Polyethylene resin composition and stretched film

MYPI2025005691A0Undetermined Publication Date: 2024-09-23IDEMITSU KOSAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005691
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2023-12-28
Publication Date
2024-09-23

AI Technical Summary

Technical Problem

Polyethylene films face challenges with high crystallinity leading to breakage during stretching, limited stretchable temperature range, and uneven film thickness, while low-density polyethylene films lack rigidity and transparency.

Method used

A polyethylene resin composition comprising high-density polyethylene, linear low-density polyethylene, and hydrogenated petroleum resin, with specific ratios and properties, allowing for a wide stretchable temperature range and improved film thickness uniformity and optical properties.

Benefits of technology

The composition enables stretched films with excellent rigidity, uniform thickness, and optical properties, enhancing formability and production efficiency without breaking during stretching.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided are: a polyethylene-based resin composition including: a high-density polyethylene (A); a linear low-density polyethylene (B); and a hydrogenated petroleum resin (C), wherein a mass ratio [(A) / (B)] of the high-density polyethylene (A) to the linear low-density polyethylene (B) is from 25 / 75 to 95 / 5, and wherein a content of the hydrogenated petroleum resin (C) is from 3 parts by mass to 25 parts by mass with respect to 100 parts by mass of a total amount of the high-density polyethylene (A) and the linear low-density polyethylene (B); and a stretched film including the polyethylene-based resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Polyethylene resin composition and stretched film

[0001] The present invention relates to a polyethylene resin composition and a stretched film.

[0002] Polyolefins have excellent mechanical properties such as tensile strength and impact strength, and are excellent in waterproofness and chemical resistance, as well as heat-sealing properties, and are therefore used in a wide range of fields, such as packaging containers. On the other hand, petroleum resins are used as tackifiers for hot-melt adhesives and adhesive tapes, and studies are being conducted to add them to plastics such as polyolefins to adjust the crystallinity of the plastics and improve their physical properties and processability.

[0003] For example, Patent Document 1 discloses a polypropylene resin composition comprising a highly stereoregular crystalline polypropylene and a petroleum resin containing no polar groups, etc., for the purpose of improving water vapor barrier properties and transparency. Also, Patent Document 2 discloses a polyethylene film containing a resin with a weight average molecular weight of less than 10,000 daltons, such as a resin derived from the polymerization of a C9 hydrocarbon feed stream, and polyethylene for the purpose of improving barrier properties, and having a reduced water vapor transmission rate compared to a film not modified with the resin.

[0004] Japanese Patent Laid-Open No. 7-076641 Japanese Patent Laid-Open No. 2009-102651

[0005] Among polyolefins, polyethylene excels in rigidity, strength, barrier properties, low-temperature properties, heat-sealing properties, etc. However, due to its high degree of crystallinity and rapid crystallization, it is prone to fracture, especially when forming stretched films at high stretch ratios. This leads to problems such as limited stretching temperature ranges and uneven film thickness. On the other hand, films based on low-density polyethylene or films using plasticizers, etc., are inferior in rigidity and transparency, which are characteristic of polyethylene. Therefore, there has been a demand for a polyethylene-based resin material that can be stretched over a wide temperature range, has high film thickness accuracy, and can produce films with excellent transparency while maintaining the rigidity characteristic of polyethylene. Therefore, the present invention aims to provide a polyethylene-based resin composition that, when used for stretched films, can be stretched over a wide temperature range and has excellent formability, thereby producing stretched films with excellent film thickness uniformity, rigidity, and optical properties, as well as a stretched film with excellent film thickness uniformity, rigidity, and optical properties.

[0006] As a result of extensive research, the present inventors have found that a polyethylene resin composition containing specific polyethylenes and specific amounts of hydrogenated petroleum resin can solve the above-mentioned problems.

[0007] That is, the present invention relates to the following items <1> to <10>. <1> A polyethylene resin composition containing high-density polyethylene (A), linear low-density polyethylene (B), and hydrogenated petroleum resin (C), wherein the mass ratio of the high-density polyethylene (A) to the linear low-density polyethylene (B) [(A) / (B)] is 25 / 75 to 95 / 5, and the content of the hydrogenated petroleum resin (C) is 3 to 25 parts by mass per 100 parts by mass of the total amount of the high-density polyethylene (A) and the linear low-density polyethylene (B). <2> The density of the high-density polyethylene (A) is 942 to 965 kg / m 3 <3> The polyethylene resin composition according to <1> above, wherein the density of the linear low-density polyethylene (B) is 890 to 938 kg / m 3<4> The polyethylene resin composition according to any one of <1> to <3>, wherein the hydrogenated petroleum resin (C) has a softening point of 115 to 160°C. <5> The polyethylene resin composition according to any one of <1> to <4>, wherein the hydrogenated petroleum resin (C) is for use in a stretched film. <6> A stretched film comprising the polyethylene resin composition according to any one of <1> to <5>. <7> The stretched film according to <6>, wherein the polyethylene resin composition is a biaxially stretched film. <8> A multilayer stretched film comprising a layer comprising the polyethylene resin composition (PE1) according to any one of <1> to <5>, and a layer comprising a polyethylene resin (PE2) that does not contain a hydrogenated petroleum resin. <9> The multilayer stretched film according to <8>, wherein the layer comprising the polyethylene resin composition (PE1) is an inner layer, and wherein layers comprising the polyethylene resin (PE2) are provided on both sides of the inner layer as outer layers. <10> A method for producing a stretched film, comprising stretching the polyethylene resin composition according to any one of <1> to <5> at a stretch ratio of 2 or more in the machine direction.

[0008] According to the present invention, it is possible to provide a polyethylene resin composition which, when used for a stretched film, has a wide temperature range in which it can be stretched and excellent formability, and therefore can give a stretched film which is excellent in thickness uniformity, rigidity, and optical properties, and to provide a stretched film which is excellent in thickness uniformity, rigidity, and optical properties.

