obtain a carboxylic acid-modified nitrile copolymer latex having a pH of 8.5.
[0089] The contents of the ionic compounds used in each example and comparative example and the weight ratio therebetween are shown in Table 1 below.
[0090] Classification (parts by weight) A. Ionic organic compounds B. Ionic inorganic compounds Weight ratio (B / A) EDTAK2SO4Na2CO3 Total content Example 10.078 0.195 0.195 0.390 5.000 Example 20.05 50.136 50.136 50.27 35.000 Example 30.03 10.078 0.078 0.15 65.000 Comparative example 10.11 20.26 30.26 30.5 264.696 Comparative example 20.14 60.30 30.30 30.60 64.151 Comparative example 30000-* Weight ratio (B / A) = Total content of ionic inorganic compounds / Content of ionic organic compounds
[0091] Experimental Example 1
[0092] The final conversion rate, initial conversion rate (after 2 hours of polymerization), average particle size, ionic conductivity, solid content, viscosity at 25°C, and zeta potential of the carboxylic acid-modified nitrile copolymer latex obtained in the above examples and comparative examples were measured and are shown in Table 2 below.
[0093] -Average particle size (Å): Measured by dynamic laser light scattering using Nanotrac 150.
[0094] -Ionic Conductivity (μS / cm): Ionic conductivity was determined by measuring resistance using an electrochemical impedance spectroscopy (EIS) using a two-electrode method and then using the Nyquist plot method. Resistance was measured under conditions of a frequency of 60 Hz to 1 kHz, a current of 10.0 mV, and a voltage range of ±10 V. Ionic conductivity was measured after correction with a standard solution within the expected range. Graphite electrodes were used as electrodes. Ionic conductivity values were corrected based on a temperature of 25°C.
[0095] -25℃ Viscosity (cps): Measured using a Brookfield viscometer at spindle speeds of 62 and 100 rpm.
[0096] -Zeta potential (mV): Zeta potential at 25℃ was measured using a Malvern Zetasizer device.
[0097] ClassificationFinal conversion rate (%)Initial conversion rate (%)Average particle size (Å)Ionic conductivity (㎲ / cm)Solid content (wt%)25℃Viscosity (cps)Zeta potential (mV)Example 196.228.01,230286.954.7290-75.9Example 297.831.01,250282.350.2210-71.1Example 398.335.01,180279.053.3280-70.3Comparative example 191.017.615,80289.354.9290-71.9Comparative example 288.011.51,620291.953.6270-74.2Comparative example 399.148.0900239.255.6>10,000-54.0
[0098] Referring to Table 2 above, all of Examples 1 to 3 exhibited high conversion rates, and compared to the latex of Comparative Example 3 without the addition of an ionic compound, the ionic conductivity was high, and the zeta potential, which indicates the electrical stability of the latex particles, was measured to be large. In addition, the latexes of Examples 1 to 3 exhibited low viscosity while achieving a large particle size of 1,000 Å or more and a high solid content of 50 wt% or more.
[0099] In the case of Comparative Examples 1 and 2, the ionic conductivity was high compared to the latex of Comparative Example 3 without the addition of an ionic compound, the zeta potential was measured to be large, and the properties similar to those of Examples 1 to 3 were exhibited in that the large particle size of 1,000 Å or more and the high solid content of 50 wt% or more were achieved while exhibiting low viscosity. However, the reaction rate was slow, so the initial conversion rate was lower than that of the examples, and it was confirmed that a relatively large amount of unreacted monomer was present even after the polymerization was completed due to the low final conversion rate.
[0100] The latex of Comparative Example 3, which did not contain any ionic compounds, was measured to have a relatively small zeta potential, and due to its low stability, it was difficult to simultaneously achieve large particle size, high solids content, and low viscosity. In addition, the reaction rate was fast, resulting in small particle size and high viscosity, and there were difficulties in product storage and reaction heat control. In particular, the latex of Comparative Example 3, which had small particle size, had a problem in that its viscosity increased rapidly when the solids content was increased through concentration.
[0101] Manufacturing example
[0102] For each 100 parts by weight of the carboxylic acid-modified nitrile copolymer latex manufactured according to the above examples and comparative examples, 1.8 parts by weight of sulfur (S), 0.7 parts by weight of zinc oxide (ZnO), and 1.2 parts by weight of zinc dibutyldithiocarbamate (ZDBC) as a vulcanization accelerator were added. Thereafter, a 4% aqueous potassium hydroxide solution and double-distilled water were added to manufacture a latex composition for dip molding having a solids concentration of 20% and a pH of 10.0.
[0103] Experimental Example 2
[0104] Rectangular specimens measuring 30 mm in width, 135 mm in length, and 0.072 to 0.074 mm in thickness were manufactured using each of the latex compositions for deep molding manufactured according to the above manufacturing examples, and the durability of the specimens was evaluated. The results are shown in Table 3 below.
