AI Technical Summary
Existing thermal spray powders face challenges in achieving high-density, low-surface roughness, and reduced phase separation in thermal spray coatings, particularly when using double oxides containing yttrium and aluminum, as they often result in coatings with non-uniform composition and increased porosity due to differences in boiling points and particle size distribution.
A thermal spray powder with a specific particle size distribution and composition, including a double oxide containing metal oxides like Y2O3, Al2O3, ZrO2, and Yb2O3, with a particle size D10 of 10 μm or more and D50 of 40 μm or less, and a boiling point difference of 500°C or more, is used to reduce phase separation and surface roughness, composed of granulated sintered or fused and pulverized secondary particles to enhance bonding and stability.
The proposed thermal spray powder effectively increases coating density, reduces surface roughness, and minimizes phase separation, resulting in improved thermal spray coatings with enhanced mechanical properties and uniformity.
Smart Images

Figure PI2025005863_DRAWING_001 
Figure PI2025005863_DRAWING_002 
Figure PI2025005863_DRAWING_003
Abstract
Description
Thermal spray powder
[0001] The present disclosure relates to a powder material used in additive manufacturing. The present disclosure also relates to a method for manufacturing the powder material. This application claims priority to Japanese Patent Application No. 2023-058418, filed on March 31, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present disclosure relates to thermal spray powders.
[0003] The thermal spray powder disclosed in Patent Document 1 contains a granulated and sintered powder of a double oxide containing yttrium and aluminum. The granulated and sintered powder is composed of secondary particles obtained by granulating and sintering primary particles. The secondary particles have a crushing strength of 15 MPa or more. The 10% particle size of the thermal spray powder is 6 μm or more. When X-ray diffraction of the thermal spray powder is measured, the ratio of the intensity of the X-ray diffraction peak derived from the (222) plane of yttria to the intensity of the maximum peak among the X-ray diffraction peak derived from the (420) plane of the garnet phase in the double oxide, the X-ray diffraction peak derived from the (420) plane of the perovskite phase in the double oxide, and the X-ray diffraction peak derived from the (−122) plane of the monoclinic phase in the double oxide is 20% or less. The publication also states that the use of such a thermal spray powder enables the formation of a good thermal spray coating of a double oxide containing yttrium and aluminum.
[0004] Patent No. 4560387
[0005] When using a thermal spray powder containing a double oxide, it is necessary to obtain a thermal spray coating that is highly dense and has low surface roughness, while also reducing the rate of phase separation in the thermal spray coating. In view of these circumstances, an object of the present invention is to provide a technology for increasing the density, reducing the surface roughness, and reducing the rate of phase separation in a thermal spray coating.
[0006] The thermal spray powder disclosed herein is a thermal spray powder containing a double oxide containing a plurality of metal oxides. The thermal spray powder is determined by determining the particle diameter (hereinafter referred to as "particle diameter D") at which the cumulative particle volume from the small particle diameter side accounts for 10% of the total particle volume in the cumulative particle diameter distribution based on the volumetric basis, as determined by a laser diffraction / scattering particle size distribution measurement method. 10 ") is 10 μm or more, and the particle diameter at which the cumulative particle volume from the small particle size side accounts for 50% of the total particle volume in the volume-based cumulative particle diameter distribution based on a laser diffraction / scattering particle size distribution measurement method (hereinafter referred to as "particle diameter D 50 The diameter (of the powder) of the thermal spray powder is 40 μm or less. Under a pressure of 1 atmosphere, the difference between the maximum and minimum boiling points of the plurality of metal oxides is 500° C. or more. By using a thermal spray powder of this configuration, it is possible to increase the density of the thermal spray coating, reduce the surface roughness, and decrease the rate of phase separation.
[0007] In a preferred embodiment of the thermal spray powder disclosed herein, the double oxide contains at least two of the following elements: lanthanoid elements consisting of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu; metalloid elements consisting of Si and Ge; typical elements consisting of Al and Ga; and transition elements consisting of Sc, Y, Ti, Zr, Hf, Nb, Ta, Mo, and W. According to this configuration, the effects of the technology disclosed herein can be appropriately achieved by using a thermal spray powder containing at least two of the above-mentioned elements.
[0008] In a preferred embodiment, the thermal spray powder disclosed herein contains at least two elements selected from the group consisting of Al, Si, Y, Zr, and Yb. With this configuration, the effects of the technology disclosed herein can be appropriately achieved by using a thermal spray powder containing at least two of the above elements.
[0009] In a preferred embodiment of the thermal spray powder disclosed herein, the plurality of metal oxides are Al 2 O 3 , SiO 2 , Y 2 O 3 , ZrO 2 , and Yb2 O 3 According to this configuration, by using a thermal spray powder of a double oxide containing at least two of the above metal oxides, the effects of the technology disclosed herein can be appropriately achieved.
[0010] In another preferred embodiment, the thermal spray powder disclosed herein contains Y 2 O 3 and Al 2 O 3 and Yb 2 O 3 and SiO 2 or a double oxide of SiO 2 and Al 2 O 3 By using a thermal spray powder of a double oxide containing the above double oxide, the effects of the technology disclosed herein can be appropriately achieved.
[0011] Preferably, the thermal spray powders disclosed herein are YAlO 3 , Y 4 Al 2 O 9 , Y 3 Al 5 O 12 , Yb 2 Si 2 O 7 , or 3Al 2 O 3 2SiO 2 By using a thermal spray powder containing the above-described double oxide, the effects of the technology disclosed herein can be appropriately achieved.