[0009] [Polyethylene Resin Composition] The polyethylene resin composition of the present invention is a polyethylene resin composition containing a high-density polyethylene (A), a linear low-density polyethylene (B), and a hydrogenated petroleum resin (C), in which the mass ratio of the high-density polyethylene (A) to the linear low-density polyethylene (B) [(A) / (B)] is 25 / 75 to 95 / 5, and the content of the hydrogenated petroleum resin (C) is 3 to 25 parts by mass per 100 parts by mass of the total amount of the high-density polyethylene (A) and the linear low-density polyethylene (B).

[0010] <High-density polyethylene (A)> The polyethylene resin composition of the present invention contains a high-density polyethylene (A), and the mass ratio of the high-density polyethylene (A) to the linear low-density polyethylene (B) described below [(A) / (B)] is 25 / 75 to 95 / 5.

[0011] Since high-density polyethylene has a high degree of crystallinity, it is believed that the use of high-density polyethylene (A) in the polyethylene resin composition of the present invention can impart particularly high rigidity to the resulting stretched film. The density of the high-density polyethylene (A) is preferably 942 to 965 kg / m 3 and more preferably 942 to 960 kg / m 3 and more preferably 945 to 960 kg / m 3 and even more preferably 950 to 960 kg / m 3 The melt flow rate (MFR) of the high-density polyethylene (A) at 190°C is preferably 0.05 to 30 g / 10 min, more preferably 0.1 to 20 g / 10 min, even more preferably 0.2 to 10 g / 10 min, still more preferably 0.3 to 5 g / 10 min, and even more preferably 0.4 to 2 g / 10 min. The MFR is measured by the measurement method specified in JIS K7210-1:2014, under conditions of a temperature of 190°C and a load of 2.16 kg. When the melt flow rate of the high-density polyethylene (A) at 190°C is within the above range, the film has good formability and can further impart rigidity to the obtained film. In particular, with regard to formability, the production rate can be increased without breakage during stretching. The melting point of the high-density polyethylene (A) is preferably 128 to 142° C., more preferably 129 to 141° C., even more preferably 130 to 140° C., and still more preferably 131 to 139° C. When the melting point of the high-density polyethylene (A) is within the above range, the stretchability of the film becomes good, and furthermore, the obtained film can be imparted with rigidity and transparency.

[0012] The high-density polyethylene (A) may be obtained by any method as long as it is polymerized using a conventionally known catalyst. However, the catalyst used for polymerization is preferably a Ziegler-based, Phillips-based, or metallocene-based catalyst, and a Ziegler-based catalyst is preferred because it can broaden the composition distribution on the high-melting point side and facilitate stretching.

[0013] The content of the high-density polyethylene (A) in the polyethylene resin composition of the present invention is preferably 25 to 95 parts by mass, more preferably 30 to 90 parts by mass, even more preferably 30 to 80 parts by mass, still more preferably 30 to 70 parts by mass, still more preferably 30 to 60 parts by mass, and still more preferably 40 to 60 parts by mass, per 100 parts by mass of the total amount of the high-density polyethylene (A) and the linear low-density polyethylene (B).

[0014] <Linear Low-Density Polyethylene (B)> The polyethylene resin composition of the present invention contains a linear low-density polyethylene (B), and the mass ratio of the linear low-density polyethylene (B) to the high-density polyethylene (A) [(A) / (B)] is 25 / 75 to 95 / 5.

[0015] It is believed that by using the linear low-density polyethylene (B) in the polyethylene resin composition of the present invention, it is possible to impart particularly good optical properties to the resulting stretched film and improve moldability.

[0016] The linear low-density polyethylene (B) is not particularly limited, but is preferably a copolymer of ethylene and an α-olefin having 4 to 18 carbon atoms (ethylene-α-olefin copolymer). Examples of the α-olefin having 4 to 18 carbon atoms include linear α-olefins and branched α-olefins, with linear α-olefins being preferred. Specific examples of linear α-olefins include 1-butene, 1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, and 1-dodecene. Among linear α-olefins, linear α-olefins having 4 to 10 carbon atoms are more preferred. These α-olefins may be used alone or in combination of two or more. The content of α-olefin units in the ethylene-α-olefin copolymer is not particularly limited and can be appropriately selected depending on the purpose. Furthermore, a small amount of a diene component may be copolymerized into the linear low-density polyethylene (B). Examples of the diene component include dicyclopentadiene, ethylennorbornene, 1,4-hexadiene, 1,9-decadiene, and vinylnorbornene.

[0017] The linear low-density polyethylene (B) is more preferably at least one selected from the group consisting of an ethylene / 1-hexene copolymer and an ethylene / 1-butene copolymer.

[0018] The linear low-density polyethylene (B) may be obtained by any method as long as it is polymerized using a conventionally known catalyst. However, the catalyst used for polymerization is preferably a Ziegler-based, Phillips-based, or metallocene-based catalyst, and metallocene-based catalysts are preferred because they can narrow the composition distribution on the low-melting point side and make the film less likely to become sticky.

[0019] The density of the linear low-density polyethylene (B) is preferably 890 to 938 kg / m 3 and more preferably 900 to 935 kg / m 3 and more preferably 905 to 930 kg / m 3 and even more preferably 910 to 920 kg / m 3The difference between the density of the high-density polyethylene (A) and the density of the linear low-density polyethylene (B) is preferably 4 to 80 kg / m 3 and more preferably 20 to 80 kg / m 3 and more preferably 30 to 70 kg / m 3 and even more preferably 30 to 60 kg / m 3 and even more preferably 30 to 50 kg / m 3 When the difference between the density of the high-density polyethylene (A) and the density of the linear low-density polyethylene (B) is within the above range, the stretchability of the film becomes good, and further, the thickness uniformity of the obtained film can be improved.

