Silver oxide particles, silver oxide powder, bonding composition, silver oxide paste, method for producing semiconductor device using said bonding composition or said silver oxide paste, and method for producing silver oxide particles or silver oxide powder

MYPI2025005783A0Undetermined Publication Date: 2024-10-17CENT GLASS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005783
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-10
Filing Date
2024-04-10
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional bonding materials for power semiconductor devices, such as solder alloys and epoxy conductive adhesives, fail to provide sufficient bonding strength at high operating temperatures, particularly when used in power semiconductor devices that require temperatures above 200°C.

Method used

The development of a silver oxide paste using nano-sized, flaky silver oxide particles with specific size and shape characteristics, along with a dispersant and dispersion medium, to create a bonding composition that can maintain bonding strength at low temperatures without cracking or peeling, achieved through bead mill pulverization and careful composition formulation.

Benefits of technology

This solution provides excellent bonding strength of 30 MPa or more at temperatures as low as 250°C, suppressing cracks and peeling, and allows for the use of silver oxide particles in semiconductor device manufacturing, enhancing the reliability and stability of power semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005783_DRAWING_001
    Figure PI2025005783_DRAWING_001
  • Figure PI2025005783_DRAWING_002
    Figure PI2025005783_DRAWING_002
  • Figure PI2025005783_DRAWING_003
    Figure PI2025005783_DRAWING_003
Patent Text Reader

Abstract

The present invention provides a bonding material that achieves good bonding strength even when bonding at low temperatures. Flake-shaped silver oxide particles or a silver oxide powder containing the particles are provided. The flake-shaped silver oxide particles have an average thickness of 10 to 100 nm and a D50 of 100 to 350 nm. Moreover, the flake-shaped silver oxide particles or silver oxide powder containing the particles may be used as a paste for bonding a semiconductor substrate with, for example, a power semiconductor chip. Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Silver oxide particles, silver oxide powder, bonding composition, silver oxide paste, method for manufacturing a semiconductor device using the bonding composition or the silver oxide paste, and method for manufacturing silver oxide particles or silver oxide powder

[0001] The present disclosure relates to a silver oxide paste and a method for manufacturing a semiconductor device using the silver oxide paste.

[0002] Power semiconductor devices have traditionally been used for power control and motor control in automobiles, power transmission systems, railways, solar cells, home appliances, etc. Until now, Si-based semiconductor devices using Si have been mainstream, but with the demand for higher currents and voltages, power semiconductor devices using SiC, GaN, etc. are being considered.

[0003] The operating temperature of power semiconductor devices is expected to reach 200°C or higher, which is higher than the operating temperature of currently mainstream Si-based semiconductor devices. This poses a problem that conventionally used bonding materials such as solder alloys and epoxy-based conductive adhesives cannot withstand such operating temperatures.

[0004] In recent years, the use of silver-based bonding materials such as silver and silver oxide has been considered as bonding materials that are durable at temperatures above 200°C, have low electrical resistance, and have excellent heat dissipation properties. Patent Document 1 discloses that silver oxide particles are used as a material for bonding a semiconductor element and a circuit layer in a power module, and that this material can keep the bonding temperature to the semiconductor element low and reduce the thermal load on the semiconductor element. Patent Document 1 also discloses silver oxide particles of 0.1 μm to 40 μm in size as the silver oxide particles, and in its examples, micron-sized silver oxide particles are tested. Typically, such fine silver oxide particles are obtained by precipitation from a silver salt solution and generally have a relatively isotropic shape, such as a spherical or approximately spherical shape.

[0005] JP 2014-96545 A

[0006] It has been found that the bonding materials made of spherical silver oxide particles discussed above may result in insufficient bonding strength when bonding at relatively low temperatures, for example, around 250° C., and that improvements are necessary for practical use. An object of the present disclosure is to provide a bonding material, such as a silver oxide paste, that can provide good bonding strength even at low temperatures.

[0007] The present inventors have focused on nano-sizing silver oxide particles, and have discovered a bonding material that can provide good bonding strength without causing cracks or peeling due to thermal shrinkage by forming the silver oxide particles into flakes.

[0008] That is, one aspect of the present disclosure relates to flake-shaped silver oxide particles having a nano-sized thickness or a silver oxide powder containing the same.

[0009] The present disclosure (1-1) relates to flake-shaped silver oxide particles or a silver oxide powder containing the same, characterized in that the flake-shaped silver oxide particles have an average thickness of 1 to 100 nm and a D50 of 100 to 350 nm.

[0010] The present disclosure (1-2) relates to the flake-shaped silver oxide particles according to the present disclosure (1-1), or a silver oxide powder containing the same, wherein the average major axis of the flake-shaped silver oxide particles is 300 to 1000 nm.

[0011] The present disclosure (1-3) relates to the flaky silver oxide particles according to the present disclosure (1-1) or (1-2), or a silver oxide powder containing the same, in which the half-width of the diffraction peak derived from the (111) plane in the X-ray diffraction spectrum of the flaky silver oxide particles is 0.80 or more.

[0012] The present disclosure (1-4) relates to the flake-shaped silver oxide particles according to any one of the present disclosures (1-1) to (1-3), or a silver oxide powder containing the same, wherein the surfaces of at least some of the flake-shaped silver oxide particles have a compound having a glycol ether skeleton in the main chain and / or side chain.

[0013] The present disclosure (1-5) relates to a bonding composition comprising: silver oxide particles having a flake shape according to any one of the present disclosures (1-1) to (1-4) or a silver oxide powder containing the same; a dispersant; and a dispersion medium.

[0014] The present disclosure (1-6) relates to the bonding composition according to the present disclosure (1-5), in which the dispersant is a compound having a glycol ether skeleton in the main chain and / or side chain.

[0015] The present disclosure (1-7) relates to the bonding composition according to the present disclosure (1-5) or (1-6), in which the dispersion medium is a compound having an ethylene-based or propylene-based glycol ether skeleton.

[0016] The present disclosure (1-8) relates to a method for producing the flake-shaped silver oxide particles or silver oxide powder containing the same according to any one of the present disclosures (1-1) to (1-4), characterized in that the silver oxide particles are pulverized using a bead mill.

[0017] The present disclosure (1-9) relates to a method for producing flake-shaped silver oxide particles or a silver oxide powder containing the same according to the present disclosure (1-8), wherein the bead milling comprises the following steps: a step of supplying the silver oxide particles, the dispersant, and the dispersion medium to a bead milling device; and a step of performing bead milling in the device to obtain a slurry containing flake-shaped silver oxide particles.

[0018] The present disclosure (1-10) relates to a method for producing flake-shaped silver oxide particles or a silver oxide powder containing the same according to the present disclosure (1-8) or (1-9), wherein the dispersant is a compound having a glycol ether skeleton in the main chain and / or side chain.

[0019] The present disclosure (1-11) relates to a method for manufacturing a semiconductor device, comprising: (1) a step of applying the bonding composition according to any one of the present disclosures (1-5) to (1-7) onto a semiconductor substrate to form a layer of the bonding composition; (2) a step of placing a semiconductor chip on the layer of the bonding composition to form a laminate; and (3) a step of heating the obtained laminate at 300°C or less while applying pressure at 0 to 30 MPa to integrate the laminate.

[0020] The present disclosure (1-12) relates to the method for manufacturing a semiconductor device according to the present disclosure (1-11), further comprising a step of drying the layer of the bonding composition between the step (1) and the step (2).

[0021] The present disclosure (1-13) relates to a method for manufacturing a semiconductor device according to the present disclosure (1-11) or (1-12), wherein the semiconductor chip is a SiC semiconductor chip.

[0022] The present disclosure (2-1) relates to a silver oxide paste comprising: flake-shaped silver oxide particles; a dispersant; and a dispersion medium, wherein the silver oxide particles have an average thickness of 1 to 100 nm and a D50 of 100 to 350 nm.

[0023] The present disclosure (2-2) relates to the silver oxide paste according to the present disclosure (2-1), further containing a proton-based additive.

[0024] The present disclosure (2-3) relates to the silver oxide paste according to the present disclosure (2-1) or (2-2), wherein the dispersant is a compound having a glycol ether skeleton in the main chain and / or side chain.

[0025] The present disclosure (2-4) relates to the silver oxide paste according to any one of the present disclosures (2-1) to (2-3), wherein the dispersion medium is a compound having an ethylene-based or propylene-based glycol ether skeleton.

[0026] The present disclosure (2-5) relates to the silver oxide paste according to any one of the present disclosures (2-1) to (2-4), wherein the average major axis of the silver oxide particles is 300 to 1000 nm.