[0012] In another preferred embodiment, the particle diameter D of the thermal spray powder disclosed herein 50 The thickness of the thermal spray coating is 23 μm or more and 38 μm or less. This configuration can further enhance the effect of reducing the rate of phase separation in the thermal spray coating. In addition, an increase in the surface roughness of the thermal spray coating can be suppressed.
[0013] In another preferred embodiment, the particle diameter D of the thermal spray powder disclosed herein 10is 12 μm or more and 21 μm or less. With this configuration, an increase in the surface roughness of the thermal spray coating can be suppressed. In addition, an increase in the surface roughness of the thermal spray coating can be suppressed.
[0014] In another preferred embodiment, the thermal spray powder disclosed herein is composed of secondary particles in which primary particles of the double oxide are bonded to each other. This configuration tends to further suppress the occurrence of phase separation in the thermal spray coating.
[0015] Preferably, the secondary particles are granulated and sintered particles. This configuration tends to further suppress the occurrence of phase separation in the thermal spray coating.
[0016] In another preferred embodiment, the thermal spray powder disclosed herein is composed of a fused and pulverized powder of a double oxide. This configuration allows the effects of the technology disclosed herein to be appropriately achieved. Furthermore, the thermal spray powder can be obtained more easily.
[0017] FIG. 1 is a cross-sectional SEM image of the thermal sprayed coating of Example 1. FIG. 2 is a cross-sectional SEM image of the thermal sprayed coating of Example 2. FIG. 3 is a cross-sectional SEM image of the thermal sprayed coating of Example 3. FIG. 4 is a cross-sectional SEM image of the thermal sprayed coating of Example 4. FIG. 5 is a cross-sectional SEM image of the thermal sprayed coating of Example 5. FIG. 6 is a cross-sectional SEM image of the thermal sprayed coating of Example 6. FIG. 7 is a cross-sectional SEM image of the thermal sprayed coating of Example 7. FIG. 8 is a cross-sectional SEM image of the thermal sprayed coating of Example 8. FIG. 9 is a cross-sectional SEM image of the thermal sprayed coating of Example 9. FIG. 10 is a cross-sectional SEM image of the thermal sprayed coating of Example 10. FIG. 11 is a cross-sectional SEM image of the thermal sprayed coating of Example 11. FIG. 12 is a cross-sectional SEM image of the thermal sprayed coating of Example 12. Fig. 13 is a cross-sectional SEM image of the thermal spray coating of Example 13. Fig. 14 is a cross-sectional SEM image of the thermal spray coating of Example 14.
[0018] Preferred embodiments of the technology disclosed herein are described below. Matters necessary for implementing the present invention other than those specifically mentioned in this specification can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The technology disclosed herein can be implemented based on the content disclosed in this specification and the technical common sense in the relevant field. In the specification, the expression "X to Y" indicating a numerical range means "X or more and Y or less" unless otherwise specified, and also means a range "greater than X and less than Y," a range "greater than X and less than Y," and a range "greater than X and less than Y."
[0019] <Definitions> In this specification, the term "thermal spray powder" refers to a powdered material used for thermal spraying. Furthermore, in this specification, the term "composite particle" refers to a particulate matter (in the form of a particle) composed of multiple different materials, which are bonded together and behave as a single particle. Examples of composite particles include granulated particles and granulated sintered particles composed of at least two types of materials. In this specification, the term "primary particle" refers to the smallest unit that can be identified as a granular matter from its appearance among the morphological components that make up the thermal spray powder. Therefore, when the composite particle that makes up the thermal spray powder disclosed herein contains secondary particles, the particles that make up the secondary particles are referred to as primary particles, for example. Here, the term "secondary particle" refers to a particulate matter in which primary particles are bonded three-dimensionally and behave as a single particle. Examples of the "secondary particle" referred to here include granulated particles and particles that have been sintered after granulation (granulated sintered particles).
[0020] Here, "bonding" refers to the direct or indirect bonding of two or more primary particles. Examples of "bonding" include bonding between primary particles due to a chemical reaction, bonding between primary particles due to simple adsorption, bonding using the anchor effect of allowing an adhesive or the like to penetrate the unevenness of the primary particle surface, bonding between primary particles due to the electrostatic attraction effect, and bonding between primary particles formed by melting the surfaces of the primary particles. Furthermore, with regard to secondary particles composed of two or more materials, "bonding" includes bonding between primary particles formed by one material and melting the other material to form the primary particles. Furthermore, in this specification, the term "raw material particles" refers to particles that form the powder in the raw material stage used to produce the thermal spray powder disclosed herein.
[0021] <Method for measuring particle diameter> In this specification, "particle diameter D 10 " refers to the particle size at which the cumulative particle volume from the small particle size side is 10% of the total particle volume in the volume-based cumulative particle size distribution based on a laser diffraction / scattering particle size distribution measurement method. 50 " refers to the particle size at which the cumulative particle volume from the small particle size side is 50% of the total particle volume in the volume-based cumulative particle size distribution based on a laser diffraction / scattering particle size distribution measurement method. Particle size can be measured using, for example, a commercially available measuring device.
[0022] When a thermal spray powder containing a double oxide containing multiple metal oxides is thermally sprayed, for example, differences in composition may occur between splats (melted and flattened particles), resulting in the formation of a thermal spray coating with a non-uniform composition. For example, among the multiple metal oxides contained in the double oxide, a metal oxide with a relatively low boiling point may vaporize during thermal spraying, resulting in the local formation of an altered phase in addition to the main phase consisting of the double oxide in the thermal spray coating. The altered phase may be a phase consisting of a metal oxide with a relatively high boiling point, or a phase containing a larger amount of a metal oxide with a relatively high boiling point. The present inventors desired to reduce the proportion of phase separation (i.e., the proportion of altered phase) in the thermal spray coating when producing a thermal spray coating by thermal spraying such a double oxide. To this end, the present inventors investigated the composition of the thermal spray powder.
