Non-oriented electrical steel sheet, core, and rotary electric machine

MYPI2025005637A0Undetermined Publication Date: 2024-10-05NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005637
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-05
Filing Date
2024-04-05
Publication Date
2024-10-05

AI Technical Summary

Technical Problem

Existing non-oriented electrical steel sheets face challenges in achieving low core loss and high magnetic flux density while maintaining plate thickness, with previous methods increasing manufacturing load and exhibiting stress sensitivity, and insufficient magnetic properties in the ±45° direction.

Method used

A non-oriented electrical steel sheet with a specific chemical composition and texture, featuring a {411}<011> orientation, is developed, which includes a higher temperature increase rate during intermediate annealing and final annealing at a higher temperature, resulting in improved magnetic properties and reduced stress sensitivity.

Benefits of technology

The solution achieves low iron loss and high magnetic flux density in the ±45° direction, reducing stress sensitivity and manufacturing costs, making it suitable for high-frequency applications in drive motors and hybrid vehicles.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

ABSTRACT NON-ORIENTED ELECTRICAL STEEL SHEET, CORE, AND ROTARY ELECTRIC MACHINE The non-oriented electrical steel sheet includes, as a chemical composition, in terms of mass%, 0.0100% or less of C, 1.50 to 4.00% of Si, 0.0001 to 1.00% of sol.Al, 0.0100% or less of S, 0.0100% or less of N, and 2.50 to 5.00% in total of one or more selected from the group consisting of Mn, Ni, and Cu, wherein, in terms of mass%, when [Mn] is defined as the Mn content, [Ni] is defined as the Ni content, [Cu] is defined as the Cu content, [Si] is defined as the Si content, [sol.Al] is defined as the sol.Al content, and [P] is defined as the P content, (2 × [Mn] + 2.5 × [Ni] + [Cu]) - ([Si] + 2 × [sol.Al] + 4 × [P]) ≥ 1.50% is satisfied; has A411-011 of 15.0% or more; has a B50D of 1.70 T or more; and has a W10D / 400D of 10.4 W / kg or less.
Need to check novelty before this filing date? Find Prior Art

Description

Non-oriented electrical steel sheets, cores, and rotating electrical machines

[0001] This application claims priority to Japanese Patent Application No. 2023-061313, filed on April 5, 2023, the contents of which are incorporated herein by reference.

[0002] Electrical steel sheets are used as core materials for electrical equipment. Examples of electrical equipment include drive motors installed in automobiles, compressor motors for air conditioners and refrigerators, and even household and industrial generators. These electrical equipment require high energy efficiency, compactness, and high output. Therefore, electrical steel sheets used as cores of electrical equipment require low iron loss and high magnetic flux density. Iron loss can be reduced by thinning the sheet thickness. However, thinning the sheet thickness reduces motor production efficiency, so a method for reducing iron loss while maintaining the sheet thickness has been required. To address this issue, texture control is one solution to achieving low iron loss and high magnetic flux density. Previously, techniques have been proposed to develop a texture (α-fiber) with an easy axis of magnetization within the steel sheet plane, which is advantageous for improving magnetic properties and can be relatively easily enriched by hot rolling and cold rolling, which are essential processes in steel sheet manufacturing. Specifically, a structure is formed in which the <110> direction is approximately parallel to the rolling direction (RD).

[0003] For example, Patent Document 1 describes that the steel sheet is cooled to 250°C or less at a cooling rate of 200°C / sec or more within 3 seconds after hot rolling, that no annealing is performed between hot rolling and cold rolling, and that the cumulative reduction in cold rolling is 88% or more. Patent Document 1 shows that this method enables the production of an electrical steel sheet in which grains are concentrated in the {100}<011> orientation on the steel sheet surface.

[0004] On the other hand, a technique for developing the {411} orientation, which is rotated 20° from the {100} orientation, has also been proposed in order to improve magnetic properties. Patent Documents 2 to 8 all disclose techniques for developing the {411} orientation, and describe optimizing the grain size in a hot-rolled sheet and strengthening the α-fiber in the texture of the hot-rolled sheet.

[0005] Specifically, Patent Document 2 describes that a hot-rolled sheet in which the concentration of the {211} orientation is higher than the concentration of the {411} orientation is cold-rolled to a cumulative reduction ratio of 80% or more, and that this enables the production of an electrical steel sheet in which the {411} orientation is concentrated on the steel sheet surface.

[0006] Furthermore, Patent Documents 3 and 4 describe that the slab heating temperature is 700°C or higher and 1150°C or lower, the start temperature of finish rolling is 650°C or higher and 850°C or lower, the end temperature of finish rolling is 550°C or higher and 800°C or lower, and further, the cumulative reduction in cold rolling is 85 to 95%. Patent Documents 3 and 4 indicate that this makes it possible to produce an electrical steel sheet in which grains are concentrated in the {100} and {411} orientations on the steel sheet surface.

[0007] Patent Document 5 describes a method for producing a non-oriented electrical steel sheet in which α-fibers are developed in a hot-rolled coil steel sheet up to the vicinity of the surface layer of the steel sheet by strip casting or the like, and the {h11}<1 / h12> orientation, particularly the {100}<012> to {411}<148> orientation, is recrystallized during subsequent annealing of the hot-rolled sheet.

[0008] Patent Document 6 discloses that in a non-oriented electrical steel sheet having an inverse pole figure {100} plane intensity of 2.4 or more, an area ratio of crystal grains having a crystal orientation of {100} orientation (within a tolerance of 20°) relative to the entire field of view as measured by electron backscatter diffraction (EBSD) of 18% or more, an average crystal grain size of 20 μm or less, a sheet thickness of 0.10 mm to 0.30 mm, and a Q value of 2.00 or more, expressed as Q=[Si]−0.5×[Mn] where the Si content (mass %) is [Si] and the Mn content (mass %) is [Mn], the probability of the presence of {411} orientation grains, which are advantageous for magnetic properties, is increased in order to improve magnetic properties and achieve low iron loss and high magnetic flux density. Patent Document 6 describes that when α-fibers are grown in the vicinity of the surface layer of a hot-rolled coil steel sheet, the {h11}<1 / h12> orientation, particularly the {100}<012> to {411}<148> orientation, is recrystallized during subsequent annealing of the hot-rolled sheet.

[0009] Patent Document 7 discloses a non-oriented electrical steel sheet that is of an α-γ transformation system and has a chemical composition, in mass %, of 2.0 to 4.5% Si, more than 3.0 to 5.0% Mn, and the balance: Fe, optional elements, and impurity elements, and that has an X-ray random intensity ratio of 0 to 15.0 for the {100}<011> crystal orientation and an X-ray random intensity ratio of 4.0 to 200 for the {411}<148> crystal orientation at a depth of ¼ of the sheet thickness from the steel sheet surface.

[0010] Patent Document 8 describes a non-oriented electrical steel sheet having an inverse pole figure {100} plane intensity of 2.4 or more, an area ratio of crystal grains having a crystal orientation of {100} orientation (within a tolerance of 20°) to the entire field of view of 18% or more when measured by electron backscatter diffraction (EBSD), an average crystal grain size of 55 μm to 200 μm, a sheet thickness of 0.10 mm to 0.30 mm, a layer containing Cr oxide having a thickness of 0.01 μm or more and 0.5 μm or less on the surface of the steel sheet, and wherein the Si content (mass%) is [Si], the Al content (mass%) is [Al], the Cr content (mass%) is [Cr], and the sheet thickness (mm) of the non-oriented electrical steel sheet is 10.00%≦2[Si]+2[Al]+[Cr]<15.00% and (2[Al]+[Cr]) / 2[Si]−10t 2It is disclosed that in order to achieve low core loss and high magnetic flux density in non-oriented electrical steel sheets that satisfy the condition of 0.35 or less, the probability of the existence of {411} oriented grains, which are advantageous in magnetic properties, is increased.

[0011] Japanese Patent Publication No. 2017-145462 Japanese Patent No. 4218077 Japanese Patent No. 5256916 Japanese Patent Publication No. 2011-111658 Japanese Patent Publication No. 2019-183185 Japanese Patent Publication No. 2020-76138 Japanese Patent Publication No. 2020-100860 Japanese Patent Publication No. 2020-139198

[0012] The inventors have studied the above-mentioned technology and found that if the {100}<011> orientation is strengthened to improve the magnetic properties as described in Patent Document 1, rapid cooling immediately after hot rolling is required, which results in a high manufacturing load. Furthermore, it has been found that when a steel sheet strengthened in the {100}<011> orientation as described in Patent Document 1 is used as a material for a crimped core, the core properties expected from the material may not be obtained. After studying the cause of this, it was found that the {100}<011> orientation exhibits a large change in magnetic properties in response to stress, specifically, a large deterioration in magnetic properties when compressive stress is applied (stress sensitivity).

