MFI zeolite and method for producing the same
Patent Information
- Application Number
- MYPI2025005865
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-22
- Filing Date
- 2024-04-04
- Publication Date
- 2024-10-07
AI Technical Summary
Existing methods for producing MFI type zeolite as an adsorbent result in large primary particle diameters, leading to aggregation and poor handling properties, and either require dispersants that affect adsorption characteristics or pulverization that reduces crystallinity and adsorption performance.
A method involving hydrothermal treatment of a composition containing a silica source, alumina source, alkali source, and n-butylamine at controlled temperatures and pressures to produce MFI type zeolite with a small average particle size and high adsorption performance without the need for dispersants or pulverization.
The method achieves MFI type zeolite with excellent handling properties and high adsorption performance for organic compounds, maintaining high crystallinity and preventing particle aggregation, thus improving slurry viscosity and adsorption efficiency.
Abstract
Description
MFI zeolite and method for producing the same
[0001] The present disclosure relates to an MFI zeolite and a method for producing the same.
[0002] MFI zeolites are used in various industrial fields as adsorbents for organic compounds. Generally, when using MFI zeolites as adsorbents, it is preferable to reduce the primary particle size and increase the specific surface area in order to increase the adsorption efficiency. For example, Patent Document 1 discloses, as an MFI zeolite suitable as an adsorbent, a pentasil zeolite with a primary particle size of about 1 μm, which is obtained by using normal propylamine as a structure-directing agent.
[0003] On the other hand, when the primary particle diameter is about 5 μm or less, the primary particles tend to aggregate and form coarse secondary particles, which results in a high viscosity when made into a zeolite slurry, making it difficult to handle.
[0004] Known methods for reducing the particle size of zeolite particles, particularly secondary particles, contained in a slurry include adding a dispersant such as an organic substance to the zeolite slurry (e.g., Patent Document 2) and pulverizing the zeolite powder.
[0005] Japanese Patent Application Publication No. 2021-11422 Japanese Patent Application Publication No. 2004-67976
[0006] In the MFI zeolite disclosed in Patent Document 1, primary particles undergo significant aggregation, resulting in the formation of coarse particles. As a result, it has not been possible to obtain MFI zeolite having a small average particle size as a powder.
[0007] On the other hand, the method of adding a dispersant disclosed in Patent Document 2 is not preferable because the dispersant affects the adsorption properties of MFI zeolite.
[0008] There is also a method of reducing the particle size by crushing MFI zeolite, but crushing reduces the particle size and the crystallinity of the zeolite, which reduces the adsorption performance.
[0009] An object of the present disclosure is to provide at least one of an MFI zeolite that has a small average particle size and high adsorption performance for organic compounds without requiring the use of a dispersant or pulverization, a method for producing the same, and an adsorbent containing the same.
[0010] The present disclosure has investigated a method for producing MFI zeolite that has excellent handleability when made into a zeolite slurry without using pulverization or a dispersant. As a result, it has been found that by manipulating the pressure inside a sealed container in the step of crystallizing the raw material, it is possible to directly crystallize MFI zeolite that has a small average particle size and high adsorption performance for organic compounds, something that could not be obtained by conventional production methods.
[0011] That is, the present invention is as set forth in the claims, and the gist of the present disclosure is as follows. [1] MFI zeolite having a D50 in an integrated volume particle size distribution of 0.5 μm or more and 5.0 μm or less, and having a peak height of the (020) plane relative to the peak height of the (101) plane in a powder X-ray diffraction pattern of 65% or more and 95% or less. [2] MFI zeolite according to the above item [1], in which the molar ratio of silica to alumina is 50 or more and 3,000 or less. [3] MFI zeolite according to any one of the above items [1] or [2], in which the frequency volume particle size distribution curve is a monomodal type. [4] MFI zeolite according to any one of the above items [1] to [3], in which the standard deviation in the volume particle size distribution is 10 μm or less. [5] MFI zeolite according to any one of the above items [1] to [4], in which the average crystal diameter is 0.1 μm or more and 5.0 μm or less. [6] BET specific surface area is 300 m 2 [7] A method for producing the MFI zeolite according to any one of [1] to [5] above, comprising a step of hydrothermally treating a composition containing a silica source, an alumina source, an alkali source, normal butylamine, and water at 100°C or higher and 150°C or lower and 0.15 MPa or higher, and then hydrothermally treating the composition at 100°C or higher and 150°C or lower while reducing the pressure at a rate of reducing pressure of 0.10 MPa / hour or higher.
[0012] According to the present disclosure, it is possible to provide at least one of an MFI zeolite that has excellent handleability when made into a zeolite slurry and has high adsorption performance for organic compounds, without requiring a method of adding a dispersant or a method of pulverizing zeolite powder, and a method for producing the same.
[0013] Hereinafter, the MFI zeolite of the present disclosure will be described with reference to an example of an embodiment. In the present disclosure, the respective configurations and parameters disclosed herein include any combination, and the upper and lower limits of the values disclosed herein include any combination. The terms used in this embodiment are as follows:
[0014] An "aluminosilicate" is a composite oxide having a structure consisting of a repeating network of aluminum (Al) and silicon (Si) via oxygen (O). Among aluminosilicates, those that have a crystalline XRD peak in their powder X-ray diffraction (hereinafter also referred to as "XRD") pattern are called "crystalline aluminosilicates," and those that do not have a crystalline XRD peak are called "amorphous aluminosilicates."
[0015] In this embodiment, the XRD pattern may be obtained by XRD measurement under the following conditions.
[0016] Acceleration current / voltage: 40 mA / 40 kV Radiation source: CuKα radiation (λ=1.5405 Å) Measurement mode: Continuous scan Scan conditions: 10° / min Measurement range: 2θ=5° to 40° Divergence vertical limiting slit: 10 mm Divergence / entrance slit: 1° Scattering slit: Open Receiving slit: Open Detector: Semiconductor detector (D / teX Ultra2) Filter: Not used XRD patterns can be measured using a general powder X-ray diffractometer (e.g., device name: Ultima IV, manufactured by Rigaku Corporation). Furthermore, crystalline XRD peaks are peaks whose peak top 2θ is identified and detected in analysis of XRD patterns using general analysis software, and examples thereof include XRD peaks whose half-width is 2θ=0.10° or less.
[0017] "Zeolite" is a compound having a regular structure in which skeleton atoms (hereinafter also referred to as "T atoms") are connected via oxygen (O), and the T atoms are at least one of metal atoms and metalloid atoms. Examples of metal atoms include one or more selected from the group consisting of aluminum (Al), titanium (Ti), iron (Fe), zinc (Zn), gallium (Ga), and tin (Sn), with aluminum being preferred. Examples of metalloid atoms include one or more selected from the group consisting of boron (B), silicon (Si), germanium (Ge), arsenic (As), antimony (Sb), and tellurium (Te), with silicon being preferred.
[0018] A "zeolite-like substance" is a compound having a regular structure in which T atoms are oxygen-mediated, and which contains at least an atom other than a metal or a metalloid in the T atom. Examples of zeolite-like substances include complex phosphorus compounds containing phosphorus (P) as the T atom, such as aluminophosphate (AlPO) and silicoaluminophosphate (SAPO).
[0019] The "skeletal structure (hereinafter also referred to as "zeolite structure")" of zeolite and zeolite-like substances is a skeletal structure specified by a skeletal structure code (hereinafter also referred to simply as a "structure code") defined by the Structure Commission of the International Zeolite Association. For example, an MFI structure is a skeletal structure specified by the structure code "MFI." The MFI structure can be identified by comparing it with the XRD pattern (hereinafter also referred to as a "reference pattern") described in the MFI Zeolite Framework Types on the IZA Structure Commission's website, http: / / www.iza-structure.org / databases / . With respect to zeolite structure, framework structure, crystalline structure or crystalline phase are used interchangeably.