[0020] The melt flow rate (MFR) of the linear low-density polyethylene (B) at 190°C is preferably 0.05 to 30 g / 10 min, more preferably 0.1 to 20 g / 10 min, even more preferably 0.3 to 10 g / 10 min, still more preferably 0.5 to 5 g / 10 min, and even more preferably 0.5 to 3 g / 10 min. When the melt flow rate of the linear low-density polyethylene (B) at 190°C is within the above range, the formability of the film is improved, and the resulting film can be imparted with rigidity. In particular, with regard to formability, the film can be stretched without breaking, and the production rate can be increased. The MFR is measured according to the measurement method specified in JIS K7210-1:2014, under conditions of a temperature of 190°C and a load of 2.16 kg. The melting point of the linear low-density polyethylene (B) is preferably 80 to 127°C, more preferably 90 to 126°C, even more preferably 100 to 126°C, and even more preferably 110 to 125°C. When the melting point of the linear low-density polyethylene (B) is within the above range, the stretchability of the film is good, and furthermore, the obtained film can be imparted with rigidity and made less sticky. The difference between the melting point of the high-density polyethylene (A) and the melting point of the linear low-density polyethylene (B) is preferably 1 to 50°C, more preferably 5 to 45°C, even more preferably 10 to 40°C, and even more preferably 15 to 35°C. When the difference between the melting point of the high-density polyethylene (A) and the melting point of the linear low-density polyethylene (B) is within the above range, stability during extrusion through an extruder is good.

[0021] The content of the linear low-density polyethylene (B) in the polyethylene resin composition of the present invention is preferably 5 to 75 parts by mass, more preferably 10 to 70 parts by mass, even more preferably 20 to 70 parts by mass, still more preferably 30 to 70 parts by mass, still more preferably 30 to 60 parts by mass, and still more preferably 40 to 60 parts by mass, per 100 parts by mass of the total amount of the high-density polyethylene (A) and the linear low-density polyethylene (B).

[0022] The mass ratio of the high-density polyethylene (A) to the linear low-density polyethylene (B) [(A) / (B)] is 25 / 75 to 95 / 5, preferably 30 / 70 to 90 / 10, more preferably 30 / 70 to 80 / 20, even more preferably 30 / 70 to 70 / 30, still more preferably 30 / 70 to 60 / 40, and even more preferably 40 / 60 to 60 / 40. When the mass ratio of the high-density polyethylene (A) to the linear low-density polyethylene (B) is within the above range, both the formability of the film and the physical properties of the resulting film can be achieved. In particular, both the transparency and rigidity of the resulting film can be improved.

[0023] <Hydrogenated Petroleum Resin (C)> The polyethylene resin composition of the present invention contains the hydrogenated petroleum resin (C), and the content of the hydrogenated petroleum resin (C) is 3 to 25 parts by mass per 100 parts by mass of the total amount of the high-density polyethylene (A) and the linear low-density polyethylene (B).

[0024] The hydrogenated petroleum resin is a petroleum resin obtained by adding hydrogen atoms to a petroleum resin. The hydrogenated petroleum resin includes a fully hydrogenated petroleum resin in which substantially no unsaturated bonds remain and a partially hydrogenated petroleum resin in which unsaturated bonds remain, and the hydrogenated petroleum resin (C) is preferably a fully hydrogenated petroleum resin.

[0025] Petroleum resins are resins obtained by polymerizing or copolymerizing olefinically unsaturated hydrocarbons having 4 to 11 carbon atoms, which are obtained as by-products during the production of olefins such as ethylene by thermal decomposition of petroleum such as naphtha. Specifically, petroleum resins are resins obtained by polymerizing or copolymerizing one or more unsaturated compounds selected from aliphatic olefins and aliphatic diolefins having 4 to 10 carbon atoms, or aromatic compounds having 8 or more carbon atoms and having an olefinically unsaturated bond. The petroleum resin is preferably an aromatic petroleum resin, an aliphatic-aromatic copolymer petroleum resin, or an aliphatic petroleum resin, and more preferably an aliphatic-aromatic copolymer petroleum resin. Aromatic petroleum resins are petroleum resins obtained by polymerizing aromatic compounds having an olefinically unsaturated bond, aliphatic-aromatic copolymer petroleum resins are petroleum resins obtained by copolymerizing aliphatic olefins or aliphatic diolefins with aromatic compounds having an olefinically unsaturated bond, and aliphatic petroleum resins are petroleum resins obtained by polymerizing aliphatic olefins or aliphatic diolefins.

[0026] The aromatic compound having an olefinically unsaturated bond is preferably an aromatic compound having an olefinically unsaturated bond having 8 or more carbon atoms, and specific examples thereof include styrenes such as styrene, α-methylstyrene, β-methylstyrene, vinyltoluene, and vinylxylene, and indenes such as indene, methylindene, and ethylindene. The aliphatic olefins are preferably aliphatic olefins having 4 to 10 carbon atoms, and specific examples thereof include butene, pentene, hexene, and heptene. The aliphatic diolefins are preferably aliphatic diolefins having 4 to 10 carbon atoms, and specific examples thereof include butadiene, pentadiene, isoprene, piperylene, cyclopentadiene, dicyclopentadiene, and methylpentadiene. Furthermore, it is not necessary for all of the raw material compounds for this petroleum resin to be by-products during the production of olefins by thermal decomposition of petroleum such as naphtha; chemically synthesized unsaturated compounds may also be used.

[0027] Suitable examples of petroleum resins include dicyclopentadiene-styrene petroleum resins obtained by copolymerizing cyclopentadiene or dicyclopentadiene with styrenes, C9 petroleum resins obtained by polymerizing C9 monomers such as indene or vinyltoluene, dicyclopentadiene petroleum resins obtained by polymerizing cyclopentadiene or dicyclopentadiene, and C5 petroleum resins obtained by polymerizing isoprene or piperylene.