[0013] Furthermore, it was found that although the techniques disclosed in Patent Documents 2 to 8 develop the {411} orientation, the concentration of the in-plane orientation in the <011> orientation is weak, and the magnetic properties in the direction at 45° to the rolling direction of the steel sheet, which is a characteristic of α-fiber, are not sufficiently high. The in-plane orientation not being aligned with the <011> orientation, i.e., the large deviation from α-fiber, is a factor that inhibits the concentration of the {411} orientation as a plane orientation, and it is thought that this may be the reason why the magnetic properties are not sufficiently improved.

[0014] In view of the above problems, the present invention aims to provide a non-oriented electrical steel sheet that has low stress sensitivity and excellent magnetic properties in directions of ±45 degrees relative to the rolling direction (45 degrees and 135 degrees), based on a manufacturing method that does not impose a heavy manufacturing load. Another object of the present invention is to provide a core (iron core) manufactured using this non-oriented electrical steel sheet, and a rotating electrical machine such as a motor or generator manufactured using this core.

[0015] The inventors conducted further studies, focusing on the {411} plane, a plane orientation rotated 20° from the {100} plane. As a result, they discovered that developing the special {411}<011> orientation further improves magnetic properties (particularly magnetic properties in directions ±45° relative to the rolling direction). They also found that steel sheets with developed {411}<011> orientation have lower stress sensitivity than steel sheets with developed {100}<011> orientation. Furthermore, as a result of their studies, they also found that increasing the heating rate during intermediate annealing and setting the final annealing temperature higher than conventional temperatures depending on the chemical composition are effective in improving magnetic properties.

[0016] Based on this finding, the present inventors have conducted further intensive research and have come up with the following aspects of the invention.

[0017] [1] A non-oriented electrical steel sheet according to one embodiment of the present invention comprises, in mass%, C: 0.0100% or less, Si: 1.50% to 4.00%, sol. Al: 0.0001% to 1.00%, S: 0.0100% or less, N: 0.0100% or less, one or more selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total, Co: 0.000% to 1.000%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total, and the Mn content, Ni content, Cu content, Si content, sol. The alloy has a chemical composition satisfying the following formula (1), where the Al content is [sol. Al] and the P content is [P], with the balance consisting of Fe and impurities. When the area ratio of {hkl}<uvw> oriented crystal grains to the entire field of view as measured by SEM-EBSD on a plane parallel to the rolled surface at a depth of 1 / 2 of the sheet thickness from the surface, is expressed as Ahkl-uvw, A411-011 is 15.0% or more, B50D, which is the average of the magnetic flux density in a 45-degree direction with respect to the rolling direction and the magnetic flux densities in a 135-degree direction with respect to the rolling direction, is 1.70 T or more, and W10D / 400D, which is the average of the iron loss in a 45-degree direction with respect to the rolling direction and the iron loss in a 135-degree direction with respect to the rolling direction, is 10.4 W / kg or less. (2×[Mn]+2.5×[Ni]+[Cu])−([Si]+2×[sol.Al]+4×[P])≧1.50% (1) [2] In the non-oriented electrical steel sheet according to [1], when the average of the magnetic flux density in a direction of 0 degrees with respect to the rolling direction and the magnetic flux density in a direction of 90 degrees with respect to the rolling direction is defined as B50L, the B50D and the B50L may satisfy the following formula (2):B50D / B50L≧1.05 (2) [3] A core according to another aspect of the present invention is a core made of a non-oriented electrical steel sheet, wherein the non-oriented electrical steel sheet contains, in mass %, C: 0.0100% or less, Si: 1.50% to 4.00%, sol. Al: 0.0001% to 1.00%, S: 0.0100% or less, N: 0.0100% or less, one or more selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total, Co: 0.000% to 1.000%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total, and the Mn content, Ni content, Cu content, Si content, sol. The alloy has a chemical composition that satisfies the following formula (1), where the Al content is [sol. Al] and the P content is [P], with the balance consisting of Fe and impurities. When the area ratio of crystal grains of {hkl}<uvw> orientation to the entire field of view when a plane parallel to the rolled surface at a depth of 1 / 2 of the sheet thickness from the surface is measured by SEM-EBSD is expressed as Ahkl-uvw, A411-011 is 15.0% or more, B50D, which is the average of the magnetic flux density in a 45-degree direction with respect to the rolling direction and the magnetic flux densities in a 135-degree direction with respect to the rolling direction, is 1.70 T or more, and W10D / 400D, which is the average of the iron loss in a 45-degree direction with respect to the rolling direction and the iron loss in a 135-degree direction with respect to the rolling direction, is 10.4 W / kg or less.(2×[Mn]+2.5×[Ni]+[Cu])−([Si]+2×[sol.Al]+4×[P])≧1.50% (1) [4] A rotating electric machine according to another aspect of the present invention comprises a stator, a rotor arranged on the inner periphery of the stator, and a case that is in close contact with the stator from the outer periphery of the stator and fixes the stator, wherein a non-oriented electrical steel sheet that constitutes a core of at least one of the stator and the rotor contains, in mass %, C: 0.0100% or less, Si: 1.50% to 4.00%, sol. Al: 0.0001% to 1.00%, S: 0.0100% or less, N: 0.0100% or less, one or more selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total, Co: 0.000% to 1.000%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total, and the Mn content, Ni content, Cu content, Si content, sol. The alloy has a chemical composition satisfying the following formula (1), where the Al content is [sol. Al] and the P content is [P], with the balance consisting of Fe and impurities. When the area ratio of {hkl}<uvw> oriented crystal grains to the entire field of view as measured by SEM-EBSD on a plane parallel to the rolled surface at a depth of 1 / 2 of the sheet thickness from the surface, is expressed as Ahkl-uvw, A411-011 is 15.0% or more, B50D, which is the average of the magnetic flux density in a 45-degree direction with respect to the rolling direction and the magnetic flux densities in a 135-degree direction with respect to the rolling direction, is 1.70 T or more, and W10D / 400D, which is the average of the iron loss in a 45-degree direction with respect to the rolling direction and the iron loss in a 135-degree direction with respect to the rolling direction, is 10.4 W / kg or less. (2×[Mn]+2.5×[Ni]+[Cu])−([Si]+2×[sol.Al]+4×[P])≧1.50% (1).

[0018] According to the above-described aspects of the present invention, it is possible to provide a non-oriented electrical steel sheet having low stress sensitivity and excellent magnetic properties in directions of ±45 degrees relative to the rolling direction (sometimes simply referred to as the ±45 degree directions), a core manufactured using this non-oriented electrical steel sheet, and a rotating electric machine manufactured using this core.

[0019] Hereinafter, a non-oriented electrical steel sheet according to one embodiment of the present invention (non-oriented electrical steel sheet according to this embodiment), a core (core according to this embodiment), and a rotating electric machine (rotating electric machine according to this embodiment), as well as preferred manufacturing methods thereof, will be described.

[0020] [Non-oriented electrical steel sheet] The non-oriented electrical steel sheet according to this embodiment has a predetermined chemical composition, and when the area ratio of {hkl}<uvw> oriented crystal grains to the entire field of view measured by SEM-EBSD on a surface parallel to the rolled surface at a depth of half the sheet thickness from the surface is expressed as Ahkl-uvw, the A411-011 is 15.0% or more, the B50D, which is the average of the magnetic flux density in a direction at 45 degrees to the rolling direction and the magnetic flux density in a direction at 135 degrees to the rolling direction, is 1.70 T or more, and the W10D / 400D, which is the average of the iron loss in a direction at 45 degrees to the rolling direction and the iron loss in a direction at 135 degrees to the rolling direction, is 10.4 W / kg or less. The rolling direction of the non-oriented electrical steel sheet according to this embodiment can be determined by visually observing the rolling marks. These rolling marks can also be observed in the core after the non-oriented electrical steel sheet has been processed.

