Method for manufacturing printed wiring board
Patent Information
- Application Number
- MYPI2025005738
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-03-06
- Publication Date
- 2024-09-23
AI Technical Summary
Current methods for manufacturing printed wiring boards face challenges in suppressing pattern defects while achieving excellent high-frequency characteristics, particularly with the miniaturization of circuits and the use of copper foils with smooth surfaces and small roughening particles.
A method involving the preparation of an insulating base material with a roughened surface, followed by electroless plating with controlled peak density and curvature, and the application of a photoresist to form a wiring pattern, which effectively reduces pattern defects and enhances high-frequency characteristics.
This approach significantly suppresses pattern defects such as short circuits and protrusions while maintaining excellent high-frequency performance, making it suitable for advanced electronic devices.
Smart Images

Figure PI2025005738_DRAWING_001 
Figure PI2025005738_DRAWING_002 
Figure PI2025005738_DRAWING_003
Abstract
Description
Printed wiring board manufacturing method
[0001] The present invention relates to a method for manufacturing a printed wiring board.
[0002] In recent years, the demand for miniaturization and high density in printed wiring boards has led to a demand for finer circuitry (fine pitch). The semi-additive process (SAP process) has been widely adopted as a manufacturing method for printed wiring boards suitable for achieving this. The SAP process is a technique suitable for forming extremely fine circuits, and one example of this process is performed using a carrier-attached roughened copper foil. For example, as shown in FIGS. 8 and 9 , a roughened copper foil 110 is pressed against an insulating resin substrate 111 having a base substrate 111a and a lower layer circuit 111b, using a prepreg 112 and a primer layer 113 (step (a)). After the carrier (not shown) is peeled off, via holes 114 are formed by laser drilling as needed (step (b)). The roughened copper foil 110 is then removed by etching to expose the primer layer 113 with a roughened surface profile (step (c)). After electroless copper plating 115 is applied to this roughened surface (step (d)), it is masked with a predetermined pattern by exposure and development using a dry film 116 (step (e)), and electrolytic copper plating 117 is applied (step (f)). After removing the dry film 116 to form wiring portions 117a (step (g)), unnecessary electroless copper plating 115 between adjacent wiring portions 117a, 117a is removed by etching (step (h)), and wiring 118 formed in a predetermined pattern is obtained.
[0003] In this way, in the SAP method using a roughened copper foil, the roughened copper foil itself is removed by etching after laser perforation (step (c)). The uneven shape of the roughened surface of the roughened copper foil is transferred to the laminate surface from which the roughened copper foil has been removed, ensuring adhesion between the insulating layer (e.g., the primer layer 113, or the prepreg 112 if the primer layer is not present) and the plated circuit (e.g., the wiring 118) in subsequent steps. However, since the surface profile suitable for improving adhesion to the plated circuit generally tends to be rough and uneven, the etching resistance to electroless copper plating in step (h) is likely to be reduced. In other words, since the electroless copper plating penetrates into the rough unevenness, more etching is required to remove the residual copper.
[0004] Therefore, a method has been proposed in which the roughening particles are made small and have a constricted shape, thereby achieving good etching properties while ensuring the necessary plating circuit adhesion when used in the SAP method. For example, Patent Document 1 (WO 2016 / 158775) discloses a roughened copper foil having a roughened surface on at least one side, the roughened surface having a plurality of approximately spherical protrusions made of copper particles, and the average height of the approximately spherical protrusions is 2.60 μm or less. Furthermore, Patent Document 2 (WO 2018 / 211951) discloses a roughened copper foil having a roughened surface on at least one side, the roughened surface having primary roughening particles with constricted portions and secondary roughening particles on the surfaces of the primary roughening particles, and the roughened surface has a low ten-point average roughness Rz of 1.7 μm or less.
[0005] Furthermore, in order to further miniaturize circuits, it has been considered to form circuits in the SAP method by using copper foil with a smooth surface and small roughening particles and thinly applying electroless plating. However, circuits formed in this manner may suffer from pattern defects such as short circuits and protrusions. A method for manufacturing a printed wiring board that addresses this problem has been proposed. For example, Patent Document 3 (WO 2020 / 196105) discloses a method for manufacturing a printed wiring board, including a step of applying electroless plating to an insulating substrate with a roughened surface to form an electroless plated layer with a thickness of less than 1.0 μm, the electroless plated layer having a surface with an arithmetic mean waviness Wa of 0.10 μm or more and 0.25 μm or less and a kurtosis Sku of 2.0 or more and 3.5 or less. In addition, Patent Document 4 (WO 2020 / 196106) describes a method in which the arithmetic mean waviness Wa is 0.10 μm or more and 0.25 μm or less, and the void volume Vvv of the valley portion is 0.010 μm. 3 / μm 2 More than 0.028 μm 3 / μm 2 It is also disclosed that an electroless plating layer having the following surface is formed. According to the methods disclosed in Patent Documents 3 and 4, it is said that it is possible to effectively suppress pattern defects and produce a printed wiring board that is excellent in fine circuit formability.
[0006] International Publication No. WO 2016 / 158775 International Publication No. WO 2018 / 211951 International Publication No. WO 2020 / 196105 International Publication No. WO 2020 / 196106
[0007] When a printed wiring board is manufactured using the methods disclosed in Patent Documents 3 and 4, the problem of pattern defects can be resolved to some extent. However, further suppression of pattern defects is desired. In addition, with the recent increase in the functionality of portable electronic devices and the like, signals are becoming increasingly high-frequency in order to process large amounts of information at high speed, and printed wiring boards suitable for high-frequency applications such as 5G, millimeter waves, and base station antennas are also required. However, it is not easy to achieve both suppression of pattern defects and good high-frequency characteristics.
