Process for dividing single-crystal substrates
Patent Information
- Application Number
- MYPI2025005757
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-03-14
- Publication Date
- 2024-09-23
AI Technical Summary
Conventional methods for dividing single crystal substrates often result in chipping and scattering of pieces due to the adhesive dicing tape and protective films, leading to contamination and dielectric breakdown issues during semiconductor device manufacturing.
A method involving a break plate shifted by a predetermined amount from the cleavage plane, calculated using the thickness and off-angle of the substrate, to reduce chipping by aligning the break line away from the intersection line between the scribe and break planes, allowing controlled cleavage along the cleavage plane.
This approach effectively reduces chipping during the breaking process, improving the yield and quality of semiconductor chips by minimizing the scattering of broken pieces and preventing contamination, thus facilitating smoother post-process handling.
Smart Images

Figure PI2025005757_DRAWING_001 
Figure PI2025005757_DRAWING_002 
Figure PI2025005757_DRAWING_003
Abstract
Description
Method for dividing a single crystal substrate
[0001] The present invention relates to a method for dividing a single crystal substrate.
[0002] 1, in manufacturing a semiconductor device by dividing a cleavable single crystal substrate 1 made of SiC, Si, or the like, an adhesive dicing tape 9 (wafer-fixing tape) is attached to the scribe surface 3 of the single crystal substrate 1, and the opposite break surface 2 is protected by a non-adhesive (including slightly adhesive) protective film 10. In other words, the single crystal substrate 1 on the side of the protective film 10, which is the surface, is in an unconstrained state.
[0003] The single crystal substrate 1 is placed on the break table 11 with the scribe surface 3 to which the dicing tape 9 is attached facing downward. A camera 12 disposed below the break table 11 detects the scribe line L formed on the single crystal substrate 1.
[0004] A break plate 13 having a blade 14 at its tip is lowered from a break surface 2 on the front surface side, which is directly opposite the scribe line L, so as to contact the single crystal substrate 1, and is then pushed further downward to apply an external force and break the single crystal substrate 1. For example, Patent Documents 1 and 2 disclose techniques for dividing a substrate.
[0005] In Patent Document 1, a wafer having a crystal orientation oblique to the surface is uniformly divided by pushing the wafer up with a blade along a dicing line on the surface to create a crack. That is, Patent Document 1 aims to, in a wafer cracking method and apparatus, when cutting and separating a wafer having a crystal orientation oblique to the surface at an angle, to reliably separate the wafer into individual chips without causing cracks in the chips or misaligned cracks that would cause both chips to become defective, and to perform the separation operation.
[0006] In Patent Document 2, when dividing a bonded substrate at the boundary between a cell region and an intermediate scrap region where a sealing material exists, if an intermediate scrap exists that shifts the contact position of the break bar from the scribe line toward the cell region, the break bar is brought into contact with the cell region side to suppress shape defects. In other words, Patent Document 2 aims to suitably divide a bonded substrate that has a predetermined encapsulating material enclosed therein at the portion where the sealing material exists.
[0007] Japanese Patent Publication No. 05-055373 and Japanese Patent Publication No. 2020-070202
[0008] First, the mechanism by which the single crystal substrate 1 is broken will be described.
[0009] As shown in FIG. 2 , when manufacturing a semiconductor device, depending on the purpose of the product and the operation of the process, a single crystal substrate 1 may be used in which an adhesive dicing tape 9 is attached to the scribe surface 3 (back surface) on which the scribe line L is formed, and the break surface 2 (front surface) opposite the scribe surface 3 is protected by a non-adhesive protective film 10.
[0010] The single crystal substrate 1 is placed on a break table 11 of a breaking device with the scribe surface 3 to which the dicing tape 9 is attached facing downward, and a break plate 13 having a blade 14 at its tip is pressed against the protective film 10 side, which is the obverse surface, to break the single crystal substrate 1. In such a case, the following problems arise.
[0011] The entire single crystal substrate 1 sinks on the break table 11. Furthermore, since the back side of the single crystal substrate 1 is fixed with adhesive dicing tape 9, it becomes difficult to open the substrate in the horizontal direction.
[0012] In this situation, the single crystal substrate 1 is difficult to deform into a "V" shape, so the load on the portion being pressed by the break plate 13 increases, causing chipping on the surface, the break surface 2, where the single crystal substrate 1 breaks into small pieces.
[0013] For reference, a method for breaking the single crystal substrate 1 as shown in FIG. 3 is also used, and this method will be described below.
[0014] As shown in FIG. 3, a non-adhesive protective film 10 is attached to the scribe surface 3 (rear surface) of the single crystal substrate 1 on which the scribe line L is formed, and an adhesive dicing tape 9 is attached to the opposite break surface 2 (front surface).