[0021] <Chemical Composition> First, the chemical composition of the non-oriented electrical steel sheet according to this embodiment will be described. In the following description, the unit of content of each element, "%", means "mass %" unless otherwise specified. Furthermore, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0022] The non-oriented electrical steel sheet according to this embodiment has a chemical composition in which ferrite-austenite transformation (hereinafter, α-γ transformation) can occur to some extent (a chemical composition in which a certain amount of γ is produced when heated, even if the entire structure is not transformed into γ), and contains C: 0.0100% or less, Si: 1.50% to 4.00%, sol. The alloy has a chemical composition containing 0.0001% to 1.00% Al, 0.0100% or less S, 0.0100% or less N, 2.50% to 5.00% in total of one or more elements selected from the group consisting of Mn, Ni, and Cu, 0.000% to 1.000% Co, 0.000% to 0.400% Sn, 0.000% to 0.400% Sb, 0.000% to 0.400% P, and 0.0000% to 0.0100% in total of one or more elements selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd, with the balance being Fe and impurities. Furthermore, the contents of Mn, Ni, Cu, Si, sol. Al, and P satisfy the specified conditions described below. Examples of impurities include those contained in raw materials such as ore and scrap, and those contained in the manufacturing process.

[0023] (C: 0.0100% or less) C is an element that precipitates as fine carbides. Such fine carbides inhibit grain growth, thereby increasing iron loss and causing magnetic aging. Therefore, the lower the C content, the better. This phenomenon becomes more pronounced when the C content exceeds 0.0100%. For this reason, the C content is set to 0.0100% or less. The C content is preferably 0.0050% or less, more preferably 0.0025% or less. There is no particular lower limit for the C content, but in consideration of the cost of decarburization treatment during refining, the C content is preferably 0.0005% or more.

[0024] (Si: 1.50% to 4.00%) Si is an element that increases electrical resistance, reduces eddy current loss, and reduces iron loss. Si is also an element that increases the yield ratio and improves punching workability into a core. If the Si content is less than 1.50%, these effects cannot be fully obtained. Therefore, the Si content is set to 1.50% or more. On the other hand, if the Si content exceeds 4.00%, the magnetic flux density decreases, punching workability decreases due to an excessive increase in hardness, and cold rolling becomes difficult. Therefore, the Si content is set to 4.00% or less.

[0025] (Sol. Al: 0.0001% to 1.00%) Sol. Al is an element that increases electrical resistance, reduces eddy current loss, and reduces iron loss. Sol. Al also contributes to improving the relative magnitude of magnetic flux density B50 with respect to saturation magnetic flux density. Here, magnetic flux density B50 is the magnetic flux density in a magnetic field of 5000 A / m. If the sol. Al content is less than 0.0001%, these effects cannot be fully obtained. Al also has the effect of promoting desulfurization in steelmaking. Therefore, the sol. Al content is set to 0.0001% or more. The sol. Al content is preferably 0.001% or more, more preferably 0.10% or more. On the other hand, if the sol. Al content exceeds 1.00%, the magnetic flux density decreases. Therefore, the sol. Al content is set to 1.00% or less.

[0026] (S: 0.0100% or less) S is not an essential element, but is contained, for example, as an impurity in steel. S precipitates as fine MnS and inhibits recrystallization and grain growth during annealing. Therefore, the lower the S content, the better. Such an increase in iron loss and a decrease in magnetic flux density due to the inhibition of recrystallization and grain growth are significant when the S content exceeds 0.0100%. For this reason, the S content is set to 0.0100% or less. There is no particular lower limit for the S content, but in consideration of the cost of desulfurization treatment during refining, the S content is preferably set to 0.0003% or more.

[0027] (N: 0.0100% or less) N is an element that deteriorates magnetic properties through the formation of fine precipitates such as TiN and AlN. Therefore, the lower the N content, the better. Such deterioration of magnetic properties becomes significant when the N content exceeds 0.0100%, so the N content is set to 0.0100% or less. There is no particular lower limit for the N content, but in consideration of the cost of denitrification treatment during refining, the N content is preferably set to 0.0010% or more.

[0028] (One or more elements selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total) These elements are necessary for inducing the α-γ transformation. In the non-oriented electrical steel sheet according to this embodiment, at least one of these elements is contained in a total amount of 2.50% or more. On the other hand, if the content of these elements exceeds 5.00% in total, not only will the cost increase, but the magnetic flux density may also decrease. Therefore, the total amount of at least one of these elements is set to 5.00% or less.

[0029] The contents of Mn, Ni, and Cu are not limited, but from the viewpoint of resistivity, the Mn content is preferably 1.50% or more.

[0030] Furthermore, the following condition must be satisfied in order for the α-γ transformation to occur and for good magnetic properties to be obtained: That is, when the Mn content (mass%) is [Mn], the Ni content (mass%) is [Ni], the Cu content (mass%) is [Cu], the Si content (mass%) is [Si], the sol. Al content (mass%) is [sol. Al], and the P content (mass%) is [P], the following formula (1) is satisfied: (2×[Mn]+2.5×[Ni]+[Cu])-([Si]+2×[sol. Al]+4×[P])≧1.50% (1) If the formula (1) is not satisfied, the α-γ transformation will not occur, or even if it does occur, the transformation point will be high, and therefore sufficient magnetic flux density will not be obtained even when the manufacturing method described below is applied.

[0031] The chemical composition of the non-oriented electrical steel sheet according to this embodiment basically contains the above elements, with the balance consisting of Fe and impurities (impurities other than those mentioned above). However, instead of a portion of the balance Fe, Co, Sn, Sb, P, Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd may be contained in the ranges shown below. These elements do not necessarily have to be contained, so the lower limit is 0%. Furthermore, it is permissible for these elements to be contained as impurities without being intentionally added.

[0032] (Co: 0.000% to 1.000%) Co is an element that increases magnetic flux density. Therefore, it may be contained as needed. On the other hand, excessive Co content increases costs. Therefore, the Co content is set to 1.000% or less.

[0033] (Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%) Sn and Sb are elements that improve the texture after cold rolling and recrystallization, and increase the magnetic flux density. Therefore, one or two of these elements may be contained as needed. When further effects such as magnetic properties are to be imparted, it is preferable to contain one or more elements selected from the group consisting of 0.020% to 0.400% Sn and 0.020% to 0.400% Sb. On the other hand, if these elements are contained in excess, the steel becomes embrittled. Therefore, the Sn content and Sb content are both set to 0.400% or less.

[0034] (P: 0.000% to 0.400%) P is an element that is effective in ensuring the hardness of the steel sheet after recrystallization. P is also an element that has a favorable effect on magnetic properties. Therefore, it may be contained. To obtain these effects, the P content is preferably 0.020% or more. On the other hand, if excessive P is contained, the steel becomes embrittled. Therefore, the P content is set to 0.400% or less.

[0035] (One or more elements selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total) Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd are elements that react with S in molten steel during casting to form precipitates of sulfides or oxysulfides, or both. Hereinafter, Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd may be collectively referred to as "coarse precipitate-forming elements." The particle size of precipitates of coarse precipitate-forming elements is about 1 μm to 2 μm, which is much larger than the particle size (about 100 nm) of fine precipitates such as MnS, TiN, and AlN. Therefore, these fine precipitates adhere to the precipitates of the coarse precipitate forming elements and are less likely to inhibit recrystallization and grain growth during annealing such as intermediate annealing. To fully obtain these effects, the total content of these elements is preferably 0.0005% or more, and more preferably 0.0010% or more. On the other hand, if the total content of these elements exceeds 0.0100%, the total amount of sulfides or oxysulfides, or both, becomes excessive, inhibiting recrystallization and grain growth during annealing such as intermediate annealing. Therefore, the total content of the coarse precipitate forming elements is set to 0.0100% or less.

[0036] The chemical composition is determined by the following method. The chemical composition may be measured by a general steel analysis method. For example, the chemical composition may be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Specifically, the chemical composition is determined by measuring a test piece taken from the steel sheet using a predetermined measuring device under conditions based on a pre-created calibration curve. C and S may be measured using the combustion-infrared absorption method, and N may be measured using the inert gas fusion-thermal conductivity method. If the non-oriented electrical steel sheet has an insulating coating on its surface, this may be mechanically removed using a disc grinder or the like before analysis.

