Hexagonal boron nitride powder, resin composition, and resin sheet

MYPI2025005733A0Undetermined Publication Date: 2024-09-28TOKUYAMA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005733
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-02-14
Publication Date
2024-09-28

AI Technical Summary

Technical Problem

Conventional hexagonal boron nitride powders exhibit thermal anisotropy, leading to reduced thermal conductivity in resin sheets, and require high filling amounts to achieve desired thermal conductivity, which increases costs.

Method used

A hexagonal boron nitride powder with a tapped bulk density ratio of 2.1 or more and an average particle diameter of 15 μm or more, featuring a complex agglomerated structure and surface irregularities, allowing for increased packing density and efficient heat transfer at lower filling amounts.

Benefits of technology

The hexagonal boron nitride powder achieves good thermal conductivity with a lower packing density than conventional powders, reducing the required filling amount and associated costs while maintaining thermal performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005733_DRAWING_001
    Figure PI2025005733_DRAWING_001
Patent Text Reader

Abstract

Achieved is hexagonal boron nitride powder and the like that can exhibit a more favorable thermal conductivity with a smaller filling amount than conventional art. Hexagonal boron nitride powder has a tap bulk density of not less than 0.50 g / cm3 and having an average particle diameter of not less than 15 μm, a ratio of the tap bulk density to a loose bulk density of the hexagonal boron nitride powder being not less than 2.1.
Need to check novelty before this filing date? Find Prior Art

Description

Hexagonal boron nitride powder, resin composition and resin sheet

[0001] The present invention relates to a hexagonal boron nitride powder, a resin composition, and a resin sheet.

[0002] In recent years, as electronic components have become smaller and more powerful, the amount of heat generated by them has become an issue. Therefore, materials with excellent thermal conductivity are being developed to efficiently dissipate heat from electronic components.

[0003] Hexagonal boron nitride powder can be blended with resins used in electronic components to improve the thermal conductivity of the resin. Conventional hexagonal boron nitride powders contain primary particles with a scale-like structure derived from the crystalline structure. These scale-like particles have thermal anisotropy, so when filled into a sheet or the like, there is a direction in which the thermal conductivity is low.

[0004] In order to improve such thermal anisotropy, for example, Patent Document 1 proposes a hexagonal boron nitride powder containing hexagonal boron nitride aggregates.

[0005] Japanese Patent Application Publication No. 2011-98882

[0006] In conventional hexagonal boron nitride powders such as those described in Patent Document 1, heat is transferred through the contact areas between the agglomerated particles contained therein, and therefore, the thermal conductivity tends to improve as the density increases during packing. Therefore, in order to achieve high thermal conductivity, the packing amount of hexagonal boron nitride powder per unit volume tends to be large.

[0007] An object of one aspect of the present invention is to provide a hexagonal boron nitride powder or the like that can exhibit good thermal conductivity with a smaller filling amount than conventional powders.

[0008] In order to solve the above problems, the hexagonal boron nitride powder according to one embodiment of the present invention has a tapped bulk density of 0.50 g / cm 3 The ratio of the tapped bulk density to the loose bulk density is 2.1 or more, and the average particle size is 15 μm or more.

[0009] According to one aspect of the present invention, it is possible to realize a hexagonal boron nitride powder or the like that can exhibit good thermal conductivity with a smaller filling amount than conventional powders.

[0010] 1 is a schematic diagram showing an outline of hexagonal boron nitride powder, in which the diagram indicated by reference numeral 101 is a conventional example, and the diagram indicated by reference numeral 102 is an example of the present invention.

[0011] Hereinafter, one embodiment of the present invention will be described in detail. In this specification, unless otherwise specified, the expression "A to B" representing a range of numerical values ​​means "A or more and B or less."

[0012] <Hexagonal boron nitride powder> The hexagonal boron nitride powder according to one embodiment of the present invention (hereinafter, may be referred to as "the present hexagonal boron nitride powder") has a tapped bulk density of 0.50 g / cm 3 or more, the ratio of tapped bulk density to loose bulk density is 2.1 or more, and the average particle size is 15 μm or more.

[0013] Hexagonal boron nitride forms scaly primary particles due to its crystalline structure. When filled into a resin to form a resin sheet, for example, these primary particles are oriented in the plane direction of the resin sheet. This reduces the thermal conductivity of the resin sheet in the thickness direction. To improve this thermal anisotropy, hexagonal boron nitride powder containing agglomerated particles of hexagonal boron nitride has been proposed. Agglomerated particles of hexagonal boron nitride can be made to have a shape closer to a sphere than primary particles, thereby reducing the problem of thermal anisotropy.

[0014] Hexagonal boron nitride powder is used, for example, as a heat dissipation material, as a filler for resins to obtain resin compositions. The thermal conductivity of such resin compositions tends to increase as the packing density of the hexagonal boron nitride powder increases.