[0008] The present inventors have now discovered that by applying electroless plating to an insulating substrate having a roughened surface to form an electroless plated layer having a surface in which the peak density Sds and peak curvature Ssc are each controlled within a predetermined range, it is possible to produce a printed wiring board in which pattern defects are more effectively suppressed and which also has excellent high-frequency characteristics.
[0009] SUMMARY OF THE INVENTION It is therefore an object of the present invention to provide a method for manufacturing a printed wiring board that more effectively suppresses pattern defects and has excellent high-frequency characteristics.
[0010] The present invention provides the following aspects: [Aspect 1] A method for producing a printed wiring board, comprising the steps of: (a) preparing an insulating substrate having a roughened surface; and (b) electroless plating the roughened surface of the insulating substrate to produce a printed wiring board having a peak density Sds of 0.90 μm as measured in accordance with EUR 15178N. -2 1.30 μm or more -2 and the peak curvature Ssc measured in accordance with EUR15178N is 1.00 μm or less. -1 4.00 μm or more -1 (c) laminating a photoresist on the surface of the electroless plated layer, (d) exposing and developing the photoresist to form a resist pattern, (e) electroplating the electroless plated layer through the resist pattern, (f) peeling off the resist pattern, and (g) removing by etching unnecessary portions of the electroless plated layer exposed by peeling off the resist pattern to form a wiring pattern. [Aspect 2] The method for manufacturing a printed wiring board according to Aspect 1, wherein the surface of the electroless plated layer has an interface developed area ratio Sdr of 5.00% or more and 10.00% or less, as measured in accordance with EUR 15178N. [Aspect 3] The surface of the electroless plated layer has an interface developed area ratio Sdr of 5.00% or more and 10.00% or less, as measured in accordance with EUR 15178N. -1 3.50 μm or more -1A method for producing a printed wiring board according to aspect 1 or 2, wherein the step (a) is: (a-1) a peak density Sds measured in accordance with EUR15178N is 1.00 μm or less. -2 1.50 μm or more -2 The peak curvature Ssc measured in accordance with EUR15178N is 4.00 μm or less. -1 6.00 μm or more -1 A method for producing a printed wiring board according to any one of Aspects 1 to 3, comprising: (a-2) providing a surface-treated copper foil having a treated surface in which the developed area ratio Sdr of the interface is 20.00% or less and 40.00% or less, as measured in accordance with EUR 15178N; (a-3) laminating an insulating base material on the treated surface of the surface-treated copper foil to transfer the surface shape of the treated surface to the surface of the insulating base material; and (a-4) removing the surface-treated copper foil by etching to obtain an insulating base material having the roughened surface. [Aspect 5] A method for producing a printed wiring board according to any one of Aspects 1 to 4, wherein the electroless plating layer has a thickness of 0.3 μm or more and 1.0 μm or less. [Aspect 6] A method for producing a printed wiring board according to any one of Aspects 1 to 5, wherein the photoresist comprises a dry film resist. [Aspect 7] A method for producing a printed wiring board according to Aspect 6, wherein the dry film resist has a thickness of 2 μm or more and 35 μm or less. [Embodiment 8] The method for producing a printed wiring board according to any one of embodiments 1 to 7, wherein the wiring pattern has a thickness of 2 μm or more and 30 μm or less.
[0011] FIG. 1 is a process flow diagram showing the first half of the steps (steps (a) to (c)) in an example of the manufacturing method of the present invention. FIG. 2 is a process flow diagram showing the second half of the steps (steps (d) to (g)) in an example of the manufacturing method of the present invention. FIG. 3 is a process flow diagram showing an example of a procedure for preparing an insulating substrate having a roughened surface. FIG. 4 is a diagram for explaining the influence of surface foreign matter during exposure and development when the surface after electroless plating does not have a sufficient uneven shape. FIG. 5 is a diagram for explaining the influence of surface foreign matter during exposure and development when the surface after electroless plating has a sufficient uneven shape. FIG. 6 is a diagram for explaining the procedure for evaluating the number of detected dust particles in the examples. FIG. 7 is a diagram for explaining the peak density Sds measured in accordance with EUR15178N, where Sds=5 μm-2 1 is a diagram illustrating an example of the surface and peaks in the case of 1 μm. -2 1 is a diagram showing an example of the surface and peaks in the case of FIG. 2. FIG. 3 is a process flow diagram for explaining the SAP method, showing the first half of the process (steps (a) to (d)). FIG. 4 is a process flow diagram for explaining the SAP method, showing the second half of the process (steps (e) to (h)).
[0012] DEFINITIONS The following are definitions of the parameters used to define the present invention.
[0013] As used herein, "peak density Sds" or "Sds" is a parameter representing the number of peaks per unit area, measured in accordance with EUR 15178N. As shown in Figures 7A and 7B, in calculating Sds, a point higher than eight neighboring points N is considered to be a peak S. A larger value indicates a denser presence of bumps (see Figure 7A). Conversely, a smaller value indicates a sparser presence of bumps (see Figure 7B).
