Cold-rolled high-strength steel plate with excellent phosphating performance, and manufacturing method therefor

MYPI2025005766A0Undetermined Publication Date: 2024-09-23BAOSHAN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005766
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2024-03-22
Publication Date
2024-09-23

AI Technical Summary

Technical Problem

In the existing technology, when producing cold-rolled high-strength steel, the external oxidation of alloy elements Si and Mn affects the nucleation and growth of the phosphating film, resulting in poor phosphating performance, and the method of controlling the annealing atmosphere is costly and has strong limitations.

Method used

By controlling the peak mass percentage of Mn and Si elements in the depth range of 0-1000nm on the steel plate surface, ensuring that Mn ≤ 10.0% and Si ≤ 4.0%, and located at a depth of at least 50nm, using glow discharge emission spectrum detection, combined with a unique continuous Annealing process forms a ferrite surface layer to prevent the diffusion of alloy elements and ensure excellent phosphating performance.

Benefits of technology

It achieves excellent phosphating properties of cold-rolled high-strength steel plates, improves coating quality, and reaches ≥780MPa in tensile strength, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005766_DRAWING_001
    Figure PI2025005766_DRAWING_001
  • Figure PI2025005766_DRAWING_002
    Figure PI2025005766_DRAWING_002
  • Figure PI2025005766_DRAWING_003
    Figure PI2025005766_DRAWING_003
Patent Text Reader

Abstract

Disclosed in the present invention is a cold-rolled high-strength steel plate with excellent phosphating performance. On the element mass percentage content-depth distribution curve with a depth in the range of 0-1000 nm from the surface of the steel plate, the Mn mass percentage peak Mnp is less than or equal to 10.0%, the Si mass percentage peak Sip is less than or equal to 4.0%, and the Mn mass percentage peak Mnp and the Si mass percentage peak Sip are both located at a depth position greater than or equal to 50 nm from the surface of the steel plate. Correspondingly, further disclosed in the present invention is a manufacturing method for the cold-rolled high-strength steel plate, and a unique continuous annealing process is used in the manufacturing method.
Need to check novelty before this filing date? Find Prior Art

Description

A cold-rolled high-strength steel plate with excellent phosphating performance and a manufacturing method thereof Technical Field

[0001] The present invention relates to a steel plate and a manufacturing method thereof, and in particular to a cold-rolled steel plate and a manufacturing method thereof. Background Art

[0002] High-strength steel is an increasingly popular material. Cold-rolled high-strength steel typically requires the addition of high levels of alloying elements such as C, Si, Mn, Cr, and Al, combined with continuous annealing processes and phase transformation strengthening to achieve a certain level of strength and formability.

[0003] Phosphating is a pretreatment process before automotive electrophoretic coating. By immersing steel plates or parts made of steel plates in phosphating solution, a layer of insoluble phosphating film is formed on the surface of the steel plates or parts, thereby improving the adhesion of the paint film.

[0004] However, when using continuous annealing to produce cold-rolled high-strength steel, alloying elements such as Si and Mn in the steel can form external oxidation on the surface of the annealed strip. This Si and Mn oxidation on the steel surface can affect the nucleation and growth of the phosphate film, thereby affecting the coating quality of automotive parts. Consequently, the phosphating performance of high-strength steel has gained increasing attention in recent years.

[0005] For example, the Chinese patent application with publication number CN107419185A, publication date December 1, 2017, and titled “A Cold-rolled Steel Sheet with Excellent Phosphating Performance and Production Method” mainly produces cold-rolled sheets with excellent phosphating performance by precisely controlling the composition, and simultaneously through hot rolling, pickling, five-stand full six-roller cold rolling, continuous annealing, and leveling processes.

[0006] For example, the Chinese patent application with publication number CN111910123A, publication date November 10, 2020, and titled "A cold-rolled and continuously annealed ultra-high strength steel with excellent phosphating performance and its preparation method" discloses an annealing process for obtaining excellent phosphating performance of cold-rolled and continuously annealed ultra-high strength steel. It limits the H2 content of the annealing atmosphere to 6% to 15%, the dew point to -45°C to -41°C, and the oxygen content to 2ppm to 5ppm. The purpose is to inhibit the selective oxidation of alloying elements through the above parameters, thereby obtaining excellent phosphating performance.

[0007] It can be seen that in the prior art, in order to obtain excellent phosphating performance, controlling the content of alloy elements is one method, but limiting the content of alloy elements will affect the performance of the material properties.

[0008] Controlling the annealing atmosphere is another method for improving the phosphating properties of high-alloy cold-rolled steel sheets. However, maintaining both the dew point and oxygen content at low levels is difficult and expensive, while maintaining a high dew point can cause surface decarburization, thus limiting this method.