[0015] As shown in the reference example denoted by reference numeral 101 in Fig. 1, conventional hexagonal boron nitride powder can improve packing density by containing two or more types of agglomerated particles with different particle sizes. This is because the packing density can be easily increased by the infiltration of small agglomerated particles into the gaps between agglomerated particles with a relatively large particle size.

[0016] However, increasing the packing density of hexagonal boron nitride powder to obtain a desired thermal conductivity also increases the amount of hexagonal boron nitride powder required, leaving room for improvement in terms of cost. In this regard, the present hexagonal boron nitride powder can obtain thermal conductivity equivalent to that of conventional hexagonal boron nitride powders with a lower packing amount than conventional powders. The present hexagonal boron nitride powder will be described below.

[0017] (Packing density) The hexagonal boron nitride powder has a ratio of tapped bulk density to loose bulk density (tapped bulk density / loose bulk density, hereinafter sometimes referred to as "density ratio") of 2.1 or more. Loose bulk density refers to the packing density of a powder in a loosely packed state in which the powder is loosely packed in a container. Tapped bulk density refers to the packing density of a powder in a densely packed state in which the container filled with the powder is tapped a predetermined number of times.

[0018] The tapped bulk density of the present hexagonal boron nitride powder can be obtained, for example, using a Tap Denser KYT-5000 manufactured by Seishin Enterprise Co., Ltd. under the measurement conditions described in the Examples below. The loose bulk density of the present hexagonal boron nitride powder can be obtained by measuring the packing density of the powder loosely packed in a container before tapping to measure the tapped bulk density. The packing density of the present hexagonal boron nitride powder in a container is determined by mass / volume.

[0019] The present hexagonal boron nitride powder having the density ratio described above exhibits a large increase in packing density upon tapping. This does not limit the mechanism of action, but indicates that the present hexagonal boron nitride powder has a complex agglomerated structure or surface irregularities, and therefore particles can exist in a state of loose contact with each other to the extent that the packing density is greatly increased by tapping. In such a loosely bonded state, heat is transferred between particles through contact between the particles, and the present hexagonal boron nitride powder can achieve good thermal conductivity in the packed material.

[0020] The present hexagonal boron nitride powder having such a density ratio has a tapped bulk density of 0.50 g / cm when the average particle size is 15 μm or more. 3Therefore, with this hexagonal boron nitride powder, it is possible to obtain a thermal conductivity equivalent to that of conventional hexagonal boron nitride powders at a lower packing density than conventional powders.

[0021] From the viewpoint of obtaining good thermal conductivity with a relatively low packing density, the density ratio of the present hexagonal boron nitride powder is sufficient to be 2.1 or more, and preferably 2.2 or more, and may be 4.0 or less, or 3.5 or less.

[0022] The loose bulk density of this hexagonal boron nitride powder is 0.15 g / cm 3 0.35g / cm or more 3 If the present hexagonal boron nitride powder has such a loose bulk density, the tapped bulk density can be adjusted to a relatively small value while maintaining a density ratio of 2.1 or more, and therefore the amount of the present hexagonal boron nitride powder to be filled can be reduced.

[0023] (Average particle size) From the viewpoint of improving thermal conductivity, the average particle size of the present hexagonal boron nitride powder may be 15 μm or more, or may be 20 μm or more, or may be 25 μm or more. From the viewpoint of improving flowability, the average particle size may be 100 μm or less, or may be 75 μm or less, or may be 50 μm or less.

[0024] (First Agglomerated Particles and Second Agglomerated Particles) The hexagonal boron nitride powder satisfying the above-described parameters preferably includes at least two types of agglomerated particles, for example, first agglomerated particles and second agglomerated particles having a particle size different from that of the first agglomerated particles. Both the first agglomerated particles and the second agglomerated particles are agglomerated particles of hexagonal boron nitride primary particles.

[0025] The first agglomerated particles refer to agglomerated particles in the present hexagonal boron nitride powder having a particle diameter of 20 μm or more and 50 μm or less. The first agglomerated particles preferably have an average area circularity of 0.1 or more and less than 0.6, and an average area envelopment ratio of 0.4 or more and less than 0.9.

[0026] The areal circularity is closer to 1.0 as the shape of the aggregated particles approaches a perfect sphere. Therefore, the first aggregated particles having the above-described average areal circularity can be said to be aggregated particles having a distorted shape that is far from a sphere. The areal circularity of each aggregated particle can be calculated by using a two-dimensional projection image of the aggregated particles and calculating "4π × projected area / (perimeter)" 2 " is required.