[0028] The bromine number of the hydrogenated petroleum resin (C) is preferably 0.5 to 5 g / 100 g, more preferably 1.0 to 4 g / 100 g, even more preferably 1.5 to 3.5 g / 100 g, and even more preferably 2.0 to 3.0 g / 100 g. When the bromine number of the hydrogenated petroleum resin (C) is within the above range, compatibility with polyethylene raw materials is improved, and the effects of improving stretchability and physical properties are improved. The bromine number can be determined by electrotitration based on JIS K 2605:1996. The weight-average molecular weight of the hydrogenated petroleum resin (C) is preferably 600 to 5,000, more preferably 800 to 4,000, even more preferably 1,000 to 3,000, and even more preferably 1,200 to 2,000. When the weight-average molecular weight of the hydrogenated petroleum resin (C) is within the above range, compatibility with the polyethylene raw material is good, and the stretchability and physical properties, particularly the rigidity-modifying effect, are excellent. The weight-average molecular weight can be determined by gel permeation chromatography (GPC). The glass transition temperature of the hydrogenated petroleum resin (C) is preferably 50 to 120°C, more preferably 55 to 110°C, even more preferably 60 to 100°C, and even more preferably 65 to 90°C. When the glass transition temperature of the hydrogenated petroleum resin (C) is within the above range, compatibility with the polyethylene raw material is good, and the stretchability and physical properties, particularly the rigidity-modifying effect, are excellent. The glass transition temperature can be determined by differential scanning calorimetry (DSC) measurement. The softening point of the hydrogenated petroleum resin (C) is preferably 80 to 180°C, more preferably 110 to 160°C, even more preferably 115 to 160°C, still more preferably 120 to 160°C, and even more preferably 130 to 150°C. When the softening point of the hydrogenated petroleum resin (C) is within the above range, compatibility with the polyethylene raw material is improved, and the effect of improving the stretchability and physical properties, particularly rigidity, is improved. The softening point can be measured by the ring and ball method.

[0029] The content of the hydrogenated petroleum resin (C) in the polyethylene resin composition of the present invention is 3 to 25 parts by mass, preferably 3 to 24 parts by mass, more preferably 4 to 23 parts by mass, even more preferably 5 to 23 parts by mass, still more preferably 5 to 22 parts by mass, still more preferably 6 to 20 parts by mass, and still more preferably 8 to 15 parts by mass, per 100 parts by mass of the total amount of the high-density polyethylene (A) and the linear low-density polyethylene (B).

[0030] <Characteristics of polyethylene resin composition> The density of the polyethylene resin composition is preferably 903 to 964 kg / m 3 and more preferably 911 to 962 kg / m 3 and more preferably 919 to 960 kg / m 3 and even more preferably 923 to 958 kg / m 3 and even more preferably 930 to 955 kg / m 3 and even more preferably 935 to 955 kg / m 3When the density of the polyethylene resin composition is within the above range, both the formability of the film and the physical properties of the resulting film can be achieved. In particular, both the transparency and rigidity of the resulting film can be improved. The melt flow rate (MFR) of the polyethylene resin composition at 190°C is preferably 0.1 to 30 g / 10 min, more preferably 0.3 to 20 g / 10 min, even more preferably 0.5 to 15 g / 10 min, and even more preferably 0.7 to 10 g / 10 min. When the melt flow rate of the polyethylene resin composition at 190°C is within the above range, the film formability is improved and the resulting film can be imparted with rigidity. In particular, with regard to formability, the production rate can be increased without breakage during stretching. The MFR is measured according to the measurement method specified in JIS K7210-1:2014, under conditions of a temperature of 190°C and a load of 2.16 kg. The polyethylene resin composition preferably has two or more endothermic peaks, or one or more endothermic peaks and one or more shoulders tangent to the endothermic peaks, between 40 and 140° C. in a DSC curve obtained by differential scanning calorimetry. It is more preferable that the polyethylene resin composition has substantially no endothermic peaks in the temperature range below 40° C. and above 140° C. Having substantially multiple peaks or a peak and a shoulder within the above-mentioned range of the DSC curve can impart rigidity and transparency to the resulting film, making it less likely to become sticky.

[0031] The polyethylene resin composition of the present invention may further contain additives such as antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, nucleating agents, dyes, pigments, natural oils, synthetic oils, waxes, fillers, and elastomers, as needed, provided that the objectives of the present invention are not impaired. Examples of antioxidants that can be used include hindered phenols, sulfur-containing compounds, lactones, organic phosphites, and organic phosphonite-containing antioxidants, as well as combinations of several of these antioxidants. The antioxidant is preferably incorporated in an amount of 0.01 to 5 parts by mass per 100 parts by mass of the resin composition. Examples of slip agents that can be used include amides of saturated or unsaturated fatty acids such as lauric acid, palmitic acid, oleic acid, stearic acid, erucic acid, and behenic acid, as well as bisamides of these saturated or unsaturated fatty acids. Among these, erucic acid amide and ethylene bisstearamide are preferred. The slip agent is preferably blended in an amount of 0.01 to 5 parts by mass per 100 parts by mass of the resin composition. Examples of antiblocking agents include finely powdered silica, finely powdered aluminum oxide, finely powdered clay, powdered or liquid silicone resin, polytetrafluoroethylene resin, and finely powdered crosslinked resin such as crosslinked acrylic resin or methacrylic resin powder. Of these, finely powdered silica and finely powdered crosslinked resin are preferred.

[0032] The polyethylene resin composition of the present invention is preferably used for stretched films because it has a wide temperature range in which it can be stretched and has excellent formability when used for stretched films as described above. Furthermore, stretched films obtained using the polyethylene resin composition of the present invention are excellent in thickness uniformity, rigidity, and optical properties.

[0033] <Method for Producing Polyethylene-Based Resin Composition> The polyethylene-based resin composition of the present invention can be produced by blending high-density polyethylene (A), linear low-density polyethylene (B), and hydrogenated petroleum resin (C). Melt-kneading is a preferred blending method. The composition is preferably produced by melt-kneading the high-density polyethylene (A), linear low-density polyethylene (B), and hydrogenated petroleum resin (C), and optionally adding the additives. For example, pellets of each resin can be dry-blended and then placed in the hopper of an extruder for melt-kneading. Alternatively, after producing one of the polyethylenes using a polymerization apparatus, pellets of the other polyethylene and pellets of the hydrogenated petroleum resin can be added, followed by melt-kneading using an extruder connected to the polymerization apparatus. Alternatively, polyethylene can be added to a solvent containing the hydrogenated petroleum resin, followed by solvent removal and drying to obtain pellets or lumps. Kneading can be carried out using a mixer / kneader. Examples of mixer / kneaders include a high-speed mixer, a Banbury mixer, a continuous kneader, a single-screw or twin-screw extruder, a roll, and a Brabender plastograph. After blending using a kneader other than an extruder, pelletization using the extruder may also be performed.