[0009] Based on this, it is desired to provide a new cold-rolled high-strength steel sheet that achieves excellent phosphating performance.

[0010] Summary of the Invention

[0011] One of the objects of the present invention is to provide a cold-rolled high-strength steel plate with excellent phosphating performance, which achieves excellent phosphating performance by controlling the Mn and Si elements not to be enriched on the surface of the steel plate.

[0012] Based on the above invention purpose, the present invention provides a cold-rolled high-strength steel plate with excellent phosphating performance, wherein the peak value of the Mn element mass percentage Mn on the element mass percentage-depth distribution curve within the depth range of 0-1000nm from the steel plate surface is p ≤10.0%, Si mass percentage peak Si p ≤4.0%, and the peak value of Mn element mass percentage is Mn p And the Si element mass percentage peak Si p The peak values ​​of Mn element mass percentage are located at a depth of ≥50nm from the surface of the steel plate. p and Si element mass percentage peak Si p The results were obtained by glow discharge optical emission spectroscopy (GDOES).

[0013] In the present invention, the peak value of Mn mass percentage on the element mass percentage-depth distribution curve within the depth range of 0-1000nm from the surface of the steel plate detected by glow discharge optical emission spectroscopy (GDOES) is p ≤10.0%, Si mass percentage peak Si p A content of ≤4.0% is key to achieving excellent phosphating properties in cold-rolled high-strength steel. This is because, in cold-rolled high-strength steel produced through continuous annealing, alloying elements such as Mn and Si form external oxidation on the surface of the annealed steel sheet, resulting in significant surface enrichment of Si and Mn. The peak mass percentage of Mn or Si on the steel sheet can reach several to dozens of times that of the matrix Mn or Si. These oxides hinder the reaction between the phosphating solution and the steel sheet, thereby affecting the phosphating properties of the high-strength steel.

[0014] The inventors have found through research that when the depth range from 0 to 1000 nm from the surface of the steel plate is within the range of 0 to 1000 nm, the peak value of Mn mass percentage on the element mass percentage-depth distribution curve is p >10% or Si mass percentage peak Sip When Mn>4%, the phosphating performance of the steel plate is poor. p ≤10%,Si p ≤4%. In some embodiments, the present invention controls Mn p ≤8.5%,Si p ≤3.0%. In some embodiments, Mn p Between 5.0% and 10.0%, Si p Between 0.1 and 3.0%.

[0015] In order to achieve excellent phosphating performance, the present invention controls Mn p 、Si p Depth t pMn ≥50nm, t pSi ≥50nm. This is because the inventors found through research that when Mn p 、Si p When the depth is less than 50nm, even if Mn p ≤10% or Si p ≤4%, the external oxidation of Si and Mn in local positions cannot be avoided, and the local phosphating performance is poor.

[0016] Furthermore, in the cold-rolled high-strength steel sheet with excellent phosphating performance of the present invention, the peak value of the Mn element mass percentage is Mn p And the Si element mass percentage peak Si p They are all located at a depth of 50-500nm from the surface of the steel plate.

[0017] Although when t pMn >500nm,t pSi When the thickness is greater than 500nm, the phosphating performance of cold-rolled high-strength steel is also excellent, but in order to obtain t pMn >500nm,t pSi >500nm, a higher pre-oxidation temperature and a longer pre-oxidation time are required. Therefore, the preferred t pMn ≤500nm, t pSi ≤500nm. In some embodiments, the present invention controls t pMn Between 100nm and 450nm, control t pSi Between 100nm and 450nm.

[0018] Furthermore, in the cold-rolled high-strength steel sheet with excellent phosphating performance of the present invention, on the element mass percentage-depth distribution curve within the depth range of 0-1000nm from the steel sheet surface, the peak value of Fe element mass percentage is Fe p ≥85%, and the peak value of Fe element mass percentage is Fe pLocated 0-t from the steel plate surface pSi Depth range, where t pSi Indicates the peak value Si by mass percentage of Si element p In the present invention, Fe p It refers to the distance from the steel plate surface to 0-t pSi Fe element mass percentage peak within the depth range.

[0019] When the Fe p When the content is ≥85%, it can ensure that there is enough Fe on the surface of the cold-rolled high-strength steel to react with the phosphating solution during phosphating treatment, thereby obtaining excellent phosphating performance.

[0020] Further preferably, when Fe p When it is ≥90%, the phosphating performance will be better.

[0021] Furthermore, the cold-rolled high-strength steel plate with excellent phosphating performance described in the present invention includes a base layer, a surface layer and a transition layer located between the base layer and the surface layer in the thickness direction of the steel; the microstructure of the surface layer is ferrite.