[0037] <Texture> In the non-oriented electrical steel sheet according to this embodiment, the texture is controlled when a surface parallel to the rolled surface at a depth of half the sheet thickness (a position half the sheet thickness in the sheet thickness direction) from the surface (when an insulating coating is present on the surface, the surface of the steel sheet (base steel sheet) excluding the insulating coating; the same applies hereinafter) is measured using a scanning electron microscope with electron backscatter diffraction (SEM-EBSD). Specifically, when the area ratio of crystal grains with the {hkl}<uvw> orientation (within a tolerance of 10°) to the entire field of view obtained by the above measurement is expressed as Ahkl-uvw, the A411-011 (hereinafter sometimes referred to as the {411}<011> ratio) is set to 15.0% or more. If the {411}<011> ratio is less than 15.0%, excellent magnetic properties cannot be obtained. The {411}<011> ratio is preferably 25.0% or more, more preferably 30.0% or more, even more preferably 35.0% or more, and even more preferably 40.0% or more, or 55.0% or more. There is no particular upper limit, but it may be 80.0% or less from the viewpoint of production load.

[0038] Furthermore, in the non-oriented electrical steel sheet according to this embodiment, it is preferable that the proportion of the {111} orientation ({111}<uvw> orientation) is small. The {111} orientation is an orientation that hinders in-plane magnetization, and by setting the proportion of the {111} orientation (sometimes referred to as the {111} ratio) to 10.0% or less, better magnetic properties can be obtained. The {111} ratio is preferably 8.0% or less, more preferably 7.0% or less, and even more preferably 5.0% or less. The lower limit is not particularly limited, but may be 1.0% or more from the viewpoint of production load.

[0039] The area ratio of specific orientation grains in the non-oriented electrical steel sheet according to this embodiment can be measured by the following method. Specifically, the area ratio of specific orientation grains is measured by extracting the specific orientation of interest from a measurement area (with a tolerance of 10°, hereinafter referred to as "within 10°") using a scanning electron microscope (SEM) equipped with electron backscatter diffraction (EBSD) functionality, observed under the following measurement conditions, using OIM Analysis 7.3 (manufactured by TSL Solutions Co., Ltd.). The extracted area is divided by the area of ​​the measurement area to obtain a percentage. This percentage is the area ratio of specific orientation grains. In this embodiment, the "area ratio of crystal grains having a crystal orientation of {hkl}<uvw> orientation (within a tolerance of 10°) relative to the measurement region" and the "area ratio of crystal grains having a crystal orientation of {hkl} orientation (within a tolerance of 10°) relative to the measurement region" may also be simply referred to as the "{hkl}<uvw> ratio" and the "{hkl} ratio," respectively. In describing the crystal orientation, the tolerance is set to be within 10°.

[0040] The details of the measurement conditions for determining the area ratio (Ahkl-uvw) of each orientation grain are as follows: - Measurement equipment: SEM model number "JSM-6400 (manufactured by JEOL)", EBSD detector model number "HIKARI (manufactured by TSL Solutions Co., Ltd.)", or a similar equipment is used - Step interval: 5.0 μm - Magnification: 100x - Measurement object: A surface parallel to the rolled surface at a depth of 1 / 2 the plate thickness from the surface - Measurement area: A rectangular area of ​​1000 μm or more x 1000 μm or more

[0041] <Average Grain Size> In the non-oriented electrical steel sheet according to this embodiment, if the average grain size is too small without the grains becoming coarse, there is a concern that iron loss may worsen. On the other hand, if the grains become excessively coarse and the average grain size is too large, not only may workability deteriorate, but eddy current loss may also deteriorate. Therefore, the average grain size of the non-oriented electrical steel sheet is preferably 50 to 150 μm, and more preferably 70 to 120 μm. The average grain size can be measured, for example, at any cross section using the cutting method of JIS G0551:2020. For example, the measurement range is a rectangular region of 1000 μm or more across the entire sheet thickness direction and in a direction perpendicular to the sheet thickness direction.

[0042] <Sheet Thickness> The thickness of the non-oriented electrical steel sheet according to this embodiment is not particularly limited. Typically, as the sheet thickness decreases, the iron loss decreases, but the magnetic flux density also decreases. In light of this, if the sheet thickness is 0.20 mm or more, the iron loss becomes lower and the magnetic flux density becomes higher. Furthermore, if the sheet thickness is 0.50 mm or less, low iron loss can be maintained. Therefore, the sheet thickness of the non-oriented electrical steel sheet according to this embodiment is preferably 0.20 to 0.50 mm. More preferably, it is 0.25 to 0.35 mm.

[0043] <Magnetic Properties> As described above, the non-oriented electrical steel sheet according to this embodiment has a controlled chemical composition and texture. As magnetic properties, B50D, which is the average of the magnetic flux density B50 in the direction at 45 degrees to the rolling direction and the magnetic flux density B50 in the direction at 135 degrees to the rolling direction, is 1.70 T or more, and W10D / 400D, which is the average of the iron loss W10 / 400 in the direction at 45 degrees to the rolling direction and the iron loss W10 / 400 in the direction at 135 degrees to the rolling direction, is 10.4 W / kg or less. B50D is preferably 1.73 T or more, more preferably 1.76 T or more. Furthermore, W10D / 400D is preferably 10.0 W / kg or less. The angle with respect to the rolling direction refers to the angle formed by the rolling surface with the rolling direction, with the 0-degree direction being the rolling direction (L direction) and the 90-degree direction being the width direction (C direction). W10 / 400 is the iron loss under a magnetic field of 1.0 T and 400 Hz. The magnetic flux density and iron loss can be measured by conducting tests in accordance with the method for measuring the magnetic properties of electromagnetic steel strips using a single sheet tester specified in JIS C 2556:2015. Instead of obtaining test pieces of the size specified in JIS, smaller test pieces, for example, 55 mm wide x 55 mm long, may be obtained and measured in accordance with the single sheet magnetic property test method of JIS C 2556:2015 using a corresponding small single sheet tester. Furthermore, if a 55 mm wide x 55 mm long test piece cannot be obtained, two 8 mm wide x 16 mm long test pieces may be used to obtain a 16 mm wide x 16 mm long test piece, and measurements in accordance with the single sheet magnetic property test method may be performed.

[0044] Generally, the magnetic properties of non-oriented electrical steel sheets are often evaluated as the average value in the rolling direction (coil longitudinal direction, L direction) and the perpendicular direction (coil width direction, C direction) of the steel sheet. This is because of the in-plane anisotropy of the sheet. Many conventional non-oriented electrical steel sheets have been proposed with low magnetic anisotropy. However, these conventional non-oriented electrical steel sheets often have poorer magnetic properties in the ±45° direction (coil diagonal direction) relative to the rolling direction compared to the two directions (L and C directions). This poses a problem when used as a split core designed to have the primary magnetization direction of the core in the ±45° direction relative to the rolling direction of the steel sheet. In contrast, the non-oriented electrical steel sheet according to the present embodiment has excellent magnetic properties in the 45° direction and the 135° direction (i.e., the ±45° direction relative to the rolling direction) as described above. Therefore, the non-oriented electrical steel sheet according to this embodiment is particularly suitable for use as a split core designed so that the main magnetization direction of the core is at an angle of ±45° to the rolling direction of the steel sheet, and further suitable for split cores for drive motors of electric vehicles or hybrid vehicles, which are used in the high frequency range of 1000 Hz or more.

[0045] When the average of the magnetic flux density B50(T) in the direction of 0 degrees to the rolling direction and the magnetic flux density B50(T) in the direction of 90 degrees to the rolling direction is defined as B50L(T), it is preferable that B50D and B50L satisfy the following formula (2). In this case, it is more suitable for the above-mentioned applications. B50D / B50L≧1.05 (2)

[0046] Furthermore, the non-oriented electrical steel sheet according to this embodiment has a controlled chemical composition and texture as described above, and therefore exhibits little deterioration in magnetic properties (stress sensitivity) when subjected to compressive stress. The stress sensitivity can be evaluated, for example, by the iron loss deterioration rate calculated from the iron loss W10 / 50 (45° direction) without stress and the iron loss W10 / 50 (45° direction) under a compressive stress of 10 MPa.

