Coated ultrahigh-strength steel with excellent spot welding performance and manufacturing method therefor
Patent Information
- Application Number
- MYPI2025005866
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-26
- Publication Date
- 2024-09-27
AI Technical Summary
Existing zinc-coated ultra-high-strength steels are prone to welding cracks during spot welding, resulting in poor welding performance and becoming an application obstacle in the automotive field.
By designing a reasonable chemical composition on the steel substrate, including the ratio of carbon, silicon, manganese, chromium and other elements, and using optimized manufacturing processes, such as hot rolling, pickling, continuous annealing and zinc-containing plating, the steel plate is controlled The microstructure and coating reduce the sensitivity of solder joint surface cracks.
It achieves the excellent performance of ultra-high-strength steel during spot welding. The crack depth on the surface of the welding point is less than 5% of the plate thickness. It also meets high mechanical performance requirements and significantly improves the stability and safety of welding.
Smart Images

Figure PI2025005866_DRAWING_001
Abstract
Description
A kind of ultra-high strength steel with coating having excellent spot welding performance and its manufacturing method Technical Field
[0001] The present invention relates to high-strength steel and a manufacturing method thereof, and in particular to ultra-high-strength steel with a coating and a manufacturing method thereof. Background Art
[0002] With the advancement of automobile lightweighting and the increasing requirements of the automotive industry for vehicle corrosion resistance, many automakers have an increasing demand for ultra-high-strength steel with coatings. For cold-stamped steel, the coating is mainly zinc-containing coatings, such as hot-dip pure zinc, hot-dip galvanized iron, and electroplated pure zinc. Resistance spot welding has become the most important connection method in automotive welding production due to its advantages such as fast welding speed and low cost. Many zinc-coated ultra-high-strength steel joints often exhibit good quasi-static mechanical properties when spot welded, but a welding crack appears on the surface of the steel plate in contact with the electrode and in the surrounding area. This welding crack is called a spot welding crack. Figure 1 schematically shows a schematic diagram of the spot welding crack of ultra-high-strength steel with zinc coating. However, it is very difficult to suppress the formation of this crack. Therefore, this crack has become an important obstacle and bottleneck for the application of zinc-coated ultra-high-strength steel in the automotive field.
[0003] There are some known technical solutions for controlling welding cracks in the prior art, but there are still many disadvantages:
[0004] For example, the Chinese patent document with publication number CN108015401A, publication date May 11, 2018, and titled “Resistance spot welding method for galvanized high-strength steel with good joint performance” discloses a method for suppressing spot weld surface cracks while ensuring that the performance of the weld joint is not reduced through innovation in the spot welding process.
[0005] For example, the Chinese patent document with publication number CN109385515A, published on February 26, 2019, and titled "Multi-layer steel and method for reducing liquid metal embrittlement", discloses a method for suppressing the occurrence of spot welding cracks in high-strength steel. The method suppresses the occurrence of spot welding cracks by first decarburizing the high-strength steel and then galvanizing it, so as to control the thickness of the decarburized layer to between 10 and 50 microns.
[0006] Another example is the Chinese patent document CN110892087A, published on March 17, 2020, and titled "Zinc-Coated Steel Sheet with High Resistance Spot Weldability." It discloses a technical solution for reducing spot weld cracking by increasing the dew point to form an inner oxide layer on the steel sheet, thereby improving the surface composition distribution. However, this technical solution suffers from the difficulty in controlling the thickness and uniformity of the inner oxide layer and the uniformity of the surface composition distribution of the steel sheet.
[0007] Based on this, it is expected to provide a coated ultra-high strength steel that has ultra-high strength and excellent spot welding performance.
[0008] Summary of the Invention
[0009] One of the purposes of the present invention is to provide a coated ultra-high strength steel with excellent spot welding performance, which not only meets the performance requirements of coated high-strength steel and the mechanical properties of spot welded joints, but also has low spot weld crack sensitivity.
[0010] To achieve the above objectives, the present invention provides a coated ultra-high-strength steel with excellent spot welding performance, comprising a steel substrate and a zinc-containing coating on the surface of the steel substrate, wherein the steel substrate contains Fe and unavoidable impurity elements, and further contains the following chemical elements in the following mass percentages:
[0011] C: 0.10~0.22%; Si: 0.30~0.79%; Mn: 1.00~2.50%; Cr: 0.50~5.00%; Al: 0.03~1.0%.
[0012] Furthermore, in the coated ultra-high strength steel of the present invention, the mass percentage of each chemical element of the steel substrate is:
[0013] C: 0.10~0.22%; Si: 0.30~0.79%; Mn: 1.00~2.50%; Cr: 0.50~5.00%; Al: 0.03~1.0%; the balance is Fe and inevitable impurity elements.
