Slurry homogenization process and use thereof

MYPI2025005811A0Undetermined Publication Date: 2024-10-27EVE POWER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005811
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2023-12-07
Publication Date
2024-10-27

AI Technical Summary

Technical Problem

The traditional lithium-ion battery cathode homogenization process has problems such as large equipment footprint, high energy consumption, high noise, high investment, high maintenance costs, cumbersome process steps, poor slurry uniformity, and low solid content, making it difficult to effectively improve the fineness of the slurry. degree and solid content.

Method used

A new homogenization process is adopted, which includes premixing the main material, the first conductive agent and the binder, adding the first solvent for dispersion, and then adding the conductive slurry for premixing and dispersion, combined with the degassing and cooling step to optimize The mixing and dispersing process of slurry.

Benefits of technology

It simplifies the pulping process, shortens the pulping time of a single batch, and improves the fineness, fluidity and solid content of the slurry. The solid content is increased from 55% to 60%, saving solvents and manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005811_DRAWING_001
    Figure PI2025005811_DRAWING_001
  • Figure PI2025005811_DRAWING_002
    Figure PI2025005811_DRAWING_002
Patent Text Reader

Abstract

ABSTRACT SLURRY HOMOGENIZATION PROCESS AND USE THEREOF A slurry homogenization process and a use thereof, including the following steps: performing a first pre-mixing on a main material, a first conductive agent, and a binder to obtain a first mixture, while performing a second mixing on a first solvent independently; adding the first mixture into the first solvent, and sequentially performing a second pre-mixing and a first dispersing to obtain a third mixture; and adding a conductive slurry into the third mixture, sequentially performing a third pre-mixing and a second dispersing, and defoaming and cooling to obtain a homogenized slurry. FIG. 1
Need to check novelty before this filing date? Find Prior Art

Description

A homogenization process and its application

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 27, 2023, with application number 202310470925.1. The entire contents of the above application are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of lithium-ion batteries, for example, to a homogenization process and its application. Background Art

[0003] In the related art, the lithium-ion battery positive electrode homogenization process generally adopts a double planetary stirring process, which is further divided into a dry homogenization process or a prefabricated gel wet process. The above methods have the following main disadvantages: (1) The double planetary equipment occupies a large area. Under the same production capacity, 3 sets or more of equipment are required to meet the production capacity requirements; (2) The equipment has high energy consumption. The equipment requires a high-power explosion-proof motor to drive the stirring paddle and dispersion wheel, and the equipment generates a lot of noise during operation; (3) The equipment investment and subsequent maintenance costs are high; (4) Using double planetary equipment, running a dry process or a prefabricated gel wet process: It generally takes 4-7 hours to complete a single batch of finished slurry, and the process steps are cumbersome and inefficient; (5) The slurry obtained by the traditional process generally has poor uniformity, and there are tiny particles inside the slurry, which has an adverse effect on the quality of the coated membrane and the membrane resistance. (6) The solid content of the traditional pulping process is as low as about 55%. The solid content of the slurry can be increased by developing a new homogenization process.

[0004] In order to solve the shortcomings of traditional homogenization process and develop new homogenization process, people in this field have conducted a lot of research.

[0005] For example, the binder, conductive agent, and main ingredients are mixed in a mixer at once, and then the solvent is added twice for stirring. However, the two additions of solvent do not have a beneficial effect on the fineness and solid content of the slurry. Therefore, it is necessary to further improve the feeding method to improve the fineness and solid content of the slurry.

[0006] For example, the homogenization process of a lithium-ion positive electrode slurry includes solution preparation, V-type blender stirring, premixing stirring, high-speed stirring, viscosity adjustment and vacuum degassing. However, when using a V-type blender for stirring, the fineness and fluidity of the slurry are difficult to guarantee, and the production cost is too high.

