AI Technical Summary
Current sun protection coatings for windows face challenges such as significant color change during thermal annealing, poor mechanical and chemical resistance, and inefficient solar control properties, limiting their market applicability and sustainability.
A glass pane coating comprising a lower high-index dielectric layer, an IR-reflecting titanium carbide (TiC) layer, and an upper high-index dielectric layer, which provides infrared reflection, chemical, and mechanical resistance while minimizing color shift after thermal annealing, and is suitable for both thermally annealed and non-thermally annealed products.
The coating achieves high chemical and mechanical resistance, negligible color change after thermal annealing, and effective solar control with reduced heat radiation, making it cost-effective and environmentally friendly for widespread use in windows.
Smart Images

Figure PI2025005834_DRAWING_001 
Figure PI2025005834_DRAWING_002 
Figure PI2025005834_DRAWING_003
Abstract
Description
[0001] SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT Pane with a titanium carbide coating. The invention relates to a pane with a coating, its production, and its use. Panes with coatings with low light transmission and a functional layer with TiN stacks are known from WO 2018 / 129135 A1, TiN / NiCr(N) stacks from WO 2018 / 129125 A1, and TiN / ITO stacks from US 2018 / 0237336 A1. Nb and NbN functional layers are known from WO 2009 / 112759 A2, WO 01 / 21540 A1, and WO 2021 / 069616 A1. Furthermore, EP 0693574 B2 and JP H11-114704 A disclose tools in which TiC is used to improve the mechanical stability of the tools. Furthermore, CN 105970177 A discloses a solar-selectively absorbing high-temperature coating based on TiC for use in the technical field of solar energy utilization. Accordingly, these disclosures relate to significantly different technical fields than the field of coated panes.Furthermore, the use of TiC stacks in coated substrates is known from EP 3515871 A1 and EP 0 718 250 B2. In these documents, the TiC layer is used as a barrier layer against the diffusion of alkali ions and oxygen, while an IR-reflecting layer based on silver is used. US 2002 / 045073 A1 describes methods for obtaining photoactive coatings and / or anatase crystalline phases of titanium oxides and articles produced therefrom. The article comprises a substrate and a coating, wherein a functional coating can be arranged between the coating and the substrate. The functional coating is intended to modify one or more physical properties of the substrate. This means that the functional coating, if present, is arranged directly on the substrate. SR Reineck et al., Colloque international sur les plasmas et la pulverisation cathodique, Société Française du Vide, Vol.Colloque 4, September 13, 1982, pp. 385-395, describes high-rate sputtering for the production of architectural glass coatings. A glass substrate with a titanium carbide coating is disclosed. However, no lower and upper high-index dielectric layer or layer sequence, nor the thickness of the titanium carbide coating, is described. C.G. Granqvist, "Solar Energy Materials and Solar Cells," Vol. 91, No. 17, 2007, pp. 1529-1598, discloses transparent conductors as solar energy materials. While TiN offers good thermal performance in terms of low emissivity combined with solar control properties, the TiN-containing coating undergoes a drastic color change during thermal annealing, precluding the application of the same coating for thermally annealed and non-thermally annealed products and thus reducing the overall market volume.In comparison, Nb coatings offer little color change after thermal annealing and low emissivity, but poor solar control properties. Conversely, using NbN, solar control properties and little color change after thermal annealing can be achieved, but low emissivity is not achieved with this material. The object of the present invention is to provide a cost-effective and sustainable solar control coating for windows that has high chemical and mechanical resistance and exhibits negligible color shift after thermal annealing. A further object of the invention is to provide an economical and environmentally friendly process for producing a sustainable solar control coating for windows.Finally, it is an object of the present invention to provide a use for the sun protection coating according to the invention for windows. The object of the present invention is achieved according to the invention by a pane according to claim 1, a method according to claim 12 and a use according to claim 14. Preferred embodiments are evident from the subclaims. The pane is intended to separate the interior of a window opening from the exterior environment. The pane according to the invention comprises at least one glass pane and a coating. The glass pane has two surfaces (main surfaces), namely an exterior surface and an interior surface, and a circumferential edge surface between the two main surfaces. The exterior SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT surface refers to the main surface which, in the installed position, faces the exterior environment.The interior-side surface refers to the main surface that faces the interior in the installed position. The coating is applied to said exterior surface or the interior-side surface of the glass pane. The coating is preferably applied to the interior-side surface of the glass pane, as this particularly protects the coating from impairment by mechanical and / or chemical influences from the environment. According to the invention, starting from the glass pane, the coating comprises at least in the following order: - a lower (optically) highly refractive dielectric layer or layer sequence, - an IR-reflecting layer based on titanium carbide (TiC), and - an upper (optically) highly refractive dielectric layer or layer sequence.The major advantage of the present invention is that the pane according to the invention, in addition to its infrared (IR)-reflecting properties, exhibits high chemical and mechanical resistance and, even after possible thermal annealing, shows little color change. The IR-reflecting properties are provided in particular by the IR-reflecting layer based on titanium carbide and relate to the near infrared range, so that the coating acts as a solar control coating and (partially) reflects the IR components of solar radiation. The IR-reflecting properties also relate to thermal radiation in the mid-IR range, so that it also acts as an emissivity-reducing coating (low-E coating) and reduces the radiation of heat from the pane into the interior.Furthermore, it is not susceptible to corrosion, so that it can be used on an exposed surface, which is necessary for emissivity-reducing coatings (exposed surface on the interior side) and is unavoidable anyway with monolithic panes because only exposed surfaces are available. According to the invention, an "exposed surface" refers to an external or exposed surface that forms an interface with the surrounding atmosphere and is accessible and touchable by people. Furthermore, with the coating according to the invention, a light transmission of the pane of 50% or less can be achieved, which is advantageous, for example, for use as a rear window or roof window of a motor vehicle or rail vehicle or as a pane for a building.Furthermore, due to the chemical resistance of titanium carbide, only minimal color change occurs during thermal annealing. Furthermore, since titanium is a common element, titanium carbide can be considered a sustainable material, while also enabling cost-effective production. By using the upper high-index dielectric layer or layer sequence, oxidation of the IR-reflecting titanium carbide-based layer during any thermal treatment, such as thermal annealing, can be further reduced or prevented. The coating is preferably applied over the entire surface so that the entire surface is completely covered by the coating.However, it is also possible for areas of the surface to be uncoated, for example a peripheral edge area or a local uncoated area, which acts as a data transmission window to improve the permeability for electromagnetic radiation (antenna signals). Such a data transmission window may be necessary or