Hardening accelerator for hydraulic materials, cement composition, and hardened substance

MYPI2025005839A0Undetermined Publication Date: 2024-09-28DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005839
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-26
Publication Date
2024-09-28

AI Technical Summary

Technical Problem

Hydraulic materials using existing hardening accelerators lose fluidity quickly after mixing with water, making compaction labor-intensive and reducing productivity, while also affecting initial strength development and fluidity retention.

Method used

A curing accelerator composition containing 20.0 to 80.0% calcium formate, 15.0 to 70.0% inorganic calcium compounds, and 0.5 to 30.0% inorganic sulfates other than calcium sulfate, along with calcium sulfoaluminate, which improves fluidity retention, coagulation properties, and initial strength development of hydraulic materials.

Benefits of technology

The proposed solution enhances fluidity retention and initial strength development, allowing for efficient compaction and accelerated curing, thereby improving productivity in construction processes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a hardening accelerator for a hydraulic material, containing 20.0 to 80.0 mass% of calcium formate, 15.0 to 70.0 mass% of an inorganic calcium compound, and 0.5 to 30.0 mass% of an inorganic sulfate excluding calcium sulfate.
Need to check novelty before this filing date? Find Prior Art

Description

Hardening accelerators for hydraulic materials, cement compositions, and hardened products

[0001] The present invention relates to a hardening accelerator for hydraulic materials, and a cement composition and a hardened product containing said accelerator.

[0002] Hydraulic materials such as cement used in civil engineering and construction fields are usually mixed with water and allowed to harden by standing for a predetermined period of time. The hardening speed of hydraulic materials can be affected by the ratio of the material to water, the ambient temperature, and the curing method, but the time it takes for hydraulic materials to harden can be shortened by using admixtures that accelerate hardening, i.e., hardening accelerators.

[0003] Reducing the time it takes for hydraulic materials to harden leads to improved productivity at work sites. For example, hardened concrete used in precast construction methods for reinforced concrete buildings and the like can generally be obtained by pouring a cement composition into a formwork, leaving it to stand for a predetermined period of time, and then curing it by steam curing or the like. However, the use of a hardening accelerator can reduce the time it takes for the concrete to reach an initial strength that allows it to be removed from the form, allowing for efficient production of hardened concrete.

[0004] Furthermore, after pouring the cement composition, it is usually "compacted" using a vibrator or the like to distribute the cement composition evenly within the formwork. However, if the fluidity of the cement composition is reduced immediately after pouring, compaction requires time and effort, resulting in reduced productivity.

[0005] Regarding hardening accelerators, for example, Patent Document 1 discloses a hardening accelerator for hydraulic materials containing predetermined amounts of inorganic sulfate, calcium sulfoaluminate, and inorganic hydroxide. Patent Document 2 discloses a hardening accelerator for hydraulic materials containing a material having a Blaine specific surface area of ​​4000 cm 2 The document discloses a cement admixture containing calcium sulfoaluminate in an amount of 1 / g or more and one or more salts selected from the group consisting of formates, acetates and lactates.

[0006] JP 2014-19618 A JP 2010-235399 A

[0007] However, hydraulic materials using the above-mentioned hardening accelerators lose their fluidity immediately after mixing with water, and compaction after pouring requires effort and time, which raises concerns about reduced productivity.

[0008] In view of the above, an object of the present invention is to provide a hardening accelerator for hydraulic materials that can improve the fluidity retention, setting properties, and early strength development of hydraulic materials.

[0009] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the problems can be solved by a hardening accelerator for hydraulic materials containing calcium formate, an inorganic calcium compound, and an inorganic sulfate other than calcium sulfate in a predetermined ratio, and have arrived at the present invention.