[0015] In manufacturing the single crystal semiconductor device 15, the single crystal substrate 1 is placed on the break table 11 of the breaking device with the non-adhesive protective film 10 side facing back, and the break plate 13 with a blade 14 at its tip is pressed against the adhesive dicing tape 9 side, which forms the front surface, to break the single crystal substrate 1. In this case, the following situation occurs.
[0016] On the break table 11, the single crystal substrate 1 is deformed and sinks as a whole when a break plate 13 is pressed against it. The back side of the single crystal substrate 1 is protected by a protective film 10. This protective film 10 is not adhesive, and the single crystal substrate 1 is not fixed, so it can be easily opened in the horizontal direction.
[0017] As a result, the single crystal substrate 1 is easily deformed into a "V" shape, so the load on the portion being pressed by the break plate 13 is small, and chipping on the break surface 2 side, which is the surface, is less likely to occur.
[0018] 2, chipping occurs, in which the single crystal substrate 1 breaks into small pieces, at the break surface 2 that serves as the mounting surface for the SiC semiconductor device 15. The chipping causes the peeled substrate to fly apart, causing problems in subsequent processes.
[0019] For example, the semiconductor device 15 is contaminated by the broken pieces, making it impossible to transport the semiconductor device 15 to a device for a subsequent process.Furthermore, the broken pieces make the semiconductor device 15 more susceptible to dielectric breakdown.
[0020] In particular, chipping, in which the single crystal substrate 1 breaks into small pieces, is likely to occur when adhesive dicing tape 9 is attached to the scribe surface on the back side that contacts the break table 11. Furthermore, when the single crystal substrate 1 is cut along a scribe line L2 that is perpendicular to the orientation flat 8, chipping, in which the single crystal substrate 1 breaks into small pieces, is likely to occur at the break surface 2 on the front side.
[0021] That is, when the single crystal substrate 1 is placed on the break table 11 and broken, the dicing tape 9 attached to the scribe surface 3 has adhesiveness and does not stretch in the horizontal direction, making it difficult for the single crystal substrate 1 to deform, resulting in chipping, in which the single crystal substrate 1 breaks into small pieces, on the surface that becomes the break surface 2. The present invention is directed to such a single crystal substrate 1.
[0022] In Patent Document 1, the blade is abutted at a position opposite the scribe line, which may cause chipping. Patent Document 2, on the other hand, deals with glass substrates, COS substrates, and intermediate scraps, which differs from the present invention. Furthermore, in Patent Document 2, the break bar shift amount is large at 100 μm, which may cause chipping.
[0023] In view of the above problems, the present invention aims to provide a method for dividing a single crystal substrate, which can reduce chipping, in which the single crystal substrate breaks into small pieces at the break surface on the front side, by positioning a break plate that is offset a predetermined amount from the cleavage plane that is the intended separation line when breaking the single crystal substrate.
[0024] In order to achieve the above object, the present invention provides the following technical means.
[0025] The present invention relates to a method for dividing a single crystal substrate having a cleavage plane inclined at an off-angle relative to a scribe plane and a break plane, the method comprising the steps of: forming a scribe line on the scribe plane; attaching an adhesive dicing tape to the scribe plane; inverting the single crystal substrate and placing it on a break table so that the scribe plane is in contact with the scribe plane; abutting a break plate along a break line located in a direction away from an intersection line extending from the scribe line and where the cleavage plane and the break plane intersect, based on a reference line where a vertical plane extending along the scribe line intersects with the break plane; and applying an external force from the break plate to the break plane to divide the single crystal substrate along the cleavage plane.
[0026] The distance (a) between the reference line and the intersection line on the break plane is expressed by the following equation using the thickness (t) of the single crystal substrate and the off-angle (θ): a=t×tan θ (1)
[0027] The break line is positioned in a direction away from the intersection line by a predetermined shift distance from the reference line.
[0028] The predetermined shift distance is determined by the thickness of the single crystal substrate and the off-angle.
[0029] When the thickness of the single crystal substrate is 0.1 mm to 0.5 mm and the off-angle is 4°, the predetermined shift distance may be 1 μm to 50 μm.
[0030] When the thickness of the single crystal substrate is 0.1 mm and the off-angle is 4°, the predetermined shift distance may be 10 μm to 30 μm.
[0031] When the thickness of the single crystal substrate is 0.35 mm and the off-angle is 4°, the predetermined shift distance may be 24.5 μm to 50 μm.
[0032] When the thickness of the single crystal substrate is 0.5 mm and the off-angle is 4°, the predetermined shift distance may be 35 μm to 50 μm.
