Method for producing oxygen carrier, method for producing hydrogen, and apparatus for producing hydrogen

MYPI2025005840A0Undetermined Publication Date: 2024-09-28JAPAN CARBON FRONTIER ORGANIZATION +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005840
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-25
Publication Date
2024-09-28

AI Technical Summary

Technical Problem

Current oxygen carriers used in chemical looping combustion, such as natural iron ores, have low reaction activity and are expensive, making it difficult to produce a highly active oxygen carrier at a low cost.

Method used

A method involving the reaction of iron titanate particles with an alkali component at high temperatures to form high melting point alkali titanate and liberate highly dispersed iron oxide, creating a highly active oxygen carrier, which can be used in hydrogen production processes.

Benefits of technology

The method produces a highly active oxygen carrier at a low cost, enhancing reaction activity for chemical looping combustion, gasification, and hydrogen production, with improved reactivity in reduction and steam oxidation reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005840_DRAWING_001
    Figure PI2025005840_DRAWING_001
  • Figure PI2025005840_DRAWING_002
    Figure PI2025005840_DRAWING_002
  • Figure PI2025005840_DRAWING_003
    Figure PI2025005840_DRAWING_003
Patent Text Reader

Abstract

Problem Provided is a method for producing a highly active oxygen carrier at low cost, and a method for producing hydrogen and an apparatus for producing hydrogen using the highly active oxygen carrier. Solution A method for producing an oxygen carrier of the present invention is a method for producing an oxygen carrier formed of an activated iron titanate containing an alkali titanate and an iron oxide by calcining a mixture of iron titanate particles and an alkali component. The mixture of the iron titanate particles and the alkali component is prepared by any of: physically mixing the iron titanate particles and an alkaline compound; and spraying an aqueous solution of the alkaline compound to the iron titanate particles or impregnating the iron titanate particles with the aqueous solution of the alkaline compound and then drying the sprayed or impregnated iron titanate particles. Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Oxygen carrier manufacturing method, hydrogen manufacturing method, and hydrogen manufacturing device

[0001] The present invention relates to a method for producing an oxygen carrier, a method for producing hydrogen, and a hydrogen production device.

[0002] The chemical looping combustion method is a method of burning fuel without direct contact of the fuel with air by using an oxygen carrier. In this combustion method, the fuel is burned with oxygen in the oxygen carrier, and high concentrations of carbon dioxide are recovered (see, for example, Patent Document 1). The chemical looping technology is also used for fuel gasification. In such chemical looping technology, an inexpensive and highly active oxygen carrier is required.

[0003] Iron oxide-based materials have been widely used as oxygen carriers for chemical looping combustion. However, natural iron ores (hematite, magnetite, ilmenite, etc.) do not meet the requirements due to their low reactivity. Examples of oxygen carriers made of synthetic materials include FeO / Al 2 O 3 These materials are expensive and have the drawback of being easily powdered.

[0004] JP 2018-58002 A

[0005] Although there is a demand for a highly active oxygen carrier that can be produced inexpensively, one has not yet been obtained. Therefore, an object of the present invention is to provide a method for producing a highly active oxygen carrier inexpensively, and a method and apparatus for producing hydrogen using the highly active oxygen carrier.

[0006] As a result of extensive research aimed at solving the above problems, the present inventors have noticed that alkaline components such as potassium tend to preferentially bond with titanium oxide in iron titanate at high temperatures to form alkali titanate, which then liberates highly dispersed iron oxide. They have discovered that a mixture of iron titanate and an alkaline component can be reacted at high temperatures to form a high-melting-point alkali titanate in the iron titanate, thereby liberating highly dispersed iron oxide, and have completed the present invention.

[0007] The present invention is a method for producing an oxygen carrier consisting of activated iron titanate containing an alkali titanate and iron oxide by firing a mixture of iron titanate particles and an alkali component, characterized in that the mixture of iron titanate particles and an alkali component is prepared by either physically mixing the iron titanate particles with an alkali compound, or by spraying or impregnating the iron titanate particles with an aqueous solution of the alkali compound, followed by drying.