[0010] [1] A hardening accelerator for hydraulic materials containing 20.0 to 80.0 mass% calcium formate, 15.0 to 70.0 mass% inorganic calcium compound, and 0.5 to 30.0 mass% inorganic sulfates excluding calcium sulfate. [2] The hardening accelerator for hydraulic materials according to [1] above, wherein the inorganic calcium compound is at least one selected from the group consisting of calcium sulfate, calcium hydroxide, calcium carbonate, and calcium oxide. [3] The hardening accelerator for hydraulic materials according to [1] or [2] above, wherein the inorganic sulfate is at least one selected from the group consisting of sulfate, thiosulfate, sulfite, bisulfite, pyrosulfate, and pyrobisulfite. [4] The hardening accelerator for hydraulic materials according to any one of [1] to [3] above, further containing 4.5 to 65.0 mass% calcium sulfoaluminate. [5] A cement composition containing the hardening accelerator for hydraulic materials according to any one of [1] to [4] above and cement. [6] The cement composition according to [5] above, in which the content of the hardening accelerator for hydraulic materials is 0.5 to 10 mass%. [7] A hardened body obtained by hardening the cement composition according to [5] or [6] above. [8] A method for producing a hardened body, in which a cement composition containing the hardening accelerator for hydraulic materials according to any one of [1] to [4] above, cement, and water is hardened by steam curing at a maximum temperature of 40 to 80°C for 2 to 8 hours.

[0011] According to the present invention, it is possible to provide a hardening accelerator for hydraulic materials that can improve the fluidity retention, setting properties, and early strength development of hydraulic materials.

[0012] Hereinafter, one embodiment of the present invention (the present embodiment) will be described in detail, but the present invention is not limited to this embodiment. In the present invention, the term "hydraulic material" refers to a material that hardens when kneaded with water, and the term "hardened product" refers to hardened cement paste, mortar, concrete, etc. In addition, "%" and "parts" in this specification are based on mass unless otherwise specified.

[0013] [Hydraulic material hardening accelerator] The hydraulic material hardening accelerator according to this embodiment contains 20.0 to 80.0 mass% calcium formate, 15.0 to 70.0 mass% inorganic calcium compound, and 0.5 to 30.0 mass% inorganic sulfates excluding calcium sulfate. The hydraulic material hardening accelerator not only accelerates the hardening of the hydraulic material when the hydraulic material is mixed with water and hardened, but may also harden itself while accelerating the hardening.

[0014] (Calcium formate) The hardening accelerator for hydraulic materials contains 20.0 to 80.0 mass% of calcium formate, preferably 30.0 to 70.0 mass%, and more preferably 40.0 to 65.0 mass%. If the calcium formate content is less than 20.0 mass%, the fluidity retention, setting properties, and early strength development of the hydraulic material may not be improved, while if it exceeds 80.0 mass%, the fluidity retention, setting properties, and early strength development may not be improved.

[0015] (Inorganic calcium compound) The hardening accelerator for hydraulic materials contains 15.0 to 70.0 mass% of an inorganic calcium compound, preferably 18.0 to 60.0 mass%, and more preferably 20.0 to 40.0 mass%. If the content of the inorganic calcium compound is less than 15.0 mass%, the fluidity retention, setting properties, and early strength development of the hydraulic material may not be improved, and if it exceeds 70.0 mass%, the fluidity retention, setting properties, and early strength development of the hydraulic material may not be improved.

[0016] In this embodiment, the inorganic calcium compound is preferably one or more selected from the group consisting of calcium sulfate, calcium hydroxide, calcium carbonate, and calcium oxide. When two or more inorganic calcium compounds are used, the total content of each is taken as the content of the inorganic calcium compounds. In this embodiment, from the viewpoint of early strength development, calcium sulfate, calcium hydroxide, and / or calcium oxide are preferably used, and calcium sulfate is more preferred. When calcium sulfate is used, it is more preferred that it is anhydrous.

[0017] (Inorganic Sulfates) The hardening accelerator for hydraulic materials contains 0.5 to 30.0 mass %, preferably 1.0 to 25.0 mass %, and more preferably 3.0 to 15.0 mass % of inorganic sulfates excluding calcium sulfate. If the content of inorganic sulfates excluding calcium sulfate is outside the range of 0.5 to 30.0 mass %, the fluidity retention, setting properties, and early strength development of the hydraulic material may not be improved.