[0020] In the present embodiment, "-type zeolite", such as "MFI zeolite", means a zeolite having a zeolite structure with the structure code, and preferably means a crystalline aluminosilicate having a zeolite structure with the structure code. A zeolite having a zeolite structure with the structure code "MFI" is any zeolite having an XRD peak in its XRD pattern that is identified as an MFI zeolite structure, and preferably has at least an XRD peak that can be identified as an MFI zeolite structure.
[0021] Each peak in the XRD pattern of MFI zeolite can be assigned to a lattice plane (hkl) (h, k, and l are integers) by comparing it with a reference pattern.
[0022] The "average crystal size" refers to the average particle size of primary particles, and primary particles are the smallest unit particles that can be observed independently in scanning electron microscope (hereinafter also referred to as "SEM") observation under the following conditions: SEM observation can be performed using a general scanning electron microscope (for example, device name: JSM-IT200, manufactured by JEOL Ltd.).
[0023] Acceleration voltage: 6 kV Magnification: 10,000±5,000x The average crystal size can be determined by first extracting 100±10 primary particles whose contours are observed without interruption in the SEM image, measuring the longest diameter of each extracted primary particle, and calculating the average value, which can be used as the average crystal size. The number of SEM images may be any number that allows the above-mentioned number of primary particles to be observed, and one or more SEM images may be used.
[0024] "D10," "D50," and "D90" are the particle diameters [μm] when the cumulative amount of the frequency of particle diameters in the cumulative volume particle size distribution is 10%, the particle diameters [μm] when the cumulative amount of the frequency of particle diameters is 50%, and the particle diameters [μm] when the cumulative amount of the frequency of particle diameters is 90%, respectively. D50 is used interchangeably with "median diameter."
[0025] The cumulative and frequency volume particle size distributions, as well as D10, D50, and D90 of MFI zeolite may be measured under the following conditions using a general laser diffraction / scattering particle size distribution measuring device (for example, device name: Microtrac MT3300EXII, manufactured by Microtrac BEL Co., Ltd.).
[0026] Measurement range: 0.02 to 2000 μm Particle refractive index: 1.66 Particle permeability: permeable Particle shape: non-spherical Solvent refractive index: 1.333 "Solid concentration" is the mass proportion of zeolite in the slurry, and is the concentration calculated by the following formula.
[0027] Solid content concentration [mass %] = (zeolite mass [g] / slurry mass [g]) × 100. The slurry mass in the above formula is a value obtained by measuring the mass of the slurry. The zeolite mass is a value measured by measuring the mass of the zeolite after drying the slurry after measuring the mass to obtain a solid content, and treating the solid content in air at 600°C for 1 hour.
[0028] The MFI zeolite of this embodiment will be described below.
[0029] The MFI zeolite of the present embodiment has a D50 of 0.5 μm or more and 5.0 μm or less, and in a powder X-ray diffraction pattern, the ratio of the peak height of the (020) plane to the peak height of the (101) plane (hereinafter also referred to as the "(020) / (101) peak ratio") is 65% or more and 95% or less.
[0030] The MFI zeolite of this embodiment has a D50 of 0.5 μm or more and 5.0 μm or less. MFI zeolite with a D50 of less than 0.5 μm has a high viscosity when made into a slurry and has extremely poor handleability (operability). Furthermore, if the D50 exceeds 5.0 μm, the viscosity of the slurry at high shear rates tends to increase, resulting in reduced fluidity. The D50 of the MFI zeolite of this embodiment is 1.0 μm or more or 1.5 μm or more, and can be 3.0 μm or less, preferably 1.0 μm or more and 3.0 μm or less, and more preferably 1.5 μm or more and 3.0 μm or less.
[0031] The MFI zeolite of the present embodiment preferably has a frequency volume particle size distribution curve of a monomodal type. In the present embodiment, the frequency volume particle size distribution curve being a monomodal type means that the frequency volume particle size distribution curve has a shape with a distribution having one peak, in other words, the frequency volume particle size distribution curve obtained by measuring the cumulative volume particle size distribution has a shape with one peak, preferably a curve having a shape with one inflection point of the particle diameter frequency in the frequency volume particle size distribution curve.
[0032] The MFI zeolite of this embodiment preferably has a standard deviation in its volume particle size distribution (hereinafter also simply referred to as "standard deviation") of 10 μm or less. The standard deviation of the MFI zeolite of this embodiment is 7 μm or less or 5 μm or less, and can also be greater than 0 μm or greater than 0.5 μm, preferably greater than 0 μm and less than 7 μm, and more preferably 0.5 μm or greater and less than 5 μm. When the standard deviation satisfies this range, when the MFI zeolite of this embodiment is made into a slurry, the viscosity of the resulting slurry is less likely to increase.
[0033] The "standard deviation" in this embodiment is a value obtained by dividing the difference between D90 and D10 in the cumulative volume particle size distribution by 2, and can be calculated using the following formula.
[0034] Standard deviation [μm] = (D90 [μm] - D10 [μm]) / 2 The MFI zeolite of this embodiment has a (020) / (101) peak ratio in its XRD pattern of 65% or more and 95% or less. If the (020) / (101) peak ratio is outside the above range, the amount of organic compounds adsorbed will be small. If MFI zeolite is subjected to an operation that applies strong stress to the particles, such as crushing, the (020) / (101) peak ratio tends to increase. This is thought to be because the crystallinity of the MFI zeolite is reduced, and as a result, the amount of organic compounds adsorbed will tend to be small. From the above points, the (020) / (101) peak ratio of the MFI zeolite of this embodiment can be 70% or more or 75% or more, and can be 85% or less, preferably 70% or more and 85% or less, and more preferably 75% or more and 85% or less.
[0035] In the MFI zeolite of this embodiment, the peak height of the (101) plane relative to the peak height of the (501) plane in its XRD pattern (hereinafter also referred to as the "(101) / (501) peak ratio") is preferably 50% or more and 140% or less. The (101) / (501) peak ratio is thought to be a value attributable to the 10-membered oxygen ring in the framework structure of MFI zeolite, and this value tends to increase when the structure-directing agent (hereinafter also referred to as "SDA") and alkali metal elements in the 10-membered oxygen ring are removed in the structure-directing agent removal step and cation exchange step described below. Since the adsorption amount of organic compounds at an equilibrium pressure of 0.01 kPa or more is likely to be improved, the (101) / (501) peak ratio of the MFI zeolite of this embodiment is 80% or more or 90% or more, and 140% or less or 110% or less, preferably 80% or more and 140% or less, and more preferably 90% or more and 110% or less.
[0036] In this embodiment, the "(101) plane peak" refers to an XRD peak in the XRD pattern of MFI zeolite where the lattice spacing d is 11.10±0.50 Å, the "(020) plane peak" refers to an XRD peak in the XRD pattern of MFI zeolite where the lattice spacing d is 9.97±0.10 Å, and the "(501) plane peak" refers to an XRD peak in the XRD pattern of MFI zeolite where the lattice spacing d is 3.87±0.03 Å.
[0037] The XRD pattern does not indicate the crystal structure by individual independent XRD peaks themselves, but by a single XRD pattern consisting of a group of multiple XRD peaks having specific relative intensities, and indicates the crystal structure of MFI zeolite. A change in the lattice spacing and relative intensities of the XRD peaks means a change in the crystal structure. Therefore, the crystal structure of the MFI zeolite of this embodiment can be identified by the group of XRD peaks having these relative intensities. Therefore, a change in the crystal structure changes the lattice spacing and relative intensities of the multiple XRD peaks.