[0007] Therefore, how to develop a new homogenization process that can reduce the operating costs of the enterprise while improving the quality of the slurry is an important research direction in this field. Technical issues

[0008] The present application provides a homogenization process and its application, which can reduce the operating costs of the enterprise and improve the quality of the slurry. Technical Solutions

[0009] In a first aspect, an embodiment of the present application provides a homogenization process, the homogenization process comprising the following steps:

[0010] The main material, the first conductive agent and the binder are pre-mixed to obtain a first mixture, and the first solvent is pre-mixed independently to obtain a second mixture;

[0011] adding the first mixture to the first solvent and sequentially performing a second premixing and a first dispersion to obtain a third mixture;

[0012] Adding conductive paste to the third mixture, performing third premixing and second dispersion in sequence, and degassing and cooling to obtain a homogenous slurry.

[0013] In a second aspect, an embodiment of the present application provides an application of a homogenization process as described in one of the purposes, wherein the homogenization process is applied in the field of lithium-ion batteries. Beneficial effects

[0014] Beneficial effects of the present application: The homogenization process of the present application simplifies the pulping process, and the pulping time of a single batch is shortened to less than 1.3 hours. Through the homogenization process of the present application, the quality of the slurry can be improved, so that the slurry fineness, screening performance and fluidity all meet the process specification requirements. Through the homogenization process of the present application, the solid content of the slurry can be effectively improved, and the solid content of the slurry is increased from 55% to 60%, saving solvent and saving manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] FIG1 is a flow chart of the homogenization process in Examples 1-7 of the present application.

[0016] FIG2 is a flow chart of the homogenization process in Comparative Example 1 of the present application. Modes for Carrying Out the Invention

[0017] Example 1

[0018] This embodiment provides a homogenization process, the flow chart of which is shown in FIG1 :

[0019] (1) According to the formula ratio, a certain amount of main material lithium iron phosphate, conductive agent (SP), conductive paste (multi-walled carbon nanotubes), binder (PVDF), and solvent (NMP) are weighed; the weighed main material, conductive agent, and binder are poured into the premixing bin in the order of main material (48%), conductive agent (2%), binder (2%), and main material (48%), and then premixed for 18 minutes; a certain amount of solvent is added to the circulation tank, and then the solvent is circulated between the pulping machine and the circulation tank through a rotor pump or a screw pump to achieve a stable circulation flow;

[0020] (2) When the solvent circulation flow is stable and the powder premixing is completed, the pulping machine linear speed is set to 24m / s and the circulation tank linear speed is 24m / s; the powder is fed into the pulping machine through the feeding screw and premixed with the solvent for 27min; after the premixing is completed, the pulping machine linear speed is maintained at 24m / s and the dispersion is continued for 22min;

[0021] (3) After the slurry is dispersed, it is temporarily stored in a circulation tank. The last material, a conductive slurry (5% multi-walled carbon nanotubes, 1.5% dispersant, and 93.5% NMP), is added. The conductive slurry accounts for 10% of the slurry in the circulation tank by mass. The mixture is premixed in the circulation tank for 10 minutes at a linear speed of 24 m / s. The slurry is dispersed. The slurry is pumped through a rotor pump or a screw pump to achieve a stable circulation flow between the pulper and the circulation tank. The linear speed of the pulper reaches 24 m / s, and the linear speed of the circulation tank reaches 24 m / s. The dispersion time is 22 minutes. After the dispersion is completed, the slurry is slowly stirred in the circulation tank for vacuum degassing and cooling for 22 minutes to obtain a homogenous slurry. Example 2

[0022] This embodiment provides a homogenization process, the flow chart of which is shown in FIG1 :

[0023] (1) According to the formula ratio, a certain amount of main material lithium iron phosphate, conductive agent (SP), conductive paste (4% multi-walled carbon nanotubes, 1% dispersant and 95% NMP), binder (PVDF), and solvent (NMP) are weighed; the weighed main material, conductive agent, and binder are poured into the premixing bin in the order of main material (40%), conductive agent (4%), binder (6%), and main material (50%), and then premixed for 5 minutes; a certain amount of solvent is added to the circulation tank, and then the solvent is circulated between the pulping machine and the circulation tank through a rotor pump or a screw pump to achieve a stable circulation flow;