[0034] [Stretched film and multilayer stretched film] The stretched film of the present invention is a stretched film made of the polyethylene resin composition (polyethylene resin composition (PE1)) (in this specification, the "polyethylene resin composition of the present invention" explained above will also be referred to as the "polyethylene resin composition (PE1)"). Furthermore, the multilayer stretched film of the present invention is a multilayer stretched film including a layer made of the polyethylene resin composition (PE1) and a layer made of a polyethylene resin (PE2) that does not contain hydrogenated petroleum resin.

[0035] The stretched film of the present invention is a uniaxially stretched film or a biaxially stretched film, preferably a biaxially stretched film. Regarding the stretching ratio of the stretched film of the present invention, the areal ratio, obtained by multiplying the stretching ratio in the machine direction (MD) by the stretching ratio in the direction perpendicular to the machine direction (TD), is preferably 3 times or more, more preferably 4 times or more, and even more preferably 9 times or more. The areal ratio is preferably 100 times or less. Films stretched to the above ratios have excellent rigidity and transparency.

[0036] When the stretched film is a uniaxially stretched film, the stretching ratio in the machine direction (MD) is preferably 2 times or more, more preferably 3 times or more, even more preferably 4 times or more, and even more preferably 4.5 times or more. The stretching ratio in the machine direction (MD) is preferably 12 times or less, but in the case of the stretched film of the present invention using the polyethylene resin composition, a film with a stretching ratio in the machine direction (MD) of 12 times or more can also be obtained. Films stretched at such a high ratio have excellent rigidity and transparency even when they are thin.

[0037] When the stretched film is a biaxially stretched film, the stretching ratio in the machine direction (MD) is preferably 2 times or more, more preferably 3 times or more, even more preferably 4 times or more, and even more preferably 4.5 times or more. The stretching ratio in the machine direction (MD) is preferably 12 times or less, but when the stretched film of the present invention uses the polyethylene-based resin composition, a film with a stretching ratio in the machine direction (MD) of 12 times or more can be obtained. Films stretched to such high ratios have excellent rigidity and transparency even when thin. When the stretched polyethylene film is a biaxially stretched film, the stretching ratio in the direction perpendicular to the machine direction (TD) is preferably 2 times or more, more preferably 4 times or more, even more preferably 6 times or more, and even more preferably 8 times or more. The stretching ratio in the direction perpendicular to the machine direction (TD) is preferably 12 times or less, but when the stretched polyethylene film of the present invention uses the polyethylene-based resin composition, a film with a stretching ratio in the direction perpendicular to the machine direction (TD) of 12 times or more can be obtained. Films stretched at such a high ratio have excellent rigidity and transparency even though they are thin.

[0038] The thickness of the stretched film of the present invention is preferably 1 to 200 μm, more preferably 4 to 80 μm, even more preferably 7 to 50 μm, and still more preferably 10 to 30 μm.

[0039] The tensile modulus in the MD direction of the stretched film of the present invention is preferably 500 MPa or more, more preferably 600 MPa or more, even more preferably 700 MPa or more, and even more preferably 800 MPa or more. There is no upper limit, and a higher tensile modulus is preferred, but it is usually 2,000 MPa or less. When the stretched polyethylene film is a biaxially stretched film, the tensile modulus in the TD direction of the stretched film of the present invention is preferably 1,000 MPa or more, more preferably 1,200 MPa or more, even more preferably 1,400 MPa or more, and even more preferably 1,600 MPa or more. There is no upper limit, and a higher tensile modulus is preferred, but it is usually 3,000 MPa or less. If the tensile modulus of the stretched film is within the above range, the film will have excellent rigidity. In terms of practical properties, when the film is used as a packaging material, it is preferable because the film can stand on its own. The tensile modulus can be measured by the method described in the examples. The haze of the stretched film of the present invention is preferably 11% or less, more preferably 10% or less, even more preferably 8% or less, even more preferably 5% or less, and even more preferably 3% or less. The lower limit may be 0% or more. If the haze of the stretched film is within the above range, the film will have excellent transparency. In terms of practical properties, when the film is used as a packaging material, the contents can be visually confirmed, which is preferable. Haze can be measured by the method described in the Examples. The stretched film of the present invention is characterized by having a uniform thickness. The thickness precision (coefficient of variation) of the stretched film of the present invention is preferably 11% or less, more preferably 10% or less, even more preferably 9% or less, even more preferably 8% or less, even more preferably 7% or less, and even more preferably 6% or less. The lower limit may be 0% or more. If the thickness precision of the stretched film is within the above range, there will be no deviation in the rigidity or transparency of the film, and the film as a whole will have excellent rigidity and transparency. Furthermore, in terms of practical properties, wrinkles will not occur when the film is wound up, which is preferable. The film thickness precision (coefficient of variation) can be measured by the method described in the examples.

[0040] The stretched film of the present invention may be a multilayer stretched film as long as it contains a layer obtained by stretching the polyethylene resin composition (PE1). When the stretched film of the present invention is a multilayer stretched film, a sealant layer or a skin layer may be provided adjacent to the layer made of the polyethylene resin composition (PE1). Resins used for the sealant layer and the skin layer include polyolefins, resins with gas barrier properties (such as ethylene-vinyl alcohol copolymers), and rigid resins (such as nylon). Furthermore, the innermost and outermost layers of the multilayer stretched film may be provided with thin films with gas barrier properties.