[0014] As used herein, "peak curvature Ssc" or "Ssc" refers to a parameter that represents the average principal curvature at the peak of a surface peak, measured in accordance with EUR15178N. The smaller this value, the more rounded the point of contact with other objects. On the other hand, the larger this value, the more pointed the point of contact with other objects. Note that while the parameters specified in ISO25178 only consider significant peaks remaining after segmentation, the parameters specified in EUR15178N detect local peaks and significant peaks without distinguishing between them. Therefore, when the surface shape is the same, the Ssc specified in EUR15178N will be greater than the Spc specified in ISO25178 (Spc<Ssc).
[0015] As used herein, "interface developed area ratio Sdr" or "Sdr" is a parameter that indicates how much the developed area (surface area) of a defined region has increased relative to the area of the defined region, as measured in accordance with EUR15178N. In this specification, the interface developed area ratio Sdr is expressed as the increase in surface area (%). The smaller this value, the closer the surface shape is to flatness, and the Sdr of a completely flat surface is 0%. On the other hand, the larger this value, the more irregular the surface shape is. For example, if the Sdr of a surface is 10%, this indicates that the surface area of this surface has increased by 10% from a completely flat surface.
[0016] Sds, Ssc, and Sdr can each be calculated by measuring the surface profile of a predetermined measurement area (e.g., a two-dimensional area of 64.397 μm × 64.463 μm) on the roughened surface using a commercially available laser microscope. In this specification, Sds, Ssc, and Sdr are measured under conditions without cutoff by the S filter and L filter. Other preferred measurement and analysis conditions for the surface profile using a laser microscope are shown in the examples described below.
[0017] The present invention relates to a method for manufacturing a printed wiring board, which includes the steps of (a) preparing an insulating substrate, (b) forming an electroless plating layer, (c) laminating a photoresist, (d) forming a resist pattern, (e) forming an electroplating layer, (f) stripping the resist pattern, and (g) forming a wiring pattern.
[0018] Each of the steps (a) to (g) will be described below with reference to FIGS.
[0019] (a) Preparation of Insulating Substrate As shown in FIG. 1( a), an insulating substrate 20 having a roughened surface 20a is prepared. The insulating substrate 20 may have roughened surfaces 20a on both sides or only one side. The insulating substrate 20 preferably contains an insulating resin. The insulating substrate 20 is preferably a prepreg and / or a resin sheet. Prepreg is a general term for composite materials in which a substrate such as a synthetic resin plate, a glass plate, a woven glass fabric, a nonwoven glass fabric, or paper is impregnated with a synthetic resin. Preferred examples of insulating resins impregnated into prepregs include epoxy resins, cyanate resins, bismaleimide triazine resins (BT resins), polyphenylene ether resins, and phenolic resins. Examples of insulating resins constituting resin sheets include insulating resins such as epoxy resins, polyimide resins, and polyester resins. The insulating substrate 20 may contain filler particles made of various inorganic particles such as silica and alumina to improve insulation properties. The thickness of the insulating substrate 20 is not particularly limited, but is preferably from 1 μm to 1000 μm, more preferably from 2 μm to 400 μm, and even more preferably from 3 μm to 200 μm. The insulating substrate 20 may be composed of multiple layers.
[0020] The roughened surface 20a of the insulating substrate 20 may be formed by any method, but is typically formed by transferring the irregularities of the treated surface of a surface-treated copper foil to the surface of the insulating substrate 20. According to a preferred embodiment of the present invention, the roughened surface 20a using a surface-treated copper foil is formed by (a-1) preparing a surface-treated copper foil having a predetermined treated surface, (a-2) laminating an insulating substrate onto the treated surface of the surface-treated copper foil to transfer the surface shape of the treated surface to the surface of the insulating substrate, and then (a-3) removing the surface-treated copper foil by etching to obtain an insulating substrate with a roughened surface. The specific procedures for each step are as follows.
[0021] (a-1) Preparation of Surface-Treated Copper Foil As shown in FIG. 3(a-1), a surface-treated copper foil 10 having a treated surface 10a on at least one side is prepared. The treated surface 10a is a surface that has been subjected to some kind of surface treatment, typically a roughened surface. The treated surface 10a typically comprises multiple nodules (e.g., roughening particles). In either case, the surface-treated copper foil 10 may have the treated surface 10a on both sides, or only one side. When the treated surface 10a is present on both sides, the surface on the laser irradiation side (the surface opposite the surface that is adhered to the insulating substrate) is also surface-treated when used in the SAP method. This increases laser absorbency and improves laser perforation properties. The surface-treated copper foil 10 may also be in the form of a carrier-attached copper foil. In this case, the carrier-attached copper foil typically comprises a carrier, a release layer provided on the carrier, and the surface-treated copper foil 10 provided on the release layer with the treated surface 10a facing outward. However, the carrier-attached copper foil can have a known layer structure, except that the surface-treated copper foil 10 is used.