[0038] The MFI zeolite of the present embodiment has an XRD peak identified as an MFI structure in its XRD pattern, and preferably has an XRD pattern including at least the following XRD peaks:
[0039] In this embodiment, the XRD pattern may include each of the XRD peaks in the above table, and may also include other XRD peaks attributed to the MFI structure.
[0040] It is more preferable that the MFI zeolite of the present embodiment contains at least the following XRD peaks in its XRD pattern.
[0041] It is more preferable that the MFI zeolite of the present embodiment contains at least the following XRD peaks in its XRD pattern.
[0042] In addition to the above-described peaks, the MFI zeolite of this embodiment may include XRD peaks having a relative intensity of less than 1%. However, these low-intensity XRD peaks do not need to be taken into consideration when identifying the crystal structure.
[0043] The MFI zeolite of the present embodiment has a molar ratio of silica to alumina (hereinafter referred to as "SiO 2 / Al 2 O 3 It is preferable that the SiO ratio is 50 or more and 3000 or less. 2 / Al 2 O 3 When the ratio is within the above range, the adsorption performance for organic compounds is likely to be high. The SiO of the MFI zeolite of this embodiment is advantageous in that it is likely to exhibit high adsorption properties for organic compounds even in the presence of water. 2 / Al 2 O 3 The ratio is preferably 100 or more and 3000 or less, more preferably 1000 or more and 3000 or less, and even more preferably 2000 or more and 3000 or less. On the other hand, the SiO of the MFI zeolite of this embodiment is preferred because it is easy to increase the amount of organic compounds adsorbed. 2 / Al 2 O 3 The ratio is preferably 50 or more and 2,000 or less, more preferably 100 or more and 1,000 or less, and even more preferably 170 or more and 500 or less.
[0044] In the MFI zeolite of the present embodiment, the ratio of the alkali metal content (hereinafter also referred to as "alkali metal content") to the total content (hereinafter also referred to as "metal content") of the silicon (Si) content, the aluminum (Al) content, and the alkali metal (M) content of the MFI zeolite is 0% by mass or more or more than 0% by mass, and can be 0.5% by mass or less or 0.1% by mass or less, preferably 0% by mass or more and 0.5% by mass or less, more preferably more than 0% by mass and 0.1% by mass or less, and even more preferably 0% by mass or more and 0.05% by mass or less.
[0045] When MFI zeolite contains two or more alkali metal elements, the alkali metal content may be the total value of the contents of the respective metal elements. For example, when the alkali metal elements include sodium (Na) and potassium (K), the alkali metal content may be the ratio of the total content of sodium and potassium to the metal content of the MFI zeolite (hereinafter also referred to as the "(Na + K) content"), and may be calculated as follows.
[0046] (Na+K) content [mass%] = {(Na+K)[g] / (Si+Al+Na+K)[g]}×100 SiO 2 / Al 2 O 3 The ratio and alkali metal content can be determined from the measured values of Si, Al, and M obtained by preparing a sample solution by dissolving MFI zeolite in a mixed aqueous solution of hydrofluoric acid and nitric acid, and measuring the sample solution by inductively coupled plasma atomic emission spectrometry (ICP-AES) using a general ICP device (for example, device name: OPTIMA 5300DV, manufactured by PerkinElmer).
[0047] The MFI zeolite of the present embodiment may contain SDA to the extent that it does not affect the adsorption performance for organic compounds. For example, when the mass (weighed value) of the entire MFI zeolite including SDA is taken as 100 mass%, the mass ratio of SDA contained in the MFI zeolite (hereinafter also referred to as "SDA content") may be 0 mass% or more and less than 6.0 mass%.
[0048] The average crystal size of the MFI zeolite of this embodiment is 0.1 μm or more, 0.5 μm or more, or 1.0 μm or more, and can be 5.0 μm or less, 3.0 μm or less, or 1.5 μm or less, and is preferably 0.1 μm or more and 5.0 μm or less, more preferably 0.5 μm or more and 3.0 μm or less, and even more preferably 1.0 μm or more and 1.5 μm or less. When the average crystal size of the MFI zeolite is within the above range, when the MFI zeolite of this embodiment is made into a slurry, it tends to exhibit low viscosity regardless of the shear rate.
[0049] The average crystal size is the average size of primary particles of MFI zeolite, and is different from the average sizes of secondary particles including aggregated particles, such as D10, D50, and D90. Furthermore, when the frequency volume particle size distribution curve shows a monomodal volume particle size distribution, the average crystal size tends to be larger than D10 and smaller than D90. The MFI zeolite of the present embodiment preferably satisfies D10 < average crystal size < D90 (unit: μm), and more preferably the frequency volume particle size distribution curve shows a monomodal volume particle size distribution and satisfies D10 < average crystal size < D90 (unit: μm).
[0050] The MFI zeolite of this embodiment has a BET specific surface area of 300 m 2 / g or more is preferred.
[0051] Since the amount of organic compounds adsorbed tends to be large, the BET specific surface area of the MFI zeolite of this embodiment is 330 m 2 / g or more or 350m 2 / g or more, and 2 / g or less or 500m 2 / g or less, and 2 / g or more 800m 2 / g or less is preferable, and 350m 2 / g or more 500m 2 / g or less is more preferable.
[0052] The BET specific surface area can be determined by measurements in accordance with JIS Z 8830:2013. That is, the BET specific surface area of a measurement sample can be measured by a single-point method using a general automatic specific surface area measurement device (for example, a device named BELSORP-mini II, manufactured by Microtrac-Bell Corporation) and nitrogen as the adsorption gas. As a pretreatment, the measurement sample can be kept in a vacuum atmosphere (10 Pa or less) at 350±50°C for 1 hour to 5 hours.
[0053] The MFI zeolite of the present embodiment has high crystallinity compared to conventional MFI zeolite after crystallization, but when made into a slurry, it has a low viscosity. For example, when the MFI zeolite of the present embodiment is made into a slurry using pure water as a solvent and having a solid content concentration of 51 mass%, it has a low viscosity at a shear rate of 1100 s -1 The viscosity at a shear rate of 1100 s is preferably 50 mPa·s or less, 30 mPa·s or less, or even 20 mPa·s or less. -1 If the viscosity at 2000 kJ / min is 1 mPa·s or more, and further 3 mPa·s or more, the adsorbent has a fluidity suitable for application to a carrier.
[0054] In this embodiment, the shear rate is 1100 s -1 The viscosity of the sample slurry can be measured using a general viscometer (for example, MCR 92, manufactured by Anton Paar) by the following method. MFI zeolite is mixed with pure water to prepare a zeolite slurry with a solid content of 51% by mass. 2 mL of the sample slurry is dropped onto the stage of a measuring device equipped with a parallel plate measuring jig (PP50), and the sample slurry is heated at a shear rate of 1100 s -1 During the measurement, the stage temperature is set to 20° C., and the gap between the measuring jig and the stage is set to 0.2 mm.
[0055] The MFI zeolite of this example preferably has an adsorption amount of toluene relative to the mass of the zeolite at an equilibrium pressure of 0.005 kPa (hereinafter also referred to as "toluene adsorption amount") of 5.0 mass% or more, more preferably 5.5 mass% or more, and even more preferably 6.0 mass% or more. The toluene adsorption amount at an equilibrium pressure of 0.01 kPa is preferably 5.0 mass% or more, more preferably 6.0 mass% or more, and even more preferably 7.0 mass% or more. The toluene adsorption amount at an equilibrium pressure of 0.1 kPa is preferably 6.0 mass% or more, more preferably 7.0 mass% or more, and even more preferably 8.0 mass% or more. The toluene adsorption amount at an equilibrium pressure of 1 kPa is preferably 8.0 mass% or more, more preferably 8.5 mass% or more, and even more preferably 9.0 mass% or more. The higher the toluene adsorption amount at each equilibrium pressure, the better, but the physical upper limit of the toluene adsorption amount can be 25.0 mass% or less or 20.0 mass% or less. Furthermore, it is preferable that the toluene adsorption power at equilibrium pressures of 0.005 kPa, 0.01 kPa, 0.1 kPa and 1 kPa all satisfy the above-mentioned values.