[0027] The present disclosure (2-6) relates to any one of the present disclosures (2-1) to (2-5), wherein the half-width of the diffraction peak derived from the (111) plane in the X-ray diffraction spectrum of the silver oxide particles is 0.80 or more. The silver oxide paste relates to any one of the present disclosures (2-1) to (2-5).

[0028] The present disclosure (2-7) relates to the silver oxide paste according to any one of the present disclosures (2-1) to (2-6), wherein the content of the dispersant is 12 mass% or less relative to the mass of the entire silver oxide paste.

[0029] The present disclosure (2-8) relates to the silver oxide paste according to the present disclosure (2-2), in which the content of the proton-based additive is 0.5 to 10 mass% relative to the mass of the total silver oxide paste.

[0030] The present disclosure (2-9) relates to a silver oxide paste according to any one of the present disclosures (2-1) to (2-8), which is used for joining purposes.

[0031] The present disclosure (2-10) relates to a method for manufacturing a semiconductor device, comprising: (1) a step of applying the silver oxide paste according to any one of the present disclosures (2-1) to (2-9) onto a first substrate to form a layer of the silver oxide paste; (2) a step of placing a second substrate on the layer of the silver oxide paste to form a laminate; and (3) a step of heating the obtained laminate at 300°C or less while applying pressure at 0 to 30 MPa to integrate the laminate.

[0032] The present disclosure (2-11) relates to the method for manufacturing a semiconductor device according to the present disclosure (2-10), further comprising a step of drying the layer of silver oxide paste between the step (1) and the step (2).

[0033] The present disclosure (2-12) relates to the method for manufacturing a semiconductor device according to the present disclosure (2-10) or (2-11), in which the second substrate is a semiconductor chip.

[0034] The present disclosure makes it possible to provide a bonding material such as silver oxide paste that can provide good bonding strength even at low temperatures.

[0035] 1 is a diagram showing a method for bonding power semiconductors using a paste as a composition containing flake-shaped silver oxide particles according to the present disclosure; 2 is an electron microscope photograph used when measuring (a) the average major axis and (b) the average thickness of flake-shaped silver oxide particles; 3 is a photograph, in place of a drawing, of raw silver oxide particles (before dispersion treatment) used in Comparative Examples 2 to 5; 4 is a photograph, in place of a drawing, showing the cross section of the bonding layer of (a) Example 3 and (b) Comparative Example 6; and 5 is a photograph, in place of a drawing, showing the cross section of the bonding layer of Example 3.

[0036] The present disclosure will be described in detail below, but the following description of the constituent elements is an example of an embodiment of the present disclosure, and the present disclosure is not limited to these specific details. Various modifications can be made within the scope of the gist of the present disclosure.

[0037] In this specification, unless otherwise specified, the expression "X to Y" in the description of a numerical range means at least X and at most Y. For example, "1 to 5% by mass" means "at least 1% by mass and at most 5% by mass."

[0038] The silver oxide paste of the present disclosure comprises flake-shaped silver oxide particles, a dispersant, and a dispersion medium, wherein the silver oxide particles have an average thickness of 1 to 100 nm and a D50 of 100 to 350 nm. This allows for good bonding strength to be obtained even at low temperatures (e.g., 250°C).

[0039] The present disclosure will be described in detail below. (Flake-shaped silver oxide particles, silver oxide powder) In the present disclosure, the flake-shaped silver oxide particles constituting the silver oxide powder do not refer to individual flake-shaped silver oxide particles, but rather to an aggregate of flake-shaped silver oxide particles or a group of flake-shaped silver oxide particles. The silver oxide powder of the present disclosure contains flake-shaped silver oxide particles, and is characterized in that the average thickness (average thickness) of the flake-shaped silver oxide particles is 1 to 100 nm and the D50 is 100 to 350 nm. Note that "flake-shaped silver oxide particles" refers to silver oxide particles that have a flake shape and exhibit an average thickness and D50 within the above ranges. The inventors' studies have found that by using the above-mentioned flake-shaped silver oxide particles instead of the conventionally used spherical silver oxide particles, good bonding strength can be obtained even at low temperatures.

[0040] Furthermore, in one aspect of the present disclosure, the inventors' studies have found that, as the particle size of flake-shaped silver oxide particles decreases, they are more easily reduced at low temperatures of 250°C or less. However, they also found that the smaller the particle size, the greater the shrinkage upon heating, making them more susceptible to cracking, peeling, and the like. Furthermore, it has been found that the shrinkage is also thought to be due to oxygen elimination during the reduction of silver oxide, and tends to occur more easily when silver oxide particles are used than when silver particles are used. On the other hand, as the particle size increases, cracking, peeling, and the like become less likely to occur, but reduction at the above-mentioned low temperature range becomes more difficult. One aspect of the present disclosure is that by making the silver oxide particles flake-shaped, it is possible to achieve both ease of reduction and suppression of cracking and peeling.

[0041] The silver oxide powder of the present disclosure may contain non-flake-shaped silver oxide particles as long as the content does not adversely affect various performances. The content of such silver oxide particles is not particularly limited, but may be, for example, 30% by mass or less, where the silver oxide powder is taken as 100.

[0042] The term "flake-shaped" refers to a non-spherical structure having at least an upper surface, a lower surface, and a thickness, with the upper and lower surfaces being substantially flat. In this case, the upper and lower surfaces may be partially uneven or deformed, and the overall structure may be a flat plate or a thin rectangular parallelepiped (thickness smaller than length). It may also refer to a flat, plate-like shape such as a flake or scale shape (flaky: "plate-like shape" as defined in JIS Z2500:2000). More specifically, a sample that can be observed from the cross-sectional direction of silver oxide particles is prepared according to the method described in the measurement of average thickness below, and the sample is observed using a scanning electron microscope. The distance between the upper and lower surfaces of the central part of a particle is defined as the particle thickness. If the length of the side intersecting the thickness direction of the particle is greater than the thickness, the particle is determined to have a flake shape.

[0043] By setting the average thickness of the flake-shaped silver oxide particles to 1 to 100 nm, the ease of reduction (particularly during bonding) at 250°C or less can be improved, and the bonding strength can be increased to 30 MPa or more. The average thickness may also be set to preferably 5 to 90 nm, more preferably 10 to 50 nm, and even more preferably 15 to 40 nm.

[0044] The D50 of the flake-shaped silver oxide particles is a value indicating the median diameter (center value) when each particle is considered as a sphere. By setting the D50 to 100 to 350 nm, good bonding strength can be obtained. It has also been found that as the particle size of the silver oxide particles decreases, cracks and peeling at the bonded portion tend to occur more easily due to thermal shrinkage. On the other hand, by setting the D50 to 100 to 350 nm, it is possible to achieve both suppression of cracks and peeling at the bonded portion and good bonding strength. From the viewpoint of further suppressing cracks and peeling at the bonded portion, a diameter of 180 to 350 nm may be preferable, and a diameter of 200 to 320 nm may be more preferable. Here, cracks and peeling due to thermal shrinkage can occur during each step of the process involving heating, such as during the reduction of silver oxide, drying of the silver oxide paste (hereinafter also referred to simply as paste) described below, sintering, and bonding. In particular, when D50 is 200 nm or more, it is preferable because the occurrence of the above-mentioned cracking and peeling can be easily suppressed even without containing a component (such as a plasticizer described later) that helps suppress cracking and peeling that occurs during the reduction of silver oxide or the drying of the paste.

[0045] From another perspective, the average value of the major axes (average major axis) of the flake-shaped silver oxide particles may be, for example, 300 to 1000 nm, preferably 300 to 900 nm, more preferably 300 to 700 nm, and even more preferably 400 to 700 nm. A value within the above range is suitable from the viewpoint of suppressing the occurrence of cracks and peeling at joints. From yet another perspective, the average value of the major axes (average major axis) of the flake-shaped silver oxide particles is, for example, preferably 300 to 1000 nm, and even more preferably 400 to 900 nm from the viewpoint of suppressing the occurrence of cracks and peeling at joints.

[0046] From another perspective, in the X-ray diffraction spectrum of flake-shaped silver oxide particles, the half-width of the diffraction peak derived from the (111) plane of silver oxide is preferably 0.80 or more, and more preferably 0.85 or more. The upper limit is not particularly limited, but may be, for example, 1.20 or less, preferably 1.12 or less. Furthermore, the (111) plane of the silver oxide has a main peak at 32° to 33°. When the half-width is within the above range, the bonding strength tends to be improved compared to spherical silver oxide particles with a similar D50, which is preferable. This is because when the half-width is 0.80 or more, the crystallinity of the silver oxide is low, and the bonding strength of the Ag—O that constitutes the crystal is thought to be reduced, making reduction more likely to occur at lower temperatures. The decrease in crystallinity of the silver oxide is thought to be due to the milling process described below. When raw silver oxide particles are crushed, they become smaller to a certain size, but once they reach the limit, they become indestructible and undergo plastic deformation into flakes, and it is believed that this plastic deformation reduces the crystallinity.