[0027] The smoother the contour of the agglomerated particles, the closer the area envelopment value is to 1.0. The first agglomerated particles having the above-described average area envelopment value can be said to be agglomerated particles with a rough contour and a distorted shape. The area envelopment value of each agglomerated particle can be calculated by "area wrapped around the actual perimeter / area wrapped around the envelope perimeter" using a two-dimensional projection image of the agglomerated particles.

[0028] The first agglomerate particles having such a distorted shape may have a branched shape, such as a plurality of spherical agglomerate particles connected together. Such first agglomerate particles are likely to come into contact with other agglomerate particles even when the packing density is low. The contact between the agglomerate particles efficiently transfers heat between the agglomerates, so the shape of the first agglomerate particles described above contributes to improving thermal conductivity. As a result, the hexagonal boron nitride powder having the above configuration can exhibit high thermal conductivity even when the tapped bulk density is relatively low, and the amount of the hexagonal boron nitride powder used for packing can be reduced.

[0029] The average area circularity of the first aggregate particles may be 0.1 or more, or may be 0.2 or more, and may be less than 0.6, 0.5 or less, or 0.4 or less.

[0030] The average area coverage of the first aggregate particles may be 0.4 or more, or may be 0.5 or more, and may be less than 0.9, 0.8 or less, or 0.7 or less.

[0031] The proportion of the first agglomerate particles relative to the entire hexagonal boron nitride powder may be 20% by volume or more, 25% by volume or more, or 30% by volume or more. The proportion of the first agglomerate particles may be 70% by volume or less, 65% by volume or less, or 60% by volume or less. If the hexagonal boron nitride powder contains the first agglomerate particles in such a proportion, the above-mentioned density ratio is likely to be obtained.

[0032] The second agglomerated particles refer to agglomerated particles in the present hexagonal boron nitride powder having a particle diameter of 60 μm or more and 110 μm or less. The second agglomerated particles preferably have an average area circularity of 0.4 or more and an average area envelopment ratio of 0.4 or more and 0.9 or less.

[0033] The second agglomerated particles having such a configuration are agglomerated particles that have a smoother, more spherical shape than the first agglomerated particles. In the packed state after tapping of the hexagonal boron nitride powder, the first agglomerated particles are efficiently positioned in the gaps between the second agglomerated particles and come into contact with each other, thereby improving the thermal conductivity.

[0034] The proportion of the second agglomerated particles relative to the entire hexagonal boron nitride powder may be 20% by volume or more, 25% by volume or more, or 30% by volume or more. The proportion of the second agglomerated particles may be 70% by volume or less, 65% by volume or less, or 60% by volume or less. If the hexagonal boron nitride powder contains the second agglomerated particles in such a proportion, the thermal conductivity during filling is likely to be improved.

[0035] The present hexagonal boron nitride powder may further contain agglomerated particles other than the first agglomerated particles and the second agglomerated particles, and may also contain unagglomerated primary particles. The unagglomerated primary particles contained in the present hexagonal boron nitride powder are preferably 20 volume % or less.

[0036] According to the above-described configuration, even when gaps exist between the agglomerated particles, as in the example of the present invention shown by reference numeral 102 in FIG. 1 , the contact area can be increased while maintaining gaps between the irregularly shaped first agglomerated particles and the larger second agglomerated particles. Therefore, in fillers such as resin compositions, the desired thermal conductivity can be achieved with a smaller filling amount than conventional fillers, thereby reducing the amount of hexagonal boron nitride powder used in the production of resin compositions. This effect also contributes to the achievement of Goal 12 of the United Nations' Sustainable Development Goals (SDGs), "Ensure sustainable consumption and production patterns."

[0037] <Method for Producing Hexagonal Boron Nitride Powder> The method for producing the present hexagonal boron nitride powder is not particularly limited, but it can be produced, for example, by the following production method.

[0038] First, an oxygen-containing boron compound, a carbon source, an oxygen-containing calcium compound, and boron carbide are mixed in the ratio shown below to obtain a mixture. The ratio B / C (element ratio) of the mass of the oxygen-containing boron compound converted into B to the mass of the carbon source converted into C is set to 0.75 to 1.05. 2 O 3 The oxygen-containing calcium compound is 5 to 20 parts by mass in terms of CaO relative to 100 parts by mass of the total of the converted mass of the oxygen-containing boron compound and the converted mass of the carbon source. 2 O 3 The boron carbide is contained in an amount of 5 to 45 parts by mass relative to 100 parts by mass of the total amount of the converted mass of C and CaO.

[0039] Next, the resulting mixture is heated to a temperature of 1600 to 1950°C in a nitrogen atmosphere to carry out a reduction-nitridation reaction. The particle size distribution of the resulting hexagonal boron nitride powder is adjusted by crushing. By-products other than boron nitride present in the reduction-nitridation reaction product may be removed by pickling. The hexagonal boron nitride powder after pickling is re-fired by heating to a temperature of 1700 to 2050°C in a nitrogen-containing gas atmosphere.