[0022] Furthermore, in the cold-rolled high-strength steel plate with excellent phosphating performance described in the present invention, the thickness of the surface layer is 50-500 nm.

[0023] When the thickness of the surface layer, that is, the ferrite layer, is 50-500nm, it can be ensured that the peak value of Mn and Si mass percentage on the element mass percentage-depth distribution curve obtained by glow discharge optical emission spectroscopy (GDOES) is p 、Si p Depth t p 50-500nm.

[0024] In the high-strength steel with excellent phosphating performance described in the present invention, when the thickness of the surface layer is 50-500 nm, the Mn and Si elements diffused outward from the matrix during annealing are mainly enriched in the transition layer, and the ferrite surface layer can effectively prevent the diffusion of alloying elements such as Mn and Si to the ferrite surface, thereby ensuring that the Mn and Si mass percentage peak Mn on the element mass percentage-depth distribution curve obtained by glow discharge optical emission spectroscopy (GDOES) is p 、Si p Depth t p 50-500nm.

[0025] Furthermore, in the cold-rolled high-strength steel sheet with excellent phosphating performance described in the present invention, the microstructure of the base layer is martensite+ferrite, or martensite+ferrite+retained austenite.

[0026] Furthermore, in the cold-rolled high-strength steel with excellent phosphating performance described in the present invention, the transition layer contains oxides of Mn, Si, and Fe and / or composite oxides of Mn, Si, and Fe. The oxides of Mn, Si, and Fe refer to oxides of Mn, Si, or Fe. The composite oxides of Mn, Si, and Fe refer to oxides of two or three of the elements Mn, Si, and Fe.

[0027] Furthermore, the oxides of Mn, Si and Fe are at least one of the following: MnO, MnO2, SiO2, FeO, Fe2O3 and Fe3O4; the composite oxides of Mn, Si and Fe are at least one of the following: MnSiO3, Mn2SiO4, Mn2FeO3, Mn2FeO4, FeSiO3, Fe2SiO3 and Fe2SiO4.

[0028] Furthermore, the tensile strength of the cold-rolled high-strength steel sheet with excellent phosphating performance described in the present invention is ≥780 MPa. Furthermore, the tensile strength of the cold-rolled high-strength steel sheet with excellent phosphating performance described in the present invention is ≥980 MPa. Furthermore, the tensile strength of the cold-rolled high-strength steel sheet with excellent phosphating performance described in the present invention is ≥1180 MPa.

[0029] This application does not specifically limit the type and elemental composition of cold-rolled high-strength steel. Various cold-rolled high-strength steels known in the art are prepared by the method of the present invention, thereby having the structure (such as the element distribution described herein) and phosphating performance described herein.

[0030] In some embodiments, the cold-rolled high-strength steel sheet with excellent phosphating performance of the present invention contains the following elements in the following mass percentages:

[0031] C: 0.07-0.30%, Si: 0.07-3.0%, Mn: 1.5-5.0%.

[0032] Furthermore, the chemical element mass percentages of the cold-rolled high-strength steel sheet with excellent phosphating performance described in the present invention are:

[0033] C: 0.07-0.30%, Si: 0.07-3.0%, Mn: 1.5-5.0%, and one or more of Nb, Ti, Al, B, Cr, Mo, Ni, and V, with the total mass percentage of Nb, Ti, Al, B, Cr, Mo, Ni, and V being less than or equal to 2.0%; the balance being Fe and unavoidable impurities.

[0034] The inevitable impurities are mainly S and P, and it is desired that the content thereof is as low as possible. In some embodiments, P can be controlled to be ≤ 0.05% and S to be ≤ 0.02%.

[0035] The design principles of the above elements are:

[0036] C: is a solid solution strengthening element necessary for obtaining strength in steel. When the C content is too low, the strength of the steel is low, while when the C content is too high, the weldability of the steel is poor. Therefore, the present invention controls the C content by mass to be 0.07-0.30%.

[0037] Si: It has the function of improving both the strength and formability of steel. However, when the Si content is too high, the manufacturing difficulty increases. Therefore, the present invention controls the Si content to be 0.07-3.0% by mass.

[0038] Mn: An element that increases austenite stability, reduces the critical cooling rate during quenching, and improves the steel's hardenability. Mn also enhances the steel's work-hardening properties, thereby increasing its strength. Therefore, the present invention controls the Mn content to 1.5-5.0% by weight.