[0008] The present invention also provides a method for producing an oxygen carrier comprising activated iron titanate containing an alkali titanate and iron oxide by calcining a mixture of iron titanate particles and an alkali component, characterized in that the iron titanate particles are brought into contact with the alkali component in a high-temperature reactor.

[0009] Furthermore, the present invention provides a hydrogen production method comprising: an air combustion step of burning fuel in the presence of iron titanate particles; a fuel reaction activation step of bringing the iron titanate particles into contact with an alkali component to produce activated iron titanate containing an alkali titanate and iron oxide; and a hydrogen production step of producing hydrogen by reacting the iron oxide produced in the fuel reaction activation step with water vapor.

[0010] Furthermore, the present invention provides a hydrogen production device comprising: an air combustion tower that combusts fuel in the presence of iron titanate particles; a fuel reaction activation tower that brings the iron titanate particles into contact with an alkali component to produce activated iron titanate containing alkali titanate and iron oxide; and a hydrogen production tower that produces hydrogen by reacting the iron oxide produced in the fuel reaction activation tower with water vapor.

[0011] According to the present invention, it is possible to provide a method for inexpensively producing a highly active oxygen carrier, and a method and apparatus for producing hydrogen using the highly active oxygen carrier.

[0012] FIG. 1 is a schematic diagram illustrating a hydrogen production method of the present invention. FIG. 2 is a graph showing the results of equilibrium composition calculation. FIG. 3 is a graph showing the results of equilibrium composition calculation. FIG. 4 is a graph showing the results of equilibrium composition calculation. FIG. 5 is a graph showing the results of equilibrium composition calculation. FIG. 6 is an XRD profile of activated ilmenite. FIG. 7 is an XRD profile of activated ilmenite. FIG. 8 is an XRD profile of activated ilmenite. FIG. 9 is a schematic diagram of an apparatus used for an oxidation-reduction reaction of activated ilmenite. FIG. 10 is a graph showing the mass change rate in the reduction reaction of activated ilmenite. FIG. 11 is a graph showing the mass change rate in the steam oxidation reaction of activated ilmenite. FIG. 12 is a graph showing the effect of the potassium loading amount on the reduction reactivity of activated ilmenite. FIG. 13 is a graph showing the effect of the (K / Ti) ratio on the reduction reactivity of activated ilmenite. FIG. 14 is a graph showing the effect of the potassium loading amount on the steam oxidation reactivity of activated ilmenite.

[0013] The method for producing an oxygen carrier, the method for producing hydrogen, and the hydrogen production device of the present invention are described below. In the present invention, an oxygen carrier is produced by activating iron titanate particles by reacting them with an alkali component. Natural iron titanate (ilmenite) is known as an inexpensive natural sand-like mineral. The content of titanium oxide in iron titanate is not particularly specified, but it is preferable that the titanium oxide content is at least half. The alkali component refers to potassium, sodium, etc.

[0014] Among iron titanates, Fe 2 TiO 5 When a mixture of ilmenite and alkali is calcined, high-melting potassium titanate is formed as shown in the following formula (1), which liberates harmless iron oxide. In this specification, potassium titanate (K 2 TiO 3 ) and iron oxide (hematite: Fe 2 O 3 The combination of Fe and FeO is called activated ilmenite. Activated ilmenite is useful as a highly active oxygen carrier. Since ilmenite is a natural sandy ore, it has become possible to produce a highly active oxygen carrier at low cost. 2 TiO5 +K 2 CO 3 ⇒ K 2 TiO 3 +Fe 2 O 3 +CO 2 (1)

[0015] Ilmenite particles having a particle diameter of about 10 to 500 μm can be used. The ilmenite particles can be physically mixed with an alkali compound to prepare a mixture. Specific examples of the alkali compound include potassium carbonate, potassium bicarbonate, potassium hydroxide, sodium carbonate, sodium bicarbonate, and sodium hydroxide. It is preferable to mix about 10 parts by mass of the alkali compound with 100 parts by mass of the ilmenite particles. For example, the desired mixture can be obtained by stirring for about 1 to 10 minutes using potassium carbonate or the like.

