Plated steel material

MYPI2025005678A0Undetermined Publication Date: 2024-10-11NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005678
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-11
Filing Date
2024-04-11
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing plated steel materials lack effective red rust resistance and corrosion resistance for the base metal, despite advancements in corrosion resistance for the plating layer.

Method used

A plated steel material with a Zn-Al-Mg alloy layer containing specific elements like La and Ce, and a ternary eutectic structure where the (100) plane of the η-Zn phase is oriented parallel to the surface, enhancing sacrificial corrosion protection and corrosion resistance.

Benefits of technology

The solution provides excellent red rust resistance and base metal corrosion resistance by ensuring the (100) plane of the η-Zn phase is oriented parallel to the surface, improving the sacrificial corrosion protection and corrosion resistance of the plated steel material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005678_DRAWING_001
    Figure PI2025005678_DRAWING_001
Patent Text Reader

Abstract

ABSTRACT PLATED STEEL MATERIAL The plated steel material includes a steel material and a plated layer disposed on a surface of the steel material, and the plated layer has a predetermined chemical composition, and the plated layer has a diffraction intensity obtained from a result of X-ray diffraction measurement, the diffraction intensity satisfying a predetermined formula. FIG. 1
Need to check novelty before this filing date? Find Prior Art

Description

Plated steel

[0001] This application claims priority to Japanese Patent Application No. 2023-064063, filed on April 11, 2023, the contents of which are incorporated herein by reference.

[0002] Steel materials having a Zn-plated layer containing Al and Mg formed on the surface thereof (Zn-Al-Mg-plated steel materials) have excellent corrosion resistance, and therefore are widely used as materials for structural members that require corrosion resistance, such as building materials.

[0003] For example, Patent Document 1 describes a plated steel sheet comprising a steel sheet and a plating layer formed on the surface of the steel sheet, the plating layer containing, in average, 0 to 90 mass % Al, 0 to 10 mass % Mg, with the remainder containing Zn and impurities, a patterned portion and a non-patterned portion arranged to have a predetermined shape, the patterned portion and the non-patterned portion each including one or two of a first region and a second region, the absolute value of the difference between the area ratio of the first region in the patterned portion and the area ratio of the first region in the non-patterned portion being 30% or more, the first region being a region having an orientation ratio of 3.5 or more, and the second region being a region having an orientation ratio of less than 3.5.

[0004] Patent Document 2 describes a Zn-Al-Mg-plated steel sheet that includes a steel sheet and a plating layer containing 4 mass % or more and 22 mass % or less of Al, 1 mass % or more and 5 mass % or less of Mg, with the balance being Zn and unavoidable impurities, in which a diffraction intensity ratio I(200) / I(111), which is the ratio of the X-ray diffraction intensity I(200) of the (200) plane of the Al phase to the X-ray diffraction intensity I(111) of the (111) plane of the Al phase, in a cross section of the plating layer parallel to the surface of the plating layer, is 0.8 or more.

[0005] In recent years, plated steel materials for building applications such as roofing and wall materials have been required to have excellent red rust resistance, which inhibits the occurrence of red rust on the steel substrate when the steel substrate is exposed, and excellent base steel corrosion resistance, which inhibits an increase in the corrosion depth of the steel substrate. However, in the prior art, there has been little research into improving both red rust resistance and base steel corrosion resistance.

[0006] Patent Document 1 discloses that the diffraction peak intensity I of the (0002) plane of the Zn phase 0002 and the diffraction peak intensity of the (10-11) plane I 10-11 When a region where the intensity ratio to the non-patterned portion is 3.5 or more is defined as a first region, and a region where the intensity ratio is less than 3.5 is defined as a second region, it is possible to intentionally make characters, designs, etc. appear on the surface of the plating layer by making the difference between the area ratio of the first region in the patterned portion and the area ratio of the first region in the non-patterned portion 30% or more, but red rust resistance and corrosion resistance of the base steel are not considered.

[0007] In Patent Document 2, the orientation of the Al phase in the plating layer is controlled to give the plating layer a fine-grained, smooth, pear-skin appearance with many shiny portions, but red rust resistance and corrosion resistance of the base steel are not considered.

[0008] Japanese Patent Application Publication No. 2021-85086 International Publication No. 2011 / 001662

[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a plated steel material that is excellent in red rust resistance and base steel corrosion resistance.

[0010] In order to solve the above problems, the present invention employs the following configuration: [1] A steel material and a plating layer on the steel material, wherein the plating layer has a chemical composition, in mass %, of Al: 6.0 to 30.0%, Mg: 3.0 to 15.0%, Fe: 0.01 to 15.00%, Si: 0 to 2.0%, and Ca: 0 to 2.00%, and wherein the plating layer contains one or both of La and Ce in a total amount of 0.005 to 0.500%. Sb: 0-0.50%, Pb: 0-0.50%, Cu: 0-1.00%, Sn: 0-1.00%, Ti: 0-1.00%, Cr: 0-1.00%, Nb: 0-1 .00%, Zr: 0 to 1.00%, Ni: 0 to 1.000%, Mn: 0 to 1.00%, Mo: 0 to 1.00%, Ag: 0 to 1.00%, Li: 0 to 1.00%, B A plated steel material containing one or more elements selected from the group consisting of: I(100), Y(100), P(100), Sr(100), Co(100), Bi(100), In(100), V(100), and W(100), with a total content of these elements being 0 to 5.0%, and the balance consisting of Zn and impurities, wherein the diffraction intensity obtained from X-ray diffraction measurement of the plated layer satisfies the following formula (1): 0.15≦I(100) Zn / {I(002) Zn +I(101) Zn +I(100) Zn}≦3.00 ... (1) where I(100) in formula (1) Zn is the diffraction intensity of (100) of the η-Zn phase, and I(002) Zn is the diffraction intensity of (002) of the η-Zn phase, and I(101) Zn is the diffraction intensity of (101) of the η-Zn phase, and I(100) Znis the (100) diffraction intensity of the η-Zn phase. [2] The plated steel material according to [1], wherein the Al and Mg contents of the plating layer are 10.0 to 25.0% Al and 4.5 to 15.0% Mg, respectively. [3] The plated steel material according to [1] or [2], wherein the total content of one or both of La and Ce in the plating layer is 0.010 to 0.500%, and the number of at least one of the LaCe-containing intermetallic compound phase, the La-containing intermetallic compound phase, and the Ce-containing intermetallic compound phase is 1 or more within a 200 μm × 200 μm field of view of the surface texture when the plating layer is viewed in plan. [4] The plated steel material according to any one of [1] to [3], wherein the total content of one or two of La and Ce in the plated layer is 0.050 to 0.500%, and the number of at least one of LaCe-containing intermetallic compound phases, La-containing intermetallic compound phases, and Ce-containing intermetallic compound phases in a 200 μm × 200 μm field of view in a plan view of the plated layer is 3 or more. [5] The surface structure of the plated layer in a plan view contains [α / MgZn 2 [6] The plated steel material according to any one of [1] to [4], wherein the area ratio of the eutectic structure is 5 to 70%. [6] The plated steel material according to any one of [1] to [5], wherein the diffraction intensity obtained from the X-ray diffraction measurement of the plated layer satisfies the following formula (2): 0.25≦I(100): Zn / {I(002) Zn +I(101) Zn +I(100) Zn}≦3.00 ... (2) [7] The Sn content of the plating layer is, in mass%, Sn: 0.05 to 0.50%, and the X-ray diffraction measurement result of the plating layer shows that Mg 2 The plated steel material according to any one of [1] to [6], in which a Sn phase is detected.