[0033] The single crystal substrate may have a direction specifying member that specifies the crystal direction of the cleavage plane of the single crystal substrate by its shape.
[0034] The direction specifying member has an orientation flat, the step of forming the scribe line includes forming a first scribe line extending in a direction perpendicular to the orientation flat and a second scribe line extending in a direction parallel to the orientation flat, and the step of abutting the break plate includes a step of abutting the break plate along the break line located in a direction away from the intersection line where the cleavage plane extending from the first scribe line intersects with the scribe surface, based on the reference line where the vertical plane extending along the first scribe line intersects with the break surface.
[0035] The step of forming the scribe line may include forming a crack extending from the scribe line toward the break surface, and the step of dividing the single crystal substrate may include dividing the single crystal substrate along the cleavage surface extending from the crack.
[0036] According to the method for dividing a single crystal substrate of the present invention, when breaking the single crystal substrate, the break plate is positioned at a predetermined distance from the cleavage plane that is the intended separation line, thereby reducing chipping that occurs at the break plane on the front side, in which the single crystal substrate breaks into small pieces.
[0037] 1 is a cross-sectional view showing an example of a conventional technique for breaking a single crystal substrate. 2 is a cross-sectional view showing a state in which chipping occurs on the break surface when breaking a single crystal substrate having an adhesive dicing tape attached to the scribe surface (rear surface) and an adhesive dicing tape attached to the break surface (front surface). 3 is a cross-sectional view showing a state in which a single crystal substrate having an adhesive dicing tape attached to the scribe surface (rear surface) protected by a protective film and an adhesive dicing tape attached to the break surface (front surface). 4 is a cross-sectional view showing a schematic outline of a method for dividing a single crystal substrate according to the present invention. 5 is an enlarged view of the (Z) portion of the cleavage plane of the single crystal substrate shown in FIG. 4, showing a method for deriving the shift amount of the break plate. 6 is a graph showing the relationship between the thickness (t) of the single crystal substrate and the shift amount (a) of the break plate when the off-angle (θ) is 4°. 7 is a perspective view showing a schematic outline of an example of a single crystal substrate from which a semiconductor device can be obtained.
[0038] Hereinafter, an embodiment of the method for dividing a single crystal substrate according to the present invention will be described with reference to the drawings. Note that the embodiment described below is an example of the present invention, and the configuration of the present invention is not limited to this specific example.
[0039] First, the semiconductor wafer 1 that is the base material of the semiconductor device 15, the breaking device, etc. will be described.
[0040] The semiconductor device 15 obtained by the present invention is suitable for semiconductor power devices, semiconductor high frequency devices, HEMTs (High Electron Mobility Transistors), other compound semiconductors, etc. In the following description, the semiconductor device 15 may also be simply referred to as a chip 15.
[0041] 7 is a perspective view schematically illustrating an example of a semiconductor wafer 1, which is a brittle material substrate. The semiconductor wafer 1, which serves as the base material for the chip 15, will be described using a single crystal substrate 1 (single crystal semiconductor wafer 1) as an example. In the single crystal substrate 1 of this embodiment, a 4H—SiC single crystal will be described as an example of a SiC single crystal having an off-angle and made of a hexagonal crystal.
[0042] 7, the single crystal substrate 1 is disk-shaped and serves as a base material for the chip 15. The single crystal substrate 1 has a thickness of approximately 0.5 mm or less.
[0043] The single crystal substrate 1 has a first wafer main surface 2 on one side, a second wafer main surface 3 on the other side, and a wafer side surface 4 connecting the first wafer main surface 2 and the second wafer main surface 3 .
[0044] The first wafer main surface 2 faces the {0001} plane (silicon face (Si face)) of the SiC single crystal. A plurality of element formation regions 5 (mounting surfaces) corresponding to chips 15 are formed on the first wafer main surface 2.
[0045] In the following description of the present invention, the first wafer main surface 2 is referred to as the break surface 2 because it is located on the break plate 13 side when the single crystal substrate 1 is broken. In addition, the first wafer main surface 2 is also referred to as the pattern surface 2 because the element formation region 5 is formed on it.
[0046] The second wafer main surface 3 faces the {0001] plane (carbon plane (C-plane)) of the SiC single crystal. When the second wafer is cut into chips 15, the second wafer main surface 3 becomes the surface (non-mounting surface) that is fixed to a support of the chip 15.
[0047] In the following description of the present invention, the second wafer main surface 3 is also referred to as the scribe surface because a scribe line L is formed thereon. A back electrode film 6 is provided on the scribe surface 3 side (see FIG. 1). This scribe surface 3 is also referred to as the metal surface. In other words, the single crystal substrate 1 has a break surface 2 and a scribe surface 3 that face each other.