[0024] (2) When the solvent circulation flow is stable and the powder premixing is completed, the pulping machine linear speed is set to 30m / s and the circulation tank linear speed is 30m / s; the powder is started to be fed into the pulping machine through the feeding screw and premixed with the solvent for 15 minutes; after the premixing is completed, the pulping machine linear speed is maintained at 30m / s and the dispersion is continued for 15 minutes;

[0025] (3) After the slurry is dispersed, it is temporarily stored in a circulation tank. The last material, a conductive slurry (4% multi-walled carbon nanotubes, 2% dispersant, and 94% NMP), is added. The conductive slurry accounts for 5% of the slurry in the circulation tank by mass. The mixture is premixed in the circulation tank for 5 minutes, with a linear velocity of 30 m / s. The slurry is dispersed. The slurry is pumped through a rotor pump or a screw pump to achieve a stable circulation flow between the pulper and the circulation tank. The linear velocity of the pulper reaches 30 m / s, and the linear velocity of the circulation tank reaches 30 m / s. The dispersion time is 15 minutes. After the dispersion is completed, the slurry is slowly stirred in the circulation tank for 15 minutes to degas and cool under vacuum to obtain a homogenous slurry. Example 3

[0026] This embodiment provides a homogenization process, the flow chart of which is shown in FIG1 :

[0027] (1) According to the formula ratio, a certain amount of main material lithium iron phosphate, conductive agent (SP), conductive paste (6% multi-walled carbon nanotubes, 2% dispersant and 92% NMP), binder (PVDF), and solvent (NMP) are weighed; the weighed main material, conductive agent, and binder are poured into the premixing bin in the order of main material (50%), conductive agent (5%), binder (5%), and main material (40%), and then premixed for 30 minutes; a certain amount of solvent is added to the circulation tank, and then the solvent is circulated between the pulping machine and the circulation tank through a rotor pump or a screw pump to achieve a stable circulation flow;

[0028] (2) When the solvent circulation flow is stable and the powder premixing is completed, the pulping machine linear speed is set to 18m / s and the circulation tank linear speed is 18m / s; the powder is fed into the pulping machine through the feeding screw and premixed with the solvent for 40 minutes; after the premixing is completed, the pulping machine linear speed is maintained at 18m / s and the dispersion is continued for 30 minutes;

[0029] (3) After the slurry is dispersed, it is temporarily stored in a circulation tank. The last material, a conductive slurry (6% multi-walled carbon nanotubes, 1% dispersant, and 93% NMP), is added. The conductive slurry accounts for 60% of the slurry in the circulation tank by mass. The mixture is premixed in the circulation tank for 15 minutes at a linear speed of 18 m / s. The slurry is dispersed. The slurry is pumped through a rotor pump or a screw pump to achieve a stable circulation flow between the pulper and the circulation tank. The linear speed of the pulper reaches 18 m / s, and the linear speed of the circulation tank reaches 18 m / s. The dispersion time is 15 minutes. After the dispersion is completed, the slurry is slowly stirred in the circulation tank for vacuum degassing and cooling for 15 minutes to obtain a homogenous slurry.

[0030] Comparative Example 1

[0031] In this comparative example, except that the order of adding the main material, binder, solvent, conductive agent and conductive paste is replaced with the order shown in FIG2 , other conditions are the same as those in Example 1.

[0032] The homogenates prepared in Examples 1-3 and Comparative Example 1 were tested for solid content, slurry fineness, sieving performance and fluidity. The test results are shown in Table 1.

[0033] The solids content of the homogenate is determined as follows: Weigh 1-2 grams of the homogenate and dry it in a 103°C oven for four hours using an analytical balance. Record the weight of the weighing bottle before weighing (A g), the weight of the homogenate (B g), and the weight after drying (including the sample and weighing bottle) (C g). Calculate (CA) / B × 100% to determine the solids content of the homogenate.

[0034] Table 1

[0035]

[0036] From the above results, it can be concluded that the homogenization process method in the present application effectively increases the solid content of the slurry from about 55% to about 60%, saving solvent and reducing manufacturing costs.