[0040] As described above, by using two boron sources, i.e., an oxygen-containing boron compound and boron carbide, as raw materials, the present hexagonal boron nitride powder containing first agglomerated particles and second agglomerated particles can be obtained. Specifically, it is believed that the oxygen-containing boron compound, the carbon source, and the oxygen-containing calcium compound serve as the sources of the first agglomerated particles, and the boron carbide serves as the nuclei of the second agglomerated particles.

[0041] (Raw Material) As the oxygen-containing boron compound, a compound containing boron and oxygen atoms may be used. Examples of oxygen-containing boron compounds include boric acid, boric anhydride, metaboric acid, perboric acid, hypoboric acid, sodium tetraborate, and sodium perborate. Among these, boric acid or boron oxide, which are easily available, may be preferably used.

[0042] The oxygen-containing calcium compound forms a complex oxide with the oxygen-containing boron compound, which forms a complex oxide with a high melting point and plays a role in preventing the oxygen-containing boron compound from volatilizing.It has also been confirmed that the oxygen-containing calcium compound plays a role in the direct nitriding reaction of boron carbide.

[0043] Examples of oxygen-containing calcium compounds include calcium carbonate, calcium bicarbonate, calcium hydroxide, calcium oxide, calcium nitrate, calcium sulfate, calcium phosphate, and calcium oxalate. These compounds can be used alone or in combination. Among these, calcium oxide or calcium carbonate is preferred.

[0044] Examples of carbon sources include amorphous carbon such as carbon black, activated carbon, and carbon fiber, as well as crystalline carbon such as diamond, graphite, and nanocarbon, and pyrolytic carbon obtained by pyrolyzing a monomer or polymer. Among these, highly reactive amorphous carbon is preferred, and carbon black is particularly preferred because of its industrial quality control. Examples of carbon black include acetylene black, furnace black, and thermal black.

[0045] As the boron carbide, known boron carbide may be used. The particle size of the boron carbide is preferably 1 to 500 μm, more preferably 10 to 400 μm, and even more preferably 20 to 300 μm.

[0046] The mixture containing the raw materials may be supplied to the reduction-nitridation reaction in the form of, for example, powder, or may be formed into granules. The raw materials can be mixed using a mixer such as a vibration mill, a bead mill, a ball mill, a Henschel mixer, a drum mixer, a vibration agitator, or a V-shaped mixer.

[0047] (Reductive nitridation) In the reductive nitridation reaction, the nitrogen source can be supplied to the reaction system by known means. For example, the most preferred method is to circulate nitrogen gas through the reaction system of a reactor, which will be exemplified later. The nitrogen source to be used is not limited to nitrogen gas, and is not particularly limited as long as it is a gas that can be nitrided in the reductive nitridation reaction. Specifically, ammonia gas can be used in addition to nitrogen gas. It is also possible to mix nitrogen gas or ammonia gas with a non-oxidizing gas such as hydrogen, argon, or helium and use it.

[0048] In order to obtain a highly crystalline hexagonal boron nitride powder, the heating temperature in the reduction-nitridation reaction can be 1600 to 1950° C., preferably 1650 to 1900° C., and more preferably 1680 to 1880° C. That is, if the heating temperature is less than 1600° C., the reduction-nitridation reaction will not proceed and it will be difficult to obtain hexagonal boron nitride with high crystallinity, whereas if the heating temperature exceeds 1950° C., the effect will plateau and it will be economically disadvantageous.

[0049] The time for the reduction-nitridation reaction is determined appropriately, but is, for example, about 10 to 30 hours.

[0050] (Particle Size Adjustment) The hexagonal boron nitride powder obtained after the reduction-nitridation reaction may be adjusted to a predetermined particle size distribution by crushing. Crushing is preferably carried out gently using a jet mill, ball mill, hammer mill, stone mill, or the like. Furthermore, the particle size of the crushed powder may be appropriately adjusted by classification treatment using air classification or sieving.

[0051] After disintegration and before re-firing, it is preferable to adjust the volume frequency of agglomerated particles having a particle size of 10 μm or less and the volume frequency of agglomerated particles having a particle size of more than 10 μm and 50 μm or less in the hexagonal boron nitride powder within predetermined ranges.

[0052] Specifically, the volume frequency of agglomerated particles having a particle size of 10 μm or less is preferably less than 10%, more preferably 7% or less, and even more preferably 5% or less. The hexagonal boron nitride powder before re-firing does not necessarily need to contain agglomerated particles having a particle size of 10 μm or less.

[0053] The volume frequency of aggregated particles having a particle size of more than 10 μm and not more than 50 μm may be 20% or more, preferably 25% or more, and more preferably 30% or more, and the volume frequency of aggregated particles having a particle size of more than 10 μm and not more than 50 μm may be 65% or less, preferably 60% or less.