[0048] A notch 8 is formed on the wafer side surface 4. This notch 8 is called an orientation flat (OF) 8 and is a mark that indicates the crystal orientation of the SiC single crystal. For example, one or two orientation flats 8 are provided. By dividing the single crystal substrate 1, a plurality of chips 15 (SiC semiconductor devices 15) are cut out.
[0049] The scribe line L 1 is formed in the X-axis direction of the single crystal substrate 1 and is parallel to the orientation flat 8 .
[0050] The scribe line L2 is formed in the Y-axis direction of the single crystal substrate 1, and is perpendicular to the orientation flat 8. When the single crystal substrate 1 is divided and cleaved by the crack propagating from the scribe line L2, the side surface of the chip 15 becomes the crystal surface (cleavage plane 7) of the SiC single crystal.
[0051] The single crystal substrate 1 has a scribe surface 3 (C-surface 3) on which scribe lines L1 and L2 are formed in a grid pattern attached to the center of a dicing tape 9 (adhesive film) stretched over an annular ring member (dicing ring), and the opposite break surface 2 (Si-surface 2) is protected by a protective film 10.
[0052] The single crystal substrate 1 thus set to be broken is placed on the breaking table 11 of the breaking device with the scribe surface 3 to which the dicing tape 9 is attached facing back.
[0053] Here, an example of the configuration of a breaking device for dividing the single crystal substrate 1 on which the scribe line L is formed will be briefly described.
[0054] The breaking device separates the single crystal substrate 1 into chips 15 (unit substrates) by pressing a breaking plate 13 from above against the break surface 2 along the scribe line L of the single crystal substrate 1 on which a scribe line L has been formed by the scribing device.
[0055] The breaking device includes a break table 11 on which the single crystal substrate 1 to be broken is placed, a break plate 13 that divides the mounted single crystal substrate 1 along a scribe line L, and a beam oscillator (a beam having an intensity distribution of a flat-top file) that is attached in a suspended manner to the break plate 13 and covers the upper part of the break table 11. Note that the break table 11 is rotatable, for example, around an axis in the Z-axis direction.
[0056] The break plate 13 (break bar 13) is a member that is long in the X-axis direction. The tip (lower end) of the break plate 13 is provided with a linear ridge (blade 14) that divides the single crystal substrate 1 along the scribe lines L1 and L2.
[0057] As the break table 11 rotates, the break plate 13 breaks the single crystal substrate 1 along the scribe line L1 in the X-axis direction and the scribe line L2 in the Y-axis direction, and separates each chip 15.
[0058] The break plate 13 can be raised and lowered in the Z-axis direction relative to the beam by an elevation mechanism. A pair of receiving blades may be provided below and facing the break plate 13 to receive the pressure from the single crystal substrate 1 against which the break plate 13 is pressed during breaking.
[0059] This breaking device is not limited to the device configuration exemplified above. For example, the break plate 13 may be rotatable about an axis in the Z-axis direction. Alternatively, for example, the breaking device may have a first break plate that divides the single crystal substrate 1 along a scribe line L1 in the X-axis direction and a second break plate that divides the single crystal substrate 1 along a scribe line L2 in the Y-axis direction.
[0060] The single crystal substrate 1 is divided into chips 15 using a breaking device equipped with a break table 11, for example, as follows.
[0061] 1, a single crystal substrate 1 has an adhesive dicing tape 9 (wafer-fixing tape) attached to a scribe surface 3 (C-face 3), and the opposite break surface 2 (Si-face 2) is protected by a non-adhesive (including slightly adhesive) protective film 10. In other words, the single crystal substrate 1 on the side of the protective film 10, which is the front surface, is in an unconstrained state.
[0062] The single crystal substrate 1 is placed on the break table 11 with the scribe surface 3 to which the dicing tape 9 is attached facing downward. A camera 12 disposed below the break table 11 detects the scribe line L formed on the single crystal substrate 1.
[0063] A break plate 13 with a blade 14 at its tip is lowered from a break surface 2 on the front surface side, which is directly opposite to the scribe line L, to contact the single crystal substrate 1, and is further pressed downward to apply an external force and break the single crystal substrate 1.
[0064] Specifically, the break plate 13 is lowered and the cutting edge 14 (blade 14) attached to the tip of the break plate 13 is pressed against the break surface 2 (pattern surface 2) along the scribe line L1 in the X-axis direction (parallel to the orientation flat 8), thereby breaking the single crystal substrate 1. Thereafter, the break plate 13 is raised.
[0065] Thereafter, the break table 11 is rotated 90° around the Z axis, and the break plate 13 is lowered, and the blade 14 at the tip of the break plate 13 is pressed against the break surface 2 on the surface along the scribe line L2 in the Y axis direction (perpendicular to the orientation flat 8), thereby breaking the single crystal substrate 1.