[0047] From the viewpoint of suppressing cracking and peeling at the bonded portion, it is preferable that the aspect ratio (l / t) of the average major axis (l) to the average thickness (t) is usually 8 to 20, and preferably 14 to 18. The aspect ratio may be a value calculated from the average thickness and average major axis of the flake-shaped silver oxide particles.

[0048] Furthermore, it is preferable that the surface of at least some of the flake-shaped silver oxide particles contained in the silver oxide powder contains a compound having a glycol ether skeleton in the main chain and / or side chain, as this facilitates reduction at low temperatures. This compound is the same compound as the dispersant in the composition described below. Furthermore, "having on the surface" refers to a state in which the compound is attached to the surface of the flake-shaped silver oxide particles by chemical bonding, physical adsorption, or the like. It is more preferable that the compound is attached to all of the flake-shaped silver oxide particles that make up the silver oxide powder. The particle shape, D50, average thickness, average major axis, and XRD half-width can each be confirmed or measured using the measurement methods described in detail below.

[0049] (Method for producing flake-shaped silver oxide particles) The flake-shaped silver oxide particles of the present disclosure can be obtained, for example, by pulverizing commercially available silver oxide particles (which are generally spherical or nearly spherical and have a particle size of about 1 to 20 μm) using a bead mill as a raw material. Typically, silver oxide particles having a particle size of a microparticle or less are spherical particles obtained by precipitation from a silver salt solution, as disclosed in JP 2005-104825 A. In contrast, the silver oxide particles of the present disclosure are formed by pulverizing using a bead mill, and the particles are obtained in a flake shape.

[0050] In the grinding process using a bead mill, raw silver oxide particles (raw silver oxide particles) are introduced into a grinding chamber in the bead mill together with a dispersant and a dispersion medium that suppress particle aggregation, and the raw silver oxide particles are ground by rotating the stirring mechanism (rotor) at high speed (high peripheral speed) and causing beads, which serve as grinding media in the grinding chamber, to collide with the raw silver oxide particles.

[0051] The dispersant used is not particularly limited, and various dispersants can be used as long as they can disperse the raw silver oxide particles, the silver oxide particles being pulverized, and the flaky silver oxide particles after pulverization in the dispersion medium and do not particularly affect the physical properties of the raw silver oxide particles. Furthermore, the dispersant typically adheres to the surface of at least some of the flaky silver oxide particles and remains thereon even after the solids are separated and dried, as described below, thereby preventing the flaky silver oxide particles from agglomerating under strong forces. Examples of such dispersants include commercially available dispersants based on polyacrylates, aliphatics, polyesters, polyurethanes, and polyethers. Dispersants may be used alone or in combination of two or more. Compounds having a glycol ether skeleton in the main chain and / or side chain, as described below, can also be suitably used as dispersants.

[0052] As the dispersion medium, a medium that does not react with silver oxide (e.g., reduction reaction) is used because strong energy is applied to the raw silver oxide particles when milling with beads. Furthermore, various dispersion media can be used without particular limitations as long as they can maintain the raw silver oxide particles, the silver oxide particles during milling, and the flake-shaped silver oxide particles after milling in a dispersed state. For example, water can be used as such a dispersion medium. The dispersion media may be used alone or in combination of two or more.

[0053] The milling media (beads) used are not particularly limited, and various types of beads can be used as long as they are conventionally used in the field of bead mill milling. Examples of such beads include beads made from materials such as glass, zirconia, alumina, silica, and steel. These may be used alone or in combination of two or more types. Since bead sizes that are too large or too small tend to result in insufficient milling, it is desirable to use beads with a diameter of 0.01 to 0.5 mm. By ensuring the diameter falls within the above range, silver oxide particles having a flake shape of the desired size and shape can be obtained.

[0054] The average thickness, D50 value, and average major axis of the intended flake-shaped silver oxide particles can be adjusted by appropriately adjusting the grinding time using a bead mill, the rotor circumferential speed, the bead packing ratio, and the like. The grinding time depends on the desired size of the flaky silver oxide powder, but may be, for example, about 100 to 500 minutes. As the grinding time increases, the grinding progresses and the D50 value tends to decrease. The rotor circumferential speed is preferably, for example, about 5 to 20 m / s, and the bead packing ratio is preferably, for example, about 70 to 95% by volume. Those skilled in the art can appropriately set the grinding conditions by confirming the particle morphology of the flaky silver oxide particles described below under these conditions. Depending on the desired size of the flaky silver oxide particles, grinding may be performed in stages, using beads of different diameters or types, two or more times to gradually reduce the size. A known cooling mechanism or temperature control mechanism may be installed to prevent the bead mill or the grinding chamber from becoming excessively hot.

[0055] The amount of raw silver oxide particles to be bead milled is not particularly limited, as long as it is sufficiently pulverizable. For example, when the amount of material to be processed supplied to the milling chamber of the bead mill device is taken as 100, it may be 2 to 60% by mass, preferably 5 to 40% by mass. The dispersion medium may be, for example, 28 to 90% by mass, preferably 30 to 90% by mass, and more preferably 60 to 88% by mass. The dispersant is not particularly limited as long as it can disperse raw silver oxide particles and flaky silver oxide particles. The dispersant may be 8 to 70% by mass, preferably 10 to 70% by mass, and more preferably 15 to 60% by mass, based on the raw silver oxide particles used. In this way, a slurry containing flaky silver oxide particles (hereinafter sometimes simply referred to as "slurry") is obtained. The solids are separated from the slurry and dried to obtain a silver oxide powder containing flaky silver oxide particles. Furthermore, when a silver oxide paste composition (preferably a bonding composition) is subsequently prepared, the liquid in the slurry may be replaced to obtain the silver oxide paste described below without going through the step of drying the solids.

[0056] The method for separating the solids is not particularly limited as long as it does not impair the various properties of the silver oxide powder. For example, a simple method is to separate the solids from the supernatant using a known centrifugation method. The method for drying the solids is not particularly limited as long as it does not cause reduction of silver oxide. For example, the supernatant is removed and the solids are vacuum-dried at room temperature to obtain solid silver oxide powder. To purify the flake-shaped silver oxide particles or remove excess dispersant, the solids may be dispersed again in a new dispersion medium and the same procedure repeated. Other drying methods, such as spray drying, can also be used.

[0057] (Composition such as a paste (preferably a bonding composition) containing flake-shaped silver oxide particles) The composition (e.g., the silver oxide paste of the present disclosure) contains the above-described flake-shaped silver oxide particles, a dispersion medium, and a dispersant. The dispersion medium and the dispersant may be used alone or in combination of two or more. As described above, the dispersant used during production adheres to the surface of the flake-shaped silver oxide particles and remains even after the solids are separated and dried. When this dispersant is a dispersant for a paste described below, a composition (e.g., a silver oxide paste) can be obtained simply by adding a dispersion medium for the paste. Alternatively, the silver oxide powder obtained by drying the slurry may be mixed with a dispersion medium for the paste, and optionally a dispersant for the paste, and the mixture may be stirred to obtain a uniform dispersion, thereby obtaining a composition (e.g., a silver oxide paste).

[0058] When preparing a composition (e.g., a silver oxide paste) from the above slurry without a drying step, it is preferable to obtain the desired composition by separating the slurry into a solid fraction and a supernatant by centrifugation, removing the supernatant, and then adding a dispersing medium to the resulting solid fraction to redisperse the solid fraction. If a different dispersing agent is used, the desired dispersing agent may be added simultaneously with the dispersing medium to replace the dispersing agent. Alternatively, the desired composition may be prepared by repeating the centrifugation, replacement of the dispersing medium and dispersing agent, and redispersion multiple times. A predetermined amount of dispersing medium is added to the solid fraction obtained after the above procedure, followed by stirring, to prepare a composition (e.g., a silver oxide paste) containing flake-shaped silver oxide particles as a uniform dispersion. If necessary, further dispersing agent may be added. As a result of the above, a composition (e.g., a silver oxide paste) is obtained as a uniform dispersion, and the composition may be further stirred as necessary.

[0059] When the silver oxide powder is obtained by drying the slurry, it is possible to obtain a composition (e.g., a silver oxide paste) as a uniform dispersion by mixing at least the silver oxide powder with a dispersion medium for a paste and stirring the mixture. If necessary, any dispersant, dispersion medium, etc. may be further mixed.