[0054] If the hexagonal boron nitride powder before re-firing is adjusted to have the particle size distribution described above, it is possible to suitably obtain the present hexagonal boron nitride powder after re-firing having a density ratio of 2.1 or more.

[0055] (Pickling) The reaction product obtained by the reduction-nitridation reaction described above contains impurities such as a composite oxide composed of boron oxide and calcium oxide in addition to the hexagonal boron nitride powder, and is therefore preferably washed with an acid. The method for this pickling is not particularly limited, and any known method may be used without limitation. For example, a method may be used in which the by-product-containing boron nitride powder obtained after the reduction-nitridation reaction is placed in a container, and dilute hydrochloric acid (10 to 20% by mass HCl) is added in an amount 5 to 10 times the amount of the by-product-containing boron nitride powder, followed by contact for 4 to 8 hours.

[0056] The acid used in pickling may be hydrochloric acid, or may be nitric acid, sulfuric acid, acetic acid, or the like.

[0057] After pickling, water washing with pure water may be carried out to wash away any remaining acid. As a method of water washing, the acid used in pickling may be filtered, and then the pickled hexagonal boron nitride powder may be dispersed in pure water in the same amount as the acid used, followed by filtering again.

[0058] (Drying) After pickling or water washing, the hydrous aggregate may be dried. Drying conditions are preferably, for example, in the atmosphere at 50 to 250°C or under reduced pressure. There is no particular restriction on the drying time, but it is preferable to dry until the moisture content approaches 0%.

[0059] (Re-firing) The nitrogen-containing gas atmosphere in which re-firing is carried out may be, for example, an atmosphere containing nitrogen. The nitrogen source may be supplied to the reaction system in the re-firing in the same manner as in the reduction-nitridation.

[0060] The heating temperature for re-firing can be 1700 to 2050° C., preferably 1800 to 2000° C., and more preferably 1900 to 2000° C. Such a heating temperature can suitably produce the present hexagonal boron nitride powder having a density ratio of 2.1 or more.

[0061] The reduction-nitriding reaction and re-baking described above can be carried out using a known reaction apparatus capable of controlling the reaction atmosphere, such as an atmosphere-controlled high-temperature furnace that performs heat treatment by high-frequency induction heating or heater heating, or a batch furnace or a continuous heating furnace such as a pusher-type tunnel furnace or a vertical reactor.

[0062] <Resin Composition> The present hexagonal boron nitride powder can be used, for example, as a filler in a resin composition. That is, a resin composition according to one embodiment of the present invention (hereinafter, sometimes referred to as "the present resin composition") may contain the present hexagonal boron nitride powder. In such a present resin composition, the present hexagonal boron nitride powder may be used as a filler to be mixed with a resin described below for the purpose of improving electrical insulation or imparting thermal conductivity. By being filled with the present hexagonal boron nitride powder, the present resin composition has high electrical insulation and thermal conductivity.

[0063] The present resin composition can be used for various applications, and by forming a thermally conductive resin composition or a thermally conductive molded article, it may be preferably used for applications such as thermal interface materials such as polymer-based heat dissipation sheets and phase change sheets, organic heat dissipation sheets such as heat dissipation tapes, heat dissipation greases, heat dissipation adhesives and gap fillers, heat dissipation paints such as heat dissipation paints and heat dissipation coats, heat dissipation resin substrates such as PWB-based resin substrates and CCL-based resin substrates, insulating layers for metal-based substrates such as aluminum-based substrates and copper-based substrates, and sealing materials for power devices.

[0064] The resin composition may contain a thermally conductive filler such as aluminum nitride and aluminum oxide, which are known high thermal conductivity insulating fillers.

[0065] Examples of the resin include thermoplastic resins such as polyolefin, vinyl chloride resin, methyl methacrylate resin, nylon, and fluororesin; thermosetting resins such as epoxy resin, phenol resin, urea resin, melamine resin, unsaturated polyester resin, silicone resin, and bismaleimide triazine resin; and synthetic rubber.

[0066] Furthermore, the present resin composition may contain, as necessary, known compounding agents for resin compositions, such as polymerization initiators, curing agents, polymerization inhibitors, polymerization retarders, coupling agents, plasticizers, ultraviolet absorbers, pigments, dyes, antibacterial agents, organic fillers, and organic-inorganic composite fillers. Furthermore, the present resin composition may contain other inorganic fillers to the extent that the effects of the present invention are not impaired.

[0067] <Resin Sheet> A resin sheet according to one embodiment of the present invention (hereinafter sometimes referred to as "the present resin sheet") may be made of the present resin composition described above. The use of the present resin sheet is not particularly limited, but it can be used, for example, for circuit boards and insulating layers in multilayer printed wiring boards.