[0039] Nb, Ti, Al, B, Cr, Mo, Ni, and V have the effects of solid solution strengthening, refining structure, and improving hardenability. Adding a small amount of them helps to further improve the strength and toughness of steel. Therefore, the present invention may also contain one or more of Nb, Ti, Al, B, Cr, Mo, Ni, and V, and control their total amount to be less than or equal to 2.0% by mass. In some embodiments, when contained, the content of Nb may be 0.01-0.1%, the content of Ti may be 0.01-0.05%, the content of Al may be 0.01-1.5%, the content of B may be 0.0002-0.0008%, the content of Cr may be 0.01-0.5%, the content of Mo may be 0.1-0.3%, the content of Ni may be 0.0001-0.03%, and the content of Ni may be 0.01-0.1%.

[0040] Another object of the present invention is to provide a method for manufacturing a cold-rolled high-strength steel plate with excellent phosphating performance. The manufacturing method adopts a unique continuous annealing process to control the enrichment position and enrichment amount of Mn and Si elements in the steel plate, thereby achieving excellent phosphating performance.

[0041] Based on the above-mentioned invention objectives, the present invention provides a method for manufacturing the above-mentioned cold-rolled high-strength steel plate with excellent phosphating performance, which comprises the steps of: smelting, casting, hot rolling, pickling, cold rolling and continuous annealing; wherein in the continuous annealing step: the cold-rolled plate is heated in an oxidizing atmosphere for a first stage, then heated and soaked in a reducing atmosphere for a second stage, and then cooled and coiled.

[0042] In the manufacturing method described herein, smelting, casting, hot rolling, pickling, and cold rolling all utilize existing conventional processes. In an exemplary method, during the hot rolling step, the heating temperature is controlled to be 1150-1260°C, the start temperature of the finishing rolling is 1100-1220°C, and the final temperature of the finishing rolling is 900-950°C. During the cold rolling step, the cold rolling reduction ratio is controlled to be ≥50%. In some embodiments, commercially available cold-rolled steel can be used to carry out the annealing process of this application.

[0043] In the continuous annealing step, the purpose of selecting an oxidizing atmosphere for the first heating stage is to form iron oxide on the surface of the steel plate during the first heating process, and the purpose of selecting a reducing atmosphere for the second heating and soaking stage is to reduce the iron oxide formed during the first heating process to form ferrite, thereby forming a surface layer composed entirely of ferrite, so that Mn and Si elements cannot be enriched on the surface of the steel plate.

[0044] Furthermore, in some embodiments of the manufacturing method of the present invention, the oxidizing atmosphere in the first stage of heating is obtained by controlling the air-fuel ratio of the direct-fired furnace to be 0.95-1.05.

[0045] In some embodiments, when the first stage of heating utilizes a direct-fire furnace, an oxidizing atmosphere can be achieved by adjusting the air-fuel ratio. When the air-fuel ratio is less than 0.95, oxidation is insufficient, while when the air-fuel ratio is greater than 1.05, excessive oxidation occurs. Therefore, the air-fuel ratio is controlled within a range of 0.95-1.05.

[0046] Furthermore, in some other embodiments of the manufacturing method of the present invention, the oxidizing atmosphere in the first heating stage is a N2+O2 mixed gas, wherein the volume percentage of O2 is 0.01-1%.

[0047] In other embodiments, when the first heating stage utilizes an infrared radiation furnace, an oxidizing atmosphere is achieved by using a mixture of N2 and O2. When the volume percentage of O2 is less than 0.01%, oxidation is insufficient. When the volume percentage of O2 is greater than 1%, further addition of O2 may result in excessive oxidation. Therefore, the volume percentage of O2 is controlled to be between 0.01% and 1%.

[0048] Furthermore, in the manufacturing method described in the present invention, the heating rate of the first heating stage is 1-50°C / s, the first heating stage is heated from room temperature to the heating end temperature T1, and the mass percentage of T1 and Si satisfies: 570+4000×Si≤T1≤600+9000×Si.

[0049] The thickness of the oxide layer on the surface of the steel plate will increase as the end temperature T1 of the first heating stage increases. Therefore, in order to obtain a suitable oxide layer thickness, it is necessary to control the upper and lower limits of the T1 temperature. The inventors' research found that when the T1 temperature is the same, the thickness of the iron oxide on the surface of the steel plate is also affected by the composition of the steel plate, among which the Si content has the most significant impact. When the Si content in the steel plate is high, in order to obtain the same thickness of iron oxide in the first heating stage, a higher T1 temperature is required. When the T1 temperature and the Si content of the steel plate satisfy the following relationship 570+4000×Si≤T1≤600+9000×Si, a suitable iron oxide thickness can be obtained. In some embodiments, T1 is 580~800℃. Preferably, the thickness of the oxide layer formed by the first heating stage is 50-500nm.