[0060] The stirring may be carried out using a known disperser or kneading device used for pastes or paints under conditions that do not cause further pulverization, such as various mixers, three-roll mills, paint shakers, etc. The flake-shaped silver oxide particles or silver oxide powder containing the same may be used after removing extremely large or extremely small particles by known classification or the like.

[0061] (Paste composition (preferably bonding composition)) A paste composition (preferably a bonding composition) that is one of preferred embodiments of the present disclosure will be described below. Note that the present disclosure is not limited to this embodiment.

[0062] The paste preferably contains flake-shaped silver oxide particles, a compound having an ethylene- or propylene-based glycol ether skeleton as a dispersion medium that maintains the flake-shaped silver oxide particles in a dispersed state, and a compound having a glycol ether skeleton in the main chain and / or side chain as a dispersant for dispersing the flake-shaped silver oxide particles. By using the composition, it is possible to obtain a paste that does not undergo a reduction reaction at room temperature and promotes the reduction of silver oxide in a temperature range of 100 to 150°C. Furthermore, because the reduction reaction does not occur at room temperature (20 to 30°C), the paste has a good pot life and can be used after storage for a certain period of time (e.g., one month or more) after preparation, rather than immediately after preparation.

[0063] The amount of flake-shaped silver oxide particles contained in the composition does not need to be particularly limited as long as the composition has suitable coatability during application, but is preferably 70 to 95 mass %, and more preferably 75 to 85 mass %, based on the mass of the entire composition.

[0064] The dispersion medium for the paste used in the above paste may be a compound having coating properties suitable for application, having an ethylene or propylene glycol ether skeleton, and capable of volatilizing during the bonding process. Examples include diethylene glycol methyl ether (methyl carbitol), triethylene glycol methyl ether (methoxy triglycol), diethylene glycol methyl ether (carbitol), triethylene glycol methyl ether (ethoxy glycol), ethylene glycol propyl ether (propyl cellosolve), ethylene glycol monobutyl ether (butyl cellosolve), diethylene glycol monobutyl ether (butyl carbitol), triethylene glycol n-butyl ether (butoxy triglycol), ethylene glycol hexyl ether (hexyl cellosolve), diethylene glycol hexyl ether (hexyl carbitol), ethylene glycol n-butyl ether acetate (butyl cellosolve), and the like. Suitable examples of the propylene glycol methyl ether include propylene glycol methyl ether, dipropylene glycol methyl ether, tripropylene glycol methyl ether, propylene glycol n-propyl ether, dipropylene glycol n-propyl ether, propylene glycol n-butyl ether, dipropylene glycol n-butyl ether, tripropylene glycol n-butyl ether, propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol diacetate, and propylene glycol phenyl ether. These may be used alone or in combination of two or more. Of these, diethylene glycol monobutyl ether is preferred.

[0065] The dispersion medium may be used in an amount of, for example, 8 to 30% by mass, preferably 10 to 25% by mass, and more preferably 13 to 20% by mass, based on the total mass of the composition. When two or more dispersion media are used, the above amount refers to the total amount. The same applies to other similar descriptions.

[0066] Suitable dispersants for use in the paste include compounds having a glycol ether skeleton in the main chain and / or side chain. Various dispersants can be used without particular limitation, as long as they can maintain flake-shaped silver oxide particles in a dispersed state in a dispersion medium. Examples of such dispersants include polymeric compounds having a skeleton of styrene, maleic acid, acrylic acid, methacrylic acid, aminoethyl methacrylate, or the like in the main chain and a glycol ether polymer with a molecular weight of 100 or more in the side chain. These may be used alone or in combination of two or more. The upper molecular weight limit of the dispersant may be, for example, 100,000 or less. Furthermore, the carboxyl groups of maleic acid, acrylic acid, or methacrylic acid in the main chain may form salts with amine compounds to adjust the acid value and amine value. Suitable examples of such polymeric compounds include BYK-190, BYK-194N, and BYK-2055 (all manufactured by BYK-Chemie).

[0067] The dispersant may be contained in an amount of, for example, 12% by mass or less relative to the mass of the entire composition. It may be used in an amount of preferably 5% by mass or less, more preferably 3.5% by mass or less. Furthermore, as long as dispersion is possible, the lower limit is not particularly limited, but may be, for example, 0.5% by mass or more, preferably 1% by mass or more, more preferably 2% by mass or more. When the content of the dispersant is 3.5% by mass or less relative to the mass of the entire composition, better bonding strength tends to be obtained.

[0068] Generally, the reduction reaction of silver oxide powder proceeds as follows: (1) Reduction of silver oxide → (2) Sintering of Ag → (3) Grain growth (bonding; sintering and grain growth of Ag). Generally, silver oxide begins to decompose in air at around 200°C, and heating to 300°C or higher is required for complete reduction to metallic silver. If a reducing agent is not added at low temperatures below 250°C, the reduction reaction of silver oxide ((1) → (2)) does not proceed sufficiently, and there is a risk of unreduced silver oxide remaining in the bonded or sintered layer obtained after the process for (3). Residual unreduced silver oxide may adversely affect bonding strength, thermal conductivity, and electrical conductivity. On the other hand, when a reducing agent is added, the reduction reaction of silver oxide ((1)) can proceed sufficiently even at the above low temperature range. However, in systems with strong reducing properties, the reduction reaction (1) proceeds gradually even when left at room temperature. If this system is subjected to a heat treatment for a predetermined time for drying or the like, the reaction will proceed up to the step (3) of the above (1) → (2) → (3), and it is said to be difficult to stop the reaction at the reduction reaction step.

[0069] In the invention described in Patent Document 1, a strong reducing agent such as diethylene glycol is used to obtain a bonding layer exhibiting sufficient bonding strength. However, if the coating layer after applying the above-mentioned paste is heated and dried, the reaction proceeds from (1) to (2) to (3), and even if the semiconductor chip or substrate to be bonded is then placed, the desired bonding may not be achieved. Therefore, pastes containing reducing agents have either not been heated and dried, or bonding has had to be performed in an insufficiently dried state in order to remove the dispersion medium to a degree that does not volatilize the reducing agent. The bonding layer obtained in this manner is more prone to voids (gaps) in the bonding layer due to the volatilization of the dispersion medium and reducing agent that occurs during bonding, compared to when the coating layer is dried. This may adversely affect the stability of the semiconductor device during repeated use. Furthermore, if a paste contains a strong reducing agent such as diethylene glycol, reduction may progress during storage, making the paste unusable as a bonding material.

[0070] In one preferred embodiment of the present disclosure, it is preferable that the paste does not contain a reducing agent. "No reducing agent in the paste" means that no reducing agent is intentionally added to the paste, and even if a reducing agent is mixed in, the amount is 1% by mass or less, preferably 0.5% by mass or less. The reducing agent is considered to be an organic substance having reducing properties, and in the present disclosure, is a polyhydric alcohol or an organic acid. Examples of polyhydric alcohols include ethylene glycol, diethylene glycol, glycerin, 2,5-dimethyl-2,5-hexanediol, 2,2-dimethyl-1,3-propanediol, 1,6-hexanediol, 1,2,6-hexanetriol, and 1,10-decanediol. Examples of organic acids include saturated fatty acids such as butanoic acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid, tetradecanoic acid, pentadecanoic acid, hexadecanoic acid, heptadecanoic acid, octadecanoic acid, and nonanedecanoic acid.

[0071] On the other hand, in the present disclosure, since the silver oxide has a nano-sized flake shape, unlike the reduction reaction of general silver oxide described above, it has been found to undergo the following process: (1) reduction of silver oxide → (2) precipitation of nano Ag → (3) sintering of nano Ag → (4) grain growth (bonding; Ag sintering and grain growth). The precipitation of nano Ag during reduction allows for the sintering of Ag particles to proceed, even at low temperatures below 250°C, resulting in high bonding strength. In one preferred embodiment of the present disclosure, a proton-based additive is preferably used instead of a known reducing agent for silver oxide. While the use of a proton-based additive facilitates the reduction reaction of silver oxide, the reduction reaction proceeds much more slowly than when using a reducing agent. This allows the paste to be heated and dried, and the dried coating layer can be used to bond to a chip, etc. This reduces the likelihood of voids occurring within the bonding layer.

[0072] As described above, it is preferable that the paste further contains a proton-based additive. This facilitates the reduction reaction of silver oxide even without the addition of a reducing agent, thereby reducing the amount of unreduced silver oxide in the bonding layer. Even if a small amount of unreduced silver oxide is present in the bonding layer, it does not significantly affect the bonding strength, but it may have a negative effect on thermal conduction and electrical conductivity. Furthermore, since the paste can be heated and dried, the dried coating layer can be used to bond to a chip or the like, making it less likely that voids will form in the bonding layer.