[0066] In this way, the break table 11 is rotated 90° around the Z axis, and the blade 14 of the break plate 13 is pressed against all of the lattice-shaped scribe lines L1 and L2 to break the single crystal substrate 1 and separate each chip 15 as shown in Figure 7.
[0067] After breaking, the single crystal substrate 1 is removed from the break table 11 and sent to a subsequent process. The chips 15 obtained from the single crystal substrate 1 include, for example, a SiC semiconductor layer and are approximately 5 mm x 5 mm in size.
[0068] FIG. 4 is a cross-sectional view that schematically illustrates an outline of a method for dividing a single crystal substrate 1 according to the present invention.
[0069] As shown in FIG. 4, the present invention is a technology that can be applied to the manufacture of semiconductor devices 15 (chips 15) by forming scribe lines L on a single crystal substrate 1 and then dividing the substrate along the scribe lines L by applying an external force with a break plate 13.
[0070] The single crystal substrate 1 that is the subject of the present invention has an adhesive dicing tape 9 (adhesive film) attached to at least the scribe surface 3 (C surface 3, i.e., scribe surface 3, which becomes the back surface when placed on the break table 11) on which the scribe line L is formed. In other words, the single crystal substrate 1 is held by the adhesive dicing tape 9.
[0071] On the other hand, the break surface 2, which is the surface opposite to the scribe surface 3, is protected by a protective film 10 (which may or may not be adhesive). The thickness (t) of the single crystal substrate 1 that is the subject of the present invention is 0.5 mm or less.
[0072] The single crystal substrate 1 is placed so that the scribe surface 3 side to which the dicing tape 9 is attached is in contact with the break table 11. An external force is applied by the break plate 13 along the scribe line L, and the substrate is divided from the break surface 2 side (the Si surface 2 that becomes the surface when placed on the break table 11, i.e., the break surface 2).
[0073] In particular, when dividing the single crystal substrate 1 along a scribe line L2 perpendicular to an orientation flat (OF) 8 provided on the single crystal substrate 1, the contact position of the break plate 13 with the single crystal substrate 1 is shifted in a direction away from the inclination direction of the cleavage plane 7 (planned separation line) formed by the crack propagation from the scribe line L2 perpendicular to the orientation flat (OF) 8.
[0074] That is, as shown in FIG. 4, the contact position 13 of the break plate with respect to the break surface 2 of the single crystal substrate 1 is shifted from the scribe line L2 perpendicular to the orientation flat 8 toward the line of separation to be cleaved by the crack propagation (the direction in which the cleavage surface 7 is inclined).
[0075] Here, we will describe a phenomenon that has conventionally occurred when dividing the single crystal substrate 1 that is the subject of the present invention. That is, when dividing the single crystal substrate 1 having the scribe surface 3, to which dicing tape 9 is attached, as the back surface and the break surface 2, to which protective film 10 is attached, as the front surface, the following situation may occur.
[0076] Specifically, at the current breaking position when dividing the single crystal substrate 1 along the scribe line L2 perpendicular to the orientation flat 8, the relationship between the dividing plane {11-20} (cleavage plane 7) formed by the crack propagation from the scribe line L2 perpendicular to the orientation flat L2 and the {0001} plane, which is another cleavage plane, makes it easy for chipping to occur, in which the single crystal substrate 1 breaks into small pieces at the break plane 2 (pattern plane 2) on the front surface side. This chipping causes the peeled substrate to fly apart, causing problems in subsequent processes.
[0077] Therefore, when dividing the single crystal substrate 1 along the scribe line L2 perpendicular to the orientation flat 8, the contact position of the break plate 13 is shifted in a direction away from the intended separation line (cleavage plane 7) (see the arrow indicating the shift direction in FIG. 4). Here, the intended separation line is intended to be a "plane" that is parallel to the cleavage plane 7 along which a crack propagates from the scribe line L2 toward the break plane in the Y-Z plane shown in FIG. 4 and that extends in the X direction, but is referred to as a "line" for convenience.
[0078] That is, when dividing the single crystal substrate 1, it is advisable to shift the break plate 13 in a direction away from the cleavage plane 7 that cleaves at the crack that occurs on the break plane 2 directly below the scribe line L2 that is perpendicular to the orientation flat 8 (to the right side of the drawing, in the direction in which the cleavage plane 7 is inclined).
[0079] More specifically, in the above process of forming the scribe line L on the single crystal substrate 1, the scribe lines L1 and L2 are formed on the single crystal substrate 1 so that the single crystal substrate 1 has a first scribe line L1 extending in a direction parallel to the orientation flat 8 (the X-axis direction shown in FIG. 7 ) and a second scribe line L2 extending in a direction perpendicular to the orientation flat 8 (the Y-axis direction shown in FIG. 7 ).