[0047] [Core (iron core)] The core according to this embodiment is made of the non-oriented electrical steel sheet according to this embodiment. Specifically, it is made by laminating a plurality of non-oriented electrical steel sheets according to this embodiment that have been processed into a predetermined shape. Since the above-mentioned characteristics of this non-oriented electrical steel sheet do not change due to processing, the non-oriented electrical steel sheet that constitutes the core has the same characteristics as the non-oriented electrical steel sheet according to this embodiment described above. Specifically, in mass %, C: 0.0100% or less, Si: 1.50% to 4.00%, sol. Al: 0.0001% to 1.00%, S: 0.0100% or less, N: 0.0100% or less, one or more selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total, Co: 0.000% to 1.000%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total, and the Mn content, Ni content, Cu content, Si content, sol. The alloy has a chemical composition satisfying the following formula (1), where the Al content is [sol. Al] and the P content is [P], with the balance consisting of Fe and impurities. When the area ratio of {hkl}<uvw> oriented crystal grains to the entire field of view as measured by SEM-EBSD on a plane parallel to the rolled surface at a depth of 1 / 2 of the sheet thickness from the surface, is expressed as Ahkl-uvw, A411-011 is 15.0% or more, B50D, which is the average of the magnetic flux density in a 45-degree direction with respect to the rolling direction and the magnetic flux densities in a 135-degree direction with respect to the rolling direction, is 1.70 T or more, and W10D / 400D, which is the average of the iron loss in a 45-degree direction with respect to the rolling direction and the iron loss in a 135-degree direction with respect to the rolling direction, is 10.4 W / kg or less. (2×[Mn]+2.5×[Ni]+[Cu])-([Si]+2×[sol.Al]+4×[P])≧1.50%...(1)

[0048] For example, the core according to this embodiment is a divided core of a drive motor for an electric vehicle or a hybrid vehicle. The core (iron core) according to this embodiment includes both a stator core and a rotor core.

[0049] [Rotating Electric Machine] The rotating electric machine according to this embodiment includes a stator, a rotor disposed on the inner periphery of the stator, and a case that is in close contact with the stator from the outer periphery of the stator and fixes the stator, and at least one of the cores of the stator and the rotor is the core according to this embodiment. Since the characteristics of the stator and / or rotor core do not change even after being incorporated into the rotating electric machine, the stator and / or rotor core included in the rotating electric machine according to this embodiment has the same characteristics as the non-oriented electrical steel sheet that constitutes the core according to this embodiment described above.

[0050] For example, the rotating electric machine according to this embodiment is a drive motor for an electric vehicle or a hybrid vehicle. When the rotating electric machine according to this embodiment is a drive motor, the non-oriented electrical steel sheet according to this embodiment used for the core has low stress sensitivity and excellent magnetic properties in directions of ±45 degrees relative to the rolling direction, thereby achieving the effect of reducing motor loss. This effect is particularly significant when the core is designed so that the main magnetization direction of the core is in directions of ±45 degrees relative to the rolling direction of the steel sheet, or when the non-oriented electrical steel sheets are laminated to form a laminated core that is fixed by crimping.

[0051] To evaluate the chemical composition, texture, and magnetic properties of a non-oriented electrical steel sheet that constitutes the core of a rotating electric machine, the rotating electric machine is disassembled using a known method, a single non-oriented electrical steel sheet is removed from the core, and the sheet is then tested and evaluated in the same manner as the non-oriented electrical steel sheet described above. While the detailed method for disassembling a rotating electric machine varies depending on the actual rotating electric machine, one example involves first removing the rotating electric machine from the machine in which it is housed. Next, a portion of the rotating electric machine's case (housing) is removed by machining. The stator and rotor are then separated. If the rotor contains permanent magnets, it is desirable to insert a spacer, such as a plastic sheet, between the stator and rotor due to the magnetic attraction. The stator is then removed from the housing. Since the stator has windings, the windings are removed or partially cut. The top of the stator laminations or any steel sheets damaged when the windings were cut are excluded, and samples are taken from other locations. In many cases, the laminations are fastened together by crimping or welding. In the case of crimping, it is possible to peel the laminations by inserting a cutter blade into the gap between the laminated steel sheets. In the case of welding, it is possible to peel the laminations by cutting the welded area with a hand grinder or similar. The coil ends of rotors are often made of a material other than electromagnetic steel. For this reason, they are separated into two pieces by machining near the longitudinal center of the rotor using a non-magnetic blade. The laminations are then peeled off in the same way as the stator described above. When doing so, it is desirable to exclude any areas that have been affected by the machining.

[0052] [Manufacturing Method] Next, an example of a method for manufacturing the non-oriented electrical steel sheet according to this embodiment, the core according to this embodiment, and the rotating electrical machine according to this embodiment will be described. Known conditions can be applied to conditions and steps not described.

[0053] The non-oriented electrical steel sheet according to this embodiment can obtain its effects as long as it has the above-mentioned characteristics, regardless of the manufacturing method. However, a manufacturing method including a hot rolling step, a cooling step, a cold rolling step, an intermediate annealing step, a second cold rolling (hereinafter referred to as a skin-pass rolling step), and a finish annealing step, which will be described later, is preferable because it can be obtained stably.

[0054] Preferred conditions for each step will be described. Well-known conditions can be applied to conditions not described. Hereinafter, in this embodiment, the Ar3 temperature, Ar1 temperature, and Ac1 temperature (all in °C) are determined by the following method. The Ar3 temperature and Ar1 temperature are determined from the thermal expansion change of the steel material (steel plate) during cooling at an average cooling rate of 1 °C / sec, and the Ac1 temperature is determined from the thermal expansion change of the steel material (steel plate) during heating at an average heating rate of 1 °C / sec. The average cooling rate and average heating rate are average values ​​in the range of room temperature to 1200 °C.

[0055] <Hot Rolling Step> In the hot rolling step, hot rolling is performed on a steel material satisfying the above-described chemical composition to produce a hot-rolled steel sheet. The hot rolling step includes a heating step and a rolling step.

[0056] The steel material is, for example, a slab produced by normal continuous casting, and steel material having the above-mentioned composition is produced by a well-known method. For example, molten steel is produced in a converter or electric furnace. The produced molten steel is subjected to secondary refining in a degassing facility or the like to produce molten steel having the above-mentioned chemical composition (the chemical composition does not change substantially in subsequent processes). The molten steel is cast into a slab by a continuous casting method or an ingot casting method. The cast slab may be bloomed.

[0057] In the heating process, it is preferable to heat the steel material having the above-mentioned chemical composition to 1000 to 1200°C. Specifically, the steel material is charged into a heating furnace or a soaking furnace and heated in the furnace. The holding time at the above heating temperature in the heating furnace or the soaking furnace is not particularly limited, but is, for example, 30 to 200 hours.

[0058] In the rolling process, the steel material heated in the heating process is subjected to multiple passes of rolling to produce a hot-rolled steel sheet. Here, "pass" means that the steel sheet passes through one rolling stand having a pair of work rolls and is subjected to rolling reduction. Hot rolling may be performed, for example, by tandem rolling using a tandem rolling mill including multiple rolling stands arranged in a row (each rolling stand having a pair of work rolls), or by reverse rolling using a pair of work rolls, to perform multiple passes. From the viewpoint of productivity, it is preferable to perform multiple rolling passes using a tandem rolling mill.

[0059] The rolling process (rough rolling and finish rolling) is preferably carried out at a temperature in the γ range (Ar3 temperature or higher). In other words, hot rolling is preferably carried out so that the temperature (finish rolling temperature FT (°C)) when passing through the final pass of finish rolling is Ar3 temperature or higher.

[0060] The finish rolling temperature FT means the surface temperature (°C) of the steel sheet at the exit side of the rolling stand where the final pass is reduced during the rolling process in the hot rolling step. The finish rolling temperature FT can be measured, for example, by a non-contact thermometer installed at the exit side of the rolling stand where the final pass is reduced. For example, when the entire length of the steel sheet is divided into 10 equal sections in the rolling direction, the finish rolling temperature FT means the average value of the temperature measurement results at the center part in the sheet width direction, excluding one section at the front end and one section at the rear end.