helpful to ensure the permeability for electromagnetic radiation (for example antenna signals), which can be attenuated or blocked by the electrically conductive TiC-based layer. Preferably, at least 80% of the surface is covered by the coating, particularly preferably at least 90%. In one embodiment of the invention, the pane is designed as a composite pane. A composite pane comprises an outer pane and an inner pane, which are connected to one another via a thermoplastic intermediate layer.For the purposes of the invention, the inner pane refers to the pane of the composite pane facing the interior. The outer pane refers to the pane facing the outside environment. The glass pane according to the invention with the coating can represent the inner pane or the outer pane of the composite pane. The coating can be located on the outer surface or the interior surface of the glass pane, which is used as the inner pane or as the outer pane. If the glass pane is used as the outer pane of the composite pane, the coating is preferably located on the interior surface of the glass pane, as this protects the coating from impairment by mechanical and / or chemical influences from the environment and also allows lower reflectivities to be achieved.Insofar as the glass pane represents the inner pane of a laminated pane, the SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT coating on both the outer surface and the inner surface of the glass pane is protected from these environmental influences. In one embodiment of the invention, the coating is located on the outer surface of the glass pane which is used as the inner pane of a laminated pane, so that lower reflectivities can be achieved. According to a further embodiment, the coating is arranged on the inner surface of the glass pane when the glass pane is used as the inner pane of a laminated pane, since it thus represents the surface of the laminated pane exposed to the interior and can therefore additionally exert an emissivity-reducing effect.Composite panes can be used, for example, in the automotive sector as so-called laminated safety glass (VSG) or in the building sector as insulating glazing. The pane can, for example, be a rear window or roof window of a motor vehicle or rail vehicle or a pane for a building. In an alternative embodiment of the invention, the pane according to the invention is a monolithic pane which is designed as a single pane of glass. Apart from the glass pane with the coating, no further pane is present. In the case of a single pane of glass, the coating is preferably applied to the interior surface of the glass pane, as this protects the coating from impairment by mechanical and / or chemical influences from the environment. The pane can in particular be used as so-called toughened safety glass (ESG), wherein the glass pane is thermally toughened.The monolithic pane can be, for example, a rear window or roof pane of a motor vehicle or rail vehicle, or a pane for a building. The IR-reflecting layer based on titanium carbide has a layer thickness of 2 nm to 50 nm, preferably 3 nm to 45 nm, particularly preferably 5 nm to 40 nm. This achieves good IR-reflecting properties and a light transmission TL of the pane of 25% or more and 50% or less. Titanium carbide (TiC) is also understood as TiCx, where x is from 0.8 to 1.2, preferably from 0.9 to 1.1, more preferably approximately 1.0. The titanium carbide is therefore preferably deposited essentially stoichiometrically, which corresponds to an atomic ratio of titanium to carbon of approximately 1:1. Titanium carbide exhibits electrical conductivity, which is also responsible for its IR-reflecting effect.The specific electrical resistance of thin layers is generally higher than the tabulated values for the solid state (bulk values). The specific resistance of the inventive IR-reflecting layer based on titanium carbide (SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT) is preferably less than 300 µΩ cm, more preferably less than 250 µΩ cm. The specific resistance depends crucially on the carbon content of the IR-reflecting layer; layer parameters such as density and crystallinity also have an influence. The specific resistance is expressed in the refractive index of the IR-reflecting layer. Strictly speaking, the specific electrical resistance is also referred to as resistivity. Its inverse is the electrical conductivity. The specific resistance can be determined using a commercially available resistance meter.The refractive index (real part of the complex refractive index) of the IR-reflecting layer based on titanium carbide is preferably in the range from 2.3 to 3.4 in a wavelength range from 400 nm to 780 nm or from 2.9 to 6.0 in a wavelength range from 780 nm to 2500 nm, particularly preferably from 2.9 to 3.3 in a wavelength range from 400 nm to 780 nm or from 3.3 to 6.0 in a wavelength range from 780 nm to 2500 nm. The extinction coefficient (imaginary part of the complex refractive index) of the IR-reflecting layer based on titanium carbide is preferably in the range from 2.0 to 3.7 in a wavelength range from 400 nm to 780 nm or from 3.5 to 6.5 in a wavelength range from 780 nm to 2500 nm. nm, particularly preferably from 2.0 to 3.5 in a wavelength range from 400 nm to 780 nm or from 3.7 to 6.5 in a wavelength range from 780 nm to 2500 nm.According to one embodiment, the refractive index (real part of the complex refractive index) of the IR-reflecting layer based on titanium carbide is in the range from 2.4 to 3.0 at a wavelength of 550 nm, more preferably in the range from 2.8 to 3.0 at a wavelength of 550 nm. According to another embodiment, the extinction coefficient (imaginary part of the complex refractive index) of the IR-reflecting layer based on titanium carbide is in the range from 2.7 to 2.9 at a wavelength of 550 nm, more preferably in the range from 2.7 to 2.8 at a wavelength of 550 nm. If a layer of the coating according to the invention is based on a material, the layer consists predominantly of this material, in particular substantially of this material alongside any impurities or dopants. The dielectric materials mentioned (oxides, nitrides) can be deposited stoichiometrically, substoichiometrically, or superstoichiometrically.Therefore, stoichiometric coefficients are omitted when specifying the empirical formulas. The empirical formulas serve merely as abbreviations; they contain no information about stoichiometry. Doping, for example, with aluminum, zirconium, titanium, or boron, can impart a certain degree of electrical conductivity to dielectric materials. However, those skilled in the art will identify them as dielectric layers in terms of their function, as is common in the field of thin films. The material of the dielectric layers preferably has an electrical conductivity (inverse of the resistivity) of less than 10. -4S / m. Unless otherwise stated, the thickness or layer thickness of a layer in the sense of the present invention always refers to the geometric thickness. If reference is made instead to the optical thickness, which results from the geometric thickness and the refractive index, this is explicitly stated in each case. Unless otherwise stated, the stated values for refractive indices are measured at a wavelength of 550 nm. The refractive index can be determined, for example, using ellipsometry. Ellipsometers are commercially available, for example from Sentech. If the absorption is very strong and an accurate measurement with ellipsometry is not possible, the refractive index can also be determined using optical models from simulations. A simulation can be carried out, for example, using software commonly used in the field, such as CODE.According to the invention, the pane comprises an upper high-index dielectric layer or layer sequence. According to one embodiment, the IR-reflecting layer based on titanium carbide and the upper high-index dielectric layer or layer sequence are in direct contact with one another. "In direct contact" in the sense of the invention means that there is no further layer between the layers that are in direct contact with one another. The upper high-index dielectric layer or layer sequence preferably has a refractive index of more than 1.9, for example between 1.9 and 2.5. It can be formed as a single