[0023] <Configuration of Thermal Spray Powder> The thermal spray powder disclosed herein contains, for example, a double oxide. The thermal spray powder is preferably made of a double oxide powder, but may contain unavoidable impurities resulting from the manufacturing process of the double oxide powder, etc. The content of the unavoidable impurities in the entire thermal spray powder is generally 5% by mass or less, preferably 3% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, and particularly preferably 0.1% by mass or less, and the closer to 0% by mass the better.
[0024] The double oxide contains, for example, multiple metal oxides. Here, under a condition of 1 atmosphere, the difference between the maximum and minimum boiling points among the multiple metal oxides is 500°C or more. It can be said that the greater the difference between the maximum and minimum boiling points of the multiple metal oxides contained in the double oxide, the more likely phase separation occurs in the formed thermal spray coating. Therefore, from the viewpoint of better realizing the effects of the technology disclosed herein, the difference between the maximum and minimum boiling points is, for example, preferably 700°C or more, preferably 1000°C or more, more preferably 1100°C or more, and even more preferably 1200°C or more or 1300°C or more. On the other hand, from the same viewpoint, the difference between the maximum and minimum boiling points is preferably approximately 3000°C or less, and may be, for example, 2500°C or less or 2300°C or less.
[0025] The plurality of metal oxides may include at least two metal oxides selected from various metal oxides, each of which has a difference between the maximum and minimum boiling points under 1 atmosphere of 500° C. or more. Examples of metal oxides include semimetallic elements such as silicon (Si), germanium (Ge), antimony (Sb), and bismuth (Bi); typical elements such as magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), zinc (Zn), aluminum (Al), gallium (Ga), indium (In), tin (Sn), and lead (Pb); scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), and the like. Examples of oxides include transition elements such as molybdenum (Mo), tungsten (W), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), silver (Ag), and gold (Au); and lanthanoid elements such as lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), terbium (Tb), europium (Er), gadolinium (Gd), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0026] Examples of metal oxides include alumina, zirconia, yttria, chromia, titania, cobalt oxide, magnesia, silica, calcia, ceria, iron oxide, nickel oxide, silver oxide, copper oxide, zinc oxide, gallium oxide, germanium oxide, strontium oxide, scandium oxide, samarium oxide, bismuth oxide, lanthanum oxide, lutetium oxide, hafnium oxide, vanadium oxide, niobium oxide, tungsten oxide, manganese oxide, tantalum oxide, terbium oxide, europium oxide, gadolinium oxide, dysprosium oxide, holmium oxide, erbium oxide, thulium oxide, praseodymium oxide, ytterbium oxide, neodymium oxide, tin oxide, antimony oxide, and molybdenum oxide.
[0027] For the boiling points of metal oxides, see, for example, the following references 1 to 3. Reference 1: G. Vesamsonov. Latest Handbook on Oxides - Physical and Chemical Properties, 2nd Revised and Expanded Edition. Nisso Tsushinsha, 1979, 209. Reference 2: G. Adachi. Science of Rare Earths. Kagaku Dojin, 1999, 198. (Source: HAIRE, RG, et al. Handbook on the Physics and Chemistry of Rare Earth, vol. 18: Lanthanide / Actinide Chemistry. 1994.) Reference 3: Chemical Society of Japan. Basic Chemistry Handbook (Revised 6th Edition). 2021.
[0028] For example, Ga 2 O 3 , GeO 2 , and Ta 2 O 5 Regarding the boiling point of Yb, the boiling point described in the above-mentioned document 1 (G. Vesamsonov, Latest Oxide Handbook - Physical and Chemical Properties, Second Revised and Expanded Edition, Japan-Soviet Press, 1979, 209.) can be referred to. 2 O 3 , CeO 2 , Nd 2 O 3 , Sm 2 O 3 , Eu 2 O 3 , Gd 2 O 3 , Dy 2 O 3 , Ho 2 O 3 , Er 2 O 3 , Tm 2 O 3 , Lu 2 O 3 , and Pr 2 O 3Regarding the boiling point of Y, reference can be made to the boiling point described in the above-mentioned document 2 (Adachi Ginya. Science of Rare Earths. Kagaku Dojin, 1999, 198. (Cited from: HAIRE, RG, et al. Handbook on the Physics and Chemistry of Rare Earth, vol. 18: Lanthanide / Actinide Chemistry. 1994.)). 2 O 3 , Al 2 O 3 , SiO 2 , ZrO 2 , W.O. 3 , and La 2 O 3 Regarding the boiling point of SiO, the boiling point described in the above-mentioned document 3 (Chemical Society of Japan, Basic Chemistry Handbook (Revised 6th Edition), 2021.) can be referred to. 2 The boiling point of tridymite (2230°C) is used as a reference.
[0029] From the viewpoint of preferably realizing the effects of the technology disclosed herein, the composite oxide preferably contains at least two of: lanthanoid elements such as La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu; semi-metal elements such as Si and Ge; typical elements such as Al and Ga; and transition elements such as Sc, Y, Ti, Zr, Hf, Nb, Ta, Mo, and W.