[0022] The treated surface 10a of the surface-treated copper foil 10 has a peak density Sds of 1.00 μm -2 1.50 μm or more -2 Preferably it is equal to or less than 1.00 μm, more preferably 1.00 μm -2 1.40 μm or more -2 or less, more preferably 1.10 μm -2 1.40 μm or more -2 Below 1.20 μm, particularly preferably -2 1.40 μm or more -2 The treated surface 10a of the surface-treated copper foil 10 has a peak curvature Ssc of 4.00 μm or less. -1 6.00 μm or more -1 Preferably it is equal to or less than 4.50 μm, more preferably 4.50 μm -1 6.00 μm or more -1 or less, more preferably 4.50 μm -1 5.00 μm or more -1or less. Furthermore, the treated surface 10a of the surface-treated copper foil 10 preferably has an interface developed area ratio Sdr of 20.00% or more and 40.00% or less, more preferably 20.00% or more and 25.00% or less. By imparting a textured shape to the insulating substrate 20 using a surface-treated copper foil 10 having a treated surface 10a with Sds, Ssc, and Sdr within these ranges, it becomes easier to form an electroless plating layer 22 having the specific surface parameters described below on the roughened surface 20a of the insulating substrate 20. The treated surface 10a having the above surface parameters can be formed by subjecting the copper foil surface to a surface treatment (typically a roughening treatment) under known or desired conditions. Alternatively, a commercially available copper foil having a treated surface 10a that satisfies the above conditions may be selectively obtained.
[0023] (a-2) Transfer of Textured Shape to Insulating Substrate As shown in FIG. 3(a-2), an insulating substrate 20' (i.e., an insulating substrate 20 without a roughened surface 20a) is laminated on the treated surface 10a of the surface-treated copper foil 10 to form a copper-clad laminate 12. This allows the surface texture of the treated surface 10a to be transferred to the surface of the insulating substrate 20'. The lamination of the insulating substrate 20' preferably involves a heat press or heat lamination process. The processing temperature and processing time for this heat press or heat lamination process can be appropriately determined based on known conditions, depending on the type of insulating substrate 20' to be laminated. The preferred types of insulating substrate 20' are as described above for the insulating substrate 20. The insulating substrate 20' may be laminated to the surface-treated copper foil 10 via a primer layer (not shown) that is applied in advance to the treated surface 10a of the surface-treated copper foil 10. In this case, the primer layer is considered to constitute part of the insulating substrate. The primer layer is preferably composed of a resin, and this resin preferably contains an insulating resin. If desired, prior to the next step of removing the surface-treated copper foil 10, via holes (not shown) may be formed in the copper-clad laminate 12 by laser drilling.
[0024] 3(a-3), the surface-treated copper foil 10 of the copper-clad laminate 12 is removed by etching to obtain an insulating substrate 20 having a roughened surface 20a. Etching of the surface-treated copper foil 10 may be performed using, for example, a sulfuric acid-hydrogen peroxide-based etching solution according to an etching technique and conditions generally used in the manufacture of printed wiring boards, and is not particularly limited.
[0025] 1(b), electroless plating (e.g., electroless copper plating) is performed on the roughened surface 20a of the insulating substrate 20 to form an electroless plated layer 22 having a thickness of 1.0 μm or less. Electroless plating may be performed using a commercially available electroless plating solution according to techniques and conditions commonly used in the manufacture of printed wiring boards, and is not particularly limited. The surface of the electroless plated layer 22 has a peak density Sds of 0.90 μm. -2 1.30 μm or more -2 or less, and the peak curvature Ssc is 1.00 μm -1 4.00 μm or more -1 In this way, by applying electroless plating to insulating substrate 20 having roughened surface 20 a to form electroless plated layer 22 having a surface in which peak density Sds and peak curvature Ssc are controlled within predetermined ranges, pattern defects are more effectively suppressed and a printed wiring board having excellent high-frequency characteristics can be manufactured.
[0026] As described above, in recent years, with the demand for finer circuits in the SAP process, it has been considered to provide an insulating substrate with a roughened surface profile by using a copper foil with a smooth surface and small roughening particles to achieve excellent etching properties. Furthermore, if a thin layer of electroless plating (e.g., 1.0 μm or less) can be applied to the surface of an insulating substrate with a roughened surface profile, this would be advantageous because it would reduce the amount of etching and allow for further finer circuits. However, when attempting to form a circuit using a copper foil with a smooth surface and small roughening particles and a thin layer of electroless plating in the SAP process, pattern defects such as short circuits and protrusions in the formed circuit can occur. The mechanism by which these pattern defects occur is not entirely clear, but is presumed to be as follows.
[0027] That is, when a surface shape is transferred to an insulating substrate using a surface-treated copper foil, the roughened surface of the insulating substrate generally reflects the surface profile of the surface-treated copper foil. Furthermore, when electroless plating is applied to the roughened surface of this insulating substrate at a thickness of 1.0 μm or less, the surface shape of the electroless plated layer generally reflects the surface shape of the roughened surface of the insulating substrate. Therefore, if a copper foil with a smooth surface and small roughening particles (in other words, a copper foil with a fine unevenness) is used as the copper foil used to transfer the surface profile to the insulating substrate, it is difficult to impart a sufficient unevenness to the surface of the electroless plated layer. Meanwhile, in a typical printed wiring board manufacturing process, to form a circuit with a predetermined pattern, as shown in FIGS. 4( i) to 4( iv) , a photoresist 24 (e.g., including a dry film resist 24 a and a support film 24 b) is further laminated on the surface of an electroless plated layer 22 laminated on an insulating substrate 20, and then exposed and developed to form a resist pattern 26. As shown in FIG. 4( i), during deposition or exposure of the photoresist 24, foreign matter F (e.g., dust or scratches on the photoresist surface, or air entrapment during deposition of the photoresist) may adhere to or become mixed into the surface of the photoresist 24. For example, in a printed wiring board manufacturing factory, clean rooms are typically operated at a cleanliness level of approximately Class 100 to Class 1000, making it difficult to completely eliminate foreign matter present in the environment. It is also difficult to detect even minute scratches on the surface of the photoresist 24. In this regard, when exposure is performed on the photoresist 24 deposited on the surface of the electroless plated layer 22 that does not have a sufficient texture, as shown in FIG. 4( ii), the incident exposure light I entering from a direction perpendicular to the main surface of the laminate is reflected by the electroless plated layer 22 and exits as reflected exposure light R in a direction 180° opposite to the incident exposure light I. As a result, the portion of the photoresist 24 (e.g., dry film resist 24a) directly below the foreign substance F, which should have been exposed, remains unexposed (see FIG. 4(iii)), resulting in the formation of a hole H after development (see FIG. 4(iv)).As a result, electroplating is applied to areas where no circuit should be formed, and this unnecessary electroplated portion is thought to cause the above-mentioned circuit shorts and protrusions, resulting in the problem of pattern defects.