[0018] In this embodiment, the inorganic sulfate is preferably one or more selected from the group consisting of sulfate, thiosulfate, sulfite, bisulfite, pyrosulfate, and pyrobisulfite. When two or more inorganic sulfates are used, the total content of the inorganic sulfate is the sum of the respective contents. As inorganic substances that form salts, alkali metals and alkaline earth metals are preferred. In this embodiment, from the viewpoint of early strength development, sulfate and / or thiosulfate are preferably used, and sodium sulfate, aluminum sulfate, sodium thiosulfate, and potassium alum are more preferred. From the viewpoint of early strength development, sodium sulfate and aluminum sulfate are even more preferred. Among them, sodium sulfate is even more preferred from the viewpoint of improving fluidity retention. When sodium sulfate is used, it is more preferred that it is anhydrous.

[0019] The hardening accelerator for hydraulic materials according to this embodiment preferably further contains calcium sulfoaluminate in an amount of 4.5 to 65.0 mass%, more preferably 15.0 to 60.0 mass%, and even more preferably 30.0 to 50.0 mass%. When the calcium sulfoaluminate content is within the above range, the hydraulic material can have better fluidity retention and early strength development. Calcium sulfoaluminate has the chemical formula xCaO.yAl 2 O 3 zCaSO 4 ・mH 2 O (x, y, z are non-zero positive real numbers, m is 0 or a positive real number), and is a general term for hydraulic substances and hydrated salts. For example, hauyne (3CaO.3Al 2 O 3 CaSO 4 ), as well as ettringite (3CaO·Al 2 O 3 3CaSO 4 ・32H 2 O), AFt phase, represented by monosulfate (3CaO.Al 2 O 3 CaSO 4 ・12H 2Calcium sulfoaluminate may be amorphous. 2 O 3 A small amount of Fe is included in part of 2 O 3 or SiO 2 etc., and CaSO 4 Part of Ca(OH) 2 or CaCO 3 In the present invention, the above chemical formula xCaO.yAl may be substituted. 2 O 3 zCaSO 4 ・mH 2 If z is 0, the fluidity of the hydraulic material cannot be maintained and there is a risk of a decrease in strength during hardening due to a phase transition, so z cannot be 0.

[0020] Calcium sulfoaluminate is produced using calcia raw materials such as lime, sulfate raw materials such as gypsum, and alumina raw materials such as bauxite (aluminum hydroxide), for example, as a calcium sulfoaluminate. 4 :Al 2 O 3 The raw materials can be blended in a predetermined ratio, such as a molar ratio of 3:3:1, fired at about 1,500°C in a kiln or the like, and pulverized to produce the product. Alternatively, silicon dioxide or the like may be added to the fired product, which may then be heat-treated and pulverized.

[0021] The Blaine specific surface area value (hereinafter simply referred to as the "Blaine value") of calcium sulfoaluminate is 1,000 to 6,000 cm 2 / g, and 2,000 to 4,000 cm 2 / g, and more preferably 2,200 to 3,800 cm 2 In the present invention, the Blaine specific surface area value is measured in accordance with the specific surface area test described in JIS R 5201:2015 "Physical testing methods for cement."

[0022] [Cement Composition] The cement composition according to this embodiment contains a hardening accelerator for hydraulic materials and cement.

[0023] The cement is not particularly limited, and examples include various Portland cements such as normal, high-early-strength, ultra-high-early-strength, low-heat, and medium-heat; various blended cements obtained by mixing these Portland cements with blast furnace slag, fly ash, silica fume, etc.; environmentally friendly cements (ecocements) produced using municipal waste incineration ash or sewage sludge incineration ash as raw materials; commercially available fine cements; and white cements. Various cements can also be finely powdered and used. Cement prepared by increasing or decreasing the amount of components (e.g., gypsum) typically used in cements can also be used. Furthermore, combinations of two or more of these can also be used. While normal Portland cement or high-early-strength Portland cement is preferred from the viewpoint of improving early strength development, early demolding is also possible using blast furnace cement or fly ash cement with low early strength development.

[0024] The cement used in the present invention has a Blaine specific surface area of ​​2,500 cm from the viewpoint of production cost and strength development. 2 / g~7,000cm 2 / g, and 2,750 cm 2 / g~6,000cm 2 / g, and more preferably 3,000 cm 2 / g~4,500cm 2 It is more preferable that the SiO2 content is 1 / g.