[0056] The amount of toluene adsorption may be measured using a common vapor adsorption measuring device (for example, device name: BELSORP-max II, manufactured by Microtrac BEL Co., Ltd.) by the following method. 3 A sample tube is filled with 20±10 mg of MFI zeolite and held in a vacuum atmosphere (10 Pa or less) at 350±50°C for 1 hour to 5 hours to prepare a measurement sample. The sample tube filled with the measurement sample is set in a vapor adsorption measurement device, and the equilibrium pressure is changed from 0.001 to 1 kPa at 25°C, and the toluene adsorption amount [mass %] is measured at 0.005 kPa, 0.01 kPa, 0.1 kPa, and 1 kPa.
[0057] The MFI zeolite of this embodiment is preferably an aluminosilicate, and more preferably a crystalline aluminosilicate. Therefore, the MFI zeolite of this embodiment preferably does not contain phosphorus, and further preferably does not contain phosphorus (P) as the T atom. The phosphorus content of the MFI zeolite of this embodiment is preferably 100 ppm by mass or less or 1 ppm by mass or less, or 0 ppm by mass or more or more than 0 ppm by mass, and examples thereof include 0 ppm by mass or more and 100 ppm by mass or less, 0 ppm by mass or more and 1 ppm by mass or less, and further more than 0 ppm by mass or less and 1 ppm by mass or less.
[0058] Next, a method for producing the MFI zeolite of this embodiment will be described.
[0059] The method for producing MFI zeolite of the present embodiment is a production method including a step of hydrothermally treating a composition containing a silica source, an alumina source, an alkali source, normal butylamine, and water (hereinafter also referred to as the "raw material composition") at 100°C or higher and 150°C or lower and 0.15 MPa or higher, and then hydrothermally treating the composition at 100°C or higher and 150°C or lower while reducing the pressure at a pressure reduction rate of 0.10 MPa / hour or higher (hereinafter also referred to as the "crystallization step"). The crystallization step allows the MFI zeolite of the present embodiment to be obtained as a crystallized product from the raw material composition.
[0060] The silica source is at least one of a silicon-containing compound and silicon (Si), and examples thereof include one or more selected from the group consisting of silica sol, fumed silica, colloidal silica, precipitated silica, sodium silicate, potassium silicate, amorphous silicic acid, crystalline aluminosilicate, and amorphous aluminosilicate. From the viewpoint of preventing the D50 of the crystallized MFI zeolite from becoming coarse, the silica source is preferably at least one of amorphous silicic acid and amorphous aluminosilicate, and more preferably amorphous aluminosilicate.
[0061] The alumina source is an aluminum compound, and is, for example, one or more selected from the group consisting of aluminum hydroxide, aluminum oxide, aluminum sulfate, sodium aluminate, aluminum chloride, and amorphous aluminosilicate. From the viewpoint of preventing the D50 of the crystallized MFI zeolite from becoming coarse, the alumina source is preferably one or more selected from the group consisting of aluminum oxide, aluminum sulfate, sodium aluminate, and amorphous aluminosilicate, and from the viewpoint of reactivity, it is more preferably at least one of aluminum sulfate and amorphous aluminosilicate, and even more preferably amorphous aluminosilicate.
[0062] Particularly preferred alumina sources and silica sources include at least one of amorphous silica, aluminum sulfate, and amorphous aluminosilicate, with amorphous aluminosilicate being preferred. 2 / Al 2 O 3 The ratio may be 10 or more, 15 or more, or 20 or more, and 10,000 or less, 1,000 or less, or 80 or less, and is preferably 10 or more and 10,000 or less, 15 or more and 1,000 or less, or 20 or more and 80 or less.
[0063] Furthermore, when another starting material contained in the raw material composition contains aluminum, it may be used as the alumina source. For example, when the silica source contains aluminum, the silica source can also be considered as the alumina source. As such a silica source, the amount of Al relative to the total mass of the silica source can be 2 O 3 An example of such an amorphous aluminosilicate is one having an aluminum content calculated as 0.001% by mass or more and 1.000% by mass or less.
[0064] The alkali source is at least one of a compound containing an alkali metal element and an alkali metal, and examples thereof include one or more selected from the group consisting of hydroxides, carbonates, sulfates, chlorides, bromides, silicates, and iodides of alkali metals. One or more selected from the group consisting of hydroxides, chlorides, bromides, and iodides is preferred, and hydroxides are more preferred.
[0065] The alkali metal element may be one or more selected from the group consisting of sodium, potassium, rubidium, and cesium, with at least one of sodium and potassium being preferred, and sodium being more preferred.
[0066] The raw material composition contains normal butylamine (hereinafter also referred to as "NBA"). This makes it difficult for the D50 of the crystallized MFI zeolite to become coarse, and makes it easier to obtain MFI zeolite with high adsorption performance for organic compounds. The raw material composition only needs to contain NBA as an SDA source, and preferably the SDA source is NBA alone. However, it may also contain an SDA source directing an MFI structure other than NBA. Examples of SDA sources other than NBA include one or more amines selected from the group consisting of di-normal butylamine, tributylamine, di-normal propylamine, tripropylamine, dipropylenetriamine, dihexamethylenetriamine, triethylenetetramine, diethylenetriamine, ethanolamine, and propanolamine; at least one quaternary ammonium cation selected from the group consisting of tetrapropylammonium and tetraethylammonium; and one or more selected from the group consisting of glycerol, alcohols, and morpholine.
[0067] The water may be at least one selected from the group consisting of distilled water, deionized water, and pure water. Furthermore, water derived from other starting materials contained in the raw material composition, such as solvents and water-containing compounds, is also considered to be water in the raw material composition.
[0068] The raw material composition does not need to contain seed crystals in order to reduce raw material costs. However, the raw material composition may contain seed crystals in an amount sufficiently small relative to the silica source and the alumina source in order to shorten the treatment time required for crystallization.
[0069] The seed crystals are preferably MFI zeolite, and the SiO 2 / Al 2 O 3 The ratio is preferably 10 or more and 4000 or less.
[0070] The seed crystals contained in the raw material composition convert aluminum and silicon in the raw material composition (excluding the seed crystals) into Al 2 O 3 and SiO 2 The aluminum and silicon in the seed crystals relative to the converted total mass are respectively Al 2 O 3 and SiO 2 The proportion of the converted total mass (hereinafter also referred to as "seed crystal content") can be 0% by mass or more, or 1% by mass or more, and 20% by mass or less, or 10% by mass or less, and preferred examples of the seed crystal content include 0% by mass or more and 20% by mass or less, more than 0% by mass and 20% by mass or less, or 1% by mass or more and 10% by mass or less.
[0071] The preferred composition of the raw material composition is the following molar composition.
[0072] SiO 2 / Al 2 O 3 Ratio = 50 or more, 200 or more, or 1000 or more, and 1500 or less, 3000 or less, or 5000 or less NBA / SiO 2 Ratio M / SiO = 0.01 or more, 0.05 or more, 0.10 or more, and 0.30 or less, 0.50 or less, 0.70 or less 2 OH / SiO ratio = 0.01 or more, 0.05 or more, or 0.10 or more, and 0.20 or less, 0.40 or less, or 0.60 or less 2 Ratio = 0.01 or more, 0.05 or more, or 0.10 or more, and 0.20 or less, 0.40 or less, or 0.60 or less H 2 O / SiO 2 Ratio = 2 or more, 6 or more, 8 or more, and 100 or less, 50 or less, 20 or less, where M represents an alkali metal element. When there are two or more alkali metal elements, M may be the total value of the metal elements. For example, when the alkali metal element M includes sodium (Na) and potassium (K), M may be expressed as M:(Na+K).