[0028] Furthermore, polyethylene terephthalate (PET) film is commonly used as the support film 24b constituting the photoresist 24. A lubricant is added to this PET film to improve fluidity and mold releasability during thermoforming. This lubricant typically has a variable particle size, with a certain percentage of particles being large (e.g., 10 μm or larger in diameter). Therefore, due to the large-sized foreign matter inevitably present in such PET film, areas that should be exposed may remain unexposed, resulting in pattern defects, as described above. While it is conceivable to peel off the PET film and expose the dry film before exposure, this exposure may cause deformation of the dry film due to oxygen. In other words, the above-mentioned pattern defects caused by the lubricant contained in the PET film are unavoidable. In this regard, conventional printed wiring board manufacturing methods such as those disclosed in Patent Document 3 (WO 2020 / 196105) and Patent Document 4 (WO 2020 / 196106) have room for improvement in terms of eliminating pattern defects caused by large foreign objects. On the other hand, it is also possible to excessively increase the roughness of the electroless plating layer surface by transferring the surface shape to the insulating substrate using a surface-treated copper foil with a high roughness of the treated surface. However, adopting such a method will result in deterioration of high-frequency characteristics. As such, it is not easy to achieve both suppression of pattern defects and good high-frequency characteristics.
[0029] In this regard, the method of the present invention makes it possible to further suppress pattern defects while also achieving good high frequency characteristics. The mechanism behind this is not entirely clear, but is thought to be as follows: That is, when the peak density Sds on the surface of the electroless plated layer 22 is set to 0.90 μm -2 1.30 μm or more -2 and the peak curvature Ssc is 1.00 μm or less. -14.00 μm or more -1 By satisfying the following conditions, the surface of the electroless plated layer 22 has a moderately uneven shape (see FIG. 5( i)). Therefore, during exposure, the incident exposure light I, which enters perpendicularly to the main surface of the laminate, is diffusely reflected by the uneven portions of the surface of the electroless plated layer 22 when it reaches the surface of the electroless plated layer 22 (see FIG. 5( ii)). As a result, the reflected exposure light R can expose the portion of the photoresist 24 (e.g., dry film resist 24 a) directly below the foreign matter F (see FIG. 5( iii)). Typically, about 60 to 70 percent of the light of the wavelength used to expose the photoresist 24 is absorbed by the electroless plated layer 22, which is made of copper or the like. Therefore, for example, if the angle between the incident exposure light I and the reflected exposure light R is too large, the reflected exposure light R may be absorbed by the electroless plated layer 22 (e.g., the uneven portions near the reflection point), and may not contribute to eliminating pattern defects caused by the foreign matter F. In this regard, by controlling the surface shape of the electroless plated layer 22 by combining the peak density Sds and peak curvature Ssc so that they fall within the above-mentioned range, it becomes easier to control the angle between the incident exposure light I and the reflected exposure light R within the desired range, thereby enabling extremely effective exposure of the portion of the photoresist 24 (e.g., dry film resist 24a) directly below the foreign matter F. In other words, even if the foreign matter F present on the surface and / or inside the photoresist 24 is large, its influence can be canceled. In this way, the formation of unexposed portions of the photoresist 24 due to the foreign matter F is effectively prevented, and the formation of unnecessary holes H during development is suppressed (see FIG. 5(iv)). This is believed to reduce the occurrence of pattern defects such as short circuits and protrusions in the circuit. Nevertheless, the surface of the electroless plated layer 22 having the peak density Sds and peak curvature Ssc within the above-mentioned ranges has a surface shape with low roughness, which is effective in reducing the skin effect, and therefore is believed to also achieve excellent high-frequency characteristics.
[0030] From the above viewpoint, the surface of the electroless plated layer 22 has a peak density Sds of 0.90 μm -2 1.30 μm or more -2 or less, preferably 0.90 μm -21.20 μm or more -2 Less than or equal to 1.10 μm, more preferably -2 1.20 μm or more -2 The following is the result.
[0031] The surface of the electroless plating layer 22 has a peak curvature Ssc of 1.00 μm. -1 4.00 μm or more -1 or less, preferably 2.30 μm -1 3.50 μm or more -1 Less than or equal to 2.30 μm, more preferably -1 3.00 μm or more -1 The following is the result.
[0032] The surface of the electroless plated layer 22 preferably has an interface developed area ratio Sdr of 5.00% to 10.00%, more preferably 5.00% to 6.00%. Within these ranges, excellent high-frequency characteristics can be achieved while further suppressing pattern defects caused by larger foreign particles F.