[0025] The content of the hydraulic material hardening accelerator in the cement composition is preferably 0.5 to 10 mass%, more preferably 1.0 to 9.0 mass%, and even more preferably 2.5 to 8.0 mass%. When the content of the hydraulic material hardening accelerator in the cement composition is within the above range, the fluidity retention, setting property, and early strength development of the hydraulic material can be improved.

[0026] The flow value of the cement composition before pouring is preferably 160 to 230, more preferably 170 to 220, and even more preferably 190 to 200. When the flow value of the cement composition is within the above range, pouring and compaction are easy, improving workability. Furthermore, the rate of change in flow value after 1 hour of mixing the cement composition (flow change rate) is preferably less than 20%, more preferably less than 15%, and even more preferably less than 10%. When the flow change rate of the cement composition is within the above range, pouring and compaction are easy, improving workability, even when pouring is performed 1 hour after mixing the cement composition. In the present invention, the flow value can be measured in accordance with the method specified in JIS R 5201:2015 "Physical Testing Methods for Cement." The flow change rate can be calculated by subtracting the value calculated by (flow value after 1 hour of mixing) / (flow value immediately after mixing) × 100 (%) from 100%.

[0027] The cement composition preferably contains aggregate. The aggregate used may be the same fine aggregate or coarse aggregate as that used in ordinary cement mortar or concrete. Specifically, river sand, river gravel, mountain sand, mountain gravel, crushed stone, crushed sand, limestone aggregate, lime sand, silica sand, colored sand, artificial aggregate, blast furnace slag aggregate, sea sand, sea gravel, artificial lightweight aggregate, heavy aggregate, etc., or a combination of these may be used.

[0028] The content of the aggregate is preferably 40 parts by mass or more and 250 parts by mass or less, more preferably 50 parts by mass or more and 230 parts by mass or less, and even more preferably 60 parts by mass or more and 200 parts by mass or less, relative to 100 parts by mass of cement in the cement composition. When the content of the aggregate is within the above range, the fluidity retention and early strength development of the hydraulic material can be improved.

[0029] The cement composition may contain an alkali metal carbonate. When the cement composition contains an alkali metal carbonate, the fluidity retention and early strength development are easily improved. Examples of the alkali metal carbonate include sodium carbonate, potassium carbonate, lithium carbonate, sodium bicarbonate, potassium bicarbonate, and lithium bicarbonate, and these may also be combined.

[0030] The content of the alkali metal carbonate is preferably 1 to 6 parts by mass, more preferably 2 to 5 parts by mass, in terms of solid content per 100 parts by mass of cement in the cement composition. When the content of the alkali metal carbonate is within the above range, it is easy to improve fluidity retention and early strength development.

[0031] The cement composition can contain a siliceous fine powder. When the cement composition contains a siliceous fine powder, it is easy to improve the fluidity retention and early strength development. Examples of the siliceous fine powder include latent hydraulic substances such as ground granulated blast furnace slag, fly ash, and pozzolanic substances such as silica fume, and among these, silica fume is preferred. The type of silica fume is not limited, but from the viewpoint of fluidity, it is preferable to use ZrO as an impurity. 2 It is more preferable to use silica fume containing 10% or less of the above-mentioned compound or acidic silica fume. Acidic silica fume is a silica fume that, when 1 g of silica fume is added to 100 cc of pure water and stirred, the supernatant liquid has an acidic pH of 5.0 or less.

[0032] The fineness of the silica fine powder is not particularly limited, but usually, the fine powder of granulated blast furnace slag and fly ash has a Blaine value of 3,000 cm 2 / g or more 9,000cm 2 / g or less, and silica fume has a BET specific surface area of ​​20,000 cm 2 / g or more 300,000cm 2 / g or less.