[0073] An example of the reduction reaction of silver oxide when a proton-based additive is used will be described below. For example, when water is used as the proton-based additive and diethylene glycol monobutyl ether (butyl carbitol) is used as the dispersion medium, the reduction reaction of silver oxide is expected to proceed as follows. In this way, the presence of a proton-based additive such as water is expected to make the reduction reaction of silver oxide more likely to proceed.

[0074] As described above, in the present disclosure, a compound having an ethylene- or propylene-based glycol ether skeleton is preferably used as the dispersion medium used in the paste. By using a dispersion medium (a compound having an ethylene- or propylene-based glycol ether skeleton) together with a proton-based additive, the aldehyde generated from the glycol ether during the reaction is oxidized and releases electrons, which tends to cause the reduction reaction of silver oxide to proceed at a more moderate rate.

[0075] The proton-based additive is not particularly limited as long as it can release a proton, and various proton-based additives can be used. Examples of such proton-based additives include water, monohydric alcohols such as methanol and ethanol, and aqueous hydrogen peroxide. These may be used alone or in combination of two or more. Of these, water is preferred. The proton-based additive may be used in an amount of, for example, 0.5 to 10% by mass, preferably 1 to 7% by mass, and more preferably 3 to 6% by mass, based on the mass of the total composition.

[0076] For example, when a composition is obtained by using water as a dispersion medium in producing flake-shaped silver oxide particles, separating a slurry containing flake-shaped silver oxide particles obtained by bead milling into a solid content and a supernatant by centrifugation, removing the supernatant, and adding a water-containing dispersion medium to the obtained solid content again to disperse the solid content, water, which is a proton-based additive, is included in the composition.Furthermore, when a composition is obtained by using water as a dispersion medium in producing the above-mentioned silver oxide particles, separating a slurry containing flake-shaped silver oxide particles obtained by bead milling into a solid content and a supernatant by centrifugation, removing the supernatant, and adding a dispersion medium different from that used in production again to the obtained solid content to replace the dispersion medium, and dispersing the solid content in a dispersion medium different from that used in production, complete replacement of the dispersion medium in the original slurry is difficult, so water, which is a proton-based additive, is included in the composition. On the other hand, when a composition is obtained as a uniform dispersion by mixing a dispersion medium and a dispersant with the silver oxide powder obtained by drying the above-mentioned slurry and stirring the mixture, the dispersion medium in the original slurry is removed, and therefore, if the proton-based additive is not contained in the dispersion medium or dispersant for the paste, it is preferable to add a predetermined amount of the proton-based additive.

[0077] The above composition may contain other optional components as long as the various performance properties of the composition are not impaired. For example, by using known plasticizers (polyethylene glycol (PEG), dibutyl phthalate, butyl benzyl phthalate, etc.), it is possible to more easily reduce the occurrence of cracks and peeling that occur during the reduction of silver oxide or paste drying in flake-shaped silver oxide particles having a D50 of less than 200 nm. In addition to the above, the composition may contain various fillers, known reducing agents, etc. as long as the various performance properties of the composition are not impaired. These may be used alone or in combination of two or more.

[0078] The total amount of the flake-shaped silver oxide particles, dispersant, and dispersion medium relative to the total mass of the composition is preferably 90% by mass or more, more preferably 95% by mass or more. This tends to result in better bonding strength even when bonding at low temperatures. The total amount of the flake-shaped silver oxide particles, dispersant, dispersion medium, and proton-based additive relative to the total mass of the composition is preferably 90% by mass or more, more preferably 95% by mass or more. This tends to result in better bonding strength even when bonding at low temperatures, and also tends to facilitate the reduction reaction of silver oxide.

[0079] The composition described above is suitable for use in bonding because it can provide good bonding strength even at low temperatures. That is, the composition described above is preferably a bonding composition.

[0080] (Bonding Method Using Silver Oxide Paste, Semiconductor Device Manufacturing Method) The composition (preferably a bonding composition) obtained in this manner is applied to a substrate 1 as shown in FIG. 1 and then dried by heating to form a bonding layer 3. A semiconductor chip 2 is placed on the bonding layer 3. The substrate 1 and the semiconductor chip 2 are then treated at a predetermined temperature under atmospheric pressure or pressure with the bonding layer 3 sandwiched therebetween, thereby achieving bonding between the bonded objects. In the present disclosure, after applying the composition to the first substrate, it is preferable to dry the composition layer before placing a semiconductor chip or the like as a second substrate. This can reduce voids in the bonding layer. Furthermore, only when good bonding is possible, after applying the composition, the composition layer may be heated and pressurized without drying while sandwiched between the substrate 1 and the semiconductor chip 2. Although the following description will be given using FIG. 1 , any other substrate or a substrate to which the semiconductor chip 2 is bonded may be used as the second substrate instead of the semiconductor chip 2. Similarly, instead of the substrate 1 which is a semiconductor substrate, any other substrate may be used as the first substrate, or a substrate to which the semiconductor chip 2 is bonded, or the like.

[0081] The composition can be painted or coated onto the substrate 1 by various printing methods. Suitable examples of such printing methods include screen printing, dispense coating, and applicator coating. The amount of the composition used is preferably such that the thickness after drying is, for example, 10 to 100 μm, preferably 20 to 50 μm.

[0082] The composition may be dried at a temperature at which the flake-shaped silver oxide particles are reduced but not exceeding the temperature at which bonding is complete, for example, 80 to 150°C, preferably 100 to 120°C. Furthermore, in the case of a paste containing the aforementioned proton-based additive, a sudden and temporary heat generation occurs within the temperature range of 100 to 150°C, accelerating the reduction reaction. Because this heat generation causes the dispersion medium to volatilize, the drying temperature may be set to the temperature at which the reduction reaction occurs. Specifically, for example, 100 to 150°C is preferred, and 100 to 120°C may also be used. The drying time varies depending on the drying temperature used, but is generally 10 minutes to 1 hour, and may be in the range of 20 to 40 minutes. When the bonding layer 3 is formed by drying the composition layer, at least a portion of the silver oxide in the bonding layer 3 has been reduced to silver, and most of the dispersion medium has been removed. Furthermore, some unreduced silver oxide may remain as long as it can be reduced by the time bonding is completed, or some dispersion medium may remain as long as it can be removed by the time bonding is completed. It has also been found that when cracks or peeling occur in the bonding layer 3, voids caused by the cracks or unbonded portions caused by peeling tend to remain in the bonding layer after bonding. This is thought to be due to the low bonding temperature and low pressure used during semiconductor device manufacturing. Therefore, it is preferable to suppress cracks and peeling in the bonding layer 3 in order to prevent cracks and peeling from occurring in the bonding layer.

[0083] As the substrate, various substrates conventionally used in the manufacture of semiconductor devices and power modules can be used. Suitable examples of such substrates include copper substrates, alumina, silicon nitride, aluminum nitride substrates, ceramic substrates, and various other heat dissipation substrates. As the semiconductor chip, various semiconductor chips conventionally employed can be used. Examples of such semiconductor chips include Si semiconductor chips, SiC semiconductor chips, GaN semiconductor chips, Ga 2 O 3 Suitable examples include semiconductor chips used in power semiconductors, and among these, SiC semiconductor chips are preferred.

[0084] The bonding pressure can be appropriately set within the range required for manufacturing power semiconductor devices. In particular, the silver oxide powder of the present disclosure has excellent bonding properties, so it can provide good bonding strength even at lower pressures and temperatures. The bonding pressure can be, for example, 0 to 30 MPa or 0 to 10 MPa, and is preferably approximately 0 to 5 MPa, and more preferably 0.5 to 5 MPa.

[0085] The bonding temperature can be appropriately selected from the range required for manufacturing power semiconductor devices. The bonding temperature may be, for example, 300°C or less, preferably 250°C or less, more preferably 230°C or less, and even more preferably 210°C or less. In the present disclosure, excellent bonding strength can be obtained even in a low temperature range close to 230°C. The lower limit is not particularly limited as long as it is a temperature at which silver can be sintered, but it may be, for example, higher than the drying temperature, preferably 160°C or more, more preferably 180°C or more.

[0086] The resulting bonding layer is composed of metallic silver formed by reducing silver oxide. By using the composition (preferably a bonding composition) of the present disclosure, it is possible to achieve a bonding strength of 30 MPa or more. It has also been found that the use of the silver oxide powder of the present disclosure can suppress the occurrence of localized voids in the bonding layer.