[0033] The electroless plated layer 22 having the above-described specific surface parameters can be formed by applying electroless plating to a thickness of 1.0 μm or less on the roughened surface 20 a of the insulating substrate 20. As described above, the surface shape of the electroless plated layer 22 can be said to largely reflect the surface shape of the roughened surface 20 a of the insulating substrate 20. The roughened surface 20 a can be preferably formed by, for example, transferring the surface shape of the surface-treated copper foil 10 having the surface parameters described in (a) above to the insulating substrate 20.
[0034] The thickness of the electroless plating layer 22 is 1.0 μm or less, and preferably 0.3 μm or more and 1.0 μm or less. With such a thickness, it is possible to reduce the amount of etching during wiring pattern formation, making it extremely suitable for forming fine circuits.
[0035] (c) Lamination of Photoresist As shown in FIG. 1(c), a photoresist 24 is laminated on the surface of the electroless plated layer 22. The lamination speed when laminating the photoresist 24 is not particularly limited, but is typically 1.0 m / min to 2.0 m / min. The photoresist 24 may be any known material commonly used in the manufacture of printed wiring boards. The photoresist 24 may be either a negative or positive type, and may be either a film type or a liquid type. Preferably, the photoresist 24 includes a dry film resist 24a. The photoresist 24 is preferably a photosensitive film, such as a photosensitive dry film. As shown in FIG. 1(c), the photoresist 24 may be formed by laminating a support film 24b, such as a polyethylene terephthalate (PET) film, on the dry film resist 24a as a photosensitive layer. The support film 24b, such as a PET film, typically contains a lubricant to improve fluidity and releasability during thermoforming. In this regard, according to the present invention, as described above, it is possible to effectively suppress pattern defects caused by lubricants, etc. The thickness of the photoresist 24 or dry film resist 24a is preferably 2 μm or more and 35 μm or less, and more preferably 5 μm or more and 24 μm or less.
[0036] (d) Formation of Resist Pattern As shown in FIG. 2(d), a resist pattern 26 is formed by exposing and developing the photoresist 24. The exposure and development may be performed according to known techniques and conditions generally used in the manufacture of printed wiring boards, and are not particularly limited. For example, as the exposure method, a mask exposure method using a negative or positive mask pattern, as well as a direct writing exposure method such as a Laser Direct Imaging (LDI) exposure method or a Digital Light Processing (DLP) exposure method, etc., can be used. The exposure dose during exposure is 5 mJ / cm. 2 150mJ / cm or more 2The following is preferable. On the other hand, the development method may be either wet development or dry development. In the case of wet development, the developer used may be a developer such as sodium carbonate, sodium hydroxide, or an amine-based aqueous solution. Note that, when the photoresist 24 includes a support film 24b, it is preferable to perform development after removing the support film 24b.
[0037] (e) Formation of Electroplated Layer Electroplating (e.g., copper electroplating) is performed on the electroless plated layer 22 via the resist pattern 26. In this manner, an electroplated layer 28 can be formed between the resist patterns 26, as shown in Fig. 2(e) . Electroplating can be performed according to various pattern plating techniques and conditions commonly used in the manufacture of printed wiring boards, such as using a copper sulfate plating solution or a copper pyrophosphate plating solution, and is not particularly limited.
[0038] (f) Removal of Resist Pattern In this step, the resist pattern 26 is removed. As a result, as shown in FIG. 2(f), the electroplated layer 28 remains in the form of a wiring pattern, and unnecessary portions of the electroless plated layer 22 that do not form the wiring pattern are exposed. The resist pattern 26 can be removed using an aqueous sodium hydroxide solution, an amine-based solution, or an aqueous solution thereof, and can be removed according to any of the various removal techniques and conditions commonly used for printed wiring boards, without any particular limitations.
[0039] (g) Formation of Wiring Pattern: The unnecessary portions of the electroless plated layer 22 exposed by the peeling of the resist pattern 26 (i.e., portions where no wiring pattern will be formed) are removed by etching to form the wiring pattern 30. Etching of the unnecessary portions of the electroless plated layer 22 can be performed using, for example, a sulfuric acid-hydrogen peroxide-based etching solution according to etching techniques and conditions commonly used in the manufacture of printed wiring boards, and is not particularly limited. The thickness (i.e., circuit height) of the wiring pattern 30 is preferably 2 μm or more and 30 μm or less. The wiring pitch of the wiring pattern 30 is preferably within the range of 10 μm (e.g., line / space = 5 μm / 5 μm) to 20 μm (e.g., line / space = 10 μm / 10 μm). By forming circuits on the electroless plated layer 22 having the predetermined surface parameters described above and a thickness of 1.0 μm or less, it is possible to form such highly fine wiring patterns. Furthermore, wiring patterns with a wiring pitch within the above range are prone to pattern defects such as short circuits and protrusions. However, as described above, the method of the present invention effectively solves these problems.
[0040] If necessary, an insulating layer and an nth wiring pattern (n is an integer of 2 or greater) may be alternately formed on the wiring pattern 30 to form a multilayer wiring board. The wiring patterns constituting the multilayer wiring board can be referred to in order as the second wiring pattern, the third wiring pattern, ..., the nth wiring pattern, with the wiring pattern 30 being the first wiring pattern. The sequentially laminated structure consisting of the first wiring pattern, the nth wiring pattern, and the insulating layer is generally referred to as a build-up layer or build-up wiring layer. The method for forming the build-up layers after the second wiring pattern is not particularly limited, and in addition to the SAP method described above, a modified semi-additive method (MSAP method), a full additive method, a subtractive method, etc. can be used. Furthermore, if necessary, solder resist, mounting bumps such as pillars, etc. may be formed on the wiring pattern on the outermost surface of the build-up layer. In any case, known methods generally used in printed wiring boards can be additionally performed as appropriate, and are not particularly limited.