[0033] The content of the siliceous fine powder is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, and even more preferably 3 to 12 parts by mass, per 100 parts by mass of cement in the cement composition. When the content of the siliceous fine powder is equal to or greater than the above-mentioned lower limit, it is easy to improve fluidity retention and early strength development. Furthermore, when the content of the siliceous fine powder is equal to or less than the above-mentioned upper limit, it is easy to further improve fluidity retention.

[0034] The cement composition may contain an antifoaming agent to the extent that it does not adversely affect performance. Antifoaming agents are used to reduce the amount of air entrained during mixing. The type of antifoaming agent is not particularly limited as long as it does not significantly adversely affect the strength properties of the hardened mortar, and both liquid and powder forms can be used. Examples include polyether-based antifoaming agents, polyhydric alcohol-based antifoaming agents such as polyhydric alcohol esters and alkyl ethers, alkyl phosphate-based antifoaming agents, and silicone-based antifoaming agents.

[0035] The content of the antifoaming agent is preferably 0.002 to 0.5 parts by mass, more preferably 0.005 to 0.45 parts by mass, and even more preferably 0.01 to 0.4 parts by mass, relative to 100 parts by mass of cement in the cement composition. When the content of the antifoaming agent is equal to or greater than the lower limit, the antifoaming effect can be sufficiently exhibited, and when the content of the antifoaming agent is equal to or less than the upper limit, the fluidity retention can be easily improved.

[0036] Furthermore, the cement composition may contain one or more of the following additives, within a range that does not adversely affect performance: gas foaming substances, water reducing agents, air entraining agents, rust inhibitors, water repellents, antibacterial agents, colorants, antifreeze agents, admixtures such as fine limestone powder, slowly cooled blast furnace slag powder, sewage sludge incineration ash and its molten slag, municipal waste incineration ash and its molten slag, and pulp sludge incineration ash; thickeners; shrinkage reducing agents; polymers; clay minerals such as bentonite and sepiolite; and anion exchangers such as hydrotalcite.

[0037] [Hardened product] The hardened product according to this embodiment is obtained by hardening a cement composition. The hardened product is usually produced by kneading the cement composition with water, causing the cement, which is a hydraulic material, to undergo a hydration reaction and harden. The amount of water used for mixing is not particularly limited, but is preferably 10 to 70 parts by mass, more preferably 14 to 65 parts by mass, and even more preferably 16 to 60 parts by mass, per 100 parts by mass of the cement composition. When the amount of water used for mixing is within the above range, it is easy to improve the initial strength development of the hydraulic material.

[0038] The hardened product is obtained by mixing the cement composition with water and then leaving it to harden, but it can also be obtained more efficiently by filling (casting) the mixture into a formwork and curing it, or by pouring it directly onto the construction site, or by spraying or applying it.

[0039] The compressive strength of the hardened body depends on the type of cement used, but is 10.5 to 15.0 N / mm 6 hours after casting. 2 It is preferable that the strength is 11.0 to 14.0 N / mm 2 More preferably, it is 12.0 to 13.0 N / mm 2 It is more preferable that the strength is 40.0 to 50.0 N / mm 2 Preferably, the strength is 41.0 to 48.0 N / mm 2 More preferably, it is 42.0 to 46.0 N / mm 2 In the present invention, the compressive strength can be measured in accordance with the method specified in JIS R 5201:2015 "Physical testing methods for cement."

[0040] [Method for Producing Hardened Product] The method for producing a hardened product according to this embodiment is a method for hardening a cement composition containing a hardening accelerator for hydraulic materials, cement, and water by steam curing for 2 to 8 hours at a maximum temperature of 40 to 80° C. The method for producing a hardened product preferably includes, in this order: a kneading step of kneading the hardening accelerator for hydraulic materials, cement, and water; a casting step of filling a formwork with the mixed cement composition; and a curing step of curing the cement composition filled in the formwork.

[0041] The mixing method in the mixing step is not particularly limited, and the materials may be mixed at the time of construction, or some or all of them may be mixed in advance. As a mixing device, any existing device such as a tilting mixer, an omni mixer, a Henschel mixer, a V-type mixer, a Plosser mixer, or a Nauta mixer can be used.