[0073] Particularly preferred compositions of the raw material composition include the following molar compositions.
[0074] SiO 2 / Al 2 O 3 Ratio = 100 or more and 5000 or less, preferably 200 or more and 4500 or less, more preferably 1000 or more and 4500 or less NBA / SiO 2 Ratio = 0.05 or more and 0.30 or less, preferably 0.10 or more and 0.30 or less M / SiO 2 Ratio = 0.01 or more and 0.30 or less, preferably 0.05 or more and 0.20 or less OH / SiO 2 Ratio = 0.01 or more and 0.30 or less, preferably 0.05 or more and 0.20 or less H 2 O / SiO 2 Ratio = 5 or more and 50 or less, preferably 8 or more and 15 or less. In this embodiment, the raw material composition preferably does not contain fluorine (F) or fluorine-containing compounds (hereinafter also referred to as "fluorine, etc."). Fluorine, etc. are particularly corrosive, and a production method using them requires special production equipment that exhibits corrosion resistance. This tends to increase production costs. Therefore, the raw material composition preferably does not contain fluorine. The fluorine content of the raw material composition is preferably 100 ppm by mass or less or 1 ppm by mass or less, or 0 ppm by mass or more or more than 0 ppm by mass. Examples of the fluorine content include 0 ppm by mass or more and 100 ppm by mass or less, 0 ppm by mass or more and 1 ppm by mass or less, and even more than 0 ppm by mass or more and 1 ppm by mass or less.
[0075] In the crystallization step, the raw material composition is subjected to a hydrothermal treatment at 100° C. to 150° C. and 0.15 MPa or higher, thereby crystallizing the raw material composition.
[0076] If the hydrothermal treatment temperature is less than 100°C, the time required for crystallization of the raw material composition becomes very long. On the other hand, if the temperature exceeds 150°C, the secondary particle diameter, particularly D50, becomes too large. Therefore, the hydrothermal treatment temperature is 100°C or higher and 150°C or lower, and preferably 115°C or higher and 150°C or lower.
[0077] The pressure of the hydrothermal treatment (hydrothermal treatment pressure) is 0.15 MPa or more. If the pressure is less than 0.15 MPa, the crystallinity of the resulting MFI zeolite will be low, and the adsorption performance will be low. The hydrothermal treatment pressure is preferably 0.15 MPa or more and 0.70 MPa or less, and more preferably 0.20 MPa or more and 0.50 MPa or less.
[0078] In this embodiment, the pressure (hydrothermal treatment pressure) may be adjusted to the above-described value, and examples thereof include one or more methods selected from the group consisting of autogenous pressure, a method of introducing or sucking an atmospheric gas, and a method of compressing or expanding the volume of a sealed container filled with the raw material composition.
[0079] In this embodiment, the value of the pressure (hydrothermal treatment pressure) refers to the value of absolute pressure, which is expressed as the sum of atmospheric pressure and gauge pressure.
[0080] In the hydrothermal treatment, the raw material composition may be stirred or left to stand, preferably stirred. The stirring speed may be adjusted appropriately depending on the scale and structure of the apparatus used for crystallization, and may be, for example, 30 rpm or more and 500 rpm or less, or 40 rpm or more and 400 rpm or less.
[0081] The time for the hydrothermal treatment may be adjusted depending on the amount of the raw material composition to be subjected to the hydrothermal treatment and the crystallization temperature. Industrially applicable crystallization times are, for example, 5 hours or more or 10 hours or more, and 300 hours or less, 200 hours or less, or 100 hours or less, and examples thereof include 5 hours or more and 300 hours or less, or 10 hours or more and 50 hours or less.
[0082] The hydrothermal treatment in the crystallization step is carried out by filling the raw material composition into a sealed container. The sealed container may be any container that can seal the raw material composition and has sufficient durability against the pressure generated during the hydrothermal treatment.
[0083] In the crystallization step, hydrothermal treatment is then performed at 100°C or higher and 150°C or lower while reducing the pressure at a pressure reduction rate of 0.10 MPa / hour or higher (hereinafter also referred to as "reduced-pressure hydrothermal treatment"). This makes it possible to directly crystallize MFI zeolite having the D50 of this embodiment from the raw material composition. The reason why MFI zeolite having the D50 of this embodiment can be directly crystallized by performing hydrothermal treatment at the above-mentioned pressure reduction rate and temperature is not clear, but it is thought that reducing the pressure at a pressure reduction rate of 0.10 MPa / hour or higher causes the raw material composition in the sealed container to tumble, suppressing aggregation of the crystallized particles, and as a result, makes it possible to directly crystallize MFI zeolite having a D50 of 0.5 μm or higher and 5.0 μm or lower.
[0084] In the crystallization step, the temperature at which heat treatment is performed while reducing the pressure (hereinafter also referred to as the "reduced-pressure hydrothermal treatment temperature") is set to 100°C or higher and 150°C or lower, thereby obtaining an MFI zeolite having the D50 of this embodiment. If the temperature is lower than 100°C, the primary particles of the MFI zeolite tend to aggregate, resulting in an excessively large D50. The reduced-pressure hydrothermal treatment temperature is 105°C or higher or 110°C or higher, and can be 140°C or lower or 130°C or lower, with 105°C or higher and 140°C or lower being preferred, and 110°C or higher and 130°C or lower being more preferred.
[0085] The pressure reduction rate in the crystallization step is 0.10 MPa / hour or more. If the pressure reduction rate is less than 0.10 MPa / hour, D50 tends to become large. The pressure reduction rate is preferably 0.10 MPa / hour or more and 0.30 MPa / hour or less, and more preferably 0.15 MPa / hour or more and 0.30 MPa / hour or less.
[0086] The pressure difference between the start and end of the reduced-pressure hydrothermal treatment is preferably 0.03 MPa or more and 0.40 MPa or less, more preferably 0.10 MPa or more and 0.40 MPa or less, and even more preferably 0.10 MPa or more and 0.35 MPa or less. This tends to make D50 smaller and improve the handleability of the slurry containing MFI zeolite.
[0087] The pressure at the start of the reduced pressure hydrothermal treatment is preferably 0.15 MPa or more and 0.70 MPa or less, and more preferably 0.20 MPa or more and 0.50 MPa or less.
[0088] The reduced pressure hydrothermal treatment may be terminated when the pressure reading is maintained at less than ±5 kPa (0.005 MPa) for at least one hour after the start of the reduced pressure hydrothermal treatment. The stable state may be maintained for at least one hour, for example, for at least one hour and up to 10 hours.
[0089] The production method of this embodiment may include, after the crystallization step, one or more steps selected from the group consisting of a washing step, a drying step, a structure-directing agent removal step, and a cation exchange step.
[0090] In the washing step, the zeolite and the liquid phase are separated into solid and liquid phases by a known method, and the zeolite obtained as a solid phase is washed with pure water.
[0091] In the drying step, moisture physically adsorbed on the zeolite is removed. Drying conditions are arbitrary, and examples include drying the zeolite in the air at 50° C. or higher and 250° C. or lower for 1 hour or longer and 120 hours or shorter using a spray dryer.
[0092] The structure-directing agent removal step removes the SDA contained in the zeolite. Examples of methods for removing the SDA include one or more methods selected from the group consisting of resin exchange treatment, pyrolysis treatment, and calcination treatment. From the viewpoint of production efficiency, the structure-directing agent removal step is preferably at least one of pyrolysis treatment and calcination treatment. In the case of calcination treatment, the calcination conditions may be appropriately adjusted depending on the amount of zeolite to be treated, and examples include calcination in air at 400°C to 700°C for 1 hour to 24 hours.