[0014] Furthermore, in the coated ultra-high strength steel of the present invention, the mass percentage of each chemical element of the steel substrate satisfies at least one of the following:
[0015] C: 0.15~0.20%;
[0016] Si: 0.50~0.79%;
[0017] Mn: 1.00~2.00%;
[0018] Cr: 1.00~3.00%.
[0019] The present invention adopts a composition design based on carbon, silicon, manganese and chromium, supplemented by the process adopted by the present invention, which fully utilizes the role of carbon, silicon, manganese and chromium elements in the phase transformation of the material, and realizes the unification of high mechanical properties and high spot welding performance of the ultra-high strength steel described in the present invention, thereby ultimately obtaining a coated steel plate product with excellent spot welding performance.
[0020] In the coated ultra-high strength steel of the present invention, the design principles of the chemical elements are as follows:
[0021] C: In the coated ultra-high-strength steel with low spot welding crack sensitivity described in the present invention, the solubility of carbon in austenite is much higher than its solubility in ferrite. This can extend the incubation period before austenite transformation and reduce the Ms temperature. The higher the mass percentage of carbon in the steel, the greater the fraction of retained austenite, and the higher the degree of carbon enrichment in the retained austenite during partitioning, which helps enhance the stability of the retained austenite, produce the TRIP effect, and improve the material's ductility. Furthermore, carbon is also the most essential solid solution strengthening element in steel. However, for the composition system of the present invention, if the carbon content in the steel is too high, more twins are likely to form after quenching (i.e., the rapid cooling to 200-300°C at a cooling rate of 50-500°C / s mentioned later in the present invention), increasing the crack sensitivity of the plate. Based on this, the mass percentage of element C in the present invention is controlled to 0.10-0.22%.
[0022] Of course, the mass percentage of the C element can be further preferably controlled between 0.15 and 0.20%.
[0023] Si: In the coated ultra-high-strength steel with excellent spot weldability described herein, silicon has extremely low solubility in carbides. This strongly inhibits cementite formation during the partitioning process, promotes carbon enrichment in retained austenite, and improves the stability of retained austenite. However, excessive silicon content can reduce the steel's high-temperature plasticity and form stable oxides on the steel surface, reducing its wettability. In particular, the inventors have discovered that silicon significantly increases the tendency of weld surface cracks. Therefore, the present invention limits the silicon content to 0.30-0.79% by mass.
[0024] Of course, the mass percentage of Si element can be further preferably controlled to be 0.5-0.79%.
[0025] Mn: In the ultra-high strength steel with excellent spot welding performance described in the present invention, manganese can expand the austenite phase region and reduce Ac3, M s and M f Points, improve the stability of austenite and the hardenability of steel, reduce the critical transformation rate, and are conducive to the preservation of retained austenite to room temperature. At the same time, manganese can also play a solid solution strengthening effect in steel. However, if the mass percentage of manganese is too high, it will aggravate the trend of grain coarsening, reduce the plasticity and toughness of steel, deteriorate corrosion resistance, and especially increase the enrichment of manganese in the shallow surface layer of the parent material under the coating, increase the surface crack sensitivity of the weld of the joint, and deteriorate welding performance. However, if the mass percentage of manganese is too low, ferrite and pearlite banded structures will be produced at a low cooling rate due to segregation. Based on this, the present invention controls the mass percentage of manganese to 1.00~2.50wt%.
[0026] Of course, the mass percentage of the Mn element can be further preferably controlled between 1.00 and 2.00%.
[0027] Cr: In the coated ultra-high-strength steel with excellent spot welding performance described in the present invention, chromium increases the strength and hardness of the steel without significantly reducing its plasticity and toughness. More importantly, chromium can reduce the concentration of manganese under the coating and alleviate the problem of reduced hardenability of the steel caused by manganese addition. Chromium can increase the hardenability of steel and has a secondary hardening effect, which can improve the hardenability and wear resistance of carbon steel without making the steel brittle. The chromium element can expand the γ phase region and improve hardenability and heat resistance, reduce the temperature range of high-temperature existence in the δ phase region, promote the δ→γ phase transformation, and inhibit the precipitation of high-temperature δ ferrite. In addition, the inventors have also found that as the chromium content increases, the tendency of high-strength steel to develop surface cracks in welds decreases; however, the chromium content in carbon steel cannot be too high. Therefore, the present invention controls the mass percentage of chromium to 0.50-5.00wt%.
[0028] Of course, the mass percentage of Cr element can be further preferably controlled between 1.00 and 3.00%.
[0029] A1: In the coated ultra-high-strength steel with excellent spot weldability described herein, aluminum in solid solution increases stacking fault energy, inhibits cementite precipitation and the gamma-to-martensite transformation, and improves austenite stability. Furthermore, aluminum forms fine, dispersed, insoluble particles with carbon and nitrogen, which refine grain size. However, aluminum's strengthening effect is weaker than silicon, and its ability to stabilize austenite is also weaker than silicon. Furthermore, excessively high aluminum mass percentages can easily form large oxide inclusions, hindering steelmaking and continuous casting. Therefore, the present invention limits the aluminum mass percentage to 0.03 to 1.00 wt%.