[0042] The casting method in the casting step can be performed by a known method. The temperature of the cement composition during casting is preferably 0 to 50°C, more preferably 10 to 40°C. When the temperature of the cement composition during casting is within the above range, it becomes easier to quickly demold the hardened body.

[0043] The method for producing a hardened body preferably further includes a compaction step after the casting step. A known method can be used for the compaction, but from the viewpoint of workability, it is preferable to use a vibrator. The cement composition containing the hardening accelerator for hydraulic materials of the present invention maintains its fluidity well just before casting, so compaction can be easily performed, the cement composition can be uniformly distributed within the formwork, and air bubbles mixed in during casting can be removed.

[0044] From the viewpoint of improving productivity, steam curing using a curing chamber, a heating sheet, or the like is preferably used as the curing method used in the curing step. Steam curing is usually performed by raising the temperature of the atmosphere around the target and maintaining a constant temperature while maintaining an appropriate humidity. Steam curing conditions are preferably a maximum temperature of 40 to 80°C and a curing time of 2 to 8 hours, more preferably a maximum temperature of 40 to 75°C and a curing time of 2.5 to 7.5 hours, and even more preferably a maximum temperature of 45 to 60°C and a curing time of 3 to 7 hours. Steam curing performed with the maximum temperature of the atmosphere around the cement composition during steam curing within the above ranges and the curing time within the above ranges makes it easier to enable early demolding of the hardened body.

[0045] The relative humidity around the cement composition during steam curing is preferably 50% RH or higher, more preferably 75% RH or higher, and even more preferably 90% RH or higher. There is no upper limit, but it may be 100% RH. When the relative humidity around the cement composition during steam curing is within the above range, it becomes easier to quickly demold the hardened body.

[0046] The curing step preferably includes a pre-curing step. The pre-curing conditions are preferably a temperature of 10 to 50°C, maintained constant for about 1 to 3 hours. By including the pre-curing step in the curing step, the temperature inside the poured cement composition can be made uniform, making it easier to prevent thermal cracking due to the temperature difference between the inside and outside.

[0047] The curing step preferably includes a heating step. As the heating method, a known method can be used, and heating is preferably performed at a temperature increase rate of 10 to 30°C / hour, more preferably at a temperature increase rate of 12 to 28°C / hour, and even more preferably at a temperature increase rate of 15 to 25°C. When the temperature increase rate in the heating step is within the above range, hardening can be further promoted while preventing thermal cracking due to a sudden temperature increase in the cement composition.

[0048] The curing step preferably includes a temperature holding step. A known method can be used as the temperature holding method, and a constant temperature is preferably maintained within a temperature range of 40 to 80°C for 1 to 8 hours, more preferably within a range of 40 to 75°C for 1 to 6 hours, and even more preferably within a range of 45 to 65°C for 2.5 to 5 hours. By maintaining a constant temperature within the above-mentioned range in the temperature holding step, the poured cement composition can be hardened uniformly, which facilitates early demolding.

[0049] The method for producing a hardened body preferably includes a natural cooling step after the curing step. In the natural cooling step, the hardened body obtained in the curing step is naturally cooled in a room temperature atmosphere. The cooling time is not particularly limited, but it is sufficient that the hardened body is cooled to a temperature at which it can be easily demolded, and may be about 0.5 to 2 hours. By including the natural cooling step after the curing step, thermal cracking of the hardened body can be prevented.

[0050] The present invention will be further explained below based on experimental examples, but the present invention is not limited to these.

[0051] Experimental Example 1: Mortar was prepared using the following materials, with a water / cement ratio of 45% and a cement / aggregate ratio of 1:2.5 (by mass). A water-reducing agent was added to the resulting mortar in the proportions shown in Table 1, and the hydraulic material hardening accelerator, having the composition shown in Table 1, was mixed in the amounts shown in Table 1 to prepare a cement composition. The flow value of the resulting cement composition was measured, and the flow rate was calculated. The initial flow time was also measured. Both results are shown in Table 1. The prepared cement composition was filled into a formwork measuring 4 × 4 × 16 cm and then steam-cured to obtain a hardened body. The steam-curing conditions were as follows: 1 hour of pre-curing at 20°C, 1.5 hours of temperature increase at a rate of 20°C / hour, 3 hours of temperature hold at 50°C, and 0.5 hours of natural cooling. The compressive strength of the resulting hardened body was measured. The results are shown in Table 1.