[0080] 5, the single crystal substrate 1 has a reference line R formed at the intersection of a vertical plane P extending from the second scribe line L2 in a direction perpendicular to the break planes 2 and 3 and the break planes 2. The vertical plane P and the reference line R are imaginary and extend in the depth direction of FIG. 5 (the X-axis direction in FIG. 7). That is, the cleavage plane 7 of the single crystal substrate 1 is inclined at an off angle θ with respect to the vertical plane P in the Y-Z cross section of FIG. 7.
[0081] 5, an intersection line C where the cleavage plane 7 of the single crystal substrate 1 and the break plane 2 intersect in the Y-Z cross section, and a distance (a) between the reference line R and the intersection line C are virtually defined. In the above-described step of displacing the break plate 13, it is considered ideal to abut the break plate 13 along a position (i.e., a straight line extending in the X-axis direction) that is spaced apart by the distance (a) calculated by the formula (1) described below. However, the inventors of the present application have confirmed that chipping can be suppressed by disposing the break plate 13 at a break line B (FIG. 4) that is located in a direction away from (displaced from) the intersection line C using the reference line R as a reference and applying an external force to break the break plate 13.
[0082] That is, as shown in FIG. 4, the inventors of the present application have confirmed that, rather than considering the position at which the chip 15 is divided due to the off-angle, shifting the break plate 13 in the direction of crack extension from the scribe line L2 perpendicular to the orientation flat 8 tends to reduce the occurrence of chipping, in which the single crystal substrate 1 is broken into small pieces at the break surface 2 on the front side (the side that becomes the pattern surface 2).
[0083] The contact position of the break plate 13 with the single crystal substrate 1 is offset from the scribe line L2 perpendicular to the orientation flat 8 in the extension direction of the cleavage plane 7 of the single crystal substrate 1 (away from the tilted direction of the cleavage plane 7).
[0084] Below, examples of the range of values for the amount (a) by which the break plate 13 is shifted in the horizontal direction from the orthogonal scribe line L2 are shown.
[0085] For example, when the thickness (t) of the single crystal substrate 1 is 0.1 mm and the off-angle (θ) is 4°, the shift amount (a) of the break plate 13 is preferably in the range of 1 to 50 μm, and more preferably in the range of 10 to 30 μm.
[0086] Furthermore, when the thickness (t) of the single crystal substrate 1 is 0.35 mm and the off-angle (θ) is 4°, the shift amount (a) of the break plate 13 is preferably in the range of 1 to 50 μm, and more preferably in the range of 25 to 50 μm.
[0087] Here, the range of the shift amount (a) for shifting the break plate 13 (blade 14) on the break surface 2 in a direction away from the scribe line L2 in the perpendicular direction will be considered.
[0088] FIG. 5 is an enlarged view of the (Z) portion of the cleavage plane 7 of the single crystal substrate 1 shown in FIG. 4, and shows a method for determining the shift amount (a) of the break plate 13.
[0089] As shown in FIG. 5 , the shift amount (a) of the break plate 13 at the intended dividing position (cleavage plane 7) on the break surface 2 (Si surface 2) from the position of the scribe line L2 perpendicular to the orientation flat 8 can be calculated using the following formula (1) based on the thickness (t) and off-angle (θ) of the single crystal substrate 1.
[0090] a = t × tan θ (1) Figure 6 is a graph showing the relationship between the thickness (t) of the single crystal substrate 1 and the shift amount (a) of the break plate 13 when the off angle (θ) is 4°. The black circles in Figure 6 represent the theoretical values of the shift amount (a) calculated from equation (1). However, the present invention is directed to single crystal substrates 1 having a thickness (t) of 0.5 mm or less. Here, the shift amount according to the present invention refers to the "shift distance" between the reference line R and the break line B in the Y-Z cross section of Figure 4. According to the present invention, as explained above, chipping can be suppressed by positioning the break plate 13 at a value (a + α) greater than the theoretical value (a) calculated from equation (1).
[0091] 6, for example, when the thickness (t) of the single crystal substrate 1 is 0.05 mm, the shift amount (a) calculated from equation (1) is approximately 3.496 μm. In other words, when the thickness (t) of the single crystal substrate 1 is 0.05 mm, the shift distance between the reference line R and the break line B may be set in the range of 3.5 μm to 50 μm.
[0092] When the thickness (t) of the single crystal substrate 1 is 0.1 mm, the shift amount (a) calculated from formula (1) is approximately 6.992 μm. In other words, when the thickness (t) of the single crystal substrate 1 is 0.1 mm, the shift distance between the reference line R and the break line B may be set in the range of 7 μm to 50 μm.