[0030] From the viewpoint of preferably achieving the effects of the technology disclosed herein, the thermal spray powder preferably contains at least two elements selected from the group consisting of Al, Si, Y, Zr, and Yb. The thermal spray powder preferably contains a double oxide containing at least two elements out of these five elements. The metal oxide contained in such a double oxide is, for example, alumina (Al 2 O 3 ), silica (SiO 2 ), yttria (Y 2 O 3 ), zirconia (ZrO 2 ), and ytterbium oxide (Yb 2 O 3The composite oxide may contain at least one or two of, for example, yttria (Y 2 O 3 ) and alumina (Al 2 O 3 ), double oxide with ytterbium oxide (Yb 2 O 3 ) and silica (SiO 2 ), or silica (SiO 2 ) and alumina (Al 2 O 3 ) is preferably a double oxide thereof.
[0031] In this case, the composite oxide is, for example, YAlO 3 (yttrium aluminum perovskite; YAP), Y 4 Al 2 O 9 (Yttrium Aluminum Monoclinic; YAM), Y 3 Al 5 O 12 (Yttrium aluminum garnet; YAG), Yb 2 Si 2 O 7 (ytterbium disilicate; YbDS), or 3Al 2 O 3 2SiO 2 By including such a compound in the double oxide, the rate of phase separation in the thermal spray coating can be reduced more effectively. Alternatively, the double oxide may contain, for example, zirconia (ZrO 2 ) and alumina (Al 2 O 3 ), double oxide with zirconia (ZrO 2 ) and silica (SiO 2 ), double oxide with ytterbium oxide (Yb 2 O 3 ) and alumina (Al 2 O 3 ) or yttria (Y 2 O 3 ) and silica (SiO 2 Alternatively, the double oxide may contain, for example, yttria (Y 2 O3 ) and alumina (Al 2 O 3 ) and silica (SiO 2 The compound may contain a double oxide containing three or more components, such as a double oxide with tungsten.
[0032] The double oxide is not limited to the above. The double oxide may be, for example, hafnium oxide (HfO 2 ) and alumina (Al 2 O 3 ), double oxide with hafnium oxide (HfO 2 ) and silica (SiO 2 ), double oxide with titania (TiO 2 ) and silica (SiO 2 ), double oxide with lanthanum oxide (La 2 O 3 ) and silica (SiO 2 ), double oxide with lanthanum oxide (La 2 O 3 ) and alumina (Al 2 O 3 ) may be contained.
[0033] The inventors' investigations have revealed that an increase in the proportion of small particles in a thermal spray powder containing a double oxide leads to the vaporization of metal oxides with relatively low boiling points during thermal spraying, making phase separation more likely to occur in the thermal spray coating. The inventors have also found that an increase in the proportion of large particles in a thermal spray powder tends to increase the porosity and surface roughness of the thermal spray coating. Furthermore, as a result of extensive investigations by the inventors, it has been found that by using a thermal spray powder with a predetermined particle size distribution, it is possible to increase the density, reduce the surface roughness, and reduce the proportion of phase separation in a thermal spray coating made from a thermal spray powder containing a double oxide.
[0034] The thermal spray powder disclosed herein has a particle diameter D 10 It is preferable that the particle diameter D is 10 μm or more. 10 As the particle diameter D increases, for example, the proportion of small particles decreases in the particle size distribution of the entire thermal spray powder. 10 The larger the particle diameter D10 On the other hand, from the viewpoint of suppressing an increase in the surface roughness of the thermal spray coating, the particle diameter D 10 is, for example, 40 μm or less, preferably 35 μm or less, more preferably 33 μm or less, more preferably 30 μm or less, more preferably 27.5 μm or less, and even more preferably 21 μm or less. 10 is 12 μm to 21 μm.
[0035] The thermal spray powder disclosed herein has a particle diameter D 50 The particle diameter D is preferably 40 μm or less. 50 The smaller the particle diameter D, the denser the thermal spray coating and the less the surface roughness. 50 On the other hand, from the viewpoint of suppressing an increase in the rate of phase separation in the thermal spray coating, the particle diameter D 50 is preferably 15 μm or more, more preferably 20 μm or more, and even more preferably 23 μm or more. 50 is 23 μm to 38 μm.
[0036] The thermal spray powder disclosed herein can be composed of composite particles produced by mixing, for example, multiple types of metal oxide particles (metal oxide powder) contained in a double oxide. Composite particles are particles containing multiple types of metal oxide particles, which are different materials, but which are integrated with each other and behave as a single particle. The thermal spray powder may be composed of, for example, secondary particles (composite particles) in which primary particles of the double oxide are bonded to each other. By using secondary particles (composite particles) of the double oxide as the thermal spray powder, the risk of metal oxides with relatively low boiling points vaporizing during thermal spraying can be reduced. This can reduce the proportion of phase separation in the thermal spray coating.
[0037] The form of the secondary particles (composite particles) is not limited, as long as, for example, primary particles of the double oxide are integrated and the effects of the technology disclosed herein can be achieved. The thermal spray powder disclosed herein preferably includes, for example, granulated and sintered particles. In other words, the secondary particles are preferably granulated and sintered particles. In this case, it is preferable to first produce granulated particles. In this case, the granulated particles can be produced, for example, by combining and mixing multiple types of metal oxide particles (primary particles) contained in the double oxide with other optional components (e.g., a binder, a solvent, etc.) and granulating the mixture. Alternatively, the granulated particles can also be produced by combining and mixing primary particles of the double oxide with other optional components (e.g., a binder, a solvent, etc.) and granulating the mixture.