[0016] The mixture of ilmenite particles and alkali can also be prepared by spraying or impregnating with an aqueous solution of an alkali compound. When spraying, for example, potassium carbonate is dissolved in pure water to prepare an aqueous solution with a concentration of 50 to 100% by mass, and the resulting aqueous solution is sprayed onto the ilmenite particles. The aqueous solution is preferably sprayed while shaking the ilmenite particles. When impregnating, for example, potassium carbonate is dissolved in pure water to prepare an aqueous solution with a concentration of 5 to 10% by mass. The ilmenite particles are stirred in the aqueous solution for about 30 to 60 minutes, allowing the alkali to be impregnated into the ilmenite particles. The ilmenite particles sprayed with or impregnated with the aqueous solution of the alkali compound are dried using a dryer or the like at 100 to 120°C for about 30 to 60 minutes, yielding the desired mixture.

[0017] The mixture is placed in an alumina container and calcined, for example, at 800 to 980°C for about 0.5 to 3 hours, to produce alkali titanate and liberate iron oxide. The calcination temperature is preferably 800 to 950°C, more preferably 900 to 920°C. The calcination time can be appropriately selected depending on the calcination temperature.

[0018] Alternatively, activated ilmenite can be produced by contacting ilmenite particles with an alkali component in a high-temperature reactor. Specifically, an alkali compound is placed in a fluidized bed or circulating fluidized bed using ilmenite particles as a fluidizing medium, and the ilmenite particles and alkali component are reacted in the fluidized bed reactor. The temperature of the high-temperature reactor is preferably 800 to 980°C. The reaction here produces activated ilmenite containing alkali titanate and iron oxide, as shown in the above formula (1).

[0019] An alkaline fuel such as biomass or lignite may be used as the alkali supply source. The alkaline fuel is introduced into a fluidized bed or circulating fluidized bed using ilmenite particles as a fluidizing medium, and the fuel is burned or gasified. In this case, too, the ilmenite comes into contact with the alkaline compounds in the fuel, and activated ilmenite containing alkali titanate and iron oxide is obtained, as shown in the above formula (1).

[0020] Activated ilmenite can be used as an activated oxygen carrier in chemical looping combustion, gasification, and hydrogen production processes. It can also be used in the steam-iron hydrogen production process. When the iron oxide liberated from activated ilmenite is reduced to iron, it becomes a highly dispersed iron catalyst, which can also be applied to catalytic synthesis processes.

[0021] The oxygen carrier produced by the method of the present invention can be applied to the production of hydrogen, which will be explained with reference to FIG.

[0022] The air combustion tower 10 contains ilmenite particles as a circulating fluidized medium (not shown), and air 20 is introduced into it. Combustion takes place in the air combustion tower 10 at a temperature of 950°C or higher. The ilmenite particles are introduced into the fuel reaction activation tower 12 together with the exhaust gas via a first cyclone 27. A portion of the combustion exhaust gas introduced into the first cyclone 27 is introduced into a second cyclone 28, where N 2 21 and ash 22 are discharged.

[0023] An alkaline fuel 24 is introduced into the fuel reaction activation tower 12 and combusted at a temperature of about 850 to 950°C. Titanate is produced by reaction with titanium in the ilmenite. Furthermore, iron oxide in the ilmenite is reduced to obtain activated ilmenite containing potassium titanate and iron oxide. The alkaline fuel 24 can be supplied as a combination of an alkaline compound and a fuel. Alternatively, alkaline fuels such as lignite and biomass can be supplied as the alkaline fuel 24.