[0011] According to the present invention, a plated steel material having excellent red rust resistance and base steel corrosion resistance can be provided.

[0012] 1 is a cross-sectional schematic view of a plated steel material according to an embodiment of the present invention.

[0013] The sacrificial corrosion protection properties of a plating layer are achieved by forming a plating layer containing an element (e.g., Zn, Mg) that has a higher ionization tendency than the base steel on the surface of a steel material, and by causing the plating layer to corrode preferentially relative to the base steel.

[0014] Therefore, the inventors of the present invention have conducted extensive research to improve the sacrificial corrosion protection of a Zn plating layer containing Al and Mg. The η-Zn phase contained in the plating layer has a hexagonal crystal structure, which includes various crystal orientation planes. The corrosion resistance of these crystal orientation planes is not uniform across all orientation planes. For example, the (002) plane of the η-Zn phase is a dense crystal orientation plane with a relatively high Zn atomic density, making Zn itself relatively difficult to dissolve and therefore considered to have relatively high corrosion resistance. On the other hand, the (100) plane of the η-Zn phase is a crystal orientation plane with a lower Zn atomic density than the (002) plane, making Zn itself relatively easy to dissolve. However, although the corrosion resistance of Zn itself is low, the corrosion products generated by the corrosion of Zn protect the base steel from corrosion, and therefore the sacrificial corrosion protection against the base steel is considered to be high. Therefore, the present inventors thought that the sacrificial corrosion protection properties of the Zn plating layer containing Al and Mg, specifically the red rust resistance and the corrosion protection properties of the base steel, could be improved by orienting the (100) plane of the η-Zn phase parallel to the surface of the plating layer.

[0015] Therefore, the inventors attempted to orient the (100) plane of the η-Zn phase contained in the coating layer parallel to the surface of the coating layer. When a Zn coating layer containing Al and Mg is solidified from a molten state, the α phase first crystallizes, followed by the MgZn phase. 2 The α-phase and η-Zn phase crystallize, and further, the α-phase and MgZn 2 The researchers discovered that a ternary eutectic structure containing the η-Zn phase and the α-Zn phase is formed. It was found that when a large amount of dendritic α-phase crystallizes, the ternary eutectic structure containing the η-Zn phase is oriented in a random direction. They then roughened the surface of the steel material and added La or Ce to the coating layer, and controlled the cooling conditions. This resulted in suppressing the crystallization of the α-phase and promoting the crystallization of the ternary eutectic structure, originating near the interface between the coating layer and the base steel. As a result, the (100) plane of the η-Zn phase contained in the ternary eutectic structure was oriented parallel to the surface of the coating layer.

[0016] Hereinafter, a plated steel material according to an embodiment of the present invention will be described. The plated steel material according to this embodiment comprises a steel material and a plating layer disposed on the surface of the steel material, and the plating layer has a chemical composition, in mass %, of Al: 6.0 to 30.0%, Mg: 3.0 to 15.0%, Fe: 0.01 to 15.00%, Si: 0 to 2.0%, Ca: 0 to 2.00%, and a total of 0.005 to 0.500% of one or two of La and Ce, Sb: 0 to 0.50%, Pb: 0 to 0.50%, Cu: 0 to 1.00%, Sn: 0 to 1.00%, Ti: 0 to 1.00%, Cr: 0 to 1.00%, Nb: 0 to 1.00%, Zr: 0 to 1.00%, and Ni: 0 to 1.00%. 0%, Mn: 0-1.00%, Mo: 0-1.00%, Ag: 0-1.00%, Li: 0-1.00%, B: 0-0.500%, Y: 0-0.50%, P: 0-0.50%, Sr: 0-0.50%, Co: 0-0.500%, Bi: 0-0.500%, In: 0-0.50%, V: 0-0.500%, and W: 0-0.50%, the total of these elements being 0-5.0%, with the balance being Zn and impurities, and the diffraction intensity obtained from X-ray diffraction measurement of the plating layer satisfies the following formula (1):

[0017] 0.15≦I(100) Zn / {I(002) Zn +I(101) Zn +I(100) Zn}≦3.00 ... (1)

[0018] However, I(100) in formula (1) Zn is the diffraction intensity of the (100) plane of the η-Zn phase, and I(002) Zn is the diffraction intensity of the (002) plane of the η-Zn phase, and I(101) Zn is the diffraction intensity of the (101) plane of the η-Zn phase, and I(100) Zn is the diffraction intensity of the (100) plane of the η-Zn phase.

[0019] In the following description, the "%" used to indicate the content of each element in the chemical composition means "mass %." The content of an element in the chemical composition may be expressed as the element concentration (e.g., Zn concentration, Mg concentration, etc.). "Red rust resistance" refers to the property of suppressing the occurrence of red rust on exposed steel parts (e.g., cut end surfaces of plated steel, cracked areas of the plated layer during processing, and areas where the steel is exposed due to peeling of the plated layer). "Base steel corrosion resistance" refers to the property of suppressing the increase in corrosion depth when the steel corrodes at exposed steel parts. "Flat surface corrosion resistance" refers to the corrosion-resistant property of the plated layer (specifically, a Zn-Al-Mg alloy layer) itself. "Plated layer" refers to a plated coating produced by a so-called hot-dip galvanizing process.

[0020] As shown in Fig. 1, the plated steel material 1 according to this embodiment has a steel material 11. There are no particular limitations on the shape of the steel material 11, and an example of the steel material 11 is a steel plate. The steel material 11 may also be a formed, bare steel material such as a steel pipe, a civil engineering and construction material (such as a fence, a corrugated pipe, a drainage ditch cover, a sand-flying prevention plate, a bolt, a wire mesh, a guardrail, a water cut-off wall, etc.), a home appliance component (such as a housing for an outdoor unit of an air conditioner), or an automobile part (such as an undercarriage component). The forming process may be any of various plastic processing techniques, such as pressing, roll forming, and bending.