[0068] <Other Applications> The hexagonal boron nitride powder can also be used as a raw material for boron nitride processed products such as cubic boron nitride or boron nitride molded products, a nucleating agent for engineering plastics, a phase change material, a solid or liquid thermal interface material, a release agent for molten metal or molten glass molds, cosmetics, and a raw material for composite ceramics.

[0069] <Summary> As described above, the hexagonal boron nitride powder according to aspect 1 of the present invention has a tapped bulk density of 0.50 g / cm 3 The ratio of the tapped bulk density to the loose bulk density is 2.1 or more, and the average particle size is 15 μm or more.

[0070] A hexagonal boron nitride powder according to Aspect 2 of the present invention is the same as in Aspect 1, and includes first agglomerated particles that are agglomerated particles of hexagonal boron nitride primary particles and have a particle diameter of 20 μm or more and 50 μm or less, and the first agglomerated particles may have an average areal circularity of 0.1 or more and less than 0.6, and an average areal envelopment ratio of 0.4 or more and less than 0.9.

[0071] A hexagonal boron nitride powder according to Aspect 3 of the present invention is the same as Aspect 2, further comprising second agglomerated particles that are agglomerated particles of hexagonal boron nitride primary particles and have a particle diameter of 60 μm or more and 110 μm or less, and the second agglomerated particles may have an average areal circularity of 0.4 or more and 0.9 or less and an average areal envelopment ratio of 0.4 or more and 0.9 or less.

[0072] A hexagonal boron nitride powder according to a fourth aspect of the present invention is the powder of any one of the first to third aspects, wherein the loose bulk density is 0.15 g / cm 3 0.35g / cm or more 3 It may be the following:

[0073] A resin composition according to a fifth aspect of the present invention comprises the hexagonal boron nitride powder according to any one of the first to fourth aspects.

[0074] A resin sheet according to a sixth aspect of the present invention comprises the resin composition according to the fifth aspect.

[0075] An embodiment of the present invention will be described below, but the present invention is not limited to each of the embodiments shown below.

[0076] <Production and Evaluation of Hexagonal Boron Nitride Powder> The hexagonal boron nitride powders according to the examples and comparative examples were each produced by the methods described below.

[0077] Example 1 Hexagonal boron nitride powder according to Example 1 was prepared by mixing 259 g of a mixture containing 141 g of boron oxide, 56 g of carbon black, 32 g of calcium oxide, and 30 g of boron carbide in a ball mill. The mixture was subjected to a reduction-nitriding treatment in a graphite Tammann furnace by holding it in a nitrogen gas atmosphere at a maximum temperature of 1750°C for 2 hours.

[0078] The obtained hexagonal boron nitride was subjected to crushing, and the volumetric proportion of agglomerated particles of 10 μm or less in the particle size distribution was adjusted to 4%, and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was adjusted to 48%. The hexagonal boron nitride powder after particle size distribution adjustment was placed in a container, and a five-fold amount of hydrochloric acid (7 mass% HCl) was added. The mixture was stirred at a rotation speed of 700 rpm for 24 hours to perform an acid pickling treatment. After the acid pickling treatment, the acid was filtered, and the hexagonal boron nitride powder obtained by filtration was dispersed in pure water in the same amount as the acid used, and then filtered again. This operation was repeated five times, and then the mixture was vacuum dried at 200°C for 6 hours.

[0079] The hexagonal boron nitride powder obtained after drying was re-fired in a graphite Tammann furnace in a nitrogen gas atmosphere at 1900° C. for 6 hours.

[0080] The hexagonal boron nitride powder obtained after re-firing was passed through a sieve with 106 μm openings to obtain a white hexagonal boron nitride powder.

[0081] Example 2 The hexagonal boron nitride powder according to Example 2 was produced under the same conditions as in Example 1, except for the crushing conditions. The particle size distribution after crushing was such that the volumetric proportion of agglomerated particles of 10 μm or less was 2%, and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was 25%.

[0082] Example 3 The hexagonal boron nitride powder of Example 3 was produced under the same conditions as in Example 1, except for the crushing conditions. The particle size distribution after crushing was such that the volumetric proportion of agglomerated particles of 10 μm or less was 5%, and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was 58%.

[0083] Example 4 The hexagonal boron nitride powder of Example 4 was produced under the same conditions as in Example 1, except for the crushing conditions. The particle size distribution after crushing was such that the volumetric proportion of agglomerated particles of 10 μm or less was 4%, and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was 45%.

[0084] Example 5 The hexagonal boron nitride powder of Example 5 was produced under the same conditions as in Example 1, except for the crushing conditions. The particle size distribution after crushing was such that the volumetric proportion of agglomerated particles of 10 μm or less was 3%, and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was 42%.