[0050] Furthermore, in the manufacturing method of the present invention, the dew point of the oxidizing atmosphere in the first stage of heating is ≥ -50°C, preferably ≥ -40°C. In some embodiments, the dew point of the oxidizing atmosphere in the first stage of heating is between -50°C and 50°C. In some embodiments, the dew point of the oxidizing atmosphere in the first stage of heating is between -50°C and 0°C.

[0051] Furthermore, in the manufacturing method of the present invention, the dew point of the reducing atmosphere in the second heating and soaking stage is ≤10°C, such as ≤0°C, ≤-10°C, or ≤-20°C. In some embodiments, the dew point of the reducing atmosphere in the second heating and soaking stage is 10°C to -50°C, such as 0°C to -50°C or -20°C to -50°C.

[0052] It should be noted that, in the present invention, the dew point of the atmosphere during the first heating stage, the second heating stage, and the soaking stage is not an essential technical feature of the present invention. In other words, even without any special control of the dew point of the atmosphere during the first heating stage, the second heating stage, and the soaking stage, the peak Mn mass percentage of the element mass percentage-depth distribution curve within the depth range of 0-1000nm from the steel plate surface can be obtained. p ≤ 10.0%, Si mass percentage peak Si p The product features a ≤4.0% concentration. This is because, during the first heating stage, when iron oxide is formed, some Mn in the matrix oxidizes along with Fe, but the oxides formed by Si are primarily located in the transition layer. During the second heating and soaking stage, when the reduced iron is reduced, regardless of the atmosphere's dew point, the selective oxidation of alloying elements such as Mn and Si in the matrix is ​​primarily concentrated below the ferrite formed after the iron oxide is reduced, i.e., in the transition layer, and does not accumulate on the ferrite surface. Therefore, the present invention differs from existing technologies that utilize an increased dew point in the reducing atmosphere to promote internal oxidation of alloying elements and reduce external oxidation.

[0053] However, the inventors have discovered that increasing the dew point of the oxidizing atmosphere during the first heating stage can help lower the T1 temperature. This is because increasing the dew point of the atmosphere during the first heating stage increases the internal oxidation of alloying elements, thereby reducing oxidation of alloying elements at the iron oxide / substrate interface, particularly Si. Therefore, the dew point of the oxidizing atmosphere during the first heating stage is preferably controlled to ≥ -40°C. Because excessively high dew points during the second heating and soaking stages can lead to decarburization, the dew point of the atmosphere during the second heating and soaking stages is preferably controlled to ≤ -20°C.

[0054] Furthermore, in the manufacturing method described in the present invention, the reducing atmosphere in the second stage of heating and soaking is a mixed gas of N2+H2, wherein the volume percentage of H2 is 0.5-20%.

[0055] Furthermore, in the manufacturing method described in the present invention, the heating rate of the second heating stage is 1-20°C / s, and the second heating stage continues from T1 to the soaking temperature of 720-920°C, and the soaking time is 30-200s.

[0056] The soaking temperature T2 is controlled at 720-920°C, and the soaking time is controlled at 30-200s, mainly to obtain suitable mechanical properties of cold-rolled high-strength steel, which has little correlation with the phosphating performance.

[0057] The cold-rolled high-strength steel sheet with excellent phosphating performance of the present invention has the following beneficial effects:

[0058] The present invention solves the problem of poor phosphating performance of cold-rolled high-strength steel by controlling the peak values ​​of Mn and Si mass percentages and their depth positions on the element mass percentage-depth distribution curve in the steel plate, thereby improving the coating performance of the cold-rolled high-strength steel.

[0059] In some more preferred embodiments, the steel plate with excellent phosphating performance also has a tensile strength of ≥780 MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] FIG1 is a comparison of the mass percentage-depth distribution curves of the Mn element within 0-1000 nm from the steel plate surface in Example A1 of the present invention and Comparative Example A1.

[0061] FIG2 is a comparison of the mass percentage-depth distribution curves of Si element within 0-1000 nm from the steel plate surface in Example A1 of the present invention and Comparative Example A1.

[0062] FIG3 is a comparison of the mass percentage-depth distribution curves of Fe element within 0-1000 nm from the steel plate surface in Example A1 of the present invention and Comparative Example A1.

[0063] FIG4 is a comparison of the mass percentage-depth distribution curves of the Mn element within 0-1000 nm from the steel plate surface in Example B1 of the present invention and Comparative Example B1.

[0064] FIG5 is a comparison of the mass percentage-depth distribution curves of Si element within 0-1000 nm from the steel plate surface in Example B1 of the present invention and Comparative Example B1.