[0021] The material of the steel material 11 is not particularly limited. The steel material 11 can be various steel materials such as general steel, Al-killed steel, ultra-low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steels containing strengthening elements such as Ni and Cr). The steel material 11 may also be a hot-rolled steel sheet, hot-rolled steel strip, cold-rolled steel sheet, or cold-rolled steel strip described in JIS G 3302:2010. There are also no particular limitations on the method for manufacturing the steel sheet (hot rolling method, pickling method, cold rolling method, etc.) and the specific manufacturing conditions thereof.

[0022] Furthermore, the steel material 11 serving as the plating base sheet may be a pre-plated steel material in which the surface of the steel material 11 is pre-plated. An example of the pre-plated steel material is a Ni pre-plated steel material having a Ni plating on the steel material 11. The pre-plated steel material can be obtained, for example, by electrolytic treatment or displacement plating. Electrolytic treatment is performed by immersing the base steel material in a sulfate bath or chloride bath containing metal ions of various pre-plating components. Displacement plating is performed by immersing the base steel material in an aqueous solution containing metal ions of various pre-plating components and having the pH adjusted with sulfuric acid, thereby causing displacement deposition of the metal.

[0023] The plated steel material 1 according to this embodiment has a plating layer 12 on a steel material 11. The plating layer 12 of the plated steel material 1 according to this embodiment is mainly composed of a Zn-Al-Mg alloy layer due to its chemical composition, which will be described later. Furthermore, the plating layer 12 of the plated steel material 1 according to this embodiment may include an Fe-Al-based interfacial alloy layer between the steel material 11 and the Zn-Al-Mg alloy layer. That is, the plating layer 12 may have a single-layer structure of a Zn-Al-Mg alloy layer, or a multilayer structure including a Zn-Al-Mg alloy layer and an Fe-Al-based interfacial alloy layer. Furthermore, the Fe-Al-based interfacial alloy layer may contain Ni.

[0024] The chemical composition of the plating layer according to this embodiment is composed of Zn and other alloying elements. The chemical composition of the plating layer will be described in detail below. Note that elements with a lower limit of 0% concentration are not essential for solving the problems of the plated steel material according to this embodiment, but are optional elements that are allowed to be included in the plating layer for the purpose of improving characteristics, etc.

[0025] <Al: 6.0 to 30.0%> Al forms an α-phase, which is a solid solution with Zn, and contributes to improving flat surface corrosion resistance, sacrificial corrosion protection, and workability. Therefore, the Al concentration is set to 6.0% or more. The Al concentration may be set to 10.0% or more, 12.0% or more, or 15.0% or more. On the other hand, if Al is excessive, the Mg concentration and Zn concentration decrease relatively, deteriorating red rust resistance and base steel corrosion protection. Therefore, the Al concentration is set to 30.0% or less. The Al concentration may also be set to 28.0% or less, 25.0% or less, or 20.0% or less.

[0026] <Mg: 3.0 to 15.0%> Mg is an essential element for ensuring flat surface corrosion resistance, red rust resistance, and corrosion resistance of the base steel. Therefore, the Mg concentration is set to 3.0% or more. The Mg concentration may be set to 4.5% or more or 6.0% or more. On the other hand, if the Mg concentration is excessive, workability, particularly powdering resistance, may deteriorate, and flat surface corrosion resistance may also deteriorate. Therefore, the Mg concentration is set to 15.0% or less. The Mg concentration may also be set to 12.0% or less, 10.0% or less, or 8.0% or less.

[0027] <Fe: 0.01% to 15.00%> The plating layer may contain 0.01% or more of Fe. It has been confirmed that an Fe concentration of 15.00% or less does not adversely affect the performance of the plating layer. The Fe concentration may be, for example, 0.05% or more, 0.10% or more, 0.50% or more, or 1.00% or more. The Fe concentration may be, for example, 10.00% or less, 5.00% or less, 2.00% or less, or 1.00% or less. Because Fe may be mixed in from the steel material, the Fe concentration may be 0.05% or more.

[0028] <Si: 0% to 2.0%> The Si concentration may be 0%. On the other hand, Si contributes to improving flat surface corrosion resistance. Therefore, the Si concentration may be 0.05% or more, 0.1% or more, 0.2% or more, or 0.5% or more. On the other hand, if the Si concentration is excessive, flat surface corrosion resistance, red rust resistance, and base steel corrosion resistance deteriorate. Therefore, the Si concentration is set to 2.0% or less. The Si concentration may also be 1.5% or less, 1.0% or less, or 0.5% or less.

[0029] <Ca: 0% to 2.00%> The Ca concentration may be 0%. On the other hand, Ca is an element that can adjust the amount of Mg elution that is optimal for imparting flat surface corrosion resistance. Therefore, the Ca concentration may be 0.05% or more, 0.10% or more, or 0.50% or more. On the other hand, if the Ca concentration is excessive, flat surface corrosion resistance and workability deteriorate. Therefore, the Ca concentration is set to 2.00% or less. The Ca concentration may also be set to 1.00% or less, 0.50% or less, or 0.10% or less.

[0030] <Total of One or Both of La and Ce: 0.005 to 0.500%> The inclusion of either or both of La and Ce in the coating layer contributes to improved red rust resistance and corrosion resistance against the steel substrate. If the total of La and Ce is less than 0.005%, the red rust resistance and corrosion resistance against the steel substrate cannot be improved. Furthermore, if the total of La and Ce exceeds 0.500%, corrosion resistance in flat portions deteriorates. Therefore, the total of one or both of La and Ce is set to 0.005 to 0.500%. The total of La and Ce may be 0.008% or more, 0.010% or more, or 0.050% or more. Furthermore, the total of La and Ce may be 0.200% or less, or 0.100% or less. The inclusion of La and Ce suppresses the crystallization of the α-phase when the coating layer solidifies, which makes it easier for the (100) plane of the η-Zn phase, which is contained in large amounts in the ternary eutectic structure, to be oriented parallel to the surface of the coating layer. This is thought to result in improved red rust resistance and corrosion protection of the base steel.

[0031] Furthermore, the plating layer according to this embodiment contains Sb: 0 to 0.50%, Pb: 0 to 0.50%, Cu: 0 to 1.00%, Sn: 0 to 1.00%, Ti: 0 to 1.00%, Cr: 0 to 1.00%, Nb: 0 to 1.00%, Zr: 0 to 1.00%, Ni: 0 to 1.000%, Mn: 0 to 1.00%, Mo: 0 to 1.00%, Ag: 0 One or more elements selected from the group consisting of: Cr: 0.00% or less, Li: 0.00% or less, B: 0.00% or less, Y: 0.00% or less, P: 0.00% or less, Sr: 0.00% or less, Co: 0.00% or less, Bi: 0.00% or less, In: 0.00% or less, V: 0.00% or less, and W: 0.00% or less may be contained. The total of these elements is 0.0% or less. If the total exceeds 5.0%, the flat corrosion resistance, red rust resistance, and base steel corrosion resistance may be reduced. Furthermore, since these elements are optional addition elements, the total amount may be 0%.