[0038] In the granulated and sintered particles, the primary particles of the double oxide are integrated by sintering. This bonding is achieved, for example, by sintering at least a portion of the primary particles of the double oxide. Therefore, in the granulated and sintered particles, the primary particles are more firmly bonded to each other by sintering, making the secondary particles less likely to break during the thermal spraying process. This makes it difficult for metal oxides with relatively low boiling points to vaporize, thereby reducing the rate of phase separation in the thermal spray coating. Furthermore, by ensuring that the boiling point difference between the oxides contained in each double oxide is equal to or greater than a predetermined value, it is possible to suppress the vaporization of metal oxides with relatively low boiling points, thereby reducing the rate of phase separation in the thermal spray coating.
[0039] <Method for producing thermal spray powder> The thermal spray powder disclosed herein can be prepared, for example, by mixing, as raw material particles (raw material powder), multiple types of metal oxide particles (metal oxide powders) contained in a double oxide that is the material for the thermal spray powder, together with other optional components, compounding, and sintering. The thermal spray powder may be, for example, a thermal spray powder constituted of granulated and sintered particles that serve as secondary particles formed by mixing, granulating, and sintering the raw material particles (primary particles), and the primary particles are three-dimensionally bonded together with gaps between them.
[0040] When the thermal spray powder disclosed herein is composed of granulated and sintered particles, a method for producing the thermal spray powder can include, for example, a granulation step, a firing step, a crushing step, and a classification step.
[0041] The granulation process is, for example, a process of granulating raw material particles. In this process, for example, multiple types of metal oxide particles are prepared so that the desired composition ratio of the double oxide contained in the thermal spray powder can be achieved, and their surfaces are stabilized as needed with a protective agent or the like. Next, the stabilized raw material particles, along with optional components such as a binder and various additives (e.g., dispersants) added as needed, are dispersed in an appropriate solvent to prepare a dispersion. For example, a mixer such as a homogenizer or a blade-type agitator, a disperser, or the like is used to disperse the raw material particles in the solvent. Next, granulated particles are produced using the obtained dispersion using a granulation method such as wet granulation.
[0042] Examples of granulation methods include tumbling granulation, fluidized bed granulation, stirring frame granulation, crushing granulation, melt granulation, spray granulation, and microemulsion granulation. Among these, spray granulation is a preferred granulation method. According to the spray granulation method, droplets are formed from the dispersion (spray liquid) obtained as described above. The droplets are carried by an air current and passed through a spray drying apparatus (spray dryer), thereby producing granulated particles.
[0043] The concentration of the raw material particles in the spray liquid is preferably, for example, 10% by mass to 80% by mass. Examples of the binder to be added include binding agents (e.g., polyvinyl butyral resin (PVB), polyvinyl alcohol resin (PVA), polyvinyl acetate resin, polyacrylic resin, etc.). Examples of the solvent that can be used include water. The amount of binder added is preferably adjusted to a ratio of 0.05% by mass to 10% by mass (e.g., 1% by mass to 5% by mass) relative to the mass of the raw material particles.
[0044] The firing step is, for example, a step of firing the granulated particles. In the firing step, the granulated particles are fired at a predetermined temperature (generally 1000°C to 2000°C) for 1 hour to 10 hours in an air atmosphere; an inert atmosphere such as a nitrogen atmosphere or a rare gas atmosphere; or a vacuum. This predetermined temperature may be, for example, the set temperature of a firing furnace. The temperature and time when firing the granulated particles can be set as appropriate so as to achieve the desired composition, etc., of the thermal spray powder.
[0045] The crushing step is, for example, a step of crushing the fired product obtained in the firing step. The fired product may be crushed, for example, by a crusher. Examples of crushers that are preferably used include jaw crushers, cone crushers, hammer crushers, roll crushers, and stone mill-type crushers. The crushing step can produce granulated sintered particles in the form of secondary particles in which primary particles are bonded (sintered) with gaps between them. The degree to which the fired product is crushed in this step can be appropriately set so as to achieve, for example, a desired particle size distribution of the secondary particles.
[0046] The classification step is, for example, a step of classifying the secondary particles obtained in the crushing step. This allows the particle size distribution of the secondary particles to be adjusted as desired. For the classification step, for example, in addition to classification using a sieve, a classifier such as an air classifier utilizing the Coanda effect, a swirling air classifier, a forced vortex centrifugal classifier, or a semi-free vortex centrifugal classifier is used.
[0047] As described above, the method for producing a thermal spray powder has been described in terms of a case where the thermal spray powder is composed of granulated and sintered particles. However, the thermal spray powder does not necessarily have to be composed of granulated and sintered particles. In other forms, the thermal spray powder may be composed of a fused and pulverized powder of a double oxide. In producing the fused and pulverized powder, for example, first, double oxide powder is prepared as a raw material. Next, the double oxide powder is heated and melted in an electric furnace or the like to obtain a molten double oxide liquid. Next, the molten double oxide liquid is rapidly cooled and solidified to obtain a solidified product. Next, the solidified product is crushed and classified to produce a fused and pulverized powder of a double oxide as the thermal spray powder. By forming the thermal spray powder from a fused and pulverized powder of a double oxide, the thermal spray powder can be obtained more easily.