[0065] FIG6 is a comparison of the mass percentage-depth distribution curves of Fe element within 0-1000 nm from the steel plate surface in Example B1 of the present invention and Comparative Example B1. DETAILED DESCRIPTION

[0066] The cold-rolled high-strength steel sheet with excellent phosphating performance and the manufacturing method thereof described in the present invention will be further explained and illustrated below in conjunction with specific embodiments and the accompanying drawings. However, such explanation and illustration do not constitute an undue limitation to the technical solution of the present invention.

[0067] Table 1 lists the steel composition ratios used in various embodiments of the present invention and comparative examples.

[0068] Table 1 (wt%, balance Fe)

[0069] Based on the steel plate compositions in Table 1, the steel plates of various embodiments of the present invention and comparative examples were prepared according to the following steps. The specific process parameters of the continuous annealing steps of the various embodiments and comparative examples are listed in Table 2:

[0070] (1) Using conventional smelting;

[0071] (2) Using conventional casting;

[0072] (3) Conventional hot rolling;

[0073] (4) Conventional pickling and cold rolling;

[0074] (5) Continuous annealing: The cold-rolled sheet is heated in an oxidizing atmosphere for the first stage; wherein the heating rate of the first stage heating is 1-50°C / s, and the first stage heating is from room temperature to T1, and the mass percentage of T1 and Si satisfies: 570+4000×Si≤T1≤600+9000×Si; then the second stage heating and soaking are carried out in a reducing atmosphere, wherein the reducing atmosphere of the second stage heating is a N2+H2 mixed gas, wherein the volume percentage of H2 is 0.5-20%; then cooling and coiling are carried out.

[0075] In some embodiments, the oxidizing atmosphere in the first heating stage is a N2+O2 mixed gas, wherein the volume percentage of O2 is 0.01-1%.

[0076] In other embodiments, the oxidizing atmosphere for the first stage of heating is obtained by controlling the air-fuel ratio of the direct-fired furnace to be 0.95-1.05.

[0077] In some embodiments, the dew point of the oxidizing atmosphere in the first heating stage can be controlled to be ≥-40°C, and the dew point of the reducing atmosphere in the second heating stage can be controlled to be ≤-20°C.

[0078] In some embodiments, the heating rate of the second heating stage is 1-20° C. / s, and the second heating stage continues from T1 to the soaking temperature of 720-920° C., and the soaking time is 30-200 s.

[0079] Table 2

[0080] In Table 2, examples with an air-fuel ratio indicated by " / " indicate that an N2+O2 mixed gas was used in the oxidizing atmosphere. Comparative Examples A1-A4, D1-D2, E1-E3, F1, and G1-G2 all have the air-fuel ratio and oxygen content indicated by " / ", indicating that no oxidizing atmosphere was used in the first heating stage of these comparative examples. The codes "A," "B," ..., "H," and "I" for each example and comparative example in Table 2 indicate that the steel plate composition corresponding to the number in Table 1 was used.

[0081] Table 3 lists the steel plate characteristics of each embodiment and comparative example produced by using the steel plate composition of AI and the process parameters listed in Table 2, as well as the corresponding phosphating properties of each steel plate. p 、Si p , t pSi , t pMn 、Fe p Obtained using GDOES detection.

[0082] Table 3

[0083] Figures 1, 2 and 3 show the mass percentage-depth distribution curves of Mn, Si and Fe elements in the range of 0-1000 nm from the surface of the steel plate for Example A1 and Comparative Example A1, respectively. The characteristic value Mn is marked on the curves. p 、Si p 、Fe p and t p t in Figure 1 p Indicates t pMn , t in Figure 2 p Indicates t pSi , t in Figure 3 p Indicates t pSi .

[0084] As shown in Table 2, Example A1 underwent the first heating stage in an oxidizing atmosphere, heating to 580°C at a heating rate of 10°C / s. The oxidizing atmosphere consisted of a mixture of N2 and O2, with an O2 volume percentage of 0.2% and a dew point of -50°C. The second heating and soaking stage was then carried out in a reducing atmosphere at a heating rate of 4°C / s, a soaking temperature of 820°C, and a soaking time of 100 seconds. The reducing atmosphere in the second heating and soaking stage consisted of a mixture of N2 and H2, with an H2 volume percentage of 2% and a dew point of -50°C.

[0085] GDOES was used to detect the element depth distribution of the surface of the annealed steel plate, and the mass percentage-depth distribution curves of Mn, Si, and Fe elements in the depth range of 0-1000 nm were obtained as shown in Figures 1 to 3.

[0086] Comparative Example A1 performed the first heating, second heating, and soaking stages in a reducing atmosphere, with the same heating rate, temperature, and time as Example A1. The surface mass percentage distribution curves of Mn, Si, and Fe over a depth range of 0-1000 nm after annealing for Comparative Example A1 are shown in Figures 1 to 3.