[0024] The reaction in the fuel reaction activation tower 12 can be expressed by the following formula, for example: 2 TiO 5 +K 2 CO 3 +1 / 2C ⇒ K 2 TiO 3 +2FeO+3 / 2CO 2

[0025] The fuel reaction activation tower 12 emits CO generated by the reaction. 2 23 is released, and activated ilmenite 25 is introduced into the hydrogen generation tower 14. Although not shown, water vapor is introduced into the hydrogen generation tower 14. In the hydrogen generation tower 14, hydrogen is produced by the following reaction: 2FeO+2 / 3H 2 O ⇒ 2 / 3Fe 3 O 4 +2 / 3H 2 The H generated here 2 26 is discharged from the hydrogen production tower 14 .

[0026] The excellent reactivity of the iron oxide liberated during the production of potassium titanate promotes the reduction reaction of the iron oxide in the fuel reaction activation tower 12. For the same reason, the hydrogen production reaction in the hydrogen production tower 14 is also promoted. The activated ilmenite produced by the method of the present invention has high reactivity and promotes the oxidation / reduction / hydrogen production reaction, so it can be effectively used for hydrogen production. In the above example, a hydrogen production method using activated ilmenite produced in a circulating fluidized bed system was described, but hydrogen can also be produced by reacting activated ilmenite produced outside the system with steam.

[0027] The present invention will be described in detail below based on examples, but the object of the present invention is not limited to these examples.

[0028] 1. Equilibrium composition calculations Using commercially available chemical equilibrium calculation software (HSC Chemistry), equilibrium calculations were performed on the formation of potassium titanate and sodium titanate from ilmenite and alkali. Initial conditions were entered for oxidizing and reducing atmospheres, and calculation results were obtained using Gibbs' principle (minimum free energy principle).

[0029] <Conditions for generating potassium titanate> Input conditions in an oxidizing atmosphere Fe 2 TiO 5 100 kmol, K 2 CO 3 20 kmol, O 2 10 kmol Input conditions in reducing atmosphere Fe 2 TiO 5 100 kmol, K 2 CO 3 20 kmol, H 2 The calculation results for the conditions for producing potassium titanate in an oxidizing atmosphere and a reducing atmosphere are shown in Figures 2 and 3, respectively.

[0030] <Conditions for generating sodium titanate> Input conditions in an oxidizing atmosphere Fe 2 TiO 5 100 kmol, Na 2 CO 3 20 kmol, O 2 10 kmol Input conditions in reducing atmosphere Fe 2 TiO 5 100 kmol, Na 2 CO 3 20 kmol, H 2 The calculation results for the conditions for producing sodium titanate in an oxidizing atmosphere and a reducing atmosphere are shown in Figures 4 and 5, respectively.

[0031] Figures 2 and 3 show that alkali components selectively bond with titanium oxide to form potassium titanate in both oxidizing and reducing atmospheres. Figures 4 and 5 also show that sodium titanate is formed in the high temperature range of 600°C to 1000°C in both oxidizing and reducing atmospheres. The above calculation results confirm that alkalis such as potassium tend to bond with titanium oxide in ilmenite at high temperatures to form alkali titanate.

[0032] 2. Production of Oxygen Carrier A mixture of ilmenite particles and alkali components was calcined to produce an oxygen carrier made of activated ilmenite by the method of the present invention.

[0033] <Physical Mixing Method> 20 g of ilmenite particles (average particle size: 120 μm) and 1.8 g of potassium carbonate were mixed by stirring to prepare a physical mixture. The obtained physical mixture was placed in an alumina container and fired at 920°C for 3 hours to produce activated ilmenite (potassium-loaded ilmenite) 1. The amount of potassium loaded in activated ilmenite 1 was approximately 2.0 wt%, and the molar ratio of potassium to titanium (K / Ti) was approximately 0.084.

[0034] <Impregnation Mixing Method> 1.8 g of potassium carbonate was dissolved in 20 mL of pure water to prepare an aqueous solution with a concentration of 10 mass %. 20 g of ilmenite particles (average particle size: 120 μm) was immersed in this aqueous solution for 60 minutes to impregnate the ilmenite particles with the aqueous solution. The ilmenite particles were removed and dried in a dryer at 120°C for approximately 60 minutes to prepare an impregnation mixture. The resulting impregnation mixture was placed in an alumina container and fired at 920°C for 3 hours to produce activated ilmenite (potassium-loaded ilmenite) 2. The potassium loading in activated ilmenite 2 was approximately 2.0 wt %, and the molar ratio of potassium to titanium (K / Ti) was approximately 0.084.