layer (in this case, an upper high-refractive-index dielectric layer is present) or as a stack of several layers (in this case, an upper SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT high-refractive-index dielectric layer sequence). In the case of a layer sequence, all layers preferably have a refractive index of more than 1.9. The upper high-refractive-index dielectric layer or layer sequence preferably has an optical thickness of 10 nm to 120 nm, particularly preferably of 20 nm to 100 nm. In an advantageous embodiment, the upper high-refractive-index dielectric layer or layer sequence contains or is formed from a nitride-based layer. This means that if an upper dielectric layer is present, it is formed from a nitride, and if an upper dielectric layer sequence is present,This contains at least one nitride-based layer. The nitride is preferably silicon nitride (SiN) or a silicon-metal mixed nitride, for example, silicon zirconium nitride (SiZrN), silicon hafnium nitride (SiHfN), silicon titanium nitride (SiTiN), or silicon aluminum nitride (SiAlN). These have suitable refractive indices (SiN: 2.0; SiZrN: 2.2), are comparatively simple and inexpensive to produce, and are commonly used for thin-film coatings on glass panes. In a further advantageous embodiment, the upper high-index dielectric layer or layer sequence contains or is formed from an oxide-based layer, in particular titanium oxide (TiO, refractive index 2.3). This allows the (average) refractive index of the upper high-index layer(s) to be further increased, which is advantageous, for example, for an anti-reflective effect.insofar as the pane, according to one embodiment, further comprises a low-refractive-index dielectric layer or layer sequence, as described below. In a particularly advantageous embodiment, that layer of the upper high-refractive-index layer or layer sequence which is in direct contact with the IR-reflecting layer based on TiC is formed on a nitride basis, in particular on a SiN or SiZrN basis. This can prevent the IR-reflecting layer from being oxidized during deposition or during a subsequent heat treatment, as could occur upon contact with an oxide layer. This can be achieved by providing an upper high-refractive-index dielectric layer based on the nitride, or by providing an upper high-refractive-index dielectric layer sequence.whose lowermost layer (i.e., closest to the IR-reflecting layer) is based on the nitride. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT In one embodiment, a single upper high-index dielectric layer is present based on a nitride, in particular based on silicon nitride (SiN) with a layer thickness of 10 nm to 60 nm, particularly preferably from 20 nm to 50 nm, for example from 30 nm to 45 nm, or based on silicon zirconium nitride (SiZrN) with a layer thickness of 10 nm to 50 nm,Particularly preferably from 15 nm to 45 nm. For other silicon-metal mixed nitrides, essentially the same layer thicknesses can be used as for SiZrN. In a further embodiment, an upper high-index dielectric layer sequence is present. This preferably comprises, from bottom to top (i.e., in the direction starting from the IR-reflecting layer based on titanium carbide), in the following order: - a first layer based on a nitride, in particular silicon nitride (SiN), or silicon-metal mixed nitride, in particular silicon zirconium nitride (SiZrN), and - a second layer based on an oxide, in particular titanium oxide (TiO). The first layer is preferably in direct contact with the IR-reflecting layer and prevents its oxidation. The second layer increases the average refractive index of the layer sequence. The second layer based on TiO preferably has a layer thickness of 5 nm to 25 nm.particularly preferably from 10 nm to 20 nm. The first layer preferably has a layer thickness of 10 nm to 30 nm, particularly preferably from 15 nm to 25 nm, if it is based on SiN. The first layer preferably has a layer thickness of 10 nm to 25 nm, particularly preferably from 15 nm to 20 nm, if it is based on SiZrN. According to the invention, the coating further comprises a lower high-refractive index dielectric layer or layer sequence formed between the glass pane and the IR-reflecting layer. By using the lower high-refractive index dielectric layer or layer sequence, it can be preventedthat during a possible heat treatment, components of the glass pane penetrate into the IR-reflecting layer based on titanium carbide. According to a preferred embodiment, the lower high-refractive-index dielectric layer or layer sequence and the IR-reflecting layer are in direct contact with each other. The lower high-refractive-index dielectric layer or layer sequence preferably has a refractive index of more than 1.9, for example, between 1.9 and 2.5. It can also be formed as a single layer (in this case, a lower high-refractive-index dielectric layer is present) or as a stack of several layers (in this case, a lower high-refractive-index dielectric layer sequence is present). In the case of a layer sequence, all layers preferably have a refractive index of more than 1.9. The lower high-index dielectric layer or layer sequence preferably has an optical thickness of 10 nm to 220 nm, particularly preferably of 20 nm to 200 nm. The materials of the lower and upper high-index dielectric layers or layer sequences can be selected independently of one another. In an advantageous embodiment, the lower high-index dielectric layer or layer sequence contains a layer based on a nitride or is formed therefrom. The nitride is preferably silicon nitride (SiN) or a silicon-metal mixed nitride, for example silicon zirconium nitride (SiZrN), silicon hafnium nitride (SiHfN), silicon titanium nitride (SiTiN), or silicon aluminum nitride (SiAlN). In a further advantageous embodiment, the lower high-index dielectric layer or layer sequence contains a layer based on an oxide or is formed therefrom.in particular titanium oxide (TiO). In a particularly advantageous embodiment, the layer of the lower high-index layer or layer sequence that is in direct contact with the IR-reflecting layer based on TiC is formed from a nitride, in particular based on SiN or SiZrN. This prevents the IR-reflecting layer from being oxidized during a subsequent heat treatment, as could occur upon contact with an oxide layer. This can be achieved by providing a lower high-index dielectric layer based on the nitride, or by providing a lower high-index dielectric layer sequence.whose top layer (i.e. closest to the IR-reflecting layer) is based on nitride. In a particularly advantageous embodiment, a single lower high-index dielectric layer is present based on a nitride, in particular based on silicon nitride (SiN) with a layer thickness of 10 nm to 110 nm, particularly preferably from 20 nm to 105 nm, in particular from 30 nm to 100 nm, or based on silicon zirconium nitride (SiZrN) with a layer thickness of 15 nm to 55 nm, particularly preferably from 20 nm to 45 nm. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT In a further embodiment, a lower high-index dielectric layer sequence is present, which, starting from the glass pane, comprises in the following order: - a first layer based on an oxide, in particular titanium oxide (TiO) and - a second layer based on a nitride, in particular silicon nitride (SiN), or silicon-metal mixed nitride,in particular silicon zirconium nitride (SiZrN). The second layer is preferably in direct contact with the IR-reflecting layer and prevents its oxidation. The first layer increases the average refractive index of the layer sequence. The first layer based on TiO preferably has a layer thickness of 5 nm to 25 nm, particularly preferably from 10 nm to 20 nm or from 10 nm to 18 nm. The second layer preferably has a layer thickness of 10 nm to 40 nm, particularly preferably from 15 nm to 35 nm, in particular from 25 nm to 35 nm or from 30 nm to 35 nm if it is based on SiN. The second layer preferably has a layer thickness of 10 nm to 35 nm, particularly preferably from 15 nm to 30 nm if it is based on SiZrN. According to one embodiment, the coating further comprises a low-refractive-index dielectric layer or layer sequence with a refractive index of less than 1.6,which is arranged on the upper high-refractive-index dielectric layer. With the help of