[0041] Furthermore, the multilayer stretched film of the present invention preferably comprises a layer made of a polyethylene-based resin composition (PE1) and a layer made of a polyethylene-based resin (PE2) that does not contain a hydrogenated petroleum resin (C). The polyethylene-based resin (PE2) may be made of one type of resin or two or more types of resin. From the viewpoint of stretchability, the polyethylene-based resin (PE2) preferably contains linear low-density polyethylene, and from the viewpoints of stretchability and rigidity, it preferably contains linear low-density polyethylene and high-density polyethylene. The linear low-density polyethylene constituting the polyethylene-based resin (PE2) is more preferably the linear low-density polyethylene (B). Therefore, its density is preferably 890 to 938 kg / m 3 and other preferred physical properties are preferably the same as those of the linear low-density polyethylene (B). The high-density polyethylene constituting the polyethylene-based resin (PE2) is more preferably the high-density polyethylene (A). Therefore, the density thereof is preferably 942 to 965 kg / m 3and other preferred physical properties are preferably similar to those of the high-density polyethylene (A). Furthermore, when the polyethylene-based resin (PE2) contains the high-density polyethylene (A) and the linear low-density polyethylene (B), the mass ratio [(A) / (B)] thereof is preferably 25 / 75 to 95 / 5. By adjusting the mass ratio in this manner, the stretchability can be matched with that of the layer comprising the polyethylene-based resin composition (PE1), and a homogeneous multilayer stretched film can be obtained. From the above viewpoint, it is preferable that the mass ratio of the high-density polyethylene (A) to the linear low-density polyethylene (B) contained in the polyethylene-based resin (PE2) is substantially similar to the mass ratio of the high-density polyethylene (A) to the linear low-density polyethylene (B) contained in the polyethylene-based resin composition (PE1).

[0042] The polyethylene resin (PE2) may further contain, as necessary, antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, nucleating agents, dyes, pigments, natural oils, synthetic oils, waxes, fillers, elastomers, etc., within the scope of the present invention. In particular, when the layer made of the polyethylene resin (PE2) is to be the outer layer, it is preferable that it contains an antistatic agent, slip agent, antiblocking agent, or lubricant, and it is more preferable that it contains an antiblocking agent.

[0043] Furthermore, the polyethylene-based resin (PE2) does not contain hydrogenated petroleum resin. However, polyethylene-based resins containing trace amounts of hydrogenated petroleum resin that do not affect the effects of the present invention are included in the polyethylene-based resin (PE2). Specifically, the content of hydrogenated petroleum resin in the polyethylene-based resin (PE2) is preferably 1% by mass or less, more preferably 0% by mass, and even more preferably no hydrogenated petroleum resin. By not including hydrogenated petroleum resin in the polyethylene-based resin (PE2), a wide stretchable temperature range can be maintained while suppressing bleed-out of the hydrogenated petroleum resin, thereby further improving moldability. Therefore, a stretched film having a uniform film thickness and excellent rigidity and optical properties can be obtained. When the multilayer stretched film of the present invention has a layer made of the polyethylene-based resin composition (PE1) and a layer made of the polyethylene-based resin (PE2), it is more preferable that the layer made of the polyethylene-based resin composition (PE1) is an inner layer, and that layers made of the polyethylene-based resin (PE2) are included as outer layers on both sides of the inner layer. This configuration allows for a multilayer stretched film that is excellent in both stretchability and rigidity.

[0044] <Method for producing stretched film> The stretched film of the present invention may be a film obtained by any production method as long as it has the above-mentioned configuration, but it is preferred to obtain a stretched film by reheating a sheet containing the polyethylene resin composition and stretching it uniaxially or biaxially simultaneously or sequentially. A suitable production method will be described below.

[0045] The polyethylene resin composition is melt-extruded and dripped from a T-shaped die in the form of a curtain. Immediately afterward, the molten film is solidified by a cooling roll submerged in a water bath to obtain a primary sheet. Subsequently, stretching is performed using a subsequent stretching device. The resin temperature during the melt-extrusion is preferably 160 to 280°C, more preferably 180 to 260°C. The cooling roll temperature is preferably 0 to 120°C, more preferably 10 to 100°C. The primary sheet obtained by extrusion is preferably further stretched by uniaxial or biaxial stretching to obtain a stretched polyethylene film. Examples of stretching methods include sequential biaxial stretching or simultaneous biaxial stretching using a tenter system, and simultaneous biaxial stretching using an inflation system. A batch-type biaxial stretching device may also be used. In the method for producing a stretched film of the present invention, the polyethylene resin composition is preferably formed by stretching the composition in the machine direction at a stretch ratio of 2 or more. The stretching ratio can be appropriately determined depending on the application of the stretched polyethylene film, but it is preferable to set it to the above-mentioned stretching ratio.

[0046] Specifically, when the stretched film is a uniaxially stretched film, the stretching ratio in the machine direction (MD) is preferably 2 times or more, more preferably 3 times or more, even more preferably 4 times or more, and even more preferably 4.5 times or more. The stretching ratio in the machine direction (MD) is preferably 12 times or less, but in the case of the stretched film of the present invention using the polyethylene resin composition, a film with a stretching ratio in the machine direction (MD) of 12 times or more can also be obtained. Films stretched at such a high ratio have excellent rigidity and transparency even when they are thin.

[0047] When the stretched film is a biaxially stretched film, the stretching ratio in the machine direction (MD) is preferably 2 times or more, more preferably 3 times or more, even more preferably 4 times or more, and even more preferably 4.5 times or more. The stretching ratio in the machine direction (MD) is preferably 12 times or less, but when the stretched film of the present invention uses the polyethylene-based resin composition, a film with a stretching ratio in the machine direction (MD) of 12 times or more can be obtained. Films stretched to such high ratios have excellent rigidity and transparency even when thin. When the stretched polyethylene film is a biaxially stretched film, the stretching ratio in the direction perpendicular to the machine direction (TD) is preferably 2 times or more, more preferably 4 times or more, even more preferably 6 times or more, and even more preferably 8 times or more. The stretching ratio in the direction perpendicular to the machine direction (TD) is preferably 12 times or less, but when the stretched polyethylene film of the present invention uses the polyethylene-based resin composition, a film with a stretching ratio in the direction perpendicular to the machine direction (TD) of 12 times or more can be obtained. Films stretched at such a high ratio have excellent rigidity and transparency even though they are thin.