[0093] The crystallized MFI zeolite may have alkali metal elements derived from the alkali source on its ion exchange sites. In the cation exchange step, these are replaced with ammonium cations (NH 4+ ) and protons (H +Cation exchange with non-metallic cations such as ammonium cations can be performed by contacting MFI zeolite with an aqueous ammonium chloride solution. Cation exchange with protons can be performed by contacting MFI zeolite with hydrochloric acid.
[0094] The present disclosure will be described below with reference to examples. However, the present disclosure is not limited to these examples. (Identification of Crystalline Phase) An XRD pattern was obtained using a powder X-ray diffractometer (device name: Ultima IV, manufactured by Rigaku Corporation) under the following conditions.
[0095] Accelerating current / voltage: 40 mA / 40 kV Radiation source: CuKα radiation (λ=1.5405 Å) Measurement mode: Continuous scan Scan conditions: 10° / min Measurement range: 2θ=5° to 40° Divergence vertical limiting slit: 10 mm Divergence / entrance slit: 1° Scattering slit: Open Receiving slit: Open Detector: Semiconductor detector (D / tex Ultra2) Filter: Not used The crystalline phase of the sample was identified by comparing the obtained XRD pattern with the XRD pattern described in the MFI of Zeolite Framework Types on the homepage of the IZA Structure Committee, http: / / www.iza-structure.org / databases / . (Volume Particle Size Distribution) The volume particle size distribution was determined by measuring the frequency curve and the cumulative curve of the volume particle size distribution using a laser diffraction / scattering particle size distribution measuring device (device name: Microtrac MT3300EXII, manufactured by Microtrac Bell Co., Ltd.) under the following measurement conditions.
[0096] Measurement range: 0.02 to 2000 μm Particle refractive index: 1.66 Particle transmittance: transmittance Particle shape: non-spherical Solvent refractive index: 1.333 Ultrasonic pretreatment: none From the obtained cumulative volume particle size distribution, D10, D50, and D90 were obtained. From the obtained D10, D50, and D90 values, the standard deviation was calculated using the following formula.
[0097] Standard deviation [μm] = (D90 [μm] - D10 [μm]) / 2 The shape of the frequency volume particle size distribution curve was also confirmed. (Average crystal diameter) SEM observation was carried out using a general scanning electron microscope (device name: JSM-IT200, manufactured by JEOL Ltd.) under the following conditions.
[0098] Acceleration voltage: 6 kV Magnification: 10,000±5,000 times The average crystal diameter was determined by first extracting 100±10 primary particles whose contours were observed without interruption in the SEM observation image, measuring the longest diameter of each extracted primary particle, and calculating the average value, which was then used as the average crystal diameter.
[0099] (Composition Analysis) For composition analysis, a sample solution was prepared by dissolving the sample in a mixed aqueous solution of hydrofluoric acid and nitric acid. The sample solution was measured by inductively coupled plasma atomic emission spectrometry (ICP-AES) using a general ICP device (device name: OPTIMA5300DV, manufactured by PerkinElmer). From the measured values of Si, Al, and Na obtained, the SiO 2 / Al 2 O 3 The ratio and Na content (alkali metal content) were determined.
[0100] (BET Specific Surface Area) The BET specific surface area of the sample was determined by measurement in accordance with JIS Z 8830:2013. A general specific surface area measuring device (device name: BELSORP-mini II, manufactured by Microtrac-Bell Corporation) was used for the measurement. As a pretreatment, the measurement sample was held in a vacuum atmosphere (10 Pa or less) at 350°C for 2 hours. For the measurement sample after the pretreatment, the BET specific surface area was measured by the single-point method using nitrogen as the adsorption gas.
[0101] (Toluene adsorption amount) The toluene adsorption amount was measured using a common vapor adsorption amount measuring device (device name: BELSORP-MAXII, manufactured by Microtrac-Bell Co., Ltd.) by the following method. 3 A sample tube was filled with 20 mg of MFI zeolite and held in a vacuum atmosphere (10 Pa or less) at 350°C for 2 hours to prepare a measurement sample. The sample tube filled with the measurement sample was set in a vapor adsorption measurement device, and the equilibrium pressure was changed from 0.001 to 1 kPa at 25°C, and the toluene adsorption amount [mass %] was measured at equilibrium pressures of 0.005 kPa, 0.01 kPa, 0.1 kPa, and 1 kPa.
[0102] (Viscosity Measurement) The viscosity was measured using a general viscometer (device name: MCR 92, manufactured by Anton Paar). The measurement sample was washed, solid-liquid separated, and then mixed with pure water to prepare a zeolite slurry with a solid content of 51% by mass. This was used as the sample slurry. 2 mL of the sample slurry was dropped onto the stage of the measurement device equipped with a parallel plate type measurement jig (PP50), and the shear rate was set to 100 s -1 From the 1200s -1 The shear rate was changed to 1100 s -1 During the measurement, the stage temperature was set to 20° C., and the gap between the measuring jig and the stage was set to 0.2 mm.
[0103] Example 1 NBA, pure water, sodium hydroxide and Al 2 O 3 Amorphous silicic acid having a content of 0.04% by mass was mixed to obtain a raw material composition having the following molar composition.
[0104] SiO 2 / Al 2 O 3 Ratio = 4100 Na / SiO 2 Ratio = 0.11 NBA / SiO 2 Ratio = 0.23H 2 O / SiO 2 Ratio = 11 OH / SiO 2 Ratio = 0.11 Seed crystals (MFI type zeolite, SiO 2 / Al2 O 3 After mixing with other ingredients (ratio: 2015, manufactured by Tosoh Corporation), 3,600 g of the raw material composition was filled into a 4 L airtight container and subjected to hydrothermal treatment at 120°C and a pressure of 0.31 MPa for 24 hours while stirring at 350 rpm, and then hydrothermal treatment was continued at 120°C while the hydrothermal treatment pressure was reduced to 0.20 MPa at a pressure reduction rate of 0.20 MPa / hour. After the hydrothermal treatment, the temperature was lowered to 70°C, and the crystallized product was recovered, and this was used as the MFI zeolite of this example.
[0105] The MFI zeolite of this example was an MFI zeolite (crystalline aluminosilicate) consisting of a single phase of MFI structure, with a (020) / (101) peak ratio of 76% and a (101) / (501) peak ratio of 67%. The XRD pattern of the zeolite is shown in the table below.
[0106] The MFI zeolite of this example is SiO 2 / Al 2 O 3 The ratio was 2500, the average crystal size was 1.25 μm, the Na content (alkali metal content) was 0.4 mass%, and the BET specific surface area was 392 m 2 / g, the particle diameters were D10 of 0.77 μm, D50 of 1.64 μm, and D90 of 3.05 μm, with a standard deviation of 1.14 μm. The frequency volume particle size distribution curve was monomodal.
[0107] Example 2 NBA, pure water, sodium hydroxide and Al 2 O 3 Amorphous silicic acid having a content of 0.77% by mass was mixed to obtain a raw material composition having the following molar composition.
[0108] SiO 2 / Al 2 O 3 Ratio = 220 Na / SiO 2 Ratio = 0.11 NBA / SiO 2 Ratio = 0.23H 2 O / SiO 2 Ratio = 11 OH / SiO 2Ratio = 0.11 Seed crystals (MFI type zeolite, SiO 2 / Al 2 O 3 After mixing with a mixture of 1000g of ammonium hydroxide, 2015g of ammonium hydroxide, manufactured by Tosoh Corporation, 3600g of the raw material composition was filled into a sealed container having a volume of 4L, and hydrothermal treatment was carried out for 36 hours at 130°C under a pressure of 0.40 MPa while stirring at 350 rpm, and then hydrothermal treatment was carried out at 130°C while reducing the pressure to 0.27 MPa at a pressure reduction rate of 0.20 MPa / hour. After the hydrothermal treatment, the sealed container was cooled to 70°C, and the crystallized product was recovered, and this was used as the MFI zeolite of this example.