this low-refractive-index dielectric layer or layer sequence, the pane can exhibit an anti-reflective effect in addition to its IR-reflecting properties. The low-refractive-index dielectric layer or layer sequence has a refractive index of less than 1.6, for example, between 1.2 and 1.6, preferably less than 1.5. It can be formed as a single layer (in which case, a low-refractive-index dielectric layer is present) or as a stack of several layers (in which case, a low-refractive-index dielectric layer sequence is present). In the case of a layer sequence, all layers have a refractive index of less than 1.6. The low-refractive-index dielectric layer or layer sequence preferably has an optical thickness of 40 nm to 130 nm.particularly preferably from 55 nm to 115 nm. This achieves particularly good antireflective properties. In an advantageous embodiment, the low-refractive-index dielectric layer or layer sequence contains a layer based on an oxide or is formed therefrom. The oxide is SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT preferably silicon oxide (SiO). This has a suitable refractive index (1.45), can be produced by thin-film technology, but also wet-chemically, and is commonly used for coatings on glass panes. In a preferred embodiment, a single low-refractive-index dielectric layer is present, in particular based on SiO with a layer thickness of 30 nm to 90 nm, particularly preferably from 40 nm to 80 nm. The low-refractive-index dielectric layer (in particular SiO layer) is, in one embodiment of the invention, a thin film,which can be produced, for example, by vapor deposition. Instead of a single low-refractive-index layer, a low-refractive-index dielectric layer sequence comprising several individual layers can also be present. The coating according to the invention has been described above in such a way that it contains or comprises certain layers or, according to embodiments, can contain or comprise certain layers. This means that, in addition to the layers mentioned, further layers can be present, for example, between the individual layers or layer sequences or as part of one or more layer sequences. According to a preferred embodiment, the coating consists only of the lower high-refractive-index layer(s), the IR-reflecting layer, and the upper high-refractive-index layer(s), with no further layers being present between, above, or below. It is further preferredthat the individual layer(s) consist only of the layers explicitly mentioned above and do not contain any further layers. According to a preferred embodiment, the pane according to the invention does not comprise a silver layer. The layers mentioned are sufficient to produce a good IR-shielding effect. Additional layers would increase the costs and complexity of production. However, according to one embodiment, the coating can further comprise the low-refractive-index layer(s) described above in order to obtain an anti-reflective effect in addition to the IR-reflecting property. According to an advantageous embodiment, the glass pane contains or consists of flat glass, preferably soda-lime glass, borosilicate glass, or quartz glass. The glass can be made of clear glass or of tinted or colored glass. Clear glass is understood to mean a glass panewhich has an integrated light transmission SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT according to ISO 9050 of at least 90%. Tinted or colored glass panes have a lower integrated light transmission. The same applies to the inner and outer panes if the pane is a laminated pane. The thickness of the glass pane can be freely selected according to the requirements of the application. The thickness of the glass pane, or the inner or outer pane, is usually between 0.5 mm and 5 mm. According to one embodiment, the pane is curved in one or more directions of space, as is common for motor vehicle windows, for example, with typical radii of curvature in the range of approximately 10 cm to approximately 40 m. The interior surface of the pane is generally concavely curved. According to another embodiment, the pane is flat, for example, when used as a window for buses,Trains or tractors or for buildings. The pane according to the invention preferably has an interior emissivity of less than 65%, particularly preferably less than 60%, most preferably less than 50%. Interior emissivity refers to the measure that indicates how much thermal radiation the pane emits into an interior, for example, a building or vehicle, in the installed position compared to an ideal heat radiator (a black body). Emissivity, in the sense of the invention, is understood to mean the normal emissivity at 283 K according to the standard EN 12898. The pane according to the invention preferably has a light transmission of 50% or less,more preferably 48% or less. According to a particularly preferred embodiment, the pane has a light transmission of 25% or more and 50% or less. A pane with such a light transmission is particularly advantageous in areas with very strong solar radiation, as a pleasant dimming of the incident light through the pane can be achieved. Light transmission here means the integrated light transmission according to ISO 9050, measured with a light source of illuminant D65. According to one embodiment, the pane according to the invention has the smallest possible color difference ΔE. The color difference ΔE is a measure of a color change, for example due to a heat treatment, and is measured according to EN ISO 11664-4. The lower the color difference,the less it is perceived by the human eye SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT. Preferably, after thermal tempering, the pane has a color difference ΔE of less than 5, more preferably less than 4, even more preferably less than 3. According to a particularly preferred embodiment, ΔE(Rc), which corresponds to the color difference measured from the coating side, is less than 5, more preferably less than 4, even more preferably less than 3. In a particularly preferred embodiment, ΔE(Rg), which corresponds to the color difference measured from the glass pane side, is less than 5, more preferably less than 4, even more preferably less than 3, most preferably less than 2. A color difference of less than 2 is virtually no longer perceptible to the human eye. If the pane is used, for example, as a pane for a building that has undergone thermal tempering,Thus, with a ΔE(Rg) of less than 2, the observer outside the building sees no color difference between such a tempered pane and a non-tempered pane. Due to the TiC-based layer, the coating according to the invention exhibits electrical conductivity, so that it can also be used as a heating coating. For this purpose, it is provided with so-called busbars, which extend along two opposite side edges of the pane and are connected to the poles of a voltage source, allowing a current to flow through the coating and thereby heat the pane. Due to the sheet resistance, particularly advantageous heating effects are achieved.if the voltage source has a voltage of 42 volts to 48 volts or even 300 V to 400 V. Such voltages are available in particular in electric vehicles. The invention also encompasses a method for producing a pane, wherein (a) a glass pane is provided with an outside surface and an inside surface, (b) a coating is applied to the outside surface or the inside surface of the glass pane by depositing the layers in the following order: - a lower high-index dielectric layer or layer sequence, - an IR-reflecting layer based on titanium carbide, and - an upper high-index dielectric layer or layer sequence. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT The upper high-index dielectric layer or layer sequence is preferably deposited by vapor deposition, for example by chemical vapor deposition (CVD).Plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD). Physical vapor deposition (PVD), for example, vapor deposition, is particularly preferred, and cathode sputtering (“sputtering”) and, in particular, magnetic field-assisted cathode sputtering (“magnetron sputtering”) are particularly preferred. According to the invention, the coating further comprises a lower high-refractive-index dielectric layer or layer sequence deposited between the glass pane and the IR-reflecting layer. The lower high-refractive-index dielectric layer or layer sequence can be produced using the same methods as the upper high-refractive-index dielectric layer or layer sequence, with magnetron sputtering being particularly preferred here as well. The IR-reflecting layer based on TiC can also be deposited using the aforementioned methods.Magnetron sputtering is also particularly preferred here. In a particularly advantageous embodiment, the IR-reflecting layer is deposited by reactive magnetron sputtering. It has been shown that this allows the production of IR-reflecting layers with particularly advantageous mechanical stability, light transmission, reflective color, and low specific resistance at a high deposition rate. These advantageous properties can be attributed to the fact that the use of reactive magnetron sputtering makes it possible to achieve excellent layer homogeneity (i.e., consistent composition, crystallinity, layer thickness, and density) with good crystallinity and density. Reactive magnetron sputtering is a special variant of magnetron sputtering, which in turn is a variant of sputtering. During sputtering, a target (cathode) is bombarded with ions, whereupon material is dissolved from the target.which is then deposited on the surface to be coated. While in simple sputtering, only an electric field is applied, in magnetron sputtering, an additional magnetic field is arranged behind the cathode plate. Due to the superposition of the electric and magnetic fields, the charge carriers no longer move parallel to the electric field lines, but rather orbit in a helical line above the target surface. This lengthens their path and increases the number of collisions per electron. The effectively higher ionization capacity of the electrons leads to an increase in the sputtering rate. Thus, significantly higher coating rates can be achieved at the same process pressure. In addition, denser layers can be produced. Reactive magnetron sputtering is a process based on this.wherein one or more reactive gases are added to an inert working gas (such as Ar). The gases react with the sputtered layer atoms on the target, in the vacuum chamber, or on the surface to be coated, forming new materials. The resulting reaction products are subsequently deposited on the surface to be coated. According to a preferred embodiment, the reactive gas is at least one of methane, acetylene, and nitrogen, more preferably at least one of methane and acetylene, and most preferably methane or acetylene is used, since the use of only one reactive gas allows the properties of the reaction product (such as stoichiometry, crystallinity, and layer thickness) to be more easily controlled. When using reactive magnetron sputtering, a titanium target is preferably used. The target and the sputtered layer can be doped with other materials, for example, nitrogen, boron, or aluminum.whereby the mechanical, electrical, chemical, and optical properties of the layer can be influenced and / or the deposition rate can be increased. According to a particularly preferred embodiment, the reactive magnetron sputtering is reactive DC (direct current) magnetron sputtering or reactive ACMF (alternating current mid-frequency) magnetron sputtering, which enable good control of the sputtering and are also cost-effective. According to another embodiment, the IR-reflecting TiC-based layer is produced by simple magnetron sputtering, using a titanium carbide target and an inert working gas (e.g., Ar). According to one embodiment, the coating further comprises a low-refractive-index dielectric layer or layer sequence with a refractive index of less than 1.6.which is deposited on the upper high-refractive-index dielectric layer. In one embodiment of the invention, the low-refractive-index dielectric layer is also deposited by the aforementioned vapor deposition methods, with magnetic-field-assisted cathode sputtering being particularly preferred here as well. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT The IR-reflecting TiC-based layer, the upper high-refractive-index dielectric layer, the lower high-refractive-index dielectric layer, and the low-refractive-index dielectric layer correspond to the layers described above for the pane according to the invention. After application of the coating, the pane is preferably subjected to a heat treatment,whereby the crystallinity of the layers is improved and the light transmission and optical properties of the pane are regularly improved. The temperature treatment can, for example, be carried out at a temperature of at least 500°C. The temperature treatment can also be carried out as part of a bending and / or tempering process. The temperature treatment described above is also referred to according to the invention as "thermal tempering" or "annealing". According to one embodiment, the pane can be subjected to a bending process after application of the coating in order to bring it into a cylindrical or spherically curved shape, as is customary for panes for use in vehicles, in particular for panes for use in passenger cars or trucks. For bending, the pane is softened by heating so that it becomes plastically formable, and then bent by methods known per se, for example gravity bending.Press bending and / or suction bending. Typical temperatures for glass bending processes range, for example, from 500°C to 700°C. If the pane is to be formed as a composite pane, the coated (and optionally bent) glass pane is bonded to the outer pane or inner pane via a thermoplastic intermediate layer. Known lamination processes are used for this, for example, autoclave processes, vacuum bag processes, vacuum ring processes, calender processes, vacuum laminators, or combinations thereof. The bonding of the glass pane to the outer pane or inner pane via the intermediate layer usually takes place under the influence of heat, vacuum, and / or pressure. The thermoplastic intermediate layer is preferably formed from at least one thermoplastic film, preferably a PVB film, EVA film, or PU film. Typical thicknesses for such films are in the range of 0.2 mm to 2 mm, in particular 0.3 mm to 1 mm. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT The invention also encompasses the use of a pane according to the invention as a window pane of a means of transport on land, water, or in the air, preferably of a motor vehicle or rail vehicle, particularly preferably as a rear window or roof pane, or as a pane for a building, preferably as a window pane, facade pane, or door pane. Various specific applications of the pane according to the invention are conceivable: - Thus, the coating can serve to provide a pane with a low light transmittance TL of 50% or less and a low emissivity, which is particularly advantageous when used as a rear window or roof pane of a motor vehicle or rail vehicle or as a pane for a building, preferably as a window pane, facade pane, or door pane.can be advantageous. - Since the coating can be used for both thermally tempered and non-thermally tempered products, since thermal tempering causes only a minimal color change of the pane, the corresponding manufacturing processes are efficient, so that the production costs for the corresponding products are low. In particular, a pane according to the invention that has been subjected to thermal tempering and a pane according to the invention that has not been subjected to thermal tempering can be used in close proximity to one another without creating a visually disadvantageous impression for the observer, since the pane according to the invention experiences at most a minimal color change during thermal tempering and thus is almost indistinguishable from the pane according to the invention.which has not been subjected to thermal tempering. - Due to the at most slight color change during thermal tempering, the pane according to the invention can be used in a variety of ways as a toughened pane without any undesirable coloring of the pane, which can be particularly advantageous when used as a rear window or roof pane of a motor vehicle or rail vehicle, or as a pane for a building, preferably as a window pane, facade pane, or door pane. The invention is explained in more detail below with reference to drawings and exemplary embodiments. The drawings are schematic