[0052] (Materials used) Cement: Ordinary Portland cement (commercially available), Blaine specific surface area 3,200 cm 2 / g, specific gravity 3.15g / cm 3 Water: Tap water Aggregate: River sand from the Himekawa River system in Niigata Prefecture Water reducing agent: Polycarboxylic acid-based high-performance water reducing agent (commercially available) Calcium formate: Reagent Calcium sulfate (inorganic calcium compound): Reagent Sodium sulfate (inorganic sulfate): Anhydrous, reagent

[0053] (Measurement items) Flow change rate: In accordance with the method specified in JIS R 5201:2015 "Physical testing methods for cement," the flow values ​​of the cement composition were measured immediately after mixing and one hour after mixing. All flow values ​​immediately after mixing were about 200. Using each measured flow value, the flow change rate was calculated as (flow change rate) = 1 - (flow value one hour after mixing) / (immediately after mixing) x 100. Initial setting time: In accordance with the method specified in JIS A 1147:2019 "Test method for setting time of concrete," the penetration resistance value was measured at 3.5 N / mm. 2Compressive strength: The compressive strength of the hardened body 6 hours after steam curing (immediately after demolding) and 7 days after steam curing was measured according to the method specified in JIS R 5201:2015 "Physical testing methods for cement."

[0054]

[0055] From the results shown in Table 1, it was confirmed that the fluidity retention, setting property, and early strength development of the cement composition can be improved by using a hardening accelerator for hydraulic materials containing calcium formate, inorganic calcium compounds, and inorganic sulfates other than calcium sulfate in a predetermined ratio.

[0056] Experimental Example 2 Mortar, cement composition, and hardened product were prepared in the same manner as in Experimental Example 1, except that calcium hydroxide, calcium carbonate, and calcium oxide were used in addition to calcium sulfate as the inorganic calcium compound contained in the hardening accelerator for hydraulic materials in the proportions shown in Table 2, and the flow rate, initial time, and compressive strength were measured. The results are also shown in Table 2.

[0057] (Inorganic calcium compounds) Calcium hydroxide: Reagent Calcium carbonate: Reagent Calcium oxide: Reagent

[0058]

[0059] From the results shown in Table 2, it was confirmed that the fluidity retention, setting property, and early strength development of the cement composition can be improved by using calcium sulfate, calcium hydroxide, calcium carbonate, and calcium oxide as the inorganic calcium compound contained in the hardening accelerator for hydraulic materials. In particular, it was confirmed that the early strength development of the cement composition can be improved when calcium sulfate is contained.

[0060] Experimental Example 3 Mortar, cement composition, and hardened product were prepared in the same manner as in Experimental Example 1, except that aluminum sulfate, potassium alum, and sodium thiosulfate were used as inorganic sulfates in the hardening accelerator for hydraulic materials in the proportions shown in Table 3. The flow rate, initial time, and compressive strength were measured. The results are also shown in Table 3.

[0061] (Inorganic sulfates) Aluminum sulfate: Reagent Potassium alum: Reagent Sodium thiosulfate: Reagent

[0062]

[0063] From the results shown in Table 3, it was confirmed that the fluidity retention, setting property, and early strength development of the cement composition can be improved by using sodium sulfate, aluminum sulfate, potassium alum, and sodium thiosulfate as inorganic sulfates contained in the hardening accelerator for hydraulic materials. In particular, it was confirmed that when sodium sulfate and aluminum sulfate are contained, the early strength development can be further improved, and in particular, when sodium sulfate is contained, the fluidity retention can also be further improved.

[0064] Experimental Example 4 Mortar, cement composition, and hardened product were prepared in the same manner as in Experimental Example 1, except that calcium sulfoaluminate was further added to the hardening accelerator for hydraulic materials in the proportions shown in Table 4, and the flow rate, initial time, and compressive strength were measured. The results are also shown in Table 4.