[0032] <Sb, Pb: 0 to 0.50% each> The concentrations of Sb and Pb may be 0%. On the other hand, Sb and Pb contribute to improving red rust resistance and corrosion resistance of the base steel. Therefore, the concentrations of Sb and Pb may be 0.05% or more, 0.10% or more, or 0.15% or more. On the other hand, excessive concentrations of Sb and Pb deteriorate the corrosion resistance of flat surfaces. Therefore, the concentrations of Sb and Pb are set to 0.50% or less. The concentrations of Sb and Pb may also be 0.40% or less, 0.30% or less, or 0.25% or less.

[0033] <Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li: 0 to 1.00% each> The concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may each be 0%. However, these elements contribute to improving red rust resistance and base steel corrosion resistance. Therefore, the concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may each be 0.05% or more, 0.08% or more, or 0.10% or more. However, excessive concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li deteriorate flat surface corrosion resistance. Therefore, the concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li are each set to 1.00% or less. The concentration of each of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may be 0.80% or less, 0.70% or less, or 0.60% or less.

[0034] <Ni: 0 to 1.000%> The Ni concentration may be 0%. However, these elements contribute to improving red rust resistance and corrosion resistance of the base steel. Therefore, the Ni concentration may be 0.050% or more, 0.080% or more, or 0.100% or more. However, if the Ni concentration is excessive, the corrosion resistance of the flat surface portion deteriorates. Therefore, the Ni concentration is set to 1.000% or less. The Ni concentration may also be 0.800% or less, 0.700% or less, or 0.600% or less.

[0035] <Sn: 0 to 1.00%> The Sn concentration may be 0%. On the other hand, Sn is an element that forms an intermetallic compound with Mg and improves the red rust resistance of the plating layer and the corrosion protection of the base steel. Therefore, the Sn concentration may be 0.01% or more, 0.05% or more, or 0.10% or more. However, if the Sn concentration is excessive, planar corrosion resistance will deteriorate. Therefore, the Sn concentration is set to 1.00% or less. The Sn concentration may also be 0.50% or less, 0.30% or less, or 0.20% or less.

[0036] <B: 0 to 0.500%> The B concentration may be 0%. On the other hand, B contributes to improving red rust resistance and base steel corrosion resistance. Therefore, each B concentration may be 0.100% or more, 0.150% or more, or 0.200% or more. On the other hand, if the B concentration is excessive, flat surface corrosion resistance deteriorates. Therefore, each B concentration is set to 0.500% or less. Each B concentration may also be set to 0.400% or less, or 0.300% or less.

[0037] <Y, P, and Sr: 0 to 0.50% each> The concentrations of Y, P, and Sr may each be 0%. On the other hand, Y, P, and Sr contribute to improving red rust resistance and base steel corrosion resistance. Therefore, the concentrations of Y, P, and Sr may each be 0.10% or more, 0.15% or more, or 0.20% or more. On the other hand, excessive concentrations of Y, P, and Sr deteriorate the corrosion resistance of flat surfaces. Therefore, the concentrations of B, Y, P, and Sr each are set to 0.50% or less. The concentrations of Y, P, and Sr may each be 0.40% or less, or 0.30% or less.

[0038] <Co, Bi, V: 0 to 0.500% each> The concentrations of Co, Bi, and V may each be 0%. On the other hand, Co, Bi, and V contribute to improving red rust resistance and base steel corrosion resistance. Therefore, the concentrations of Co, Bi, and V may each be 0.100% or more, 0.150% or more, or 0.200% or more. On the other hand, excessive concentrations of Co, Bi, and V deteriorate the corrosion resistance of flat portions. Therefore, the concentrations of Co, Bi, and V are each set to 0.500% or less. The concentrations of Co, Bi, and V may each be set to 0.400% or less, or 0.300% or less.

[0039] <In, W: 0 to 0.50% each> The concentrations of In and W may each be 0%. On the other hand, In and W contribute to improving red rust resistance and corrosion resistance of the base steel. Therefore, the concentrations of In and W may each be 0.10% or more, 0.15% or more, or 0.20% or more. On the other hand, excessive concentrations of In and W deteriorate the corrosion resistance of flat surfaces. Therefore, the concentrations of In and W are each set to 0.50% or less. The concentrations of In and W may each be set to 0.40% or less, or 0.30% or less.

[0040] <Balance: Zn and Impurities> The balance of the components of the plating layer according to this embodiment is Zn and impurities. Zn is an element that provides the plating layer with flat portion corrosion resistance, red rust resistance, and corrosion protection against steel substrate. In this embodiment, "impurities" refers to elements that are mixed in due to the manufacturing environment, etc., and elements that are tolerated within a range that does not adversely affect the properties of the plated steel according to this embodiment. For example, trace amounts of elements other than Fe may be mixed in as impurities into the plating layer due to mutual atomic diffusion between the base steel and the plating bath.

[0041] The chemical composition of the plating layer is measured by the following method. For example, a plated steel material is cut into a size of 30 mm x 30 mm to obtain a measurement sample. Next, the plating layer of the measurement sample is stripped and dissolved using a 10% aqueous hydrochloric acid solution containing 0.06 mass% of an inhibitor (Ivit 710K, manufactured by Asahi Chemical Industry Co., Ltd.) that suppresses corrosion of steel materials, to obtain an acid solution. The obtained acid solution is then subjected to ICP analysis. This allows the chemical composition of the plating layer to be obtained. Note that when cutting the plated steel material, it is preferable to avoid the edges and welds of the plated steel material. There are no particular restrictions on the type of acid, as long as it is an acid that can dissolve the plating layer. For example, 10% by volume of HCl is used. Note that the chemical composition is measured three times using the above method, and the average of the measurements is used as the chemical composition of the plating layer.

[0042] Next, the metal structure of the plating layer will be described.

[0043] The plating layer contains α-phase and MgZn 2 The α phase contains a fine Al phase and a fine Zn phase. 2 The phase is partially lamellar binary eutectic structure (α phase / MgZn2 eutectic structure of α phase / MgZn 2 However, when the α phase and MgZn eutectic structure are contained, the corrosion resistance of the flat surface of the coating layer is further improved. 2 The excessive precipitation of the phase causes the formation of the α phase / MgZn 2 When a large amount of the eutectic structure of α-Zn is contained, the proportion of the η-Zn phase becomes relatively small, and the red rust resistance and corrosion resistance of the base steel deteriorate. 2 The area ratio of the eutectic structure of [α phase / MgZn] may be in the range of 70% or less, in the range of 5 to 70%, or in the range of 10 to 70%. 2 The eutectic structure of the alloy may be 0% or more than 0%.