[0048] <Uses of Thermal Spray Powder> Thermal spray coatings can be produced on various substrates by thermal spraying the thermal spray powder disclosed herein using various thermal spraying methods. The thermal spray powder can be particularly preferably used to produce thermal spray coatings by plasma spraying methods such as atmospheric plasma spraying (APS), low-pressure plasma spraying (LPS), and pressurized plasma spraying. The thermal spray powder can also be suitably used for high-velocity oxygen-assisted flame (HVOF) thermal spraying, warm spray thermal spraying, and high-velocity air-assisted flame (HVAF) thermal spraying. The thermal spray powder may be supplied to a thermal spraying device in the form of a powder, or in the form of a slurry in which the powder is dispersed in an appropriate dispersion medium.
[0049] The type of substrate used to produce the thermal spray coating is not particularly limited. Examples of substrates include aluminum, aluminum alloys, iron, steel, copper, copper alloys, nickel, nickel alloys, gold, silver, bismuth, manganese, zinc, and zinc alloys. Among these, preferred examples include substrates made of widely used metallic materials, such as steels typified by various SUS materials (which may be so-called stainless steels) used as corrosion-resistant structural steels, aluminum alloys typified by 1000 series to 7000 series aluminum alloys useful as lightweight structural materials, and Ni-, Co-, or Fe-based corrosion-resistant alloys typified by Hastelloy, Inconel, Stellite, and Invar.
[0050] As described above, the thermal spray powder disclosed herein contains a double oxide containing a plurality of metal oxides. The thermal spray powder has a particle diameter D of 10% or more, at which the cumulative particle volume from the small particle diameter side accounts for 10% of the total particle volume in a volume-based cumulative particle diameter distribution based on a laser diffraction / scattering particle size distribution measurement method. 10 is 10 μm or more, and the particle diameter D is the particle diameter at which the cumulative particle volume from the small particle size side accounts for 50% of the total particle volume in the volume-based cumulative particle diameter distribution based on the laser diffraction scattering particle size distribution measurement method. 50 Under a condition of 1 atmosphere, the difference between the maximum and minimum boiling points of the plurality of metal oxides is 500° C. or more.
[0051] The thermal spray powder contains a double oxide containing a plurality of metal oxides, which enables the production of a thermal spray coating composed of double oxides. The thermal spray powder has a particle diameter D of 10 μm or more in a volume-based particle size distribution based on a laser diffraction scattering method. 10 This reduces the proportion of small particles. This makes it difficult for metal oxides with relatively low boiling points to vaporize during the thermal spraying process, and reduces the proportion of phase separation in the thermal spray coating. In addition, the thermal spray powder has a particle diameter D of 40 μm or less. 50 This results in a sharp particle size distribution for the thermal spray powder as a whole. This makes it possible to reduce the porosity of the thermal spray coating. It also makes it possible to reduce the surface roughness of the thermal spray coating.
[0052] Test examples relating to the present invention will be described below, but it is not intended that the present invention be limited to those shown in the following test examples.
[0053] <Production Example 1. Y 2 O 3 and Al 2 O 3 Thermal spray powder containing a double oxide of 50 Yttrium oxide powder (primary particles) having an average particle diameter D 50 The powder was mixed with aluminum oxide powder (primary particles) having a particle size of 0.5 μm, and dispersed in an aqueous solution containing 2 mass % of a binder (PVA) to prepare a slurry. This slurry was sprayed into an air stream using an atomizing granulator and dried to produce granulated particles. The resulting granulated particles were subjected to a firing treatment at 1600°C for 6 hours in an air atmosphere to sinter the primary particles and produce a fired product. The fired product was then crushed. Screen classification and air classification were then performed to obtain a thermal spray powder composed of granulated and sintered particles (secondary particles) with a uniform particle size. This thermal spray powder was used as the thermal spray powder of this example. The particle diameter D in this example was 10 is 11.4 μm, and the particle diameter D 50 The composition and particle size distribution of the thermal spray powder of this example are shown in the corresponding columns in Table 1.
[0054] Examples 2 to 11 The mixing ratio (mass ratio) of the yttrium oxide powder and the aluminum oxide powder in the raw material powder, the firing conditions, and the classification conditions were appropriately changed in producing the thermal spray powder of Example 1. In this way, thermal spray powders according to each example were produced that were composed of granulated and sintered particles of a double oxide having the composition and particle size distribution shown in the corresponding column in Table 1.
[0055] <Production example 2. Yb 2 O 3 and SiO 2 Thermal spray powder containing a double oxide of 50 Ytterbium silicate powder with a particle size of 23 μm was prepared. The raw material powder was subjected to sieve classification and air classification. This resulted in the production of a thermal spray powder composed of fused and pulverized powder with a uniform particle size distribution. The classification conditions were changed as appropriate to produce the thermal spray powders of each example. The composition and particle size distribution of the thermal spray powders of each example are shown in the corresponding columns of Table 2.
[0056] <Evaluation 1. Particle Size Distribution> The volumetric particle size distribution of each thermal spray powder was measured using a laser diffraction particle size analyzer (Malvern Panalytical, Mastersizer 3000). In this particle size distribution, the particle sizes at 3% cumulative from the fine particle side were obtained. The results are shown in the corresponding columns of "Dx(3)," "Dx(5)," "Dx(10)," "Dx(50)," and "Dx(90)" in Tables 1 and 2. Furthermore, the percentages (%) of particles having particle sizes of less than 25 μm, 20 μm or less, 15 μm or less, 10 μm or less, and 5 μm or less were obtained. The results are shown in the corresponding columns of "%-lower (25) μm", "%-lower (20) μm", "%-lower (15) μm", "%-lower (10) μm", and "%-lower (5) μm" in Tables 1 and 2.