[0048] In addition, it is generally known that when sequential biaxial stretching is performed, for example, when a film is first oriented by stretching in the MD direction and then further stretched in the TD direction, if the stretch ratio in the MD direction is too high, problems such as the film being prone to breakage when the stretch ratio in the TD direction is increased occur. When the polyethylene-based resin composition is used, good stretchability is obtained, making it possible to mold at a high stretch ratio. In sequential biaxial stretching using a tenter system, this primary film is reheated to a temperature suitable for stretching (longitudinal (MD) stretching temperature) and stretched in the machine direction (MD) between a slow (front) roll and a fast (rear) roll. Next, it enters the tenter section, and while holding both ends of the film stretched in the MD direction, it is further heated to a temperature suitable for stretching (transverse (TD) stretching temperature) and stretched in the direction perpendicular to the machine direction (TD). Finally, the stretched film is heat-treated at a heat-setting temperature to stabilize the film's physical properties, and then wound up by a winder. The obtained stretched film may be further adjusted to an appropriate width and length using a machine such as a slitter to form a shape suitable for the purpose. The stretched polyethylene film of the present invention can also be obtained using the above-mentioned biaxial simultaneous tenter stretching method in which stretching is simultaneously performed in the machine direction (MD) and the transverse direction (TD).

[0049] The longitudinal (MD) stretching temperature and transverse (TD) stretching temperature may be adjusted appropriately depending on the type of resin and stretching conditions. Both the longitudinal (MD) stretching temperature and transverse (TD) stretching temperature are preferably 90 to 140°C, more preferably 100 to 130°C, even more preferably 102 to 128°C, and even more preferably 104 to 126°C. The longitudinal (MD) stretching temperature and transverse (TD) stretching temperature do not need to be the same temperature and can be appropriately selected depending on the respective stretch ratios and stretching conditions. Having the stretching temperature within the above range improves moldability. In particular, the film does not break during molding, and sticking to the rolls and melt-induced breakage can be prevented. The heat setting temperature is preferably 100 to 175°C, more preferably 110 to 170°C. The stretched film of the present invention has a temperature range in which it can be stretched that is wider than that of films made from general polyethylene raw materials, and can maintain stable stretching even when the film is molded under molding conditions that would cause thickness unevenness or resulting film breakage and make it impossible to stretch the film with conventional polyethylene raw materials, resulting in an excellent elastic modulus.

[0050] The stretched film of the present invention may be produced using a continuous molding apparatus, for example, manufactured by Bruckner, JSW, DMT, Dornier, Andritz, etc. In these apparatuses, a polyethylene resin composition is extruded from a screw extruder, and while preheating on the line, it is continuously stretched in the machine direction (MD) in a longitudinal stretching step using a combination of low-speed rolls and high-speed rolls, and the longitudinally stretched film is further preheated while traveling, and both ends of the longitudinally stretched film along the lengthwise direction are clamped and the film is continuously transversely stretched in the direction perpendicular to the machine direction (TD) while traveling on a heated wide line, thereby making it possible to produce a stretched film that is stretched in both the machine direction (MD) and the direction perpendicular to the machine direction (TD) continuously on a single line.

[0051] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0052] [Raw material] High density polyethylene (A1) (HDPE (A1)): density 958 kg / m3 , MFR 1.0 g / 10 min, melting point 133 ° C, "HZ3600F", manufactured by Prime Polymer Co., Ltd. High density polyethylene (A2) (HDPE (A2)): density 944 kg / m 3 , MFR 0.45 g / 10 min, melting point 131 ° C., "Suntec F371", manufactured by Asahi Kasei Corporation Linear low-density polyethylene (B1) (LLDPE (B1)): density 916 kg / m 3 , MFR 2.3 g / 10 min, melting point 116 ° C, "SP2020", manufactured by Prime Polymer Co., Ltd. Linear low-density polyethylene (B2) (LLDPE (B2)): density 907 kg / m 3 , MFR 2.0 g / 10 min, melting point 100°C, "KF270", manufactured by Japan Polyethylene Corporation Hydrogenated petroleum resin (C1): softening point 140°C, "Imarve P-140", manufactured by Idemitsu Kosan Co., Ltd. Hydrogenated petroleum resin (C2): softening point 125°C, "Imarve P-125", manufactured by Idemitsu Kosan Co., Ltd.

[0053] [Production of polyethylene-based resin composition and stretched film] Example 1 50 parts by mass of high-density polyethylene (A1), 50 parts by mass of linear low-density polyethylene (B1), and 11 parts by mass of the hydrogenated petroleum resin (C1) obtained in Production Example 2 were dry-blended, and then a 1 mm thick sheet was produced in a sheet forming machine at a die temperature of 230 ° C, a chill roll temperature of 30 ° C, and a forming speed of 1 m / min. Next, the sheet was unwound at 0.6 m / min in a continuous sequential biaxial stretching machine, stretched 4 times in the longitudinal direction (MD direction) with rolls heated to 116 to 128 ° C, and then stretched 8 times in the transverse direction (TD direction) with a tenter heated to 102 to 128 ° C to form a biaxially stretched film. The temperatures of the rolls and tenter (stretching temperature) were adjusted in 1 ° C increments during stretching, and the elastic modulus and haze were evaluated using the stretched film with the best thickness accuracy. The TD stretching temperatures used to form the films for evaluation of modulus and haze are shown in Table 1. The results of stretchability (stretchable temperature range, thickness accuracy) and film properties (modulus, haze) are also shown in Table 1.