[0065] (Calcium sulfoaluminate) First-grade reagent calcium carbonate, calcium sulfate dihydrate, and aluminum hydroxide were used to prepare CaO:CaSO 4 :Al 2 O 3 The mixture was mixed so that the molar ratio was 4:3:1, and the mixture was baked at 1,400°C for 2 hours and allowed to cool to room temperature, resulting in a Blaine specific surface area of ​​3,500 cm 2 A sample product was crushed to a concentration of 1 / g.

[0066]

[0067] From the results shown in Table 4, it was confirmed that when the hardening accelerator for hydraulic materials further contains calcium sulfoaluminate, the early strength development can be improved.

[0068] Experimental Example 5 Mortar, cement composition, and hardened product were prepared in the same manner as in Experimental Example 1, except that the mixing amount of the hardening accelerator for hydraulic materials was set to the ratio shown in Table 5, and the flow rate, initial time, and compressive strength were measured. The results are also shown in Table 5.

[0069]

[0070] From the results shown in Table 5, it was confirmed that by adjusting the amount of hardening accelerator for hydraulic materials to fall within a predetermined range, the fluidity retention, setting property, and early strength development of the cement composition can be improved.

[0071] Experimental Example 6 Mortar, cement composition, and hardened product were prepared in the same manner as in Experimental Example 1, except that blast furnace cement and fly ash cement were used as the cement for the cement composition, and the flow rate, initial time, and compressive strength were measured. The results are also shown in Table 6.

[0072] (Cement) Blast furnace type B cement: commercially available product, Blaine specific surface area 3,200 cm 2 / g, specific gravity 3.15g / cm 3 Blast furnace type C cement: commercially available product, Blaine specific surface area 3,500 cm 2 / g, specific gravity 3.15g / cm 3 Fly ash cement type B: commercially available product, Blaine specific surface area 3,200 cm 2 / g, specific gravity 3.15g / cm 3

[0073]

[0074] From the results shown in Table 6, it was confirmed that even when blast furnace cement or fly ash cement is used as the cement for the cement composition, the fluidity retention, setting property, and early strength development of the cement composition can be improved.

[0075] From the above results, it was confirmed that the hardening accelerator for hydraulic materials of the present invention can improve the fluidity retention, setting properties, and early strength development of the cement composition by containing calcium formate, inorganic calcium compound, and inorganic sulfate in a predetermined ratio.

[0076] The hardening accelerator for hydraulic materials of the present invention contains calcium formate, an inorganic calcium compound, and an inorganic sulfate other than calcium sulfate in a predetermined ratio, thereby improving the fluidity retention, setting property, and early strength development of hydraulic materials. Therefore, the accelerator can be widely used in the fields of civil engineering and construction, such as for hardened concrete used in precast construction methods.

Claims

1. A hardening accelerator for hydraulic materials containing 20.0 to 80.0 mass% calcium formate, 15.0 to 70.0 mass% inorganic calcium compound, and 0.5 to 30.0 mass% inorganic sulfate other than calcium sulfate.

2. The hardening accelerator for hydraulic materials according to claim 1, wherein the inorganic calcium compound is one or more selected from the group consisting of calcium sulfate, calcium hydroxide, calcium carbonate, and calcium oxide.

3. The hardening accelerator for hydraulic materials according to claim 1 or 2, wherein the inorganic sulfate is one or more selected from the group consisting of sulfates, thiosulfates, sulfites, bisulfites, pyrosulfates, and pyrobisulfites.

4. The hardening accelerator for hydraulic materials according to claim 1 or 2, further comprising 4.5 to 65.0 mass % calcium sulfoaluminate.

5. A cement composition comprising the hardening accelerator for hydraulic materials according to claim 1 or 2 and cement.

6. The cement composition according to claim 5, wherein the content of the hardening accelerator for hydraulic materials is 0.5 to 10 mass %.

7. A hardened body obtained by hardening the cement composition according to claim 5.

8. A method for producing a hardened product, comprising hardening a cement composition containing the hardening accelerator for hydraulic materials according to claim 1 and cement by steam curing at a maximum temperature of 40 to 80°C for 2 to 8 hours.