representations and not to scale. The drawings do not limit the invention in any way. They show: SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT Fig. 1 shows a cross-section through an embodiment of the pane 1 according to the invention, Fig. 2 shows a cross-section through a further embodiment of the pane 1 according to the invention,Fig. 3 shows a cross section through a further embodiment of the pane 1 according to the invention, Fig. 4 shows a cross section through a further embodiment of the pane 1 according to the invention, Fig. 5 shows a cross section through a further embodiment of the pane 1 according to the invention, Fig. 6 shows a cross section through a general coating 20 on a glass pane 2, Fig. 7 shows a cross section through a further general coating 20 on a glass pane 2, Fig. 8 shows a cross section through a further embodiment of the coating 20 according to the invention on a glass pane 2, Fig. 9 shows a cross section through a further embodiment of the coating 20 according to the invention on a glass pane 2, Fig. 10 shows a flow diagram of an embodiment of the method according to the invention, Fig. 11 shows a spectrum of the light transmission TL versus the wavelength of the pane 1 according to the invention according to Example 1,Fig.12 shows a spectrum of the light reflection RLc versus the wavelength of the inventive pane 1 according to Example 1, Fig.13 shows a spectrum of the light transmission TL versus the wavelength of the inventive pane 1 according to Example 2, Fig.14 shows a spectrum of the light reflection RLout versus the wavelength of the inventive pane 1 according to Example 2, Fig.15 shows a spectrum of the light transmission TL versus the wavelength of the inventive pane 1 according to Example 3, Fig.16 shows a spectrum of the light reflection RLout versus the wavelength of the inventive pane 1 according to Example 3, Fig.17 shows a spectrum of the light transmission TL versus the wavelength of the inventive pane 1 according to Example 4,and Fig. 18 shows a spectrum of the light reflection RLout versus wavelength of the pane 1 according to the invention according to Example 4. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT Figure 1 shows an embodiment of a pane 1 according to the invention. The pane 1 is intended, for example, as a rear window or roof window of a motor vehicle or rail vehicle, or as a pane for a building. It is a monolithic pane (single pane of glass) and comprises a single glass pane 2 made, for example, of thermally toughened soda-lime glass with a thickness of 1.9 mm. The glass pane 2 has an exterior surface I, which, in the installed position, faces the outside environment, and an interior surface II,which, in the installed position, faces the interior. The interior-side surface II is completely covered with a coating 20 according to the invention. Figure 2 shows a further embodiment of a pane 1 according to the invention. The pane 1 is intended, for example, as a rear window or roof window of a motor vehicle or rail vehicle, or as a pane for a building. It is a monolithic pane (single pane of glass) and comprises a single glass pane 2 made, for example, of thermally toughened soda-lime glass with a thickness of 1.9 mm. The glass pane 2 has an exterior surface I, which, in the installed position, faces the outside environment, and an interior-side surface II,which, in the installed position, faces the interior. The outer surface I is completely covered with a coating 20 according to the invention. The coating 20 according to the invention has IR-reflecting properties. It therefore functions as a sun protection coating. This increases thermal comfort in the interior, as it heats up less. In addition to its infrared (IR)-reflecting properties, the coating 20 according to the invention is also chemically and mechanically resistant due to the use of TiC in the IR-reflecting layer and shows at most a slight color change after a possible thermal tempering. Both surfaces I, II of such a single glass pane are exposed, i.e., they have contact with the atmosphere. They could be coated with conventional,corrosion-prone (for example, silver-based) IR-reflecting coatings. Since the coating 20 according to the invention with IR-reflecting effect is not susceptible to corrosion, such a coating is easily possible. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT Figure 3 shows a further embodiment of a pane 1 according to the invention. The pane 1 is designed as a composite pane,wherein a glass pane 2 acts as the outer pane and is connected to an inner pane 5 via a thermoplastic intermediate layer 4. The glass pane 2 faces the outside environment in the installed position. The inner pane 5 faces the interior in the installed position. The glass pane 2 has an outside surface I and an inside surface II. The inner pane 5 also has an outside surface III and an inside surface IV. The glass pane 2 and the inner pane 5 are made, for example, of soda-lime glass with a thickness of 4 mm. The thermoplastic intermediate layer 4 is made, for example, of a film based on polyvinyl butyral (PVB) with a thickness of 0.38 mm. The pane 1 is intended, for example, as a rear window or roof window of a motor vehicle or rail vehicle, or as a pane for a building. The interior-side surface II of the glass pane 2 is completely coated with a coating 20 according to the invention. Figure 4 shows a further embodiment of a pane 1 according to the invention. The pane 1 is designed as a composite pane,wherein a glass pane 2 acts as the inner pane and is connected to an outer pane 3 via a thermoplastic intermediate layer 4. The outer pane 3 faces the outside environment in the installed position. The glass pane 2 faces the interior in the installed position. The outer pane 3 has an outside surface I and an inside surface II. The glass pane 2 also has an outside surface III and an inside surface IV. The glass pane 2 and the outer pane 3 are made, for example, of soda-lime glass with a thickness of 4 mm. The thermoplastic intermediate layer 4 is made, for example, of a film based on polyvinyl butyral (PVB) with a thickness of 0.38 mm. The pane 1 is intended, for example, as a rear window or roof window of a motor vehicle or rail vehicle, or as a pane for a building. The outer surface III of the glass pane 2 is completely coated with a coating 20 according to the invention. Figure 5 shows a further embodiment of a pane 1 according to the invention. The pane 1 is designed as a composite pane,wherein a glass pane 2 acts as the inner pane and is connected to an outer pane 3 via a thermoplastic intermediate layer 4. The outer pane 3 faces the outside environment in the installed position. The glass pane 2 faces the interior in the installed position. The outer pane 3 has an outside surface I and an inside surface II. The glass pane 2 also has an outside surface III and an inside surface IV. The glass pane 2 and the outer pane 3 are made, for example, of soda-lime glass with a thickness of 4 mm. The thermoplastic intermediate layer 4 is made, for example, of a film based on polyvinyl butyral (PVB) with a thickness of 0.38 mm. The pane 1 is intended, for example, as a rear window or roof window of a motor vehicle or rail vehicle or as a pane for a building. The interior surface IV of the glass pane 2 is completely provided with a coating 20 according to the invention. Figure 6 shows a general coating 20 on a glass pane 2. The coating 20 is arranged on the interior surface II or IV or on the exterior surface I or III of the glass pane 2. The coating 20 consists of an IR-reflecting layer 22 based on titanium carbide and an upper high-refractive index dielectric layer 23, which are arranged in this order on the glass pane 2, starting from its surfaces I, II,III or IV. The IR-reflecting effect is provided by the IR-reflecting layer 22 based on titanium carbide. The upper high-refractive-index dielectric layer 23 reduces or prevents the oxidation of the IR-reflecting layer 22 during a possible heat treatment. Figure 7 shows another general coating 20 on a glass pane 2. It differs from the pane 1 of Figure 6 in that, instead of a single upper high-refractive-index dielectric layer 23, there is an upper high-refractive-index dielectric layer sequence 23a, 23b. The layer sequence consists of a first high-refractive-index dielectric layer 23a and a second high-refractive-index dielectric layer 23b.which are arranged in this order on the IR-reflecting layer 22. The first layer 23a is a nitride layer and is in direct contact with the IR-reflecting layer 22. The second layer 23b is an oxide layer with a particularly high refractive index. The first layer 23a prevents contact between the IR-reflecting layer 22 and the oxide second layer 23b, so that unwanted oxidation of the IR-reflecting layer 22 can be prevented during the deposition of the layers or during a subsequent thermal treatment. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT Figure 8 shows an embodiment of the coating 20 according to the invention on a glass pane 2. It differs from the pane 1 of Figure 6 in that the coating 20 further comprises a lower high-index dielectric layer 21,which is formed between the glass pane 2 and the IR-reflecting layer 22. The lower high-refractive-index dielectric layer 21 can prevent components of the glass pane 2 from penetrating the titanium carbide-based IR-reflecting layer 22 during a possible heat treatment. Figure 9 shows a further embodiment of the coating 20 according to the invention on a glass pane 2. It differs from the embodiment of Figure 8 in that the coating 20 further comprises a low-refractive-index dielectric layer 24 with a refractive index of less than 1.6.which is arranged on the upper high-index dielectric layer 23. This coating 20 allows the pane to have an anti-reflective effect in addition to its IR-reflecting properties. Figure 10 shows an exemplary embodiment of the inventive method for producing a pane 1 with a coating 20 using a flow chart. Examples Example 1 A pane 1 according to the invention was produced. It was designed as a single glass pane and comprised a glass pane 2 (Planiclear® from Saint-Gobain Glass, soda-lime glass, light transmission TL of 91%) with a thickness of 1.9 mm, to whose surface a coating 20 according to the invention was applied. Starting with the glass pane 2, the layer sequence with the listed layer thicknesses and materials was as follows: - lower high-index dielectric layer 21: SiN (30 nm, refractive index 2.0), - IR-reflecting layer 22 based on titanium carbide: TiC (30 nm),and - upper high-refractive-index dielectric layer 23: SiN (30 nm, refractive index 2.0). SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT The lower high-refractive-index dielectric layer 21 and the upper high-refractive-index dielectric layer 23 were each deposited by magnetron sputtering. The IR-reflecting layer 22 was deposited by reactive magnetron sputtering using a titanium target and acetylene as the reactive gas. Properties of the pane 1 according to the invention are shown in Tables 1 and 2. The coated pane 1 was further subjected to a heat treatment at a temperature of 640°C for a period of 8 minutes ("thermal annealing"). Properties of the annealed pane 1 according to the invention are also shown in Tables 1 and 2. Comparative Example A pane according to the comparative example was also produced. It was designed as a single glass pane and included a glass pane (Planiclear® from Saint-Gobain Glass,Soda-lime glass, light transmission TL of 91%), 1.9 mm thick, with a coating applied to its surface. Starting with the glass pane, the layer sequence with the listed layer thicknesses and materials was as follows: - lower high-index dielectric layer: SiN (30 nm, refractive index 2.0), - IR-reflecting layer 22 based on titanium nitride: TiN (15 nm), and - upper high-index dielectric layer: SiN (30 nm, refractive index 2.0).0). The lower high-index dielectric layer and the upper high-index dielectric layer were each deposited by magnetron sputtering. The IR-reflecting layer was deposited by magnetron sputtering using a titanium nitride target. Properties of the pane according to the comparative example are also shown in Tables 1 and 2. The coated pane according to the comparative example was further subjected to a heat treatment at a temperature of 640°C for a period of 8 minutes ("thermal annealing"). Properties of the annealed pane according to the comparative example are also shown in Tables 1 and 2. It should be noted that RLg, a*Rg, b*Rg, ρ, and ε were not measured for the comparative example. In Tables 1 and 2, respectively, - TL is the integrated light transmission according to ISO 9050 (illuminant D65); - a*T and b*T are the values of the transmission color in the L*a*b* color space,measured with an angle of incidence of 8° and an observation angle of 2° (illuminant D65); SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT - RLc is the integrated light reflectance, measured from the coating side with an angle of incidence of 8° and an observation angle of 2° (illuminant D65); - a*Rc and b*Rc are the values of the reflection color from the coating side in the L*a*b* color space, measured with an angle of incidence of 8° and an observation angle of 2° (illuminant D65); - RLg is the integrated light reflectance, measured from the glass side with an angle of incidence of 8° and an observation angle of 2° (illuminant D65); - a*Rg and b*Rg are the values of the reflection color from the glass side in the L*a*b* color space, measured with an angle of incidence of 8° and an observation angle of 2° (illuminant D65); - ρ is the specific resistance, measured with NAGY resistance meter ZPM00052; - ^ is the normal indoor emissivity at 283 K according to EN 12898; - ΔE(T) is the color difference,related to the transmission, measured according to EN ISO 11664-4; - ΔE(Rc) is the color difference, measured from the coating side according to EN ISO 11664-4; and - ΔE(Rg) is the color difference, measured from the glass side according to EN ISO 11664-4.
[0002] SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT Table 1 IR- Temperature treatment TL a*T b*T RLc a*Rc b*Rc reflective [%] [%] layer TiC No (rt) 25.0 -1.8 0 22.5 2.1 22.2 TiC Yes (8 min at 640 °C) 26.7 -1.1 1.9 20.3 0.6 19.7 TiN No (rt) 50.9 -2.5 -4.6 13.5 1.0 5.9 TiN Yes (8 min at 640 °C) 54.9 -2.8 -2.9 11.4 2.2 -0.9 “rt” means “room temperature” Table 2 IR- Temperature- RLg a*Rg b*Rg ρ ε ΔE(T) The pane 1 according to the invention as per Example 1 has an attractive transmission color a*T and b*T and reflection color a*Rc, b*Rc, a*Rg and b*Rg and a low specific resistance ρ. In addition, it exhibits solar protection properties and a low emissivity ε.In addition, the inventive pane 1 according to Example 1 exhibited only a small color difference ΔE as a result of the heat treatment. In contrast, a significant color change was measurable for the comparative example using TiN. This is particularly evident in the ΔE(Rc) value, which was only 2.9 for the inventive pane 1 according to Example 1, while the comparative example exhibited a significantly higher value of 6.9. The higher the value of ΔE, ΔE(Rc), and ΔE(Rg), the greater the color change. Figures 11 and 12 show the light transmission and light reflection, respectively, of the inventive pane 1 according to Example 1, which was subjected to the heat treatment. The experimental measured values are shown in black. In addition, a simulation of the inventive heat-treated pane 1 according to Example 1 with the layer sequence listed above was carried out.The simulated data (shown in gray in Figures 11 and 12) show good agreement with the experimental data. Examples 2 to 4: Further heat-treated panes 1 according to the invention were simulated. They were designed as composite panes and comprised a glass pane 2 and another glass pane as the inner pane (glass pane and inner pane: Planiclear® from Saint-Gobain Glass, soda-lime glass, light transmission TL of 91%), each with a thickness of 4.0 mm, with the glass pane 2 acting as the outer pane and the coating being arranged on the interior-side surface (II) of the glass pane 2 as the outer pane.The arrangement of the panes and the coating 20 for the composite panes were as follows: Example 2: - inner pane 5: glass (4.0 mm) - thermoplastic intermediate layer 4: PVB (0.38 mm) - upper high-refractive-index dielectric layer 23: TiO 23b (15 nm), SiN 23a (23 nm), where SiN 23a has direct contact with the IR-reflecting layer 22 - IR-reflecting layer 22 based on titanium carbide: TiC (28.2 