[0105] - Durability: A pH 4 solution was prepared using citric acid and maintained at 35°C. Rectangular specimens were placed in the solution while being elongated by 20% in the longitudinal direction. The specimens were stretched to an elongation of 50% for 10 seconds, fixed for 2 seconds, and then relaxed to an elongation of 20% for 10 seconds. This process was repeated, and the time until the specimens broke was measured.
[0106] Specimen thickness (mm) Durability Example 10.0724 hours or more Example 20.0734 hours or more Example 30.0734 hours or more Comparative Example 10.0740.9 hours Comparative Example 20.0740.7 hours Comparative Example 30.0733 hours
[0107] Referring to Table 3 above, the specimens manufactured using the latex of Examples 1 to 3 exhibited superior durability in actual use compared to the specimens manufactured using the latex of Comparative Examples 1 to 3. In particular, the specimens manufactured using the latex of Comparative Examples 1 or 2 were broken within 1 hour, confirming that their durability in actual use was inadequate.
[0108] The description of this specification above is for illustrative purposes only, and those skilled in the art will readily appreciate that aspects of this specification can be readily modified into other specific forms without altering the technical concepts or essential features described herein. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single entity may be implemented in a distributed manner, and similarly, components described as distributed may be implemented in a combined manner.
[0109] The scope of this specification is indicated by the claims set forth below, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included within the scope of this specification.
Claims
1. Containing a conjugated diene monomer, an ethylenically unsaturated nitrile monomer, an ethylenically unsaturated acid monomer, an ionic organic compound, and an ionic inorganic compound, A latex polymerization composition, wherein the weight ratio of the ionic inorganic compound to the ionic organic compound is 4.7 or more.
2. In paragraph 1, A composition for latex polymerization, wherein the conjugated diene monomer is one selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, 2-chloro-1,3-butadiene, 3-butyl-1,3-octadiene, octadiene, and combinations of two or more thereof.
3. In paragraph 1, A composition for latex polymerization, wherein the ethylenically unsaturated nitrile monomer is one selected from the group consisting of acrylonitrile, methacrylonitrile, fumaronitrile, α-chloronitrile, α-cyanoethylacrylonitrile, and combinations of two or more thereof.
4. In paragraph 1, A composition for latex polymerization, wherein the ethylenically unsaturated acid monomer is one selected from the group consisting of acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, maleic anhydride, citraconic anhydride, styrenesulfonic acid, monobutyl fumarate, monobutyl maleate, mono-2-hydroxypropyl maleate, and combinations of two or more thereof.
5. In paragraph 1, A composition for latex polymerization, wherein the ionic organic compound is one selected from the group consisting of ethylenediaminetetraacetic acid (EDTA) or a sodium salt thereof, ethylene glycol tetraacetic acid (EGTA) or a sodium salt thereof, nitrilotriacetic acid (NTA) or a sodium salt thereof, iminodiacetic acid (IDA) or a sodium salt thereof, quinolinic acid (QNA) or a sodium salt thereof, and a combination of two or more thereof.
6. In paragraph 1, The above ionic inorganic compounds are potassium sulfate (K2SO4), sodium carbonate (Na2CO3), sodium chloride (NaCl), potassium chloride (KCl), calcium chloride (CaCl2), magnesium chloride (MgCl2), sodium nitrate (NaNO3), potassium nitrate (KNO3), calcium nitrate (Ca(NO3)2), magnesium nitrate (Mg(NO3)2), sodium sulfate (Na2SO4), calcium sulfate (CaSO4), magnesium sulfate (MgSO4), sodium hydroxide (NaOH), potassium hydroxide (KOH), calcium hydroxide (Ca(OH)2), magnesium hydroxide (Mg(OH)2), sodium bicarbonate (NaHCO3), potassium bicarbonate (KHCO3), potassium carbonate (K2CO3), sodium bisulfite (NaHSO4), potassium bisulfite (KHSO4), sodium pyrophosphate (Na4P2O7), A composition for latex polymerization, wherein the composition is one selected from the group consisting of potassium pyrophosphate (K4P2O7), trisodium phosphate (Na3PO4), tripotassium phosphate (K3PO4), sodium hydrogen phosphate (Na2HPO4), potassium hydrogen phosphate (K2HPO4), and combinations of two or more thereof.
7. In paragraph 1, The composition is a latex polymerization composition comprising 30 to 98 parts by weight of a conjugated diene monomer, 1 to 55 parts by weight of an ethylenically unsaturated nitrile monomer, and 0.001 to 20 parts by weight of an ethylenically unsaturated acid monomer.
8. In paragraph 1, A composition for latex polymerization, wherein the composition further comprises water, an emulsifier, a polymerization initiator, and a molecular weight regulator.
9. Latex for dip molding, comprising a copolymer derived from the latex polymerization composition of paragraph 1.
10. A deep-molded product manufactured from the latex for deep molding of Article 9.