[0044] In addition, the plating layer of this embodiment contains α-phase and MgZn 2 In addition to the α-Zn phase, the η-Zn phase is also present. The η-Zn phase is at least partially composed of the α-phase and MgZn 2 The η-Zn phase forms a ternary eutectic structure together with the η-Zn phase. The η-Zn phase may be contained in the plating layer as a massive η-Zn phase.

[0045] In addition, when the plating layer contains 0.05 to 0.5% Sn, the plating layer contains Mg 2 The Sn phase is definitely included. 2 The Sn phase may be contained even when the Sn content is 0.05% or less. 2 Since the Sn phase is present in a small amount, its presence can be confirmed by X-ray diffraction measurement. 2 The inclusion of the Sn phase further improves the red rust resistance of the plated steel material.

[0046] X-ray diffraction measurement was performed using Kα rays from a Cu tube, and if a peak was detected at 23.4±0.3°, it was determined that the Mg2Sn phase was present. Using an X-ray diffractometer (Rigaku Corporation, model number RINT-TTR III), X-ray output was 50 kV, 300 mA, copper target, goniometer TTR (horizontal goniometer), Kβ filter slit width 0.05 mm, longitudinal limiting slit width 2 mm, receiving slit width 8 mm, receiving slit 2 open, and measurement conditions were a scan speed of 5° / min, a step width of 0.01°, and a scan axis 2θ (5 to 90°).

[0047] Furthermore, the plating layer may contain one or more of a LaCe-containing intermetallic compound phase, a La-containing intermetallic compound phase, and a Ce-containing intermetallic compound phase, as described below.

[0048] The plating layer may contain other phases as the balance, such as an Al—Ca—Si phase.

[0049] Next, the crystal orientation of the η-Zn phase will be described. In the coating layer of this embodiment, the X-ray diffraction intensity obtained from the X-ray diffraction measurement of the coating layer must satisfy the relationship of the following formula (1). When the following formula (1) is satisfied, the (100) plane of the η-Zn phase is oriented parallel to the surface of the coating layer, improving both the red rust resistance and the corrosion protection of the base steel. It is more preferable that the following formula (2) is satisfied. I(100) Zn / {I(002) Zn +I(101) Zn +I(100) Zn If I(100) is less than 0.15, the orientation of the (100) plane of the η-Zn phase is insufficient, resulting in insufficient red rust resistance and corrosion resistance of the base steel. Zn / {I(002) Zn +I(101) Zn +I(100) Zn If the value of} exceeds 3.00, the corrosion resistance of the flat surface portion may decrease.

[0050] 0.15≦I(100) Zn / {I(002) Zn +I(101) Zn +I(100)Zn}≦3.00 ... (1)

[0051] 0.25≦I(100) Zn / {I(002) Zn +I(101) Zn +I(100) Zn}≦3.00 ... (2)

[0052] However, I(100) in formula (1) and formula (2) Zn is the diffraction intensity of the (100) plane of the η-Zn phase, and I(002) Zn is the diffraction intensity of the (002) plane of the η-Zn phase, and I(101) Zn is the diffraction intensity of the (101) plane of the η-Zn phase, and I(100) Zn is the diffraction intensity of the (100) plane of the η-Zn phase.

[0053] Furthermore, when the plating layer contains a total of 0.01 to 0.50% of one or both of La and Ce, it is preferable that a total of one or more of the following intermetallic compound phases be contained within a 200 μm × 200 μm field of view of the surface structure when the plating layer is viewed from above: LaCe-containing intermetallic compound phase, La-containing intermetallic compound phase, and Ce-containing intermetallic compound phase. More preferably, three or more of these intermetallic compound phases are contained within a 200 μm × 200 μm field of view. It is preferable that 10 or less of one or more of the intermetallic compound phases are contained within a 200 μm × 200 μm field of view.

[0054] The LaCe-containing intermetallic compound phase is an intermetallic compound phase containing La and Ce, the La-containing intermetallic compound phase is an intermetallic compound phase containing La, and the Ce-containing intermetallic compound phase is an intermetallic compound phase containing Ce. Elements other than La and Ce contained in these intermetallic compound phases include Al, Ca, Si, Mg, and Zn. For example, these intermetallic compound phases may include an Al-Ca-Si-Mg-Zn-(La,Ce) phase or a Ca-Zn-(La,Ce) phase. The notation (La,Ce) means either or both of La and Ce. When such intermetallic compound phases are contained, the (100) plane of the η-Zn phase is strongly oriented parallel to the surface of the coating layer, further improving red rust resistance and base steel corrosion protection.

[0055] [α phase / MgZn 2 The method for measuring the area ratio of the eutectic structure of MgZn is as follows. First, the surface of the plating layer is adjusted to be flat by mechanical polishing. Next, the surface of the plating layer is chemically polished by colloidal polishing until the surface is polished to a mirror finish. The polished surface of the plating layer is observed with an SEM. Specifically, an element distribution image is taken at a magnification of 5000 times (area of ​​200 μm vertical and 200 μm horizontal) using an SEM-EDS. In this element distribution image, a phase in which Mg and Zn coexist is identified as MgZn 2 The phase containing Al and Zn is identified as the α phase. Most of the α phase shows a dendritic morphology. The α phase and MgZn 2 phase and [α phase / MgZn 2 After identifying the eutectic structure of the α phase / MgZn 2 The area ratio of the eutectic structure is calculated by binarization using image analysis software.

[0056] I(100) in Equation (1) and Equation (2) Zn / {I(002) Zn +I(101) Zn +I(100) Zn The measurement method for the {} is as follows. First, the surface of the plating layer is mechanically polished, and if necessary, chemically polished to make the surface of the plating layer into a mirror-finished state. Then, for example, an X-ray diffraction apparatus (manufactured by Rigaku Corporation (Model No. RINT-TTR) X-ray diffraction measurements were performed using a TTR (horizontal goniometer) with an X-ray output of 50 kV, 300 mA, a copper target, a Kβ filter slit width of 0.05 mm, a longitudinal limiting slit width of 2 mm, a receiving slit width of 8 mm, and a receiving slit 2 open. Measurement conditions included a scan speed of 5 deg. / min, a step width of 0.01 deg., and a scan axis 2θ (5 to 90°). The diffraction intensity of the (100) plane of the η-Zn phase (maximum intensity in the range of 38.993 ± 0.2°), the diffraction intensity of the (002) plane (maximum intensity in the range of 36.297 ± 0.2°), and the diffraction intensity of the (101) plane (maximum intensity in the range of 43.232 ± 0.2°) were measured. The diffraction intensities were calculated by subtracting the background intensity. From the obtained diffraction intensities, the I(100)Zn / {I(002) Zn +I(101) Zn +I(100) Zn} is sought.

[0057] In addition, Mg 2 Whether or not the Sn phase is contained can be determined by examining the Mg 2 The determination is made based on whether or not a diffraction peak specific to Sn appears.