[0087] (Methods for Measuring Various Properties) (1) Measurement of Average Long Diameter The composition prepared above was diluted 1000 times with butyl carbitol, and 1 ml of the resulting diluted solution was applied to a smooth glass substrate (20 × 20 mm) by spin coating (2000 rpm), followed by vacuum drying at room temperature to obtain a deposit of flake-shaped silver oxide particles. When the flake-shaped silver oxide particles are applied to a glass substrate or the like, they are deposited with the flat portions of the flakes oriented vertically due to their shape. Next, the deposit was observed from above using a scanning electron microscope (SU-8220 manufactured by Hitachi High-Technologies Corporation), and the long diameters of 20 randomly selected particles were measured. The average value was calculated from the obtained values, and this was taken as the average long diameter of the flake-shaped silver oxide particles. Here, the longest diagonal line when observing the particles from above was taken as the long diameter of the particles. (2) Measurement of Average Thickness 1 ml of the composition prepared above was applied by screen printing to a smooth glass substrate (20 × 20 mm) and vacuum dried at room temperature to obtain a deposit of flake-shaped silver oxide particles. The glass substrate was then cut at a position including the formed deposit to obtain a sample that could be observed from the cross-sectional direction of the flake-shaped silver oxide particles. Next, using a scanning electron microscope (SU-8220 manufactured by Hitachi High-Technologies Corporation), the thicknesses of 20 particles randomly selected from the deposit on the cross section were measured, and the average value was calculated from the obtained values, which was used as the average thickness of the flake-shaped silver oxide particles. Here, the distance between the top and bottom surfaces of the central part of each particle was taken as the particle thickness.

[0088] (3) Measurement of D50 The D50 value means the median diameter (center value) when each particle is considered to be a sphere (based on the scattering intensity in the dynamic light scattering method), and is a statistical value where half of the particles in the flake-shaped silver oxide particles or the entire silver oxide powder containing them lie above this value, and the remaining half lie below this value. The D50 value is measured by diluting the composition prepared above 1000 times with butyl carbitol and measuring the resulting diluted solution using a dynamic light scattering measuring instrument (Zetasizer Nano ZS, manufactured by Malvern Panalytical).

[0089] (4) Powder X-ray Diffraction (XRD) Measurement The slurry prepared above was centrifuged (centrifugal force 20,000 × g) to separate it into a solid fraction and a supernatant. After removing the supernatant, the resulting solid fraction was vacuum-dried at room temperature to obtain a dried powder of the silver oxide powder of the present disclosure. The diffraction peaks of this dried powder were measured using a powder XRD measurement device (MINIFLEX 600 manufactured by Rigaku Corporation). The data for the main peak (32°) of the (111) plane of the flake-shaped silver oxide particles were fitted to the obtained diffraction peaks using a pseudo-Voigt function to calculate the half-width.

[0090] (5) Cross-sectional observation of the bonded body The bonded body is embedded in a two-component curing epoxy resin, cut after curing, and the cut surface is optically polished to prepare a sample for observing the bonded cross section. Next, the processed sample is subjected to cross-sectional observation using a scanning electron microscope (SU-8220 manufactured by Hitachi High-Technologies Corporation). The occurrence of cracks in the bonding layer is evaluated using ×, △, or ○, where × indicates that serious cracks are observed, △ indicates that the cracks are not serious but may reduce the bonding strength or affect the bonding stability, and ○ indicates that no cracks are observed.

[0091] (6) Confirmation of dispersant The slurry prepared above was centrifuged (centrifugal force 20,000 × g) to separate it into a solid fraction and a supernatant. After removing the supernatant, the solid fraction was vacuum-dried at room temperature to obtain a dried powder of silver oxide powder containing flake-shaped silver oxide particles. This dried powder was analyzed using a differential thermogravimetry / differential thermal analyzer (TG-DTA; Thermoplus TG8120, manufactured by Rigaku), and the content of the dispersant used (adhered to the silver oxide) was calculated from the mass loss rate.

[0092] The present disclosure will be described in further detail below with reference to examples and comparative examples, but the scope of the present disclosure is not limited by these examples and comparative examples. The following measured values ​​were obtained by the respective measurement methods described above.

[0093] Example 1 - Preparation of flake-shaped silver oxide particles The raw silver oxide particles used as a raw material were micro silver oxide (Silver Oxide PS, manufactured by DOWA Electronics) (spherical in shape, particle size: 10 μm). These raw silver oxide particles and water (dispersion medium) were mixed at a mass ratio of raw silver oxide:water = 10:90, and a dispersant (DISPERBYK-190, manufactured by BYK (a compound having a glycol ether-based skeleton in the main chain and / or side chain)) was added to the raw silver oxide in an amount of 30 mass% based on the raw silver oxide. The mixture was then placed in the grinding chamber of a bead mill (Ultra Apex Mill UAM-015, manufactured by Hiroshima Metal & Machinery) and ground to obtain a slurry containing flake-shaped silver oxide particles. In this grinding process, the beads used were spherical zirconia beads with a diameter of 0.1 mm, and the grinding process time was 200 minutes.

[0094] Preparation of Silver Oxide Paste The slurry containing flake-shaped silver oxide particles obtained in Example 1 was centrifuged (centrifugal force 20,000 × g) to separate the solids and the supernatant. The supernatant was then removed to remove excess dispersant and water. Next, butyl carbitol was added as a dispersion medium to the resulting solids, and the solids were re-dispersed. The mixture was then centrifuged (centrifugal force 20,000 × g) to separate the solids and the supernatant. The supernatant was then removed, and the water in the dispersion was replaced with butyl carbitol. Butyl carbitol was added to the resulting solids to achieve the composition shown in Table 1 below. The mixture was stirred in a planetary centrifugal mixer without a grinding function and then dispersed in a three-roll mill to prepare a silver oxide paste containing flake-shaped silver oxide particles. The moisture content of the silver oxide paste was measured by gas chromatography. The moisture content of the silver oxide paste was 3% by mass.

[0095] Example 2 A silver oxide paste was prepared in the same manner as in Example 1, except that in the production of a slurry containing flake-shaped silver oxide particles, a dispersant (DISPERBYK-190 manufactured by BYK) was added in an amount of 20% by mass relative to the raw silver oxide, and the grinding time was set to 300 minutes. Example 3 A silver oxide paste was prepared in the same manner as in Example 2, except that in the production of a slurry containing flake-shaped silver oxide particles, raw silver oxide and water (dispersion medium) were mixed in a raw silver oxide:water ratio of 40:60 (by weight), and the grinding time was set to 315 minutes. Example 4 A slurry containing flake-shaped silver oxide particles was obtained in the same manner as in Example 2. Next, a silver oxide paste was prepared in the same manner as in Example 1, except that when butyl carbitol was blended with the solid content obtained by centrifugation and solvent substitution, a dispersant was added so that the dispersant content in the paste was 4% by mass.

[0096] Example 5 A silver oxide paste was prepared in the same manner as in Example 4, except that in the production of a slurry containing flake-shaped silver oxide particles, a dispersant was added so that the dispersant content in the paste was 11 mass %.

[0097] Example 6 A slurry containing flake-shaped silver oxide particles was prepared in the same manner as in Example 2. The resulting slurry was then placed in a spray dryer (a mini spray dryer S-300 manufactured by Nippon Buchi Co., Ltd.), and the dispersion medium was evaporated by heating to obtain a dry powder containing flake-shaped silver oxide particles. Butyl carbitol was then blended with the resulting dry powder to achieve the composition shown in Table 1 below. The mixture was stirred using a planetary centrifugal mixer without a grinding function, and then dispersed using a three-roll mill to prepare a silver oxide paste. Gas chromatography analysis of the resulting silver oxide paste revealed no moisture content in the silver oxide paste. Example 7 A silver oxide paste was prepared in the same manner as in Example 6, except that water was blended with butyl carbitol in addition to the resulting dry powder to achieve the composition shown in Table 1 below. Gas chromatography analysis of the resulting silver oxide paste revealed that the moisture content in the silver oxide paste was 2% by mass. (Example 8) A silver oxide paste was prepared in the same manner as in Example 7, except that in the production of a slurry containing flake-shaped silver oxide particles, water was added so that the water content in the paste was 3.5% by mass. (Example 9) A silver oxide paste was prepared in the same manner as in Example 8, except that in the production of a slurry containing flake-shaped silver oxide particles, water was added so that the water content in the paste was 5% by mass. (Example 10) A silver oxide paste was prepared in the same manner as in Example 8, except that in the production of a slurry containing flake-shaped silver oxide particles, water was added so that the water content in the paste was 7% by mass.