nm) SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT - lower high-refractive-index dielectric layer 21: SiN (49.8 nm), and - the glass pane 2 as outer pane: glass (4.0 mm).Example 3: - inner pane 5: glass (4.0 mm) - thermoplastic intermediate layer 4: PVB (0.38 mm) - upper high-refractive-index dielectric layer 23: TiO 23b (5.8 nm), SiN 23a (37.1 nm), where SiN 23a has direct contact with the IR-reflecting layer 22 - IR-reflecting layer 22 based on titanium carbide: TiC (23.5 nm) - lower high-refractive-index dielectric layer 21: TiO (0.3 nm), and - the glass pane 2 as outer pane: glass (4.0 mm). Example 4: - Inner pane 5: glass (4.0 mm) - Thermoplastic intermediate layer 4: PVB (0.38 mm) - Upper high-refractive-index dielectric layer 23: SiN (24.8 nm) - IR-reflecting layer 22 based on titanium carbide: TiC (11.1 nm) - Lower high-refractive-index dielectric layer 21: SiN (5.6 nm), TiO (5.2 nm), with SiN having direct contact with the IR-reflecting layer 22; and - The glass pane 2 as outer pane: glass (4.0 mm). Properties of the panes 1 according to the invention of Examples 2 to 4 are shown in Table 3.The properties TL, a*T, b*T and ε listed in Table 3 correspond to the properties given above for Tables 1 and 2, respectively, although these were simulated and not measured.In addition, in Table 3 - RLin is / are the integrated light reflection, simulated by the inner pane of the laminated glass with an angle of incidence of 8° and an observation angle of 2° (illuminant D65); SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT - a*Rin and b*Rin are the simulated values of the reflection color from the inner pane of the laminated glass in the L*a*b* color space, simulated with an angle of incidence of 8° and an observation angle of 2° (illuminant D65); - RLout is the integrated light reflection, simulated by the outer pane of the laminated glass with an angle of incidence of 8° and an observation angle of 2° (illuminant D65); - a*Rout and b*Rout are the simulated values of the reflection colour from the outer pane of the laminated glazing in the L*a*b* colour space, simulated with an incidence angle of 8° and an observation angle of 2° (illuminant D65); and - g is the Solar Control value, which corresponds to the percentage of solar energy passing through the glass into a room.This factor takes into account the direct transmission of the glass and the phenomenon of energy reflectivity of the glass wall towards the interior (glass heats up due to absorption of solar rays), measured according to ISO 9050 AM 1.5. The inventive pane 1 according to Example 2 has a light transmission TL of 29%, similar internal and external reflection (RLin and RLout, respectively), as well as neutral transmission colors a*T and b*T and reflection colors a*Rin, b*Rin, a*Rout, and b*Rout with a low g-value. Furthermore, the inventive pane 1 according to Example 3 has a light transmission TL of 30% and high external reflection RLout, while having neutral transmission colors a*T and b*T and reflection colors a*Rin, b*Rin, a*Rout, and b*Rout and a low g-value. The pane 1 according to the invention according to Example 4 has a light transmission TL of 46% with similar internal and external reflection (RLin and RLin, respectively).RLout), neutral reflection color a*Rin, b*Rin, a*Rout and b*Rout and transmission color a*T and b*T and a low g-value. Figures 13 to 18 show the light transmission and light reflection of the panes 1 according to the invention according to Examples 2 to 4. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT Table 3 Coating TL a*T b*T RLin a*Rin b*Rin RLout a*Rout b*Rout ε g [%] [%] [%] [%] Example 2 29 -3.7 10.4 14.4 3.8 3.0 16.2 1.6 -2.0 47 34 Example 3 30 -1.8 7.1 8.8 2.3 0 30.5 -2.8 -1.0 50 35 Example 4 46 -1.0 4.3 12.8 -2.0 -2.5 17.0 -2.2 -5.6 60 49.
[0003] SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT List of reference symbols: (1) pane (2) glass pane (3) outer pane (4) thermoplastic intermediate layer (5) inner pane (20) coating (21) lower high-refractive-index dielectric layer (22) IR-reflecting layer based on titanium carbide (23) upper high-refractive-index dielectric layer (23a) first layer of an upper dielectric layer sequence (23b) second layer of an upper dielectric layer sequence (24) low-refractive-index dielectric layer (I) outer surface of the glass pane 2 in the case of a single glass pane / outer surface of the glass pane 2 or of the outer pane 3 in the case of a composite pane (II) interior-side surface of the glass pane 2 in the case of a single glass pane / interior-side surface of the glass pane 2 or of the outer pane 3 in the case of a composite pane (III) outer surface of the glass pane 2 or of the inner pane 5 in the case of a composite pane (IV) interior-side surfaceof the glass pane 2 or the inner pane 5 in the case of a laminated pane
Claims
SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT Patent claims 1. A pane (1), comprising - at least one glass pane (2) with an outside surface (I, III) and an inside surface (II, IV), and - a coating (20) on the outside surface (I, III) or the inside surface (II, IV) of the glass pane (2), wherein the coating (20), starting from the surface (I, II, III, IV) of the glass pane (2), comprises at least in the following order: - a lower high-refractive-index dielectric layer (21) or layer sequence, - an IR-reflecting layer (22) based on titanium carbide, and - an upper high-refractive-index dielectric layer (23) or layer sequence (23a, 23b), wherein the IR-reflecting layer (22) has a layer thickness of 2 nm to 50 nm.The pane (1) according to claim 1, wherein the high-refractive-index dielectric layer (21, 23) or layer sequence (23a, 23b) contains a layer based on silicon nitride (SiN), silicon-metal mixed nitride, or titanium oxide (TiO).
3. The pane (1) according to claim 1 or 2, wherein the refractive index of the high-refractive-index dielectric layer (21, 23) or layer sequence (23a, 23b) is greater than 1.
9.
4. The pane (1) according to any one of claims 1 to 3, wherein the upper high-refractive-index dielectric layer (23) or layer sequence (23a, 23b) has an optical thickness of 10 nm to 120 nm, preferably of 20 nm to 100 nm.
5. The pane (1) according to any one of claims 1 to 4, wherein the pane (1) has a light transmission TL of 50% or less.
6. Pane (1) according to one of claims 1 to 5, wherein the glass pane (2) contains or consists of flat glass, preferably soda-lime glass, borosilicate glass, or quartz glass. 7.Disc (1) according to one of claims 1 to 6, wherein the disc (1) does not comprise a silver layer. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT 8. Pane (1) according to one of claims 1 to 7, which is designed as a composite pane, wherein the glass pane (2) is connected to an outer pane (3) via a thermoplastic intermediate layer (4).
9. Pane (1) according to one of claims 1 to 7, which is designed as a composite pane, wherein the glass pane (2) is connected to an inner pane (5) via a thermoplastic intermediate layer (4).
10. Pane (1) according to one of claims 1 to 7, which is designed as a single glass pane.
11. Pane (1) according to one of claims 1 to 10, wherein the pane (1) has a light transmission TL of 25% or more. 12.A method for producing a pane (1), wherein (a) a glass pane (2) is provided having an outside surface (I, III) and an inside surface (II, IV), (b) a coating (20) is applied to the outside surface (I, III) or the inside surface (II, IV) of the glass pane (2) by depositing the layers in the following order: - a lower high-refractive-index dielectric layer (21) or layer sequence, - an IR-reflecting layer (22) based on titanium carbide, and - an upper high-refractive-index dielectric layer (23) or layer sequence (23a, 23b), wherein the IR-reflecting layer (22) has a layer thickness of 2 nm to 50 nm.
13. The method according to claim 12, wherein the IR-reflecting layer (22) is deposited by reactive magnetron sputtering. 14.Use of a pane (1) according to one of claims 1 to 11 as a window pane of a means of locomotion on land, on water or in the air, preferably a motor vehicle or rail vehicle, particularly preferably as a rear window or. SAINT-GOBAIN GLASS FRANCE 2023077-WO-PCT roof pane, or as a pane for a building, preferably as a window pane, facade pane or door pane.