[0093] When the thickness (t) of the single crystal substrate 1 is 0.35 mm, the shift amount (a) calculated from formula (1) is approximately 24.474 μm. In other words, when the thickness (t) of the single crystal substrate 1 is 0.35 mm, the shift distance between the reference line R and the break line B may be set in the range of 24.5 μm to 50 μm.
[0094] When the thickness (t) of the single crystal substrate 1 is 0.5 mm, the shift amount (a) calculated from formula (1) is approximately 34.963 μm. In other words, when the thickness (t) of the single crystal substrate 1 is 0.5 mm, the shift distance between the reference line R and the break line B may be set in the range of 35 μm to 50 μm.
[0095] As explained above, the inventors of the present application have confirmed that it is preferable to shift the break plate 13 in the inclination direction of the cleavage plane 7 (the direction away from the reference line R) by a shift amount (a) greater than the theoretical value, as shown in FIG. 6 (see the arrow and the trapezoidal area in FIG. 6 ).
[0096] That is, on the break surface 2 side of the single crystal substrate 1, it is preferable to shift the break plate 13 horizontally in a direction away from the scribe line L2 perpendicular to the orientation flat 8 by at least the shift amount (a) calculated by equation (1).
[0097] In other words, it is advisable to shift the break plate 13 to the position of value (a) calculated by equation (1) or in the direction from the position (a) toward the side where the angle between the break plane 2 and the cleavage plane 7 becomes obtuse.
[0098] The break plate 13 is preferably shifted by a shift amount (a) or more in the direction of inclination of the cleavage plane 7 and away from the perpendicular scribe line L2 (reference line R) from the intersection line C (planned division position) where the cleavage plane 7 and the break plane 2 intersect, which is divided by cleavage from the scribe line L2 perpendicular to the orientation flat 8.
[0099] From the above, the shift amount (a) by which the break plate 13 is shifted in the horizontal direction is determined by the thickness (t) and off-angle (θ) of the single crystal substrate 1, for example, as shown in equation (1).
[0100] However, the inventors have confirmed that a shift amount (a) of the break plate 13 exceeding 50 μm is unsuitable because problems arise. That is, shifting the break plate 13 significantly to the right in FIG. 4 is unsuitable because chipping may occur. The inventors have also confirmed that shifting the break plate 13 to the left in FIG. 4 (toward the scribe line L2 relative to the intersection line C where the cleavage plane 7 and the break plane 2 intersect) is unsuitable because chipping increases.
[0101] That is, the contact position of the break plate on the break surface 2 side with respect to the single crystal substrate 1 should be shifted by at least the shift amount (a) calculated from equation (1) toward the inclination direction of the cleavage surface 7 (the planned separation line) formed by the crack propagation from the scribe line L2 in the direction perpendicular to the orientation flat 8, away from the scribe line L2 in the perpendicular direction.
[0102] However, since the off-angle does not affect cutting along the scribe line L1 parallel to the orientation flat (OF) 8, the single crystal substrate 1 is cut perpendicularly without any problems. Therefore, there is no need to shift the contact position of the break plate 13.
[0103] In the process of forming the scribe lines L1 and L2, a crack may be formed along the cleavage plane 7, and the single crystal substrate 1 may be cleaved and divided as the crack propagates along the cleavage plane 7.
[0104] Furthermore, the single crystal substrate 1 has been described as having an orientation flat (OF) 8 as a direction specifying member that specifies the crystal orientation of the cleavage plane 7 by its shape, but the direction specifying member is not limited to this and may be a notch or any other member that specifies the crystal orientation of the cleavage plane 7 by its shape.
[0105] It is also preferable that an adhesive dicing tape 9 be attached to the scribe surface 3 (metal surface 3) which is the back surface.
[0106] On the other hand, when a non-adhesive protective film 10 is attached to the scribe surface 3, chipping on the break surface 2 is reduced to begin with (see FIG. 3).
[0107] The protective film 10 to be attached to the break surface 2 (pattern surface 2) that serves as the front surface may have any adhesive property.
[0108] As described above, according to the method for dividing a single crystal substrate 1 of the present invention, when breaking the single crystal substrate 1 along the scribe line L, particularly when dividing the single crystal substrate 1 along the scribe line L2 that is perpendicular to the orientation flat 8 provided on the single crystal substrate 1, by positioning the break plate 13 at a predetermined shift amount (a) in the inclined direction from the cleavage plane 7 (the line to be separated) formed by the scribe line L2 in the perpendicular direction, it is possible to reduce chipping, in which the single crystal substrate 1 breaks into small pieces at the break plane 2 that becomes the pattern surface 2 of the chip 15.