[0057] <Preparation of Thermal Spray Coating> Using the thermal spray powder of each example, a thermal spray coating was prepared by atmospheric plasma spraying. The substrate was an aluminum alloy (Al6061) plate (70 mm × 50 mm × 2.3 mm) whose surface had been roughened by blasting with brown alumina abrasive (A#40). The thermal spraying conditions were as follows: Thermal spraying machine: SG-100 (manufactured by Praxair) Powder feeder: Model 1264 (manufactured by Praxair) Plasma working gas: Argon (Ar) gas (50 psi (0.34 MPa)); and Helium (He) gas (50 psi (0.34 MPa)) Plasma output: 36 kW Plasma generation voltage: 40 V Plasma generation current: 900 A Supply rate of thermal spray powder: 20 g / min Spraying distance (distance from thermal spray gun to substrate): 120 mm
[0058] <Evaluation 2. Surface Roughness (Ra)> The surface roughness (arithmetic mean roughness) Ra of the thermal spray coatings produced using the thermal spray powders of each example was measured in accordance with JIS B0601:2013. The surface roughness Ra was measured at any five points on each thermal spray coating using a surface roughness measuring device (SV-3000S CNC, manufactured by Mitutoyo Corporation), and the arithmetic mean value of these measurements was obtained as the surface roughness Ra. The results are shown in the "Ra" column of Tables 1 and 2.
[0059] <Evaluation 3. Cross-sectional structure of the thermal spray coating> For the thermal spray coatings produced using the thermal spray powders of each example, the proportions of pores, altered phases, and main phases in each thermal spray coating were measured using images obtained by observing a plane (cross-section of the thermal spray coating) perpendicular to the plane of the coating when viewed in plan view using an SEM. Specifically, the thermal spray coating was first cut together with the substrate perpendicular to the substrate surface to extract the surface to be observed (cross-section of the thermal spray coating). This cross-section was observed using an SEM to obtain a cross-sectional SEM image. The cross-sectional SEM image was analyzed using image analysis software (Image-Pro Plus, manufactured by Nippon Roper Co., Ltd.) to calculate the proportions of pores, altered phases, and main phases in the total cross-sectional area. Here, a binarization process was performed to separate the pores from other parts (altered phase and main phase), and the pore proportion (porosity) (%), defined as the proportion of the area of pores in the total cross-sectional area, was calculated. Next, a binarization process was similarly performed to separate the altered phase from the other parts (pores and main phase), and the altered phase ratio (%), which is defined as the ratio of the area of the altered phase to the total cross-sectional area, was calculated. Then, based on the following formula (A): Pore ratio (%) + Altered phase ratio (%) + Main phase ratio (%) = 100(%) (A), the main phase ratio (%) was calculated by subtracting the pore ratio (porosity) and the altered phase ratio from the total cross-sectional area. The respective results are shown in the "Porosity (%)", "Altered phase (%)", and "Main phase (%)" columns in Tables 1 and 2.
[0060] For reference, cross-sectional SEM images of the thermal sprayed coatings of each example are shown in Figures 1 to 14. The scale bar in each figure indicates 100 µm. Figure 1 is a cross-sectional SEM image of the thermal sprayed coating of Example 1. Figure 2 is a cross-sectional SEM image of the thermal sprayed coating of Example 2. Figure 3 is a cross-sectional SEM image of the thermal sprayed coating of Example 3. Figure 4 is a cross-sectional SEM image of the thermal sprayed coating of Example 4. Figure 5 is a cross-sectional SEM image of the thermal sprayed coating of Example 5. Figure 6 is a cross-sectional SEM image of the thermal sprayed coating of Example 6. Figure 7 is a cross-sectional SEM image of the thermal sprayed coating of Example 7. Figure 8 is a cross-sectional SEM image of the thermal sprayed coating of Example 8. Figure 9 is a cross-sectional SEM image of the thermal sprayed coating of Example 9. Figure 10 is a cross-sectional SEM image of the thermal sprayed coating of Example 10. Fig. 11 is a cross-sectional SEM image of the thermal sprayed coating of Example 11. Fig. 12 is a cross-sectional SEM image of the thermal sprayed coating of Example 12. Fig. 13 is a cross-sectional SEM image of the thermal sprayed coating of Example 13. Fig. 14 is a cross-sectional SEM image of the thermal sprayed coating of Example 14.
[0061]
[0062] Among Examples 1 to 11, those in which Ra was less than 7 μm, porosity was less than 7%, and the altered phase was less than 5% were evaluated as having a reduced phase separation rate in the thermal spray coating, improved density, and suppressed increase in surface roughness. As shown in Table 1, the composite oxide containing yttrium oxide and aluminum oxide (here, YAG:Y 3 Al 5 O 12 , YAP: YAlO 3 , or YAM:Y 4 Al 2 O 9 For thermal spray powders containing 10 is 10 μm or more, and the particle diameter D 50 It was found that the thermal spray powders of Examples 1 to 7, in which the particle size was 40 μm or less and the difference between the maximum and minimum boiling points among the multiple metal oxides (here, yttrium oxide and aluminum oxide) was 500°C or more under a condition of 1 atmosphere, made it possible to form a thermal spray coating in which phase separation was suppressed, density was improved, and an increase in surface roughness was suppressed.