[0061] <Cooling Step> In the cooling step, the steel sheet (hot-rolled steel sheet) after the hot rolling step (after the completion of finish rolling) is cooled. This cooling transforms austenite to ferrite, resulting in high strain and moderately fine crystal grains. The cooling conditions are preferably such that cooling begins 0.10 seconds or more (after 0.10 seconds or more have elapsed) after the final pass of finish rolling, and cooling is performed so that the surface temperature of the hot-rolled steel sheet reaches 300°C or higher and Ar1 temperature or lower after 3 seconds (without immediate rapid cooling). Avoiding immediate rapid cooling in this way eliminates the need for a special rapid cooling device, which is advantageous in terms of production (cost). Furthermore, when the hot-rolled steel sheet is immediately rapid cooled, the texture becomes a structure in which unrecrystallized austenite is transformed, and the texture after the subsequent finish annealing is likely to have a texture concentrated in the {100}<011> orientation. On the other hand, if immediate rapid cooling is not performed, it is presumed that the partially recrystallized austenite will be transformed into a structure, and will be more likely to accumulate in the {411}<011> orientation in the structure after subsequent finish annealing. That is, in order to increase the {411}<011> ratio, it is important to transform the partially recrystallized austenite, and therefore it is preferable not to perform immediate rapid cooling. Furthermore, the cooling conditions are preferably set so that the average grain size in the hot-rolled steel sheet before cold rolling is 3 to 10 μm. If subsequent cold rolling is performed with a suitable grain size that is not excessively refined, α-fibers will develop after intermediate annealing, and the {411}<011> orientation, which is usually difficult to develop, can be developed after the subsequent skin pass and finish annealing. On the other hand, if the grains become too coarse, α-fibers will be less likely to develop after cold rolling and intermediate annealing, and the desired {411}<011> ratio may not be obtained. In order to make the average grain size of the hot-rolled steel sheet before cold rolling 3 to 10 μm, it is sufficient to make the temperature equal to or lower than the Ar1 temperature within 3 seconds after passing through the final pass of finish rolling. On the other hand, if the cooling stop temperature is less than 300°C, there is a concern that the average grain size of the hot-rolled steel sheet will be excessively refined. Therefore, it is preferable to make the cooling stop temperature 300°C or higher.

[0062] The temperature of the hot-rolled steel sheet (particularly the finish rolling temperature) and the surface temperature of the hot-rolled steel sheet 3 seconds after passing through the final pass of finish rolling are measured by the following method. In a hot rolling equipment line used to manufacture non-oriented electrical steel sheets, a cooling device and a conveying line (e.g., conveying rollers) are arranged downstream of the hot rolling mill, a thermometer for measuring the surface temperature of the hot-rolled steel sheet is arranged at the exit of the rolling stand that performs the final pass of the hot rolling mill, and multiple thermometers are also arranged along the conveying line on the conveying rollers arranged downstream of the rolling stand, the hot-rolling temperature and the surface temperature of the hot-rolled steel sheet 3 seconds after passing through the final pass of finish rolling can be measured using the thermometer arranged in the hot rolling equipment line. Cooling is performed using a cooling device arranged downstream of the rolling stand that performs the final pass. Multiple water cooling devices are generally arranged, and a thermometer is arranged at the entrance of each water cooling device. The cooling device may be, for example, a well-known water cooling device or a well-known forced air cooling device. Preferably, the cooling device is a water cooling device. The cooling liquid of the water cooling device may be water or a mixture of water and air.

[0063] <Cold Rolling Step> In the cold rolling step, a hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. It is preferable that the hot-rolled steel sheet is not subjected to hot-rolled sheet annealing before the cold rolling step in order to develop α-fiber after cold rolling. Here, hot-rolled sheet annealing refers to, for example, heat treatment in which the heating temperature is Ac1 temperature or lower and 300°C or higher. For example, cold rolling may be performed using a tandem rolling mill including a plurality of rolling stands arranged in a row (each rolling stand having a pair of work rolls) to perform multiple passes. Alternatively, reverse rolling may be performed using a Sendzimir rolling mill or the like having a pair of work rolls to perform single-pass or multiple-pass rolling. From the viewpoint of productivity, it is preferable to perform multiple-pass rolling using a tandem rolling mill.

[0064] In cold rolling, cold rolling is performed without performing annealing treatment during the cold rolling. For example, when performing reverse rolling and performing cold rolling in multiple passes, multiple passes of cold rolling are performed without annealing treatment between passes of cold rolling. If annealing is performed between passes, the desired orientation cannot be developed in the process described below. Cold rolling may be performed in only one pass using a reverse rolling mill. Furthermore, when performing cold rolling using a tandem rolling mill, cold rolling is performed continuously in multiple passes (passes at each rolling stand).

[0065] In this embodiment, in order to develop α-fiber, it is preferable that the reduction rate RR1 (%) in cold rolling is set to 75 to 95%. The reduction rate RR1 is more preferably 78 to 92%. Here, the reduction rate RR1 is defined as follows: Reduction rate RR1 (%) = (1 - sheet thickness after the final pass in cold rolling / sheet thickness before the first pass in cold rolling) x 100

[0066] <Intermediate Annealing Step> In the intermediate annealing step, the steel sheet (cold-rolled steel sheet) after the cold rolling step is subjected to intermediate annealing. More specifically, annealing is performed by raising the temperature (heating) at a heating rate of 400°C / s or more to an annealing temperature (intermediate annealing temperature T1) (°C) between 600°C and the Ac1 temperature or lower. A411-011 can be improved by performing the intermediate annealing step, the subsequent skin-pass rolling step, and the finish annealing step under appropriate conditions on a steel sheet having a predetermined chemical composition. If the heating rate to the annealing temperature is less than 400°C / s, sufficient recovery may not occur, and there is a concern that the desired texture may not be obtained. The heating rate is preferably 600°C / s or more, or 1000°C / s or more. A faster heating rate to the annealing temperature is preferable, also from the viewpoint of reducing the proportion of {111} orientation, which is detrimental to magnetic properties. On the other hand, a faster heating rate is preferable for texture formation, but achieving a heating rate of more than 2000°C / s requires special equipment and control, which significantly increases costs. Therefore, the heating rate may be 2000°C / s or less. More preferably, it is 1500°C / s or less. The heating rate is calculated by dividing the temperature change from room temperature (e.g., 25°C) to the annealing temperature by the time required for heating. Furthermore, if the annealing temperature of the intermediate annealing exceeds the Ac1 temperature, part of the structure of the steel sheet will transform to austenite, and due to the change in crystal orientation associated with the transformation, {411}<011> oriented grains may not grow sufficiently during the subsequent skin-pass rolling and finish annealing, resulting in an insufficient magnetic flux density. On the other hand, if the temperature of the intermediate annealing is too low, recrystallization will not occur, and {411}<011> oriented grains may not grow sufficiently during the subsequent skin-pass rolling and finish annealing, resulting in an insufficient magnetic flux density. Therefore, it is preferable that the intermediate annealing temperature T1 (°C) is 600°C or higher. The intermediate annealing temperature T1 (°C) is the sheet temperature (surface temperature) near the outlet of the annealing furnace. The holding time at the intermediate annealing temperature T1 (°C) in the intermediate annealing step may be a time known to those skilled in the art. The holding time at the intermediate annealing temperature T1 (°C) is, for example, 5 to 60 seconds, but is not limited thereto. The atmosphere during intermediate annealing is not particularly limited, but may be, for example, a 20% by volume H atmosphere. 2 and the remainder is N 2The cooling rate of the steel sheet after intermediate annealing is not particularly limited, and is, for example, 5.0 to 60.0°C / sec.

[0067] <Skin-pass rolling process> In the skin-pass rolling process, the cold-rolled steel sheet after the intermediate annealing process is rolled (cold rolling) at room temperature in the atmosphere. For the skin-pass rolling here, a reverse rolling mill, such as the Sendzimir rolling mill described above, or a tandem rolling mill is used. In the skin-pass rolling process, rolling is performed without performing an annealing treatment in between. For example, when performing skin-pass rolling in multiple passes after performing reverse rolling, multiple passes are performed without annealing treatment between passes. Skin-pass rolling may be performed in only one pass using a reverse rolling mill. Furthermore, when performing skin-pass rolling using a tandem rolling mill, rolling is performed continuously in multiple passes (passes at each rolling stand). In this embodiment, after strain is introduced into the steel sheet by hot rolling and cold rolling, the strain introduced into the steel sheet by intermediate annealing is temporarily reduced. Then, skin-pass rolling is performed. This reduces the excessive strain introduced by cold rolling during intermediate annealing, thereby suppressing preferential recrystallization of {111} grains in the steel sheet surface and leaving {411}<011> crystal orientation grains. Then, an appropriate amount of strain is introduced into each crystal grain in the steel sheet during skin-pass rolling, creating a state in which grain growth due to bulging is likely to occur during the subsequent finish annealing. The reduction ratio RR2 in skin-pass rolling is preferably 10 to 15%. If the reduction ratio RR2 is less than 10%, the amount of strain becomes too small, resulting in a long finish annealing time required for grain growth due to bulging. On the other hand, if the reduction ratio RR2 exceeds 15%, the amount of strain becomes too large, resulting in normal grain growth rather than bulging, resulting in the growth of {411}<148> and {111}<112> during finish annealing.