[0087] Example A1 and Comparative Example A1 were subjected to phosphating treatment under the same conditions. The phosphating film on the surface of Example A1 was uniform and dense, and the phosphating performance met the requirements (indicated by "○" in Table 2-2). However, the phosphating film on the surface of Comparative Example A1 was sparse, with a large area not covered by the phosphating film, and the phosphating performance did not meet the requirements (indicated by "×" in Table 2-2). In this article, the quality of the phosphating performance is judged by observing the phosphating film on the surface of the steel plate after phosphating treatment, where the phosphating film coverage is 100%, the phosphating crystal size is less than 12 microns, and the phosphating film weight is greater than 2g / m 2 The phosphating performance meets the requirements. The phosphating treatment is carried out using a commercially available treatment agent. The specific steps and process are as follows: (1) Pre-degreasing spray, 45-55℃, 1 min; (2) Degreasing spray, 45-55℃, 2.0 min; (3) Secondary water cleaning spray, room temperature, 1 min; (4) Surface conditioning spray, room temperature, 1 min; (5) Phosphating spray, 50-60℃, 2.0 min; (6) Water cleaning spray, room temperature, 1 min; (7) Drying.

[0088] Figures 4, 5, and 6 show the mass percentage-depth distribution curves of Mn, Si, and Fe elements in the depth range of 0-1000 nm from the steel plate surface for Example B1 and Comparative Example B1, respectively. The characteristic value Mn is marked on the curves. p 、Si p 、Fe p and t p t in Figure 4 p Indicates tpMn , t in Figure 5 p Indicates t pSi , t in Figure 6 p Indicates t psi .

[0089] In Example B1, the first heating stage was conducted in an oxidizing atmosphere, heating to 650°C at a heating rate of 50°C / s. The oxidizing atmosphere was achieved in a direct-fired furnace with an air-fuel ratio of 0.95 and a dew point of 50°C. The second heating and soaking stage was then conducted in a reducing atmosphere at a heating rate of 5°C / s, a soaking temperature of 870°C, and a soaking time of 180 seconds. The atmosphere for the second heating and soaking stage was a mixture of N2 and H2, with an H2 volume percentage of 2% and a dew point of -40°C.

[0090] GDOES was used to analyze the depth distribution of elements on the annealed steel sheet surface, yielding the mass percentage-depth distribution curves of Mn, Si, and Fe over a depth range of 0-1000 nm, as shown in Figures 4-6. The sample from Example B1 was phosphating, resulting in a uniform and dense phosphating film that met the required phosphating performance.

[0091] Comparative Example B1 underwent the first and second heating stages and soaking in a reducing atmosphere consisting of an N₂-H₂ gas mixture containing 2% H₂ by volume and a dew point of -20°C. The soaking temperature and soaking time were the same as those for Example B1. The mass percentage distribution curves of Mn, Si, and Fe over a depth range of 0-1000 nm from the steel sheet surface after annealing for Comparative Example B1 are shown in Figures 4-6. Phosphating treatment of the sample from Comparative Example B1 revealed an uneven and loose phosphate film, with some areas lacking phosphate film coverage, resulting in substandard phosphate performance.

[0092] The inventors also used a scanning electron microscope to observe the cross-sectional metallographic structure after etching with a nital alcohol solution to examine the microstructure of each embodiment and comparative example. They also used a focused ion beam microscope to prepare cross-sectional transmission electron microscope specimens of the surface layer and transition layer. They measured the thickness of the surface layer under a transmission electron microscope and analyzed the types of oxides in the transition layer. The test results are listed in Table 4.

[0093] Table 4

[0094] Note: In Table 4, F represents ferrite, M represents martensite, and R represents retained austenite. The surface layer of each comparative example is indicated by "-", which means that the comparative example does not have a surface layer.

[0095] The inventors also tested the tensile strength of each embodiment and comparative example according to the tensile test of national standard GB / T 228.1, and the test results are listed in Table 5.

[0096] Table 5

[0097] It can be seen that the cold-rolled steel sheet manufactured by the present invention has excellent phosphating performance and high strength.

[0098] It should be noted that the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.

[0099] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therefrom that can be directly derived from or easily conceived by those skilled in the art based on the disclosure of the present invention are intended to fall within the scope of protection of the present invention.

Claims

1. A cold-rolled high-strength steel sheet with excellent phosphating performance, characterized in that: On the element mass percentage-depth distribution curve within the depth range of 0-1000nm from the steel plate surface, the peak value of Mn element mass percentage is p ≤10.0%、Si mass percentage peak value Si p ≤4.0%, and the peak value of Mn element mass percentage is Mn p And the Si element mass percentage peak Si p All are located at a depth of ≥50 nm from the surface of the steel plate.