[0085] Example 6 The hexagonal boron nitride powder of Example 6 was produced under the same conditions as in Example 1, except for the crushing conditions. The particle size distribution after crushing was such that the volumetric proportion of agglomerated particles of 10 μm or less was 3%, and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was 30%.

[0086] (Comparative Example 1) The hexagonal boron nitride powder according to Comparative Example 1 was produced under the same conditions as in Example 1, except for the crushing conditions. The particle size distribution after crushing was such that the volumetric proportion of agglomerated particles of 10 μm or less was 10% and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was 30%.

[0087] Comparative Example 2 The hexagonal boron nitride powder of Comparative Example 2 was produced by reducing and nitriding 242 g of a mixture containing 142 g of boron oxide, 62 g of carbon black, and 38 g of calcium oxide, without adding boron carbide as a raw material. Except for this point, it was produced under the same conditions as in Example 1. The particle size distribution after crushing was such that the volumetric proportion of agglomerated particles of 10 μm or less was 30%, and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was 70%.

[0088] Comparative Example 3 Hexagonal boron nitride powder according to Comparative Example 3 was produced under the same conditions as in Example 1, except that the heating temperature in the re-firing was 1500° C. The particle size distribution after crushing was such that the volumetric proportion of agglomerated particles of 10 μm or less was 4% and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was 40%.

[0089] Comparative Example 4 The hexagonal boron nitride powder according to Comparative Example 4 was produced under the same conditions as those of Comparative Example 3, except for the crushing conditions. The particle size distribution after crushing was such that the volumetric proportion of agglomerated particles of 10 μm or less was 2% and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was 20%.

[0090] Boron carbide (B 4 The presence or absence of the use of hexagonal boron nitride powder C), the particle size distribution of the hexagonal boron nitride powder before re-firing, and the heating temperature (maximum temperature reached) for re-firing are summarized in Table 1 below. The tapped bulk density, loose bulk density, density ratio (tapped bulk density / loose bulk density), and average particle size of the resulting hexagonal boron nitride powder after re-firing are also shown in Table 1 below. Note that "10 to 50 μm" in the column for particle size distribution before re-firing in Table 1 indicates more than 10 μm and not more than 50 μm.

[0091]

[0092] (Evaluation Methods) Loose Bulk Density, Tapped Bulk Density The loose bulk density and tapped bulk density of hexagonal boron nitride powder were measured using a Tap Denser KYT-5000 manufactured by Seishin Enterprise Co., Ltd. The hexagonal boron nitride powder was loosely filled into a 100 mL sample cell, and the loose bulk density was calculated from the mass and volume immediately after the loose bulk density was calculated. Next, the 100 mL sample cell after calculating the loose bulk density was tapped at a tapping speed of 120 times / min, a tapping height of 5 cm, and 500 taps, and the tapped bulk density was calculated from the mass and volume after tapping. The sample cell consisted of a lidded cylinder with a diameter of 28 mm and a height of 163 mm.

[0093] Average Area Circularity, Average Area Envelopment Ratio, and Volume Proportion For the hexagonal boron nitride powder, the average particle size of the entire hexagonal boron nitride powder, and the average area circularity, average area envelopment ratio, and volume proportion of each of the first agglomerated particles and the second agglomerated particles were evaluated using a Morphologi G3-ID / G3SE-ID manufactured by Malvern Instruments.

[0094] Average particle size, volume percentage of 10 μm or less, and volume percentage of more than 10 μm and less than 50 μm. The hexagonal boron nitride powder was measured for its average particle size (μm), volume percentage of 10 μm or less, and volume percentage of more than 10 μm and less than 50 μm using a laser diffraction / scattering particle size analyzer MT3000 (manufactured by Microtrac Bell Co., Ltd.). Specifically, a sample prepared by adding 0.1 g of hexagonal boron nitride powder to a mixing vessel attached to the analyzer filled with 50 cc of ethanol was used for the measurement. From the measurement results, the volumetric particle size (D50), volume percentage of 10 μm or less, and volume percentage of more than 10 μm and less than 50 μm were calculated. The measurements were performed without any crushing treatment, such as ultrasonic treatment.

[0095] (Results) The hexagonal boron nitride powders according to the examples and comparative examples were evaluated for the first agglomerated particles and the second agglomerated particles, and the results are shown in Table 2 below.

[0096]

[0097] In the hexagonal boron nitride powders according to Examples 1 to 6, the average area circularity of the first agglomerate particles was 0.2 or more and 0.3 or less, and the average area envelopment ratio was 0.5 or more and 0.7 or less. This result indicates that the shape of the first agglomerate particles was distorted.

[0098] On the other hand, the first aggregate particles according to Comparative Examples 1, 3, and 4 had an average area circularity of 0.6 or more and an average area envelopment ratio of 0.8 or more. That is, the first aggregate particles according to Comparative Examples 1, 3, and 4 had a shape closer to a sphere than the first aggregate particles according to each Example.