[0068] Here, the reduction rate RR2 is defined as follows: Reduction rate RR2 (%) = (1 - thickness after the final pass of skin-pass rolling / thickness before the first pass of skin-pass rolling) x 100

[0069] The number of passes in skin pass rolling may be only one pass (i.e., only one rolling), or may be multiple passes. The skin pass rolling performed in this embodiment has a significantly different effect from skin pass rolling performed after finish annealing. A predetermined structure can be obtained by performing hot rolling, cooling, cold rolling, intermediate annealing, skin pass rolling, and finish annealing in this order under predetermined conditions.

[0070] <Finish Annealing Step> In the finish annealing step, the steel sheet after the skin-pass rolling step is annealed at an annealing temperature T2 (°C) of 850°C or higher and Ac1 temperature or lower for 2 hours or longer. Setting the finish annealing temperature T2 (°C) to 850°C or higher promotes grain growth due to bulging, thereby increasing the concentration of the {411}<011> orientation. Furthermore, if T2 is lower than 850°C, there is a concern that the above-mentioned grain growth may not occur sufficiently. Conventionally, finish annealing has often been performed at around 750°C. This is because it was believed that increasing the temperature beyond this point would not be effective and would increase costs. In contrast, the present inventors have discovered that by combining the above-mentioned intermediate annealing conditions (such as rapid heating) with the skin-pass rolling conditions, increasing the annealing temperature increases the concentration of texture and further improves magnetic properties. On the other hand, if the finish annealing temperature T2 (°C) exceeds the Ac1 temperature, a part of the structure of the steel sheet is transformed into austenite, grain growth due to bulging does not occur, and the desired {411}<011> ratio cannot be obtained. Furthermore, if the annealing time is less than 2 hours, even if the finish annealing temperature T2 (°C) is 850°C or higher and the Ac1 temperature or lower, there is a concern that grain growth due to bulging will not occur sufficiently, resulting in a decrease in the concentration of the {411}<011> orientation. On the other hand, the annealing time for the finish annealing is not particularly limited, but since the effect saturates even if the annealing time exceeds 10 hours, it may be 10 hours or shorter.

[0071] The temperature rise rate TR2 up to the finish annealing temperature T2 in the finish annealing step may be any temperature rise rate known to those skilled in the art, and may be, for example, 40°C / hour or more and less than 200°C / hour, but is not limited to this range.

[0072] The heating rate TR2 is determined by the following method. A thermocouple is attached to a steel sheet having the above chemical composition and obtained by carrying out the above steps from hot rolling to skin pass, to prepare a sample steel sheet. The sample steel sheet to which the thermocouple is attached is heated, and the time from the start of the heating until the temperature reaches the finish annealing temperature T2 is measured. The heating rate TR2 is determined based on the measured time.

[0073] The atmosphere during the final annealing step is not particularly limited. For example, the atmosphere during the final annealing step may be a 20% H 2 and the remainder is N 2 and atmospheric gas (dry) consisting of 100% hydrogen (H 2 The cooling rate of the steel sheet after the finish annealing is not particularly limited. The cooling rate is, for example, 5 to 20°C / second.

[0074] When a core is made from a non-oriented electrical steel sheet, the steel sheet is punched and / or laminated. The punching and / or lamination of the steel sheet may be performed after the finish annealing step, or may be performed after the skin-pass rolling step and before the finish annealing step. When punching and / or lamination is performed before the finish annealing step, the finish annealing (annealing time of 2 hours or more at an annealing temperature of 850°C or higher and Ac1 temperature or lower) may also be performed as stress relief annealing (in other words, stress relief annealing may be performed instead of finish annealing under conditions equivalent to those of finish annealing).

[0075] In the manufacturing method of a non-oriented electrical steel sheet according to this embodiment, for example, shot blasting and / or pickling may be performed after the cooling step and before the cold rolling step among the above manufacturing steps. In shot blasting, shot blasting is performed on the hot-rolled steel sheet to destroy and remove scale formed on the surface of the hot-rolled steel sheet. In pickling, pickling treatment is performed on the hot-rolled steel sheet. For example, the pickling treatment uses an aqueous hydrochloric acid solution as the pickling bath. Pickling removes scale formed on the surface of the steel sheet. Shot blasting may be performed after the cooling step and before the cold rolling step, and then pickling may be performed. Alternatively, pickling may be performed after the cooling step and before the cold rolling step, without shot blasting. Alternatively, shot blasting may be performed after the cooling step and before the cold rolling step, without pickling treatment. Shot blasting and pickling are optional steps. Therefore, it is not necessary to perform both the shot blasting step and the pickling step.

[0076] <Insulating Coating Forming Step> The method for producing an electrical steel sheet according to this embodiment may further include forming an insulating coating on the surface of the steel sheet (non-oriented electrical steel sheet) after the final annealing step by coating after the final annealing step. The insulating coating forming step is an optional step. Therefore, coating does not necessarily have to be performed after the final annealing.

[0077] The type of insulating coating is not particularly limited. The insulating coating may be made of either an organic component or an inorganic component, and the insulating coating may contain both an organic component and an inorganic component. Examples of inorganic components include dichromate-boric acid-based, phosphoric acid-based, and silica-based resins. Examples of organic components include general acrylic, acrylic styrene-based, acrylic silicone-based, silicone-based, polyester-based, epoxy-based, and fluorine-based resins. Considering paintability, emulsion-type resins are preferred. An insulating coating that exhibits adhesive properties when heated and / or pressurized may be applied. Examples of insulating coatings with adhesive properties include acrylic, phenol-based, epoxy-based, and melamine-based resins.

[0078] The core according to the present embodiment can be obtained by subjecting the non-oriented electrical steel sheet according to the present embodiment obtained by the above-described method to a processing step and / or an annealing (stress relief) step as necessary. For example, if the non-oriented electrical steel sheet is not punched and / or laminated before the finish annealing step, the core can be obtained by punching the non-oriented electrical steel sheet into a predetermined shape, laminating multiple sheets, and then performing stress relief annealing instead of finish annealing. The punching conditions are not particularly limited. For example, a progressive die can be used to consistently manufacture the non-oriented electrical steel sheet up to the next lamination step. The fixing method during lamination is also not particularly limited. For example, methods such as caulking, bonding, and welding can be used. When stress relief annealing is performed instead of finish annealing, annealing is performed at an annealing temperature of 850°C or higher and the Ac1 temperature or lower for 2 hours or longer. On the other hand, if the non-oriented electrical steel sheet is punched and / or laminated to form a core shape before the finish annealing step, the non-oriented electrical steel sheet after the finish annealing step can also be used as the core as is.

[0079] Furthermore, the rotating electric machine according to this embodiment is obtained by winding the core according to this embodiment to form a rotor or a stator, then combining this with another rotor or stator, and fixing the pair of rotors and stators in a case.

[0080] Next, the non-oriented electrical steel sheet of the present invention will be specifically described with reference to examples. The examples shown below are merely examples of the non-oriented electrical steel sheet according to the embodiment of the present invention, and the non-oriented electrical steel sheet according to the present invention is not limited to the examples below.

[0081] Molten steel was cast to produce ingots having the chemical compositions shown in Table 1 (units: mass %, balance: Fe and impurities). In Table 1, the left side of the formula represents the value of the left side of the formula (1). The total of coarse precipitate forming elements such as Mg represents the total of one or more elements selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd.