[0109] By following this method of reducing chipping by offset breaking of the break plate 13, it is possible to improve the yield of the chips 15 obtained from the single crystal substrate 1. In other words, it is possible to efficiently manufacture the chips 15 that will become products.
[0110] It should be noted that the embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. In particular, matters not explicitly stated in the embodiments disclosed herein, such as operating conditions, operation conditions, dimensions and weights of components, etc., do not deviate from the scope of ordinary practice by a person skilled in the art, and are matters that can be easily assumed by a person skilled in the art.
[0111] In this embodiment, an example has been described in which a 4H (Hexagonal)-SiC single crystal having an off-angle of 4° is used as an example of a SiC single crystal made of a hexagonal crystal in the single crystal substrate 1. The present invention can be applied to a Si substrate or a SiC single crystal made of a hexagonal crystal, which is a single crystal substrate and has an off-angle. A 2H-SiC single crystal or a 6H-SiC single crystal can also be applied.
[0112] REFERENCE SIGNS LIST 1 Single crystal substrate (wafer) 2 Break surface (first wafer main surface) 3 Scribe surface (second wafer main surface) 4 Wafer side wall surface 5 Device formation region 6 Back electrode film 7 Cleavage surface (planned separation line) 8 Orientation flat (OF) 9 Dicing tape 10 Protective film 11 Break table 12 Camera 13 Break plate 14 Blade 15 Semiconductor device (chip) L1 Scribe line (X-axis direction) L2 Scribe line (Y-axis direction) B Break line C Intersection line P Vertical surface R Reference line
Claims
1. A method for dividing a single crystal substrate having a cleavage plane inclined relative to a scribe plane and a break plane, comprising the steps of: forming a scribe line on the scribe plane; attaching an adhesive dicing tape to the scribe plane; inverting the single crystal substrate and placing it on a break table so that the scribe plane is in contact with the scribe plane; abutting a break plate along a break line located in a direction away from an intersection line extending from the scribe line and where the cleavage plane and the break plane intersect, based on a reference line where the break plane intersects with a vertical plane extending from the scribe line in a direction perpendicular to the scribe plane and the break plane; and applying an external force from the break plate to the break plane to divide the single crystal substrate along the cleavage plane.
2. The method for dividing a single crystal substrate according to claim 1, wherein the cleavage plane is inclined at an off-angle with respect to the vertical plane, and the distance (a) between the reference line and the intersection line on the break plane is expressed by the following formula using the thickness (t) of the single crystal substrate and the off-angle (θ): a=t×tan θ (1) 3. The method for dividing a single crystal substrate according to claim 1, wherein the break line is positioned in a direction away from the intersection line by a predetermined shift distance with respect to the reference line.
4. The method for dividing a single crystal substrate according to claim 3, wherein the predetermined shift distance is determined by the thickness and off-angle of the single crystal substrate.
5. The method for dividing a single crystal substrate according to claim 3, wherein when the thickness of the single crystal substrate is 0.1 mm to 0.5 mm and the off angle is 4°, the predetermined shift distance is 1 μm to 50 μm.
6. The method for dividing a single crystal substrate according to claim 5, wherein when the thickness of the single crystal substrate is 0.1 mm and the off angle is 4°, the predetermined shift distance is 10 μm to 30 μm.
7. The method for dividing a single crystal substrate according to claim 5, wherein when the thickness of the single crystal substrate is 0.35 mm and the off angle is 4°, the predetermined shift distance is 24.5 μm to 50 μm.
8. The method for dividing a single crystal substrate according to claim 5, wherein when the thickness of the single crystal substrate is 0.5 mm and the off angle is 4°, the predetermined shift distance is 35 μm to 50 μm.
9. The method for dividing a single crystal substrate according to claim 1, wherein the single crystal substrate has a direction specifying member that specifies the crystal direction of the cleavage plane by its shape.
10. The method for dividing a single crystal substrate as claimed in claim 1, wherein the single crystal substrate has an orientation flat, the step of forming the scribe lines comprises the steps of forming a first scribe line extending in a direction parallel to the orientation flat and a second scribe line extending in a direction perpendicular to the orientation flat, and the step of abutting the break plate comprises the step of abutting the break plate along the break line located in a direction away from the intersection line where the cleavage plane extending from the second scribe line intersects with the scribe surface, based on the reference line where the vertical plane extending along the second scribe line intersects with the break surface.
11. A method for dividing a single crystal substrate as set forth in claim 1, wherein the step of forming a scribe line includes forming a crack from the scribe line toward the break surface, and the step of dividing the single crystal substrate includes dividing the single crystal substrate along the cleavage surface extending from the crack.