2. The cold-rolled high-strength steel sheet with excellent phosphating performance according to claim 1, characterized in that: The Mn element mass percentage peak value Mn p And the Si element mass percentage peak Si p They are all located at a depth of 50-500 nm from the surface of the steel plate.

3. The cold-rolled high-strength steel sheet with excellent phosphating performance according to claim 1, characterized in that: On the element mass percentage-depth distribution curve within the depth range of 0-1000nm from the steel plate surface, the peak value of Fe element mass percentage is Fe p ≥85%, and the peak value of Fe element mass percentage is Fe p Located at 0-t from the surface of the steel plate pSi Depth range, where t pSi Indicates the mass percentage of Si element peak Si p Depth position at which it appears.

4. The cold-rolled high-strength steel sheet with excellent phosphating performance according to any one of claims 1 to 3, characterized in that: The steel plate comprises a base layer, a surface layer and a transition layer between the base layer and the surface layer in the thickness direction; wherein the microstructure of the surface layer is ferrite.

5. The cold-rolled high-strength steel sheet with excellent phosphating performance according to claim 4, characterized in that: The thickness of the surface layer is 50-500 nm.

6. The cold-rolled high-strength steel sheet with excellent phosphating performance according to claim 4, characterized in that: The microstructure of the base layer is martensite+ferrite, or martensite+ferrite+retained austenite.

7. The cold-rolled high-strength steel sheet with excellent phosphating performance according to claim 4, characterized in that: The transition layer contains oxides of Mn, Si, and Fe and / or composite oxides of Mn, Si, and Fe.

8. The cold-rolled high-strength steel sheet with excellent phosphating performance according to claim 7, characterized in that: The oxides of Mn, Si and Fe are at least one of the following: MnO, MnO2, SiO2, FeO, Fe2O3 and Fe3O4; the composite oxides of Mn, Si and Fe are at least one of the following: MnSiO3, Mn2SiO4, Mn2FeO3, Mn2FeO4, FeSiO3, Fe2SiO3 and Fe2SiO4.

9. The cold-rolled high-strength steel sheet with excellent phosphating performance according to claim 1, characterized in that: Its tensile strength is ≥780MPa.

10. The cold-rolled high-strength steel sheet with excellent phosphating performance according to claim 1, characterized in that: It contains the following elements in the following mass percentages: C: 0.07-0.30%, Si: 0.07-3.0%, Mn: 1.5-5.0%.

11. The cold-rolled high-strength steel sheet with excellent phosphating performance according to claim 10, characterized in that: The mass percentage of its chemical elements is: C: 0.07-0.30%, Si: 0.07-3.0%, Mn: 1.5-5.0%, and one or more of Nb, Ti, Al, B, Cr, Mo, Ni, and V, the total mass percentage of Nb, Ti, Al, B, Cr, Mo, Ni, and V is less than or equal to 2.0%; the balance is Fe and unavoidable impurities.

12. The method for manufacturing a cold-rolled high-strength steel sheet with excellent phosphating performance according to any one of claims 1 to 11, comprising the steps of smelting, casting, hot rolling, pickling, cold rolling and continuous annealing; characterized in that: In the continuous annealing step: the cold-rolled sheet is first heated in an oxidizing atmosphere, then heated and soaked in a reducing atmosphere, and then cooled and coiled.

13. The manufacturing method according to claim 12, characterized in that: The oxidizing atmosphere for the first stage of heating is obtained by controlling the air-fuel ratio of the direct-fired furnace to be 0.95-1.05; or, the oxidizing atmosphere for the first stage of heating is a N2+O2 mixed gas, wherein the volume percentage of O2 is 0.01-1%.

14. The manufacturing method according to claim 12, characterized in that: The heating rate of the first stage of heating is 1-50°C / s, the first stage of heating is heated from room temperature to T1, and the mass percentage of T1 and Si satisfies: 570+4000×Si≤T1≤600+9000×Si; preferably, T1 is 580-800°C.

15. The manufacturing method according to claim 12, characterized in that: The manufacturing method has one or more of the following characteristics: The dew point of the oxidizing atmosphere in the first stage of heating is ≥ -50°C; The reducing atmosphere in the second stage of heating and equalizing is a N2+H2 mixed gas, wherein the volume percentage of H2 is 0.5-20%; The dew point of the reducing atmosphere in the second stage of heating and equalization is ≤10℃; The heating rate of the second stage heating is 1-20°C / s. The second stage heating continues from T1 to the even heating temperature of 720-920°C, and the even heating time is 30-200s.