[0099] Furthermore, all of the hexagonal boron nitride powders according to Examples 1 to 6 and Comparative Examples 1, 3, and 4 contained second agglomerated particles that were more spherical than the first agglomerated particles according to each Example. The hexagonal boron nitride powder according to Comparative Example 2 consisted mostly of first agglomerated particles with a particle diameter of 20 μm or more and 50 μm or less, and no second agglomerated particles with a particle diameter of 60 μm or more were detected. Therefore, the average area circularity and average area envelopment were not evaluated.

[0100] To obtain the present hexagonal boron nitride powder, it is important to control the volumetric ratio of agglomerated particles of 10 μm or less in the particle size distribution before re-firing to less than 10%, as shown in Comparative Examples 1 and 2. It is also important to set the maximum temperature reached in re-firing to 1700° C. or higher, as shown in Comparative Examples 3 and 4.

[0101] <Evaluation of Resin Sheet Filled with Hexagonal Boron Nitride Powder> Next, resin sheets filled with hexagonal boron nitride powder according to each of the Examples and Comparative Examples were manufactured, and the thermal conductivity of the resin sheets was evaluated.

[0102] (Method for manufacturing resin sheet) The obtained hexagonal boron nitride powder was filled into an epoxy resin to prepare a resin composition, and the thermal conductivity was evaluated. A mixture of 100 parts by mass of epoxy resin (JER828 manufactured by Mitsubishi Chemical Corporation), 5 parts by mass of a curing agent (imidazole-based curing agent, Curesol 2E4MZ manufactured by Shikoku Chemical Industry Co., Ltd.), and 210 parts by mass of methyl ethyl ketone as a solvent was prepared. Next, the varnish-like mixture and hexagonal boron nitride powder were mixed in a rotation / revolution mixer (MAZERUSTAR manufactured by Kurabo Industries Co., Ltd.) to obtain a resin composition of 35% by volume of base resin and 65% by volume of the specific boron nitride powder, 40% by volume of base resin and 60% by volume of the specific boron nitride powder, or 45% by volume of base resin and 55% by volume of the specific boron nitride powder.

[0103] The resin composition was coated onto a PET film to a thickness of approximately 180 to 220 μm using a Tester Sangyo automatic coater PI-1210, dried, and cured under reduced pressure at a temperature of 200°C, a pressure of 5 MPa, and a holding time of 30 minutes to produce a sheet with a thickness of 150 μm. The sheet was analyzed using a temperature wave thermal analyzer to calculate the thermal conductivity.

[0104] (Results) The thermal conductivity (W / m·K) of the obtained resin sheet is shown in Table 3 below.

[0105]

[0106] At loading levels of 55% and 60% by volume, the resin sheets according to Examples 1 to 6 exhibited higher thermal conductivities than the resin sheets according to Comparative Examples 1 to 4. On the other hand, at loading levels of 65% by volume, the thermal conductivities of the resin sheets according to the Examples and Comparative Examples were equivalent, except for Comparative Example 2. This result demonstrates that the hexagonal boron nitride powder according to one embodiment of the present invention is effective in obtaining higher thermal conductivities than conventional powders, particularly in the range of relatively low loading levels.

[0107] The above results show that by using the hexagonal boron nitride powder according to one embodiment of the present invention, the amount of filling required to obtain a desired thermal conductivity can be reduced compared to conventional methods.

[0108] [Additional Notes] The present invention is not limited to the above-described embodiments and examples, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention.

Claims

1. Tapped bulk density is 0.50 g / cm 3 or more, a ratio of the tapped bulk density to the loose bulk density is 2.1 or more, and an average particle size is 15 μm or more.

2. The hexagonal boron nitride powder according to claim 1, comprising first agglomerated particles which are agglomerated particles of hexagonal boron nitride primary particles and have a particle diameter of 20 μm or more and 50 μm or less, and the first agglomerated particles have an average area circularity of 0.1 or more and less than 0.6, and an average area envelopment ratio of 0.4 or more and less than 0.

9.

3. The hexagonal boron nitride powder according to claim 2, further comprising second agglomerated particles which are agglomerated particles of hexagonal boron nitride primary particles and have a particle diameter of 60 μm or more and 110 μm or less, and the second agglomerated particles have an average area circularity of 0.4 or more and 0.9 or less and an average area envelopment ratio of 0.4 or more and 0.9 or less.

4. The loose bulk density is 0.15 g / cm 3 0.35g / cm or more 3 2. The hexagonal boron nitride powder of claim 1, wherein:

5. A resin composition comprising the hexagonal boron nitride powder according to any one of claims 1 to 4.

6. A resin sheet comprising the resin composition according to claim 5.