[0082] No. 8 had a chemical composition in which α was stable and α-γ transformation did not occur. The prepared ingot was heated to 1150°C and held for 1 hour, and then hot-rolled to a finish rolling temperature FT shown in Table 2. After completion of hot rolling (after passing through the final pass), the time until the start of cooling was set as shown in Table 2, and cooling was performed so that the temperature of the steel sheet 3 seconds after the start of cooling reached the temperature shown in Table 2. The hot-rolled steel sheet obtained in this manner was not subjected to hot-rolled sheet annealing, but was descaled by pickling and cold-rolled at a reduction ratio RR1 shown in Table 2. Then, in an atmosphere consisting of 20% hydrogen and 80% nitrogen by volume, the steel sheet was heated to an intermediate annealing temperature T1 shown in Table 2 at a heating rate shown in Table 2, and held at T1 for 30 seconds, thereby performing intermediate annealing. After holding, the steel sheet was cooled to 50°C or less at an average cooling rate of 20.0°C / s. After the intermediate annealing, the cold rolling was performed by skin-pass rolling at a reduction rate RR2 shown in Table 2. Next, the steel sheets after skin-pass rolling were subjected to finish annealing in a 100% hydrogen atmosphere at a temperature increase rate of 100°C / hour at the finish annealing temperature T2 shown in Table 2. At this time, the holding time at the finish annealing temperature T2 was 2 hours. In this manner, non-oriented electrical steel sheets were produced. However, since No. 7 broke into two pieces during cold rolling, subsequent processes were not performed.

[0083] To investigate the texture of the obtained non-oriented electrical steel sheets, a portion of the steel sheet was cut off to obtain a test specimen, which was then subjected to thickness reduction processing, in which the test specimen was reduced to half its thickness from the surface. The measurement surface was a surface parallel to the rolled surface at a depth of half the sheet thickness from the surface exposed by the reduction of the test specimen, and the {411}<011> ratio and {111} ratio were measured using SEM-EBSD under the conditions described above. The average grain size of the measurement surface was also measured using the intercept method of JIS G0551 (2020).

[0084] The magnetic properties of the obtained non-oriented electrical steel sheets were measured in the following manner.

[0085] <Magnetic Flux Density> Measurement samples were prepared by cutting 55 mm square (55 mm wide x 55 mm long) single sheet magnetic property test specimens in two directions: 0° and 45° to the rolling direction. The magnetic flux densities B50 of these two specimens were determined at angles of 0°, 45°, 90°, and 135° to the rolling direction in accordance with JIS C2556 (2015). The average of the magnetic flux densities at 45° and 135° to the rolling direction was designated B50D, and the average of the magnetic flux densities at 0° and 90° to the rolling direction was designated B50L.

[0086] <Iron loss and iron loss deterioration rate> For the iron loss W10 / 400, the above measurement samples were taken in a direction at 45° to the rolling direction, and the iron losses in the 45° and 135° directions relative to the rolling direction were determined in accordance with JIS C2556 (2015), and the average was taken as W10D / 400D. Furthermore, for the iron loss deterioration rate Wx [%] of the iron loss W10 / 50 under compressive stress, the iron loss W10 / 50 (45° direction) without stress was taken as W10 / 50(0), and the iron loss W10 / 50 (45° direction) under a compressive stress of 10 MPa was taken as W10 / 50(10), and the iron loss deterioration rate Wx was calculated using the following formula. Wx = {W10 / 50(10) - W10 / 50(0)} / W10 / 50(0) If the iron loss degradation rate of W10 / 50 under compressive stress in a direction at 45° to the rolling direction is 40% or less, it was determined that the iron loss degradation rate (stress sensitivity) was low.

[0087]

[0088]

[0089]

[0090] As can be seen from Tables 1 to 3, inventive examples Nos. 1 to 5 and 19, the chemical compositions and textures were within the ranges of the present invention, and the magnetic properties (magnetic flux density, iron loss, and iron loss degradation rate) were excellent. In contrast, in comparative examples Nos. 6, 8 to 18, and 20, one or more of the chemical compositions, textures, and magnetic properties were outside the ranges of the present invention.

[0091] According to the present invention, it is possible to provide a non-oriented electrical steel sheet having low stress sensitivity and excellent magnetic properties in directions at angles of ±45 degrees to the rolling direction, a core manufactured using this non-oriented electrical steel sheet, and a rotating electrical machine manufactured using this core, which have high industrial applicability.

Claims

1. In mass percent, C: 0.0100% or less, Si: 1.50% to 4.00%, sol. containing Al: 0.0001% to 1.00%, S: 0.0100% or less, N: 0.0100% or less, one or more selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total, Co: 0.000% to 1.000%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total, The Mn content, in mass%, is [Mn], the Ni content is [Ni], the Cu content is [Cu], the Si content is [Si], and the sol. Al content is [sol. a non-oriented electrical steel sheet having a chemical composition which satisfies the following formula (1) where [Al] and P content are [P], with the balance consisting of Fe and impurities; when the area ratio of crystal grains of {hkl}<uvw> orientation to a whole field of view when a plane parallel to the rolled surface at a depth of 1 / 2 the sheet thickness from the surface is measured by SEM-EBSD, and expressed as Ahkl-uvw, A411-011 is 15.0% or more; B50D which is an average of magnetic flux density in a 45 degree direction to the rolling direction and magnetic flux density in a 135 degree direction to the rolling direction is 1.70 T or more; and W10D / 400D which is an average of iron loss in a 45 degree direction to the rolling direction and iron loss in a 135 degree direction to the rolling direction is 10.4 W / kg or less. (2×[Mn]+2.5×[Ni]+[Cu])-([Si]+2×[sol.Al]+4×[P])≧1.50%...(1) 2. The non-oriented electrical steel sheet according to claim 1, characterized in that, when the average of the magnetic flux density in a 0 degree direction with respect to the rolling direction and the magnetic flux density in a 90 degree direction with respect to the rolling direction is defined as B50L, the B50D and the B50L satisfy the following formula (2): B50D / B50L≧1.05 (2) 3. A core made of a non-oriented electrical steel sheet, the non-oriented electrical steel sheet containing, in mass %, C: 0.0100% or less, Si: 1.50% to 4.00%, sol. containing Al: 0.0001% to 1.00%, S: 0.0100% or less, N: 0.0100% or less, one or more selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total, Co: 0.000% to 1.000%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total, The Mn content, in mass%, is [Mn], the Ni content is [Ni], the Cu content is [Cu], the Si content is [Si], and the sol. Al content is [sol. a chemical composition satisfying the following formula (1) where [Al] and P content are [P], with the balance consisting of Fe and impurities; when the area ratio of crystal grains of {hkl}<uvw> orientation to a whole field of view when a plane parallel to the rolling surface at a depth of 1 / 2 the sheet thickness from the surface is measured by SEM-EBSD, and expressed as Ahkl-uvw, A411-011 is 15.0% or more; B50D, which is an average of magnetic flux density in a 45 degree direction to the rolling direction and magnetic flux density in a 135 degree direction to the rolling direction, is 1.70 T or more; and W10D / 400D, which is an average of iron loss in a 45 degree direction to the rolling direction and iron loss in a 135 degree direction to the rolling direction, is 10.4 W / kg or less. (2×[Mn]+2.5×[Ni]+[Cu])-([Si]+2×[sol.Al]+4×[P])≧1.50%...(1) 4. A motor comprising a stator, a rotor arranged on the inner circumference of the stator, and a case that is in close contact with the stator from the outer circumference of the stator and fixes the stator, wherein the non-oriented electromagnetic steel sheet constituting the core of at least one of the stator and the rotor contains, in mass %, C: 0.0100% or less, Si: 1.50% to 4.00%, sol. containing Al: 0.0001% to 1.00%, S: 0.0100% or less, N: 0.0100% or less, one or more selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total, Co: 0.000% to 1.000%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total, The Mn content, in mass%, is [Mn], the Ni content is [Ni], the Cu content is [Cu], the Si content is [Si], and the sol. Al content is [sol. a rotating electric machine having a chemical composition satisfying the following formula (1) where [Al] and P content are [P], with the balance consisting of Fe and impurities; when the area ratio of crystal grains of {hkl}<uvw> orientation to a whole field of view when a plane parallel to the rolling surface at a depth of 1 / 2 the sheet thickness from the surface is measured by SEM-EBSD, and expressed as Ahkl-uvw, A411-011 is 15.0% or more; B50D which is an average of magnetic flux density in a 45 degree direction to the rolling direction and magnetic flux density in a 135 degree direction to the rolling direction is 1.70 T or more; and W10D / 400D which is an average of iron loss in a 45 degree direction to the rolling direction and iron loss in a 135 degree direction to the rolling direction is 10.4 W / kg or less. (2×[Mn]+2.5×[Ni]+[Cu])-([Si]+2×[sol.Al]+4×[P])≧1.50%...(1)