[0098] Example 11 A silver oxide paste was prepared in the same manner as in Example 2, except that in the production of a slurry containing flake-shaped silver oxide particles, a dispersant (DISPERBYK-190 manufactured by BYK) was added in an amount of 20 mass% relative to the raw silver oxide, and the grinding time was set to 360 minutes. Example 12 A silver oxide paste was prepared in the same manner as in Example 1, except that in the production of a slurry containing flake-shaped silver oxide particles, a dispersant manufactured by BYK (a compound having a glycol ether-based skeleton in the main chain and / or side chain) was used, and the grinding time was set to 270 minutes. Example 13 A silver oxide paste was prepared in the same manner as in Example 1, except that in the production of a slurry containing flake-shaped silver oxide particles, a dispersant manufactured by BYK (a compound having a glycol ether-based skeleton in the main chain and / or side chain) was used, and the grinding time was set to 160 minutes.

[0099] Example 14 - Preparation of flake-shaped silver oxide particles The silver oxide particles used as a raw material were micro silver oxide (Silver Oxide PS, manufactured by DOWA Electronics) (spherical in shape, particle size: 10 μm). These raw silver oxide particles and water (dispersion liquid) were mixed at a mass ratio of raw silver oxide:water = 10:90, and a dispersant (DISPERBYK-190, manufactured by BYK-Chemie) was added to the mixture so that the mass ratio was 30% relative to the raw silver oxide. The mixture was then placed in the grinding chamber of a bead mill (Ultra Apex Mill UAM-015, manufactured by Hiroshima Metal & Machinery). The grinding process was carried out twice to obtain a slurry containing flake-shaped silver oxide powder. The processing conditions were as follows: In the first grinding process, the beads were spherical and made of zirconia (material), with a diameter of 0.1 mm, and the grinding process time was 360 minutes. In the second crushing treatment, the beads were spherical and made of zirconia (material), with a diameter of 0.05 mm, and the crushing treatment time was 30 minutes.

[0100] Preparation of Silver Oxide Paste The slurry containing flake-shaped silver oxide particles obtained in Example 14 was centrifuged (centrifugal force 20,000 × g) to separate the solids and the supernatant, and the supernatant was removed to remove excess dispersant and water. Next, butyl carbitol was added as a dispersion medium to the obtained solids, and the solids were re-dispersed. Then, the mixture was centrifuged (centrifugal force 20,000 × g) to separate the solids and the supernatant, and the supernatant was removed. The water in the dispersion was replaced with butyl carbitol. The obtained solids were blended with butyl carbitol and polyethylene glycol (PEG 400) as a plasticizer to obtain the composition shown in Table 1 below. The mixture was stirred in a planetary centrifugal mixer and then dispersed in a three-roll mill to prepare a silver oxide paste containing flake-shaped silver oxide particles.

[0101] (Example 15) A silver oxide paste was prepared in the same manner as in Example 7, except that in the production of a slurry containing flake-shaped silver oxide particles, a dispersant (DISPERBYK-190 manufactured by BYK) was added in an amount of 50 mass% relative to the raw silver oxide, and the grinding time of the second grinding treatment was set to 150 minutes. (Example 16) - Preparation of flake-shaped silver oxide particles A slurry containing flake-shaped silver oxide particles was obtained in the same manner as in Example 2 in the production of a slurry containing flake-shaped silver oxide particles. - Preparation of silver oxide paste The slurry containing flake-shaped silver oxide particles obtained in Example 16 was centrifuged (centrifugal force 20,000 × g) to separate it into a solid content and a supernatant, and the supernatant was removed to remove excess dispersant and water. Next, butyl carbitol was added as a dispersion medium to the obtained solids, and the solids were re-dispersed. The mixture was then centrifuged (centrifugal force: 20,000 x g) to separate the solids and the supernatant, and the supernatant was removed. The water in the dispersion was then replaced with butyl carbitol. To further remove residual moisture from the obtained solids, butyl carbitol was added, the solids were re-dispersed, and the mixture was then centrifuged (centrifugal force: 20,000 x g) to separate the solids and the supernatant, and the supernatant was removed. Butyl carbitol was added to the obtained solids to obtain the composition shown in Table 1 below. The mixture was stirred in a planetary centrifugal mixer without a grinding function and then dispersed in a three-roll mill to prepare a silver oxide paste containing flake-shaped silver oxide particles. The moisture content of the silver oxide paste was measured by gas chromatography, and was found to be 1.7% by mass. (Example 17) A silver oxide paste was prepared in the same manner as in Example 16, except that in preparing a paste as a bonding composition, solvent substitution with butyl carbitol was repeated a total of three times for the purpose of removing residual moisture from the solid content. The moisture content in the silver oxide paste was measured by gas chromatography and was found to be 0.8% by mass.

[0102] Comparative Example 1 A silver oxide paste was prepared in the same manner as in Example 1, except that in the production of a slurry containing flake-shaped silver oxide particles, a dispersant (DISPERBYK-190 manufactured by BYK-Chemie) was added in an amount of 20 mass % relative to the raw material silver oxide, and the grinding time was set to 60 minutes.

[0103] Comparative Example 2 Commercially available submicron-sized silver oxide particles (see Figure 3 for shape) were used as the silver oxide particles. Silver oxide particles were mixed with water at a mass ratio of 10:90, and a dispersant (DISPERBYK-190 manufactured by BYK) was added to the mixture at a concentration of 30% by mass relative to the silver oxide particles. Ultrasonic treatment was then performed for 280 minutes to obtain a slurry in which the silver oxide particles were uniformly dispersed. The slurry was first centrifuged (centrifugal force: 20,000 x g) to separate the solids from the supernatant, and the supernatant was removed, thereby removing excess dispersant and water. Electron micrographs of the silver oxide particles contained in the slurry showed that the initial aggregates shown in Figure 3 had only partially disintegrated, and all particles were spherical. Butyl carbitol was added as a dispersion medium to the obtained solids, and the solids were dispersed again. The solids were then centrifuged to separate the solids from the supernatant, and the supernatant was removed, thereby replacing the remaining water with butyl carbitol. Butyl carbitol was added as a dispersion medium to the obtained solids so as to obtain the composition shown in Table 1 below. The mixture was stirred with a planetary centrifugal mixer and then dispersed with a three-roll mill to prepare a paste.

[0104] Comparative Example 3: Commercially available submicron-sized silver oxide particles (see FIG. 3) were used as the silver oxide particles. The silver oxide particles were mixed with water at a mass ratio of 10:90, and a dispersant (DISPERBYK-190 manufactured by BYK) was added to the mixture at a mass ratio of 30% relative to the silver oxide particles. The mixture was dispersed for 5 minutes using a paint shaker (V-type manufactured by Asada Iron Works Co., Ltd.) to partially disintegrate the silver oxide particle aggregates and obtain a slurry in which the silver oxide particles were uniformly dispersed. The dispersion treatment involved 5 minutes of spheres made of zirconia (material), each with a diameter of 0.3 mm. The slurry was first centrifuged (centrifugal force 20,000 × g) to separate the solids from the supernatant, and the supernatant was removed, thereby removing excess dispersant and water. When an electron microscope photograph of the silver oxide particles contained in the slurry was observed, the initial agglomeration state shown in Figure 3 had been broken down, and all spherical particles were observed. Butyl carbitol was added as a dispersion medium to the obtained solid content, and the solid content was dispersed again. The solid content was then separated from the supernatant by centrifugation, and the supernatant was removed, thereby replacing the remaining water with butyl carbitol. Butyl carbitol was added as a dispersion medium to the obtained solid content so as to obtain the composition shown in Table 1 below. The mixture was stirred in a planetary centrifugal mixer and then dispersed in a three-roll mill to prepare a paste.

[0105] Comparative Example 4 A paste was prepared in the same manner as in Comparative Example 3, except that in the production of a slurry containing silver oxide particles, the time of dispersion treatment in a paint shaker was changed to 15 minutes. Furthermore, when the silver oxide particles contained in the obtained slurry were observed under an electron microscope, the initial agglomerated state shown in Figure 3 had only slightly disintegrated, and all particles were observed to be spherical.

[0106] Comparative Example 5 A paste was prepared in the same manner as in Comparative Example 3, except that in the production of a slurry containing silver oxide particles, the time of dispersion treatment in a paint shaker was changed to 30 minutes. Furthermore, when the silver oxide particles contained in the obtained slurry were observed under an electron microscope, the initial agglomerated state shown in Figure 3 had only slightly disintegrated, and all particles were observed to be spherical.

[0107] Comparative Examples 6 and 7 Flake-shaped silver particles (average major axis: 6000 nm, average thickness: 100 nm) manufactured by Fukuda Metal Co., Ltd. and butyl carbitol were mixed in a mass ratio of 90:10 to prepare a paste.