[0035] <Spray Mixing Method> 1.8 g of potassium carbonate was dissolved in 2.5 mL of pure water to prepare an aqueous solution with a concentration of 72 mass %. 20 g of ilmenite particles (average particle size: 120 μm) were shaken while spraying this aqueous solution to prepare a spray mixture. The resulting spray mixture was placed in an alumina container and fired at 920°C for 3 hours to produce activated ilmenite (potassium-loaded ilmenite) 3. The amount of potassium loaded in activated ilmenite 3 was approximately 2.0 wt %, and the molar ratio of potassium to titanium (K / Ti) was approximately 0.084.

[0036] The XRD measurement results of the produced activated ilmenite 1, activated ilmenite 2, and activated ilmenite 3 are shown in Figures 6, 7, and 8, respectively. In all of the measurement results, a peak of potassium titanate and a peak of hematite clearly appear. It was confirmed that potassium titanate and hematite are present in the activated ilmenite produced by the method of the present invention.

[0037] The reducibility and steam oxidation reactivity of activated ilmenite were evaluated using the apparatus shown in Figure 9. Specifically, 0.05 g of activated ilmenite was placed in a container, and a test was conducted under the following conditions to examine the mass change rate. For comparison, the mass change rate of unactivated ilmenite (uncalcined ilmenite) was also examined in the same manner.

[0038] Reduced CO 15% / CO 2 Steam oxidation in 20% Ar atmosphere at 900°C for 30 minutes Steam oxidation in 45% Ar atmosphere at 900°C for 15 minutes

[0039] Figure 10 shows the mass change rate in the reduction reaction, and Figure 11 shows the mass change rate in the steam oxidation reaction. Physical mixing (activated ilmenite 1), impregnation mixing (activated ilmenite 2), and spray mixing (activated ilmenite 3) all had larger mass change rates than ilmenite, and it was confirmed that they have reaction activity several times higher than ilmenite.

[0040] Next, six types of activated ilmenite (potassium-loaded ilmenite) with different potassium loadings were produced by the spray mixing method, and the effect of the potassium loading on the reduction reaction and steam oxidation reaction was investigated. The potassium loading was adjusted by changing the amount of potassium carbonate in the range of 0 to 3.8 wt%.

[0041] Figure 12 shows the change in mass change rate over time during the reduction reaction. When 0.19 wt% of potassium was supported, the mass change rate increased at the beginning of the reduction reaction, indicating enhanced reduction reactivity. In this case, the molar ratio of potassium to titanium (K / Ti ratio) was 0.008. To enhance reduction reactivity, the K / Ti ratio is preferably 0.008 or higher. As the amount of potassium supported increases, the mass change rate also tends to increase, but supporting 2 wt% or more of potassium does not significantly enhance reactivity.

[0042] FIG. 13 shows the relationship between the molar ratio of potassium to titanium (K / Ti ratio) in activated ilmenite and the mass change rate. 3 -W 0 ) / t 3 ) in W 3 , W 0 , t 3 represents the following: W 3 W: Mass change (wt%) at 3 minutes 0 t: Mass change (wt%) at 0 minutes 3 :W 3 Time (min) at point Up to the K / Ti ratio of 0.008%, the mass change rate increases rapidly. Above 0.008%, the increase in the mass change rate is relatively small.

[0043] Figure 14 shows the increase in mass change rate over time during a steam oxidation reaction. When 0.19 wt% of potassium was supported, the mass change rate increased at the beginning of the reaction, indicating that steam oxidation reactivity was enhanced. To enhance steam oxidation reactivity, the K / Ti ratio is preferably 0.008 or higher. As the amount of potassium supported increases, the mass change rate also tends to increase, but even when 2 wt% or more of potassium is supported, reactivity does not increase significantly.