[0063]
[0064] Regarding Examples 12 to 14, the examples in which Ra was less than 7 μm, porosity was less than 7%, and the altered phase was less than 8% were evaluated as having a reduced phase separation rate in the thermal spray coating, improved density, and suppressed increase in surface roughness. As shown in Table 2, the composite oxide containing ytterbium oxide and silica (here, YbDS:Yb 2 Si 2 O 7 For the thermal spray powder containing 10 is 10 μm or more, and the particle diameter D 50 It was found that the thermal spray powder of Example 12, in which the particle size was 40 μm or less and the difference between the maximum and minimum boiling points among the multiple metal oxides (here, ytterbium oxide and silica) was 500° C. or more under a condition of 1 atmosphere, enabled the formation of a thermal spray coating in which phase separation was suppressed, density was improved, and an increase in surface roughness was suppressed.
[0065] While specific examples of the technology disclosed herein have been described above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above.
[0066] The technology disclosed herein encompasses the inventions according to the following items 1 to 11. [Item 1] A thermal spray powder containing a double oxide containing a plurality of metal oxides, wherein the particle diameter D is such that the cumulative particle volume from the small particle diameter side accounts for 10% of the total particle volume in a volume-based cumulative particle diameter distribution based on a laser diffraction / scattering particle size distribution measurement method. 10 and a particle diameter D at which the cumulative particle volume from the small particle size side accounts for 50% of the total particle volume in a volume-based cumulative particle size distribution based on a laser diffraction / scattering particle size distribution measurement method. 50a thermal spray powder having a diameter of 40 μm or less, and a difference between the maximum and minimum boiling points of the plurality of metal oxides of 500° C. or more under a condition of 1 atmosphere. [Item 2] The thermal spray powder according to Item 1, wherein the double oxide contains at least two selected from the group consisting of lanthanoid elements La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, metalloid elements Si and Ge, typical elements Al and Ga, and transition elements Sc, Y, Ti, Zr, Hf, Nb, Ta, Mo, and W. [Item 3] The thermal spray powder according to Item 1 or 2, containing at least two selected from the group consisting of Al, Si, Y, Zr, and Yb. [Item 4] The plurality of metal oxides are at least one of Al, Si, Y, Zr, and Yb. 2 O 3 , SiO 2 , Y 2 O 3 , ZrO 2 , and Yb 2 O 3 [Item 5] Y 2 O 3 and Al 2 O 3 and Yb 2 O 3 and SiO 2 or a double oxide of SiO 2 and Al 2 O 3 [Item 6] The thermal spray powder according to any one of Items 1 to 4, which contains a double oxide of YAlO 3 , Y 4 Al 2 O 9 , Y 3 Al 5 O 12 , Yb 2 Si 2 O 7 , or 3Al 2 O 3 2SiO 2 [Item 7] The thermal spray powder according to any one of Items 1 to 5, comprising: 50[Item 8] The thermal spray powder according to any one of Items 1 to 6, wherein the particle diameter D 10 [Item 9] The thermal spray powder according to any one of items 1 to 8, wherein the particle size is 12 μm or more and 21 μm or less. [Item 10] The thermal spray powder according to item 9, wherein the secondary particles are granulated and sintered particles. [Item 11] The thermal spray powder according to any one of items 1 to 8, wherein the particle size is 12 μm or more and 21 μm or less. [Item 12] The thermal spray powder according to any one of items 1 to 8, wherein the secondary particles are granulated and sintered particles. [Item 13] The thermal spray powder according to any one of items 1 to 8, wherein the secondary particles are fused and pulverized powder of the double oxide.
Claims
1. A thermal spray powder containing a double oxide containing multiple metal oxides, in which the particle diameter D is such that the cumulative particle volume from the small particle diameter side is 10% of the total particle volume in the volume-based cumulative particle diameter distribution based on a laser diffraction scattering type particle size distribution measurement method. 10 and a particle diameter D at which the cumulative particle volume from the small particle size side is 50% of the total particle volume in a volume-based cumulative particle size distribution based on a laser diffraction scattering particle size distribution measurement method. 50 and a difference between a maximum value and a minimum value of boiling points among the plurality of metal oxides is 500° C. or more under a condition of 1 atmospheric pressure.
2. The thermal spray powder according to claim 1, wherein the double oxide contains at least two selected from the group consisting of lanthanoid elements La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, semi-metallic elements Si and Ge, typical elements Al and Ga, and transition elements Sc, Y, Ti, Zr, Hf, Nb, Ta, Mo, and W.
3. The thermal spray powder according to claim 1 or 2, which contains at least two elements selected from the group consisting of Al, Si, Y, Zr, and Yb.
4. The plurality of metal oxides are Al 2 O 3 , SiO 2 , Y 2 O 3 , ZrO 2 , and Yb 2 O 3 The thermal spray powder according to claim 1 , comprising at least two of:
5. Y 2 O 3 and Al 2 O 3 and Yb 2 O 3 and SiO 2 or SiO 2 and Al 2 O 3 The thermal spray powder according to claim 1 or 2, which contains a double oxide of 6. YAlO 3 , Y 4 A 2 O 9 , Y 3 A 5 O 12 , Yb 2 S 2 O 7 , or 3Al 2 O 3 2SiO 2 The thermal spray powder of claim 5 , comprising:
7. The particle diameter D 50 The thermal spray powder according to claim 1 or 2, wherein the average particle size is 23 μm or more and 38 μm or less.
8. The particle diameter D 10 The thermal spray powder according to claim 1 or 2, wherein the average particle size is 12 μm or more and 21 μm or less.
9. The thermal spray powder according to claim 1 or 2, wherein the primary particles of the double oxide are composed of secondary particles bonded to each other.
10. The thermal spray powder according to claim 9, wherein the secondary particles are granulated and sintered particles.
11. The thermal spray powder according to claim 1 or 2, which is composed of a fused and pulverized powder of the double oxide.