Claims

1. A homogenization process, comprising the following steps: The main material, the first conductive agent and the binder are first premixed to obtain a first mixture, and the first solvent is independently second mixed; adding the first mixture into a first solvent and sequentially performing a second premixing and a first dispersion to obtain a third mixture; Adding conductive paste to the third mixture, performing third premixing and second dispersion in sequence, and degassing and cooling to obtain a homogenous slurry.

2. The homogenization process according to claim 1, wherein: Taking the mass fraction of the first mixture as 100%, the order of adding the main material, the first conductive agent and the binder is to add 40-60% of the main material, the first conductive agent, the binder and 60-40% of the main material in sequence; Preferably, the main material includes lithium iron phosphate; Preferably, the first conductive agent comprises SP; Preferably, the mass fraction of the first conductive agent in the first mixture is 0.2-5% by mass; Preferably, the binder comprises PVDF; Preferably, the mass fraction of the binder in the first mixture is 1.3-6% by mass; Preferably, the first premixing time is 5 to 30 minutes; Preferably, the first premixing is performed in a premixing bin.

3. The homogenization process according to claim 1 or 2, wherein: The first solvent comprises NMP; Preferably, the mass ratio of the first solvent to the first mixture is 1:(1.2-5); Preferably, the second mixing is carried out in a circulation tank and a pulper; Preferably, the second mixing end condition is that the first solvent reaches a stable circulation flow rate between the pulping machine and the circulation tank; Preferably, the flow rate of the second mixture circulating and dispersing between the pulping machine and the circulation tank is set between 50% and 65% of the pulping capacity.

4. The homogenization process according to any one of claims 1 to 3, wherein: The second premixing is carried out in a circulation tank and a pulping machine; Preferably, the linear velocity of the circulation tank in the second premixing is 18-30 m / s; Preferably, the linear speed of the pulping machine in the second premixing is 18-30 m / s; Preferably, the second premixing time is 15 to 40 minutes; Preferably, the flow rate of the second premixed material circulated and dispersed between the pulping machine and the circulation tank is set between 50% and 65% of the pulping capacity.

5. The homogenization process according to any one of claims 1 to 4, wherein: The first dispersion is carried out in a circulation tank and a pulper; Preferably, the linear velocity of the circulation tank in the first dispersion is 18-30 m / s; Preferably, the linear speed of the pulping machine in the first dispersion is 18-30 m / s; Preferably, the first dispersion time is 15 to 30 minutes; Preferably, the flow rate of the first dispersion circulating from the pulping machine to the circulation tank is set between 50% and 65% of the pulping capacity.

6. The homogenization process according to any one of claims 1 to 5, wherein: The mass fraction of the conductive paste in the homogenate is 5-20%; Preferably, based on the mass fraction of the conductive paste being 100%, the conductive paste comprises 4-6% of the second conductive agent, 1-2% of the dispersant and the second solvent; Preferably, the second conductive agent comprises carbon nanotubes; Preferably, the second solvent comprises NMP; Preferably, the third premixing is performed in a circulation tank; Preferably, the linear velocity of the circulation tank in the third premixing is 18-30 m / s; Preferably, the third premixing time is 5 to 15 minutes.

7. The homogenization process according to any one of claims 1 to 6, wherein: The second dispersion is carried out in a pulper and a circulation tank; Preferably, the condition for starting the second dispersion is that the circulation flow of the slurry between the pulping machine and the circulation tank reaches a stable state; Preferably, the flow rate of the second dispersion circulating from the pulping machine to the circulation tank is set between 50% and 65% of the pulping capacity.

8. The homogenization process according to claim 7, wherein: The linear speed of the pulping machine in the second dispersion is 18-30 m / s; Preferably, the linear velocity of the circulation tank in the second dispersion is 18-30 m / s; Preferably, the second dispersion time is 15 to 30 minutes.

9. The homogenization process according to any one of claims 1 to 8, wherein: The degassing and cooling time is 15 to 30 minutes.

10. An application of the homogenization process according to any one of claims 1 to 9, wherein the homogenization process is applied in the field of lithium-ion batteries.