[0109] The MFI zeolite of this example was a MFI zeolite (crystalline aluminosilicate) consisting of a single phase of MFI structure, with a (020) / (101) peak ratio of 78% and a (101) / (501) peak ratio of 65%. The XRD pattern of the zeolite is shown in the table below.
[0110] The MFI zeolite of this example is SiO 2 / Al 2 O 3 The ratio was 200, the average crystal size was 1.16 μm, the Na content (alkali metal content) was 0.3 mass%, and the BET specific surface area was 381 m 2 / g, the particle diameters were D10 of 1.40 μm, D50 of 2.69 μm, and D90 of 7.14 μm, with a standard deviation of 2.87 μm. The frequency volume particle size distribution curve was monomodal.
[0111] Example 3 The MFI zeolite of Example 1 was brought into contact with 7 mass % hydrochloric acid at 25°C for 5 minutes, washed with pure water, subjected to solid-liquid separation, and then dried in an air atmosphere at 110°C for 12 hours, thereby obtaining the MFI zeolite of this example.
[0112] The MFI zeolite of this example was an MFI zeolite (crystalline aluminosilicate) consisting of a single phase of MFI structure, with a (020) / (101) peak ratio of 82% and a (101) / (501) peak ratio of 105%. The XRD pattern of the zeolite is shown in the table below.
[0113] The MFI zeolite of this example is SiO 2 / Al 2 O 3 The ratio was 2500, the average crystal size was 1.25 μm, the Na content (alkali metal content) was 0.01 mass%, and the BET specific surface area was 338 m 2 / g, the particle diameters were D10 of 0.77 μm, D50 of 1.64 μm, and D90 of 3.05 μm, with a standard deviation of 1.14 μm. The frequency volume particle size distribution curve was monomodal.
[0114] Example 4 The MFI zeolite of Example 1 was heat-treated in an air atmosphere at 600°C for 2 hours to obtain the MFI zeolite of this example.
[0115] The MFI zeolite of this example was an MFI zeolite (crystalline aluminosilicate) consisting of a single phase of MFI structure, with a (020) / (101) peak ratio of 82% and a (101) / (501) peak ratio of 137%. The XRD pattern of the zeolite is shown in the table below.
[0116] The MFI zeolite of this example is SiO 2 / Al 2 O 3 The ratio was 2500, the average crystal size was 1.25 μm, the Na content (alkali metal content) was 0.4 mass%, and the BET specific surface area was 392 m 2 / g, the particle diameters were D10 of 0.77 μm, D50 of 1.64 μm, and D90 of 3.05 μm, with a standard deviation of 1.14 μm. The frequency volume particle size distribution curve was monomodal.
[0117] Example 5 NBA, pure water, sodium hydroxide and Al 2 O 3 Amorphous silicic acid having a content of 0.08% by mass was mixed to obtain a raw material composition having the following molar composition.
[0118] SiO 2 / Al 2 O 3 Ratio = 2100 Na / SiO 2 Ratio = 0.11 NBA / SiO 2Ratio = 0.23H 2 O / SiO 2 Ratio = 11 OH / SiO 2 Ratio = 0.11 Seed crystals (MFI type zeolite, SiO 2 / Al 2 O 3 After mixing with a mixture of 1000g of ammonium hydroxide, 2015g of ammonium hydroxide, manufactured by Tosoh Corporation, 3600g of the raw material composition was filled into a 4L airtight container and subjected to hydrothermal treatment at 120°C and a pressure of 0.30 MPa for 36 hours while stirring at 350 rpm. After that, hydrothermal treatment was continued at 120°C while the hydrothermal treatment pressure was reduced to 0.20 MPa at a pressure reduction rate of 0.20 MPa / hour. After the hydrothermal treatment, the temperature was lowered to 70°C, and the crystallized product was recovered, and this was designated as the MFI zeolite of this example.
[0119] The MFI zeolite of this example was a MFI zeolite (crystalline aluminosilicate) consisting of a single phase of MFI structure, with a (020) / (101) peak ratio of 95% and a (101) / (501) peak ratio of 76%. The XRD pattern of the zeolite is shown in the table below.
[0120] The MFI zeolite of this example is SiO 2 / Al 2 O 3 The ratio was 1500, the average crystal size was 1.32 μm, the Na content (alkali metal content) was 0.5 mass%, and the BET specific surface area was 310 m 2 / g, the particle diameters were D10 1.15 μm, D50 1.99 μm, and D90 3.17 μm, with a standard deviation of 1.01 μm. The frequency volume particle size distribution curve was monomodal.
[0121] Comparative Example 1 A raw material composition obtained in the same manner as in Example 1 was subjected to hydrothermal treatment for 24 hours at a pressure of 0.31 MPa and 120°C while stirring at 350 rpm. After the hydrothermal treatment, the temperature was lowered to 30°C, and the crystallized product was recovered, which was used as the MFI zeolite of this comparative example.
[0122] The MFI zeolite of this comparative example was an MFI zeolite (crystalline aluminosilicate) consisting of a single phase of MFI structure, with a (020) / (101) peak ratio of 75% and a (101) / (501) peak ratio of 65%. The XRD pattern of the zeolite is shown in the table below.
[0123] The MFI zeolite in this comparative example is SiO 2 / Al 2 O 3 The ratio was 2500, the average crystal size was 1.22 μm, the Na content (alkali metal content) was 0.4 mass%, and the BET specific surface area was 360 m 2 / g, the particle diameters were D10 2.49 μm, D50 37.1 μm, and D90 76.1 μm, with a standard deviation of 36.8 μm. The frequency volume particle size distribution curve was bimodal.
[0124] Comparative Example 2 A raw material composition obtained in the same manner as in Example 1 was subjected to hydrothermal treatment at a pressure of 0.31 MPa and 120° C. for 24 hours, and then the temperature was lowered to 70° C. After the temperature was lowered, the composition was subjected to hydrothermal treatment at 70° C. while reducing the pressure to 0.10 MPa (atmospheric pressure) at a pressure reduction rate of 0.20 MPa / hour, and then the crystallized product was recovered, and this was used as the MFI zeolite of this comparative example.
[0125] The MFI zeolite of this comparative example was confirmed to be an MFI zeolite (crystalline aluminosilicate) consisting of a single phase of MFI structure, with a (020) / (101) peak ratio of 75% and a (101) / (501) peak ratio of 73%. The XRD pattern of the zeolite is shown in the table below.
[0126] The MFI zeolite in this comparative example is SiO 2 / Al 2 O 3 The particle size ratio was 2600, the average crystal size was 1.29 μm, the Na content (alkali metal content) was 0.4 mass%, and the particle sizes were D10=1.86 μm, D50=8.29 μm, and D90=38.8 μm, with a standard deviation of 18.5 μm. The frequency volume particle size distribution curve was bimodal.
[0127] Comparative Example 3 The MFI zeolite of Comparative Example 1 was pulverized by the following method. That is, the MFI zeolite obtained in Comparative Example 1 was mixed with pure water to prepare a zeolite slurry with a solid content concentration of 30% by mass. The glass beads and the zeolite slurry were loaded into a wet pulverizer (device name: DYNO-MILL, MULTI LAB, manufactured by WAB Co.) so that the 1 mm diameter glass beads accounted for 80% by volume and the zeolite slurry accounted for 20% by volume relative to the capacity of the wet pulverizer, and the mixture was pulverized at a peripheral speed of 10 m / s for 10 minutes to obtain a pulverized product.