[0054] Examples 2 to 8 and Comparative Examples 1 to 5 Stretched films were obtained in the same manner as in Example 1, except that the type and amount of high-density polyethylene, the type and amount of linear low-density polyethylene, and the type and amount of hydrogenated petroleum resin were changed, and the roll and tenter temperatures (stretching temperatures) were changed. Evaluations of modulus and haze were performed using the stretched film with the best thickness and thickness accuracy. The TD stretching temperatures used to mold the films evaluated for modulus and haze are shown in Table 1. In Comparative Examples 4 and 5, no stretchable temperature was available, and no stretched films were obtained. The results of stretchability (stretchable temperature range, thickness and thickness accuracy) and film physical properties (modulus, haze) are shown in Table 1.

[0055] [1. Melt flow rate (MFR) of composition] The melt flow rate (MFR) of the polyethylene resin composition was measured using samples obtained by remolding the films obtained in the examples and comparative examples. The melt flow rate (MFR) was measured at a temperature of 190°C under a load of 2.16 kg according to the measurement method specified in JIS K7210-1:2014.

[0056] [2. Density of Composition] A strand of the polyethylene resin composition obtained when measuring the melt flow rate (MFR) was treated at 120°C for 2 hours, and then slowly cooled to room temperature (23°C) over 1 hour, and then the density was measured by Method D (density gradient tube) in accordance with JIS K7112:1999.

[0057] [3. Stretchable Temperature Range (Evaluation of Stretchability)] The stretchable temperature range was evaluated using the raw sheet obtained in the Examples and Comparative Examples. The raw sheet was unwound at 0.6 m / min in a continuous sequential biaxial stretching machine, stretched 4 times in the machine direction (MD direction) using rolls heated to 116 to 128°C, and then stretched 8 times in the transverse direction (TD direction) using a tenter heated to 102 to 128°C to form a biaxially stretched film. During the above formation, the tenter temperature (TD stretching temperature) was changed in 1°C increments, and the difference between the maximum tenter temperature and the minimum tenter temperature at which a stretched film could be obtained was taken as the stretchable temperature range. The larger the value of the stretchable temperature range, the better the stretchability.

[0058] 4. Thickness Precision (Variation Coefficient) (Evaluation of Stretchability) The stretched films obtained in the Examples and Comparative Examples were measured at 81 locations (9 locations lengthwise and 9 locations widthwise) at 10 cm intervals, and the average film thickness and standard deviation were calculated from the obtained data. The coefficient of variation was determined using the following formula (1). When multiple stretched films were obtained in each Example and Comparative Example, the value of the stretched film with the smallest coefficient of variation was used as the coefficient of variation for the stretched film of the corresponding Example or Comparative Example. The smaller the coefficient of variation, the higher the thickness precision, the better the film thickness uniformity, and the more excellent the stretchability. Coefficient of variation (%) = Standard deviation (μm) / Average film thickness (μm) × 100 (1)

[0059] 5. Tensile Modulus (Evaluation of Film Properties) The stretched films obtained in the Examples and Comparative Examples were punched into JIS No. 1 / 2 dumbbell shapes using a punching machine so that the tensile direction was the MD direction, and a tensile test was conducted using a tensile tester (SHIMADZU AUTOGRAPH AG-X) under conditions of a chuck distance of 40 mm and a test speed of 300 mm / min, and the tensile modulus (MD direction) was calculated. Similarly, the stretched films obtained in the Examples and Comparative Examples were punched into dumbbell shapes so that the tensile direction was the TD direction, and a tensile test was conducted to calculate the tensile modulus (TD direction). The higher the tensile modulus value, the better the rigidity (strength).

[0060] 6. Haze (Evaluation of Film Properties) The haze of the stretched films obtained in the examples and comparative examples was measured in accordance with JIS K7136: 2000, and calculated. The smaller the haze value, the better the transparency.

[0061]

[0062] The results in Table 1 show that the polyethylene resin compositions of the Examples have a wide temperature range in which they can be stretched and excellent film thickness uniformity. Furthermore, the stretched films of the Examples have a high elastic modulus and good haze, and therefore the obtained stretched films are also excellent in rigidity and optical properties. From the above, it can be seen that the polyethylene resin composition of the present invention, when used for stretched films, has a wide temperature range in which it can be stretched and excellent film thickness uniformity, and therefore has excellent formability. Furthermore, the obtained stretched films are also excellent in rigidity and optical properties.

Claims

1. A polyethylene resin composition comprising high density polyethylene (A), linear low density polyethylene (B) and hydrogenated petroleum resin (C), wherein the mass ratio of the high density polyethylene (A) to the linear low density polyethylene (B) [(A) / (B)] is 25 / 75 to 95 / 5, and the content of the hydrogenated petroleum resin (C) is 3 to 25 parts by mass per 100 parts by mass of the total amount of the high density polyethylene (A) and the linear low density polyethylene (B).

2. The density of the high-density polyethylene (A) is 942 to 965 kg / m 3 The polyethylene resin composition according to claim 1, 3. The density of the linear low-density polyethylene (B) is 890 to 938 kg / m 3 The polyethylene resin composition according to claim 1 or 2, 4. The polyethylene resin composition according to any one of claims 1 to 3, wherein the hydrogenated petroleum resin (C) has a softening point of 115 to 160°C.

5. The polyethylene resin composition according to any one of claims 1 to 4, which is for use in a stretched film.

6. A stretched film comprising the polyethylene resin composition according to any one of claims 1 to 5.

7. The stretched film of claim 6 which is a biaxially stretched film.

8. A multilayer stretched film comprising a layer made of the polyethylene resin composition (PE1) according to any one of claims 1 to 5, and a layer made of a polyethylene resin (PE2) not containing hydrogenated petroleum resin.

9. The multilayer stretched film according to claim 8, comprising an inner layer made of the polyethylene resin composition (PE1) and outer layers on both sides of the inner layer made of the polyethylene resin (PE2).

10. A method for producing a stretched film, comprising stretching the polyethylene resin composition according to any one of claims 1 to 5 at a stretch ratio of 2 or more in the machine direction.