[0041] The present invention is further illustrated by the following examples.
[0042] Examples 1 to 15: Fifteen types of surface-treated copper foil were prepared, and the surface shape was transferred to an insulating substrate using these surface-treated copper foils. Electroless plating was performed on the roughened surface of the obtained insulating substrate to prepare a laminate for evaluation, and various evaluations were performed. Specifically, the evaluations were as follows.
[0043] (1) Preparation of Surface-Treated Copper Foils Fifteen types of surface-treated copper foils 10 were prepared, each having a treated surface 10a on at least one side with the parameters shown in Table 2. Some of these surface-treated copper foils 10 were commercially available products, while the others were separately prepared based on known methods. The methods for measuring or calculating each parameter on the treated surface 10a of the prepared surface-treated copper foils 10 are as follows.
[0044] The treated surface 10a of the surface-treated copper foil 10 was measured for surface roughness by a laser microscope in accordance with EUR 15178 N. The specific measurement conditions are shown in Table 1.
[0045]
[0046] The measurement data acquired by the laser microscope was read into analysis software (Olympus Corporation, "OLS5100 LEXT (version 2.1.2.215)") and converted to LEXT file format as unprocessed data and output. This LEXT file was read into another analysis software (Digital Surf, "MountainsMap (version 9.0.9878)") and analyzed (analysis area: 64.397 μm × 64.463 μm). Specifically, "Parameter Table" and "Default Settings" were selected from the analysis target tab to display the parameter analysis screen. On the parameter analysis screen, "EUR15178N" was selected as the standard, "Linear Surface" as the wavelength processing, "Least Squares Surface" as the F operation for shape removal, and "Sds", "Ssc", and "Sdr" were selected as parameters. On the other hand, the S filter and L filter were not selected on this screen (i.e., no cutoff was performed by the S filter and L filter). Then, "Export Analysis Results" was selected to save the analysis results, and the peak density Sds, peak curvature Ssc, and interface developed area ratio Sdr were read from the analysis results. For each example, the above parameters were calculated for five different fields of view. The average values over all fields of view were used as Sds, Ssc, and Sdr of the treated surface 10a of the surface-treated copper foil 10, respectively. The results were as shown in Table 2.
[0047] (2) Preparation of Laminate for Evaluation Two sheets of prepreg (GHPL-830NSF, manufactured by Mitsubishi Gas Chemical Co., Inc., thickness 100 μm) were laminated together, and then the surface-treated copper foil 10 prepared in (1) above was laminated on the insulating substrate 20′ so that the treated surface 10a was in contact with the insulating substrate 20′ as shown in FIG. 3 . The laminate was pressed at a temperature of 220° C. for 90 minutes under a pressure of 40 kgf / cm. 2The copper-clad laminate 12 was obtained by pressing under the conditions of
[0049] . The surface-treated copper foil 10 of this copper-clad laminate 12 was completely removed using a sulfuric acid-hydrogen peroxide-based etching solution, yielding an insulating substrate 20 having a roughened surface 20a to which the surface shape of the treated surface 10a was transferred. Electroless copper plating was performed on this insulating substrate 20 using an electroless copper plating solution (Atotech MV+, manufactured by Atotech) to form an electroless plated layer 22 on the roughened surface 20a. The thickness of the electroless plated layer 22 was as shown in Table 2. In this way, a laminate (hereinafter referred to as a laminate for evaluation) was obtained immediately before a photoresist was laminated thereon in the SAP method.
[0048] (3) Measurement of Surface Profile of Evaluation Laminate The peak density Sds, peak curvature Ssc, and interface developed area ratio Sdr of the electroless plated layer 22 side surface of the obtained evaluation laminate were measured by surface roughness analysis using a laser microscope in accordance with EUR15178N. The measurement and analysis conditions for each parameter were the same as those for the surface-treated copper foil in (1) above. The results are shown in Table 2.
[0049] (4) Various Evaluations The obtained laminates or circuit boards for evaluation were evaluated for various properties as follows.
[0050] <Number of detected dust particles> The number of detected dust particles was evaluated as follows. First, a 19 μm-thick negative photoresist 24 (RY-5319, manufactured by Hitachi Chemical Co., Ltd.) was laminated on the surface of the electroless plated layer 22 side of the obtained evaluation laminate at a lamination speed of 1.5 m / min. Thereafter, as shown in FIG. 6( i ), a glass mask 25 was laminated on the surface of the photoresist 24. The glass mask 25 had circular light-shielding portions B (diameter 8 μm to 15 μm (1 μm intervals, 8 levels in total), 25 portions x 12 fields of view) in the center of each area partitioned by 100 μm x 100 μm, which were intended to accommodate foreign matter such as dust. Therefore, light was transmitted through the portions of the glass mask 25 where the light-shielding portions B were not provided, while light was not transmitted through the portions of the glass mask 25 where the light-shielding portions B were provided. The evaluation laminate after laminating the glass mask 25 was exposed to light (70 mJ / cm 2) and development to form a resist pattern 26. The surface of the evaluation laminate on the side of the resist pattern 26 after development was observed with a digital microscope (Keyence Corporation, VHX-7000) at 700x magnification, and the number of holes H formed in the resist pattern 26 was counted, as shown in FIG. 6(ii). The number of holes detected per field of view was then averaged by size of the light-shielding portion B (i.e., a maximum of 25 holes per size) to determine the number of detected dust particles. Note that the greater the number of detected dust particles (i.e., the better the resolution), the greater the risk of unnecessary electroplating in locations where circuits should not be formed, making it more likely that pattern defects will occur. Therefore, for each sample, the diameter of the largest light-shielding portion B at which the number of detected dust particles was 13 or less was considered to be the maximum dust size capable of canceling pattern defects. The results were as shown in Table 2.