[0128] The obtained pulverized product was brought into contact with 7% by mass hydrochloric acid at 25°C for 5 minutes, washed with pure water, subjected to solid-liquid separation, and then dried in an air atmosphere at 110°C for 12 hours to obtain MFI zeolite of this comparative example.
[0129] The MFI zeolite of this comparative example was an MFI zeolite (crystalline aluminosilicate) consisting of a single phase of MFI structure, with a (020) / (101) peak ratio of 99% and a (101) / (501) peak ratio of 106%. It was confirmed that the crystallinity of the MFI zeolite of this comparative example was reduced by pulverization compared to the MFI zeolite of the examples. The XRD pattern of the zeolite of this comparative example is shown in the table below.
[0130] The MFI zeolite in this comparative example is SiO 2 / Al 2 O 3 The ratio was 2500, the average crystal size was 0.96 μm, the Na content (alkali metal content) was 0.01 mass%, and the BET specific surface area was 320 m 2 / g, the particle diameters were D10 of 0.52 μm, D50 of 0.88 μm and D90 of 1.76 μm, and the standard deviation was 0.62. The frequency volume particle size distribution curve was monomodal.
[0131] Comparative Example 4 NBA, pure water, sodium hydroxide and Al 2 O 3 Amorphous silicic acid having a content of 6.0 mass % was mixed to obtain a raw material composition having the following molar composition.
[0132] SiO 2 / Al 2 O3 Ratio = 26 Na / SiO 2 Ratio = 0.20 NBA / SiO 2 Ratio = 0.23H 2 O / SiO 2 Ratio = 11 OH / SiO 2 Ratio = 0.20 Seed crystals (MFI type zeolite, SiO 2 / Al 2 O 3 After mixing with other ingredients (ratio: 2015, manufactured by Tosoh Corporation), 3,600 g of the raw material composition was filled into a 4 L sealed container and subjected to hydrothermal treatment at 150°C and a pressure of 0.41 MPa for 36 hours while stirring at 350 rpm, and then hydrothermal treatment was performed at 130°C while reducing the pressure to 0.27 MPa at a pressure reduction rate of 0.22 MPa / hour. After the hydrothermal treatment, the sealed container was cooled to 70°C, and the crystallized product was recovered, and this was used as the MFI zeolite of this comparative example.
[0133] The MFI zeolite of this comparative example was an MFI zeolite (crystalline aluminosilicate) consisting of a single phase of MFI structure, with a (020) / (101) peak ratio of 76% and a (101) / (501) peak ratio of 54%. The XRD pattern of the zeolite is shown in the table below.
[0134] The MFI zeolite in this comparative example is SiO 2 / Al 2 O 3 The ratio was 23, the average crystal size was less than 0.1 μm, the Na content (alkali metal content) was 2.1 mass%, and the BET specific surface area was 298 m 2 / g, the particle diameters were D10 5.38 μm, D50 33.7 μm, and D90 74.7 μm, with a standard deviation of 34.7 μm. The frequency volume particle size distribution curve was bimodal.
[0135] Comparative Example 5 NBA, pure water, sodium hydroxide and Al 2 O 3 Amorphous silicic acid having a content of 0.04% by mass was mixed to obtain a raw material composition having the following molar composition.
[0136] SiO2 / Al 2 O 3 Ratio = 3900 Na / SiO 2 Ratio = 0.11 NBA / SiO 2 Ratio = 0.23H 2 O / SiO 2 Ratio = 11 OH / SiO 2 Ratio = 0.11 Seed crystals (MFI type zeolite, SiO 2 / Al 2 O 3 After mixing with other ingredients (ratio: 2015, manufactured by Tosoh Corporation), 3600 g of the raw material composition was filled into a 4 L airtight container and hydrothermally treated at 170°C under a pressure of 1.0 MPa for 36 hours while stirring at 350 rpm, and then hydrothermally treated at 130°C while the hydrothermal treatment pressure was reduced to 0.27 MPa at a pressure reduction rate of 0.20 MPa / hour. After the hydrothermal treatment, the temperature was lowered to 70°C, and the crystallized product was recovered and used as the zeolite of this comparative example.
[0137] The zeolite in this comparative example was amorphous (non-crystalline aluminosilicate).
[0138] Measurement Example 1 (Viscosity Measurement of Zeolite Slurry) Each of the MFI zeolites of Example 1, Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 4 was mixed with pure water to prepare a zeolite slurry with a solid content concentration of 51 mass%, and the viscosity of each zeolite slurry was measured. The results are shown in the table below.
[0139] From the above table, the MFI type zeolite of the example is 1100s -1 The viscosity of the zeolite slurry at a shear rate of 1000 rpm was lower than that of the MFI zeolite of the comparative example. Therefore, it was confirmed that the MFI zeolite of the example has excellent handleability when made into a zeolite slurry without pulverization or the use of a dispersant, compared to the MFI zeolite of the comparative example.
[0140] Measurement Example 2 (Measurement of Toluene Adsorption Amount) The toluene adsorption amounts of the MFI zeolites of Examples 1 to 5 and Comparative Example 3 were measured. The results are shown in the table below.
[0141] From the above table, it was confirmed that the MFI zeolites of the Examples had a higher adsorption amount of toluene at each equilibrium pressure than the MFI zeolites of the Comparative Examples.
[0142] It was confirmed that the MFI zeolite of Comparative Example 3 had a (020) / (101) peak ratio of more than 95%, i.e., had a reduced crystallinity, and therefore the amount of toluene adsorbed decreased at each equilibrium pressure.
[0143] In Example 3, the Na content was 0.1 mass% or less, and therefore it was confirmed that the toluene adsorption amount was increased at each equilibrium pressure compared to Example 1. Furthermore, in Examples 3 and 4, the (101) / (501) peak ratio was 80% or more and 140% or less, and therefore it was confirmed that the toluene adsorption amount was further improved at an equilibrium pressure of 0.01 kPa or more compared to Example 1.
[0144] The entire contents of the specification, claims and abstract of Japanese Patent Application No. 2023-62985, filed on April 7, 2023, and the entire contents of the specification, claims and abstract of Japanese Patent Application No. 2023-198053, filed on November 22, 2023, are hereby incorporated by reference as the disclosure of the specification of the present disclosure.
Claims
1. An MFI zeolite having a D50 in an accumulated volume particle size distribution of 0.5 μm or more and 5.0 μm or less, and a peak height of the (020) plane relative to the peak height of the (101) plane in a powder X-ray diffraction pattern of 65% or more and 95% or less.
2. The MFI zeolite according to claim 1, wherein the molar ratio of silica to alumina is 50 or more and 3,000 or less.
3. The MFI zeolite according to claim 1 or 2, having a frequency volume particle size distribution curve of a monomodal type.
4. An MFI zeolite according to claim 1 or 2, having a standard deviation in volumetric particle size distribution of 10 μm or less.
5. An MFI zeolite according to claim 1 or 2, having an average crystal size of 0.1 μm or more and 5.0 μm or less.
6. BET specific surface area is 300m 2 The MFI zeolite according to claim 1 or 2, wherein the MFI zeolite has a molecular weight of 1 / g or more.
7. A method for producing an MFI zeolite according to claim 1 or 2, comprising a step of hydrothermally treating a composition containing a silica source, an alumina source, an alkali source, normal butylamine and water at 100°C or higher and 150°C or lower and a pressure of 0.15 MPa or higher, and then hydrothermally treating the composition at 100°C or higher and 150°C or lower while reducing the pressure at a reduction rate of 0.10 MPa / hour or higher.