[0108] A bonding test was performed on the pastes of the examples and comparative examples obtained above using the following method. As shown in Figure 1, a Cu substrate (with an Ag-plated outermost layer, surface dimensions of 20 x 20 mm, and thickness of 3 mm) with Ni-Ag plating was prepared. The pastes of the examples and comparative examples were applied to the Ag-plated layer by screen printing, and the substrate was heated at 100°C for 30 minutes to remove the dispersion medium. No visible cracks or peeling occurred in the dried bonding layer. Next, a Si chip (with an Ag-sputtered outermost layer, surface dimensions of 3 x 3 mm, and thickness of 625 μm) was placed on the dried bonding layer so that the Ag-sputtered layer was in contact with it. Pressure (1.5 MPa) and heating (set temperature 250°C) were applied from above for 4 minutes, and the Si chip and the Cu substrate were bonded using the bonding layer as a bonding layer.

[0109] (Cross-section observation) The bonded bodies obtained in Examples 3 and 11 and Comparative Examples 6 and 7 were subjected to cross-section observation by the method described above in the section "Regarding measurement methods for various properties." Cross-sectional photographs of the bonding layers in Example 3 and Comparative Example 6 are shown in FIG. 4. Furthermore, the bonded body obtained in Example 3 was subjected to cross-sectional observation by the method described above in the section "Regarding measurement methods for various properties." A cross-sectional photograph of the bonding layer in Example 3 is shown in FIG. 5.

[0110] (Bonding Strength Test) The resulting bonded body was subjected to a die shear test (shear) using a bond tester (DAGE 4000 Plus manufactured by DAGE Japan) to determine the bonding strength.

[0111] (Post-bonding reduction property) The color of the peeled surface of the bonded body after shear peeling in the above-mentioned bonding strength test was visually observed. Black areas were judged to be areas where silver oxide remained and there were unreduced parts, and silvery-white areas were judged to be areas where silver oxide had been reduced to silver. The post-bonding reduction property was evaluated with x or ◯, where x was judged to be the case where even a part of the peeled surface was black, and ◯ was judged to be the case where the entire peeled surface was silvery-white.

[0112] The properties of the silver oxide particles or metallic silver particles used in the examples and comparative examples and the compositions of the pastes containing them are shown in Table 1 below. Furthermore, the bonding strength, post-bonding reducibility, crack evaluation, and findings during bonding for the pastes obtained in this manner are also shown in Table 1 below. Note that the "BC content" in Table 1 refers to the content of diethylene glycol monobutyl ether.

[0113]

[0114] Table 1 shows that bonding between bonded objects using the silver oxide paste of the present disclosure results in an excellent bonding strength of 30 MPa or more. Furthermore, cross-sectional photographs of the bonding layer reveal that no cracks occur. On the other hand, as shown in Comparative Example 1, when the pulverization time is short in the preparation of the flake-shaped silver oxide particles used, the D50 of the flake-shaped silver oxide particles increases, and the use of a paste containing such flake-shaped silver oxide particles results in low bonding strength. Furthermore, when bonding is performed using a paste containing spherical silver oxide particles used in Comparative Examples 2 to 5, even when the D50 falls within the range of the present disclosure, the bonding strength is significantly lower, at 20 MPa or less, compared to the examples of the present disclosure. Furthermore, observation of the peeled surface after the bonding strength test revealed that unreduced silver oxide remained.

[0115] Furthermore, Example 6, which did not contain water, had high bonding strength, but some unreduced silver oxide remained on the peeled surface after the bonding strength test, resulting in low reducibility. Furthermore, as shown in Comparative Examples 6 and 7, when bonding was performed using a paste containing commercially available flaky silver particles, the commercially available flaky silver particles had an average major axis of 6000 nm, which is micron-sized. As a result, local voids occurred at the bonding interface and within the bonding layer. The occurrence of local voids makes the bonding layer uneven, which tends to result in poor bonding stability. The mechanism by which these voids occurred is unknown, but it is presumed that they were due to the overlap of large-area flaky silver particles, and that the voids could not be eliminated at temperatures as low as 250 °C.

[0116] As described above, the silver oxide paste of the present disclosure is useful for bonding a semiconductor substrate and a semiconductor chip with good bonding strength (without generating cracks).

[0117] 1. Substrate 2. Semiconductor chip 3. Bonding layer containing flake-shaped silver oxide particles of the present disclosure

Claims

1. Flake-shaped silver oxide particles or a silver oxide powder containing the same, characterized in that the flake-shaped silver oxide particles have an average thickness of 1 to 100 nm and a D50 of 100 to 350 nm.

2. The flake-shaped silver oxide particles according to claim 1, or a silver oxide powder containing the same, wherein the average major axis of the flake-shaped silver oxide particles is 300 to 1,000 nm.

3. The flake-shaped silver oxide particles according to claim 1, or a silver oxide powder containing the same, wherein in an X-ray diffraction spectrum of the flake-shaped silver oxide particles, the half-value width of a diffraction peak derived from a (111) plane is 0.80 or more.

4. The flake-shaped silver oxide particles according to claim 1, or a silver oxide powder containing the same, wherein the surface of at least a portion of the flake-shaped silver oxide particles has a compound having a glycol ether skeleton in the main chain and / or side chain.

5. A bonding composition comprising: the flake-shaped silver oxide particles according to any one of claims 1 to 4 or a silver oxide powder containing the same; a dispersant; and a dispersion medium.

6. The bonding composition according to claim 5, wherein the dispersant is a compound having a glycol ether skeleton in the main chain and / or the side chain.

7. The bonding composition according to claim 5, wherein the dispersion medium is a compound having an ethylene-based or propylene-based glycol ether skeleton.

8. A method for producing flake-shaped silver oxide particles or silver oxide powder containing the same according to claim 1, comprising crushing the silver oxide particles using a bead mill.

9. A method for producing flake-shaped silver oxide particles or a silver oxide powder containing the same according to claim 8, wherein the bead mill grinding comprises the following steps: a step of supplying the silver oxide particles, the dispersant, and the dispersion medium to a device for bead mill grinding; and a step of performing bead mill grinding in the device to obtain a slurry containing flake-shaped silver oxide particles.

10. A method for producing flake-shaped silver oxide particles or silver oxide powder containing the same, as described in claim 8 or 9, wherein the dispersant is a compound having a glycol ether skeleton in the main chain and / or side chain.

11. A method for manufacturing a semiconductor device, comprising the steps of: (1) applying the bonding composition according to claim 5 onto a semiconductor substrate to form a layer of the bonding composition; (2) placing a semiconductor chip on the layer of the bonding composition to form a laminate; and (3) heating the resulting laminate at 300°C or less while applying pressure of 0 to 30 MPa to integrate the laminate.

12. The method for producing a semiconductor device according to claim 11, further comprising the step of drying the layer of bonding composition between steps (1) and (2).

13. The method for producing a semiconductor device according to claim 11, wherein the semiconductor chip is a SiC semiconductor chip.

14. A silver oxide paste comprising: flake-shaped silver oxide particles; a dispersant; and a dispersion medium, wherein the silver oxide particles have an average thickness of 1 to 100 nm and a D50 of 100 to 350 nm.

15. The silver oxide paste of claim 14, further comprising a proton additive.

16. The silver oxide paste according to claim 14, wherein the dispersant is a compound having a glycol ether skeleton in the main chain and / or side chain.

17. The silver oxide paste according to claim 14, wherein the dispersion medium is a compound having an ethylene-based or propylene-based glycol ether skeleton.

18. The silver oxide paste according to claim 14, wherein the average major axis of the silver oxide particles is 300 to 1,000 nm.

19. The silver oxide paste according to claim 14, wherein in the X-ray diffraction spectrum of the silver oxide particles, the half-value width of the diffraction peak derived from the (111) plane is 0.80 or more.

20. The silver oxide paste according to claim 14, wherein the content of the dispersant is 12 mass% or less based on the mass of the entire silver oxide paste.

21. The silver oxide paste according to claim 15, wherein the content of the proton-based additive is 0.5 to 10 mass % based on the total mass of the silver oxide paste.

22. The silver oxide paste according to claim 14, for use in joining applications.

23. A method for manufacturing a semiconductor device, comprising: (1) a step of applying a silver oxide paste according to any one of claims 14 to 22 onto a first substrate to form a layer of the silver oxide paste; (2) a step of placing a second substrate on the layer of silver oxide paste to form a laminate; and (3) a step of heating the obtained laminate at 300°C or less while applying pressure of 0 to 30 MPa to integrate the laminate.

24. The method for producing a semiconductor device according to claim 23, further comprising the step of drying the layer of silver oxide paste between steps (1) and (2).

25. The method of claim 23, wherein the second substrate is a semiconductor chip.