[0058] Furthermore, the method for measuring the number of LaCe-containing intermetallic compound phases, La-containing intermetallic compound phases, and Ce-containing intermetallic compound phases in the surface structure of the plating layer is as follows. First, the surface of the plating layer is mechanically polished, and if necessary, chemically polished to make the surface of the plating layer mirror-finished. Next, a rectangular observation field of 200 μm in length and 200 μm in width is set on the surface of the plating layer. An element distribution image is taken of this observation field using SEM-EDS. In this element distribution image, phases containing either La or Ce, or both, are identified as any one of the LaCe-containing intermetallic compound phases, La-containing intermetallic compound phases, and Ce-containing intermetallic compound phases. Then, the number of these intermetallic compounds is counted.

[0059] The coating weight of the plating layer per side is, for example, 20 to 300 g / m 2 The amount of adhesion per side should be within the range of 20 g / m 2 By setting the coating weight per side to 300 g / m or more, the flat surface corrosion resistance, red rust resistance, and base steel corrosion resistance of the plated steel material can be further improved. 2 By setting the following, the workability of the plated steel material can be further improved.

[0060] Next, a method for producing the plated steel material according to this embodiment will be described, but the method for producing the plated steel material according to this embodiment is not particularly limited. For example, the plated steel material according to this embodiment can be obtained according to the production conditions described below.

[0061] In the method for producing a plated steel material according to this embodiment, a steel material having a surface with irregularities formed thereon is used as the base sheet for plating. This steel material is annealed in a reducing atmosphere, and the steel material immediately after annealing is immersed in a hot dip coating bath and then pulled out, thereby forming a coating layer on the surface of the steel material. Next, the coating layer is cooled from the bath temperature to 340°C at an average cooling rate of 15°C / sec or more, and then cooled in the range of 340 to 320°C at a flux of 15,000 (L / min / m 2 ) or more, the material is cooled at an average cooling rate of 7°C / sec or less while blowing cooling gas thereon.

[0062] The roughness of the surface of the steel material to be plated is the reference length L 0 Curve length L of the roughness curve p The ratio (L p / L 0 ) is 1.08 or more. p / L 0 By making the (L) equal to or greater than 1.08, nucleation sites for crystallizing a ternary eutectic structure are formed near the interface between the coating layer and the steel sheet. p / L 0 The upper limit of the reference length L is preferably 3.00 or less, and may be 2.50 or less. 0 is the longitudinal length of the plating layer when viewed in cross section, and the curve length L p is the reference length L when the plating layer is viewed cross-sectionally. 0 The curve length of the roughness curve for the surface roughness of the plating layer, i.e., the total length of the contour line of the surface of the plating layer.

[0063] The adjustment of the roughness of the steel surface is not particularly limited, and may be performed, for example, by rolling the original sheet to be plated with a rolling roll or a roll for temper rolling whose roll surface has been adjusted to a desired roughness, thereby transferring the surface shape of the roll to the original sheet. Alternatively, the adjustment may be performed by pickling.

[0064] (L p / L 0The measurement of (L) is performed using, for example, a shape measurement laser microscope (model number: VK-8700) manufactured by Keyence Corporation. The measurement conditions are, for example, scan area: 200 μm×200 μm, measurement mode: laser confocal, measurement quality: high precision, pitch: 0.75 μm, double scan: ON, optical zoom: 1x, objective lens name: Plan, γ coefficient: 0.45, offset: 0%. p / L 0 The measuring device used for measuring the temperature is not limited to the above example.

[0065] Annealing of the steel material to be plated is carried out in a reducing atmosphere. The reducing atmosphere and annealing conditions are not particularly limited. By this annealing, oxides present on the surface of the steel material are removed as much as possible.

[0066] Next, the steel immediately after annealing is immersed in a hot-dip galvanizing bath. The chemical composition of the hot-dip galvanizing bath may be appropriately adjusted so as to obtain the chemical composition of the coating layer described above. The temperature of the hot-dip galvanizing bath is not particularly limited, and a temperature at which hot-dip galvanizing can be performed may be appropriately selected. For example, the temperature of the galvanizing bath may be set to a value approximately 20°C or more higher than the melting point of the galvanizing bath.

[0067] Next, the steel material is pulled up from the hot-dip galvanizing bath. The coating weight of the coating layer can be controlled by controlling the pulling speed of the steel material. If necessary, the coating weight of the coating layer may be controlled by wiping the steel material to which the coating layer is attached. The coating weight of the coating layer is not particularly limited and can be, for example, within the above-mentioned range.

[0068] Next, the coating layer is cooled. Cooling is first performed at an average cooling rate of 15°C / sec or more until the temperature of the coating layer reaches 340°C from the bath temperature. The average cooling rate until the temperature of the coating layer reaches 340°C from the bath temperature may be 30°C / sec or less. Cooling can be performed, for example, by spraying cooling gas. When cooling by spraying cooling gas, multiple cooling gas spray nozzles may be arranged along the steel material transport path, and the cooling gas may be sprayed from the nozzles. By cooling at a rate of 15°C / sec or more in the range from the bath temperature to 340°C, the formation of dendritic α-phase, which forms in the early solidification stage, is suppressed. α-phase dendrites can serve as nucleation sites during the crystallization of a ternary eutectic structure. By suppressing the formation of the α-phase, a ternary eutectic structure is formed from nucleation sites near the interface between the steel material and the coating layer.

[0069] Next, the range of 340 to 320°C was set at a flux of 15,000 (L / min / m 2 ) or more, while blowing cooling gas at an average cooling rate of 7°C / sec or less. At this time, cooling may be performed at an average cooling rate of 2°C or more. The flux of the cooling gas during cooling is 25,000 (L / min / m 2 In this case, a plurality of cooling gas spray nozzles are arranged along the steel material transport path. 2 ) or higher, the coating layer is vibrated by blowing cooling gas without being excessively supercooled. As a result, crystallization of a ternary eutectic structure begins near the interface between the coating layer and the steel material, and the ternary eutectic structure grows toward the surface of the coating layer.

[0070] The cooling gas to be sprayed is not particularly limited, and may be a non-oxidizing gas such as nitrogen, an inert gas such as argon, or air, or a mixture of these gases.

[0071] When controlling the flux of cooling gas, the shape of the gas nozzle from which the cooling gas is ejected is, for example, in the range of 1 to 50 mm in diameter. The angle between the tip of the gas nozzle and the steel plate is, for example, in the range of 70 to 110°, more preferably 90° (right angle). The distance between the tip of the gas nozzle and the steel plate is in the range of 30 to 1000 mm. Note that the shape, angle, and distance of the gas nozzle are merely examples and are not limited to the above ranges.

[0072] The cooling conditions below 320°C are not particularly limited, and either air cooling or natural cooling may be used.

[0073] By cooling the plating layer so as to satisfy the above-mentioned conditions, a plating layer that satisfies the above formula (1) is formed. The reason for this is presumed to be as follows.