[0044] The activated ilmenite produced by the method of the present invention is a highly active oxygen carrier having high reactivity, and can therefore be effectively used in chemical looping combustion and hydrogen production.

[0045] 10...air combustion tower, 12...fuel reaction activation tower, 14...hydrogen generation tower

Claims

1. A method for producing an oxygen carrier made of activated iron titanate containing an alkali titanate and iron oxide by firing a mixture of iron titanate particles and an alkali component, characterized in that the mixture of iron titanate particles and an alkali component is prepared by either physically mixing iron titanate particles and an alkali compound, or spraying or impregnating iron titanate particles with an aqueous solution of the alkali compound, followed by drying.

2. The method for producing an oxygen carrier according to claim 1, wherein said iron titanate is ilmenite.

3. The method for producing an oxygen carrier according to claim 1 or 2, wherein the alkaline compound is potassium carbonate.

4. The method for producing an oxygen carrier according to claim 1 or 2, characterized in that the calcination is carried out at 800 to 980° C. for 0.5 to 3 hours.

5. A method for producing an oxygen carrier consisting of activated iron titanate containing an alkali titanate and iron oxide by calcining a mixture of iron titanate particles and an alkali component, the method comprising contacting the iron titanate particles with the alkali component in a high-temperature reactor.

6. The method for producing an oxygen carrier according to claim 5, wherein the high-temperature reactor is a fluidized bed or a circulating fluidized bed containing iron titanate particles as a fluidizing medium.

7. The method for producing an oxygen carrier according to claim 5 or 6, wherein the temperature of the high-temperature reaction apparatus is 800 to 1000°C.

8. The method for producing an oxygen carrier according to claim 5 or 6, wherein the alkali content is supplied separately from the fuel for combustion.

9. The method for producing an oxygen carrier according to claim 5 or 6, wherein the alkali is supplied as a fuel for combustion.

10. The method for producing an oxygen carrier according to claim 9, wherein the fuel is selected from lignite and biomass.

11. A method for producing hydrogen, comprising: an air combustion step of burning a fuel in the presence of iron titanate particles; a fuel reaction activation step of bringing the iron titanate particles into contact with an alkali component to produce activated iron titanate containing an alkali titanate and iron oxide; and a hydrogen production step of producing hydrogen by reacting the iron oxide produced in the fuel reaction activation step with water vapor.

12. The method for producing hydrogen according to claim 11, wherein the fuel reaction activation step is carried out at a temperature of 800 to 980°C.

13. The method for producing hydrogen according to claim 11 or 12, wherein the alkali is supplied separately from the fuel for combustion.

14. The method for producing hydrogen according to claim 11 or 12, wherein the alkali is supplied as a fuel for combustion.

15. The method for producing hydrogen according to claim 14, wherein the fuel is selected from lignite and biomass.

16. A hydrogen production device comprising: an air combustion tower for burning fuel in the presence of iron titanate particles; a fuel reaction activation tower for bringing the iron titanate particles into contact with an alkali component to produce activated iron titanate containing alkali titanate and iron oxide; and a hydrogen production tower for producing hydrogen by reacting the iron oxide produced in the fuel reaction activation tower with water vapor.

17. The hydrogen production device according to claim 16, wherein the temperature of the fuel reaction activation tower is 800 to 980°C.

18. The hydrogen production device according to claim 16 or 17, wherein the alkali component is an alkali compound supplied separately from the fuel for combustion.

19. The hydrogen production device according to claim 16 or 17, wherein the alkali component is contained in a fuel for combustion.

20. The hydrogen production device according to claim 19, wherein the fuel is selected from lignite and biomass.

21. A method for producing hydrogen by reacting an oxygen carrier with water vapor, wherein the oxygen carrier is produced by the method according to claim 1 or 5.

22. An oxygen carrier produced by the method of claim 3 and containing potassium titanate as the alkali titanate.

23. The oxygen carrier according to claim 22, wherein the molar ratio of potassium to titanium (K / Ti) in said potassium titanate is 0.008 or more.

24. A chemical looping combustion method using the oxygen carrier of claim 23.