[0051] <Evaluation of High-Frequency Characteristics> A high-frequency substrate (MEGTRON7, manufactured by Panasonic Corporation, two sheets of 68 μm thick) was prepared as an insulating resin substrate. Carrier-attached copper foils provided with the surface-treated copper foil 10 prepared in (1) above were laminated on both sides of this insulating resin substrate so that the treated surface 10 a of the surface-treated copper foil 10 abutted against the insulating resin substrate. Pressing was performed using a vacuum press under conditions of a pressure of 3 MPa, a temperature of 190°C, and a pressing time of 90 minutes, after which the carrier was peeled off and removed together with the release layer. The surface-treated copper foil 10 was completely removed using a sulfuric acid-hydrogen peroxide-based etching solution to obtain an insulating substrate 20 having a roughened surface 20 a onto which the surface shape of the treated surface 10 a had been transferred. Subsequently, electroless copper plating was performed on this insulating substrate 20 using an electroless copper plating solution (Atotech MV+, manufactured by Atotech) to form a 0.5 μm-thick electroless plated layer 22 on the roughened surface side. Thereafter, copper plating was carried out until the copper layer thickness reached 18 μm to prepare a copper-clad laminate. A circuit (circuit height: 18 μm, circuit width: 320 μm, circuit length: 300 mm) was formed on this copper-clad laminate by a subtractive method using a cupric chloride etching solution. Thus, a transmission loss measurement board was obtained, on which a microstrip line was formed so that the characteristic impedance was 50 Ω±2 Ω. The obtained transmission loss measurement board was measured using a network analyzer (Keysight Technologies, Inc., N5225B) under the following conditions, and the transmission loss (dB) at 50 GHz was measured. (Setting conditions) - IF Bandwidth: 100 Hz - Frequency: 10 MHz to 50 GHz - Data points: 501 points - Average: Off - Calibration method: SOLT (e-cal)
[0052] The obtained transmission loss (absolute value) at 50 GHz was ranked and evaluated according to the following criteria. The results are shown in Table 2. <High frequency characteristic evaluation criteria> - Rating A (best): Transmission loss (absolute value) is less than 13.5 dB - Rating B (good): Transmission loss (absolute value) is 13.5 dB or more and less than 15.0 dB - Rating C (poor): Transmission loss (absolute value) is 15.0 or more
[0053]
Claims
1. A method for manufacturing a printed wiring board, comprising the steps of: (a) preparing an insulating substrate having a roughened surface; and (b) electroless plating the roughened surface of the insulating substrate to obtain a peak density Sds of 0.90 μm as measured in accordance with EUR15178N. -2 1.30 μm or more -2 and the peak curvature Ssc measured in accordance with EUR15178N is 1.00 μm or less. -1 4.00 μm or more -1 (c) laminating a photoresist on the surface of the electroless plating layer; (d) exposing and developing the photoresist to form a resist pattern; (e) electroplating the electroless plating layer via the resist pattern; (f) peeling off the resist pattern; and (g) removing by etching unnecessary portions of the electroless plating layer exposed by the peeling off of the resist pattern to form a wiring pattern.
2. The method for producing a printed wiring board according to claim 1, wherein the developed area ratio Sdr of the interface on the surface of the electroless plating layer, measured in accordance with EUR15178N, is 5.00% or more and 10.00% or less.
3. The peak curvature Ssc on the surface of the electroless plating layer is 2.30 μm. -1 3.50 μm or more -1 The method for producing a printed wiring board according to claim 1 or 2, wherein:
4. The step (a) is: (a-1) the peak density Sds measured in accordance with EUR15178N is 1.00 μm -2 1.50 μm or more -2 The peak curvature Ssc measured in accordance with EUR15178N is 4.00 μm or less. -1 6.00 μm or more -1 3. The method for producing a printed wiring board according to claim 1, comprising: (a-2) laminating an insulating base material on the treated surface of the surface-treated copper foil to transfer a surface shape of the treated surface to a surface of the insulating base material; and (a-3) removing the surface-treated copper foil by etching to obtain an insulating base material having the roughened surface.
5. The method for producing a printed wiring board according to claim 1 or 2, wherein the thickness of the electroless plating layer is 0.3 μm or more and 1.0 μm or less.
6. The method for producing a printed wiring board according to claim 1 or 2, wherein the photoresist comprises a dry film resist.
7. The method for producing a printed wiring board according to claim 6, wherein the thickness of the dry film resist is from 2 μm to 35 μm.
8. The method for manufacturing a printed wiring board according to claim 1 or 2, wherein the thickness of the wiring pattern is 2 μm or more and 30 μm or less.