[0074] In the above manufacturing method, by providing irregularities on the surface of the steel material before hot-dip coating, nucleation sites of the ternary eutectic structure are formed near the interface between the steel material and the coating layer. Then, by cooling the steel material immersed in the coating bath under the above conditions when it is pulled up, the nucleation sites that serve as the starting points for crystallization of the ternary eutectic structure are directed to be near the interface between the steel material and the coating layer, rather than α-phase dendrites. Unlike crystallization originating from α-phase dendrites, the ternary eutectic structure crystallized from the vicinity of the interface between the steel material and the coating layer has a crystal orientation oriented in a fixed direction. As a result, it is believed that the (100) plane of the η-Zn phase contained in the ternary eutectic structure is oriented parallel to the surface of the coating layer, thereby satisfying the above formula (1).

[0075] Examples of the present invention will be described below. However, the conditions in the examples are merely examples adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.

[0076] A hot-rolled steel sheet having a thickness of 1.6 mm was used as the base sheet for plating. The surface roughness of the hot-rolled steel sheet was controlled in advance using a skin pass mill or the like. The surface roughness was measured by measuring the surface roughness along the reference length L 0 Curve length L of the roughness curve p The ratio (Lp / L 0 ) was adjusted to be 1.05 to 1.57.

[0077] In addition, (L p / L 0 The measurement of the surface roughness was performed using a shape measuring laser microscope (model number: VK-8700) manufactured by Keyence Corporation. The measurement conditions were as follows: measurement mode: laser confocal, measurement quality: high precision, pitch: 0.75 μm, double scan: ON, optical zoom: 1x, objective lens name: Plan, γ coefficient: 0.45, offset: 0%.

[0078] Next, the plated original sheet with the adjusted surface roughness was annealed. 2 -4% H 2 The conditions were a soaking temperature of 800°C and a soaking time of 2 minutes in a nitrogen atmosphere. 2 The steel sheets were cooled with gas to adjust the temperature at the time of immersion in the plating bath to about (plating bath temperature + 20) ° C., and then immersed in various hot dip plating baths, and then pulled up at a pulling speed of 20 to 200 mm / sec. 2 The coating weight was controlled by wiping gas. After the steel material was pulled out of the coating bath, it was cooled under the conditions shown in Table 2.

[0079] In the cooling range of 340 to 320°C, the cooling gas was N 2 The cooling gas was used, and the gas flux was controlled as shown in Table 2. The gas nozzle from which the cooling gas was ejected had a diameter of 6 mm, the angle between the tip of the gas nozzle and the steel sheet was a right angle, and the distance between the tip of the gas nozzle and the steel sheet was 35 mm. In this manner, plated steel products Nos. 1 to 47 were produced.

[0080] The chemical composition of the plating layer was as shown in Table 1. The metal structure of the plating layer was also evaluated, and the results are shown in Table 3. Furthermore, the red rust resistance and base steel corrosion resistance of the plated steel materials were evaluated, and the results are shown in Table 4.

[0081] The chemical composition of the plating layer was measured by immersing a sample cut into a size of 30 mm × 30 mm in a 10% HCl aqueous solution containing an inhibitor to pickle and remove the plating layer, and then performing ICP analysis of the elements eluted into the aqueous solution.

[0082] [α phase / MgZn 2 The area ratio of the eutectic structure of MgZn was evaluated as follows. First, the surface of the plating layer was polished to a mirror finish by mechanical polishing and colloidal polishing. Next, the plating layer surface was observed at a magnification of 5000 times (region of 200 μm long x 200 μm wide) using a field emission scanning electron microscope (FE-SEM) equipped with an energy dispersive elemental analyzer (EDS), and an element distribution image was taken using the EDS. In the element distribution image, a phase in which Mg and Zn coexist was designated as MgZn. 2 The phase containing Al and Zn is identified as the α phase, and the phase containing Al and Zn is identified as the α phase. 2 The eutectic structure of α phase / MgZn was identified. 2 The area ratio of the eutectic structure was calculated by binarization using image analysis software.

[0083] I(100) in formula (1) Zn / {I(002) Zn +I(101) Zn +I(100) Zn The measurement method for {} was as follows. First, the surface of the plating layer was polished to a mirror finish in the same manner as above. Next, X-ray diffraction measurement was performed using an X-ray diffractometer (Rigaku Corporation, model number RINT-TTR III) with an X-ray output of 50 kV, 300 mA, a copper target, a goniometer TTR (horizontal goniometer), a Kβ filter slit width of 0.05 mm, a longitudinal limiting slit width of 2 mm, a receiving slit width of 8 mm, and a receiving slit 2 open, under the measurement conditions of a scan speed of 5 deg. / min, a step width of 0.01 deg, and a scan axis 2θ (5 to 90°). Then, the diffraction intensity of the (100) plane of the η-Zn phase (maximum intensity in the range of 38.993±0.2°), the diffraction intensity of the (002) plane (maximum intensity in the range of 36.297±0.2°), and the diffraction intensity of the (101) plane (maximum intensity in the range of 43.232±0.2°) were measured. The diffraction intensity was the intensity excluding the background intensity. From the obtained diffraction intensities, the I(100) Zn / {I(002) Zn +I(101) Zn +I(100)Zn} was sought.

[0084] Mg in the plating layer 2 Whether or not the Sn phase is contained can be determined by examining the Mg 2 The determination was made based on whether or not a diffraction peak specific to Sn appeared.

[0085] Furthermore, the numbers of LaCe-containing intermetallic compound phases, La-containing intermetallic compound phases, and Ce-containing intermetallic compound phases in the surface structure of the plating layer were measured. First, the surface of the plating layer was polished to a mirror finish in the same manner as above. Next, a rectangular observation field of 200 μm in length and 200 μm in width was set on the surface of the plating layer. An element distribution image was taken of this observation field using SEM-EDS. In this element distribution image, phases containing La or Ce, or both, were identified as any one of the LaCe-containing intermetallic compound phases, La-containing intermetallic compound phases, and Ce-containing intermetallic compound phases. The numbers of these intermetallic compounds were then counted. The results are shown in Table 3. The column for "LaCe-containing intermetallic compound phase" in Table 3 shows the total number of LaCe-containing intermetallic compound phases, La-containing intermetallic compound phases, and Ce-containing intermetallic compound phases.

[0086] Red rust resistance was evaluated as follows. Plated steel was cut into 100 mm x 100 mm pieces to prepare test pieces. The plating layer in a 30 mm diameter area centered on the intersection of the diagonal lines of the test piece was removed by milling to expose the steel sheet (base steel). The exposed 30 mm diameter area of ​​the base steel was subjected to a combined cycle test specified in the JASO-M609-91 method, and evaluation was made based on the occurrence of red rust in the exposed area of ​​the base steel. The evaluation criteria for red rust resistance are as follows: "AAAA", "AAA", "AA", and "A" were considered to be passing.

[0087] AAAA: Red rust area ratio of 2% or less after 120 cycles AAA: Red rust area ratio of over 2% to 5% after 120 cycles AA: Red rust area ratio of over 5% to 10% after 120 cycles A: Red rust area ratio of over 10% to 15% after 120 cycles B: Red rust area ratio of over 15% after 120 cycles

[0088] The corrosion protection of the steel substrate was evaluated as follows. The plated steel material was cut into 100 mm x 100 mm pieces to prepare test specimens. The plating layer in a 25 mm diameter area centered on the intersection of the diagonal lines of the test specimen was removed by milling to expose the steel sheet (steel substrate). The 25 mm diameter exposed area of ​​the steel substrate was subjected to a combined cycle test specified in JASO-M609-91, and evaluation was based on the maximum steel substrate corrosion depth in the exposed steel substrate area. The evaluation criteria for steel substrate corrosion protection are as follows: "AAA", "AA", and "A" were considered to be passing.

[0089] AAA: 0.5 mm or less at 360 cycles AA: 0.5 mm or less at 240 cycles A: 0.5 mm or less at 180 cycles B: Over 0.5 mm at 180 cycles

[0090] In Nos. 1 to 32 and 42 to 47 (Examples) according to the present invention, the chemical composition and metal structure of the plating layer were appropriately controlled, and both the red rust resistance and the corrosion resistance of the base steel were excellent.

[0091] Comparative Example No. 33 had an insufficient amount of Al in the coating layer, and therefore No. 31 had insufficient corrosion protection for the base steel.

[0092] Comparative Example No. 34 had an excessive amount of Al in the coating layer. As a result, in No. 32, excessive α-phase dendrites were formed, and these dendrites functioned as nucleation sites for the η-Zn phase, making it impossible to ensure the orientation of the η-Zn phase, resulting in insufficient red rust resistance and corrosion resistance of the base steel.

[0093] Comparative Example No. 35 had an insufficient amount of Mg in the coating layer, and therefore No. 33 was insufficient in both red rust resistance and base steel corrosion resistance.

[0094] Comparative Example No. 36 had an insufficient total amount of La and Ce in the coating layer, which meant that the orientation of the η-Zn phase could not be ensured, resulting in insufficient corrosion resistance of the base steel.

[0095] Comparative Example No. 37 had an excessive amount of Mg in the plating layer, which resulted in insufficient red rust resistance in No. 35.

[0096] In Comparative Example No. 38, the gas flux of the cooling gas was insufficient during cooling in the range of 340 to 320° C. Therefore, in No. 38, the orientation of the η-Zn phase could not be ensured, and the red rust resistance was insufficient.

[0097] In Comparative Example No. 39, the cooling rate exceeded 7°C / sec in the range of 340 to 320°C. Therefore, in No. 39, the orientation of the η-Zn phase could not be ensured, and the red rust resistance was insufficient.

[0098] In Comparative Example No. 40, the cooling rate was less than 15°C / sec in the cooling range from a bath temperature of up to 340°C. Therefore, in No. 40, the orientation of the η-Zn phase could not be ensured, and the red rust resistance was insufficient.

[0099] In the comparative example No. 41, the surface roughness of the plating base sheet ((L p / L 0 ) was less than 1.08. Therefore, in No. 41, the orientation of the η-Zn phase could not be ensured, and the red rust resistance was insufficient.

[0100]

[0101]

[0102]

[0103]

[0104] The plated steel material of the present disclosure has excellent red rust resistance and base steel corrosion resistance, and therefore has high industrial applicability.

[0105] 1...plated steel material, 11...steel material, 12...plated layer

Claims

1. A steel material and a plating layer on the steel material, the plating layer having a chemical composition, in mass%, containing Al: 6.0-30.0%, Mg: 3.0-15.0%, Fe: 0.01-15.00%, Si: 0-2.0%, Ca: 0-2.00%, and one or both of La and Ce in total 0.005-0.500%. Sb: 0-0.50%, Pb: 0-0.50%, Cu: 0-1.00%, Sn: 0-1.00%, Ti: 0-1.00%, Cr: 0-1.00%, Nb: 0-1 .00%, Zr: 0-1.00%, Ni: 0-1.000%, Mn: 0-1.00%, Mo: 0-1.00%, Ag: 0-1.00%, B A plated steel material containing one or more elements selected from the group consisting of I(100), Y(100), P(100), Sr(100), Co(100), Bi(100), In(100), V(100), and W(100), with a total content of these elements being 0 to 5.0%, and the balance consisting of Zn and impurities, wherein the diffraction intensity obtained from an X-ray diffraction measurement of the plated layer satisfies the following formula (1): 0.15≦I(100) Zn / {I (002) Zn +I(101) Zn +I(100) Zn}≦3.00 ... (1) where I(100) in formula (1) Zn is the diffraction intensity of (100) of the η-Zn phase, and I(002) Zn is the diffraction intensity of (002) of the η-Zn phase, and I(101) Zn is the diffraction intensity of (101) of the η-Zn phase, and I(100) Zn is the diffraction intensity of (100) of the η-Zn phase.

2. The plated steel material according to claim 1, wherein the Al and Mg content of the plated layer is, respectively, Al: 10.0 to 25.0% and Mg: 4.5 to 15.0%.

3. The plated steel material according to claim 1 or 2, wherein the total content of one or two of La and Ce in the plating layer is 0.010 to 0.500%, and the number of at least one of a LaCe-containing intermetallic compound phase, a La-containing intermetallic compound phase and a Ce-containing intermetallic compound phase in a 200 μm × 200 μm visual field of the surface structure when the plating layer is viewed in a plane is at least 1.

4. The plated steel material according to any one of claims 1 to 3, wherein the total content of one or two of La and Ce in the plating layer is 0.050 to 0.500%, and the number of at least one of LaCe-containing intermetallic compound phases, La-containing intermetallic compound phases and Ce-containing intermetallic compound phases in a 200 μm × 200 μm visual field of the surface structure when the plating layer is viewed in a plane is 3 or more.

5. The surface structure of the plating layer when viewed in plan is [α / MgZn 2 The plated steel material according to any one of claims 1 to 4, wherein an area ratio of the eutectic structure is 5 to 70%.

6. The plated steel material according to any one of claims 1 to 5, wherein the diffraction intensity obtained from the X-ray diffraction measurement of the plated layer satisfies the following formula (2): 0.25≦I(100) Zn / {I (002) Zn +I(101) Zn +I(100) Zn}≦3.00 ... (2) 7. The Sn content of the plating layer is, by mass%, Sn: 0.05 to 0.50%, and the X-ray diffraction measurement of the plating layer shows that Mg 2 The plated steel material according to claim 1 , wherein a Sn phase is detected.