[0030] Furthermore, in the coated ultra-high strength steel of the present invention, the chemical elements of the steel substrate further include at least one of the following:
[0031] 0<Mo≤0.03%;
[0032] 0<Nb≤0.03%;
[0033] 0<Ti≤0.03%;
[0034] 0<V≤0.03%;
[0035] 0<B≤0.001%, for example, 0<B<0.001%.
[0036] Molybdenum, niobium, titanium, vanadium, and boron can further enhance the performance of the coated ultra-high-strength steel described herein. Molybdenum can improve the steel's hardenability and adjust its strength, but excessive molybdenum content can increase the steel's resistance to cold rolling deformation. Niobium, titanium, and vanadium can form fine carbides with carbon, promoting microstructure refinement. However, the formation of these fine carbides hinders carbon enrichment and stabilization in retained austenite. Boron significantly enhances the steel's hardenability. Boron easily segregates at grain boundaries, filling grain boundary defects, reducing grain boundary energy, and making it more difficult for new phases to nucleate at austenite grain boundaries, which were originally ferrite nucleation sites. The stability of austenite is enhanced, thereby improving hardenability. However, the more boron content is not necessarily better. When the grain boundary defects are filled, if there is still more boron non-equilibrium segregation, "boron phase" precipitation will form at the grain boundaries, increasing the grain boundary energy. At the same time, the "boron phase" will serve as the core of the new phase, prompting an increase in the nucleation rate, reducing the stability of austenite, and reducing the hardenability. Moreover, the precipitation of a large amount of "boron phase" will make the steel brittle, which has a negative impact on the mechanical properties of the steel.
[0037] In addition, the addition of the above elements will increase the cost of the material. Taking into account the performance and cost control of the material, at least one of the above elements can be selectively added and its content can be controlled within the above range.
[0038] In the present invention, when the steel substrate contains Mo, the mass percentage of Mo can be 0.001 to 0.03%. When the steel substrate contains Nb, the mass percentage of Nb can be 0.001 to 0.03%. When the steel substrate contains Ti, the mass percentage of Ti can be 0.001 to 0.03%. When the steel substrate contains V, the mass percentage of V can be 0.001 to 0.03%. When the steel substrate contains B, the mass percentage of B can be 0.0001 to 0.001%, for example, 0.0001 to 0.0009%.
[0039] Furthermore, in the coated ultra-high strength steel of the present invention, the mass percentage of the inevitable impurity elements of the steel substrate satisfies: P≤0.01%, S≤0.01%, and N≤0.003%.
[0040] In the above technical solution, P, S, and N elements are all impurity elements in the coated ultra-high-strength steel described in the present invention. When technical conditions permit, in order to obtain steel with better performance and higher quality, the content of impurity elements in the coated ultra-high-strength steel should be reduced as much as possible.
[0041] Among them, although P can play a role in solid solution strengthening, inhibit the formation of carbides, and is beneficial to improving the stability of retained austenite, too high a mass percentage of P will weaken the grain boundaries, increase the brittleness of the material, and deteriorate the welding performance. In other words, the positive effect of the P element is weaker than its negative effect. Therefore, it is preferred to control the mass percentage of P to P≤0.01%.
[0042] The S element in steel easily forms a low-melting eutectic at the grain boundaries. When its mass percentage is too high, the plasticity of the material will be significantly deteriorated. Therefore, the mass percentage of the S element is controlled to S≤0.01%.
[0043] Too high a mass percentage of nitrogen will bring difficulties to steelmaking and continuous casting, and is not conducive to inclusion control. Therefore, it is preferred to control the mass percentage of nitrogen to N≤0.003wt%.
[0044] Furthermore, in the coated ultra-high strength steel of the present invention, the microstructure of the steel substrate is ferrite+martensite+retained austenite.
[0045] Furthermore, in the coated ultra-high strength steel of the present invention, the volume proportion of ferrite is 25% to 45%; and / or the volume proportion of martensite is 45% to 65%.
[0046] Furthermore, in the coated ultra-high-strength steel of the present invention, the volume fraction of grains 10 μm or smaller in the ferrite is ≥ 85%, and the volume fraction of grains 5 μm or smaller is ≥ 55%. In some embodiments, the volume fraction of grains 10 μm or smaller in the ferrite is 85-96%. In some embodiments, the volume fraction of grains 5 μm or smaller in the ferrite is 55-75%.
[0047] Furthermore, in the coated ultra-high-strength steel of the present invention, the average grain size of the retained austenite is ≤ 2 μm; and / or the average carbon content of the retained austenite is ≥ 1.0%. In some embodiments, the average carbon content of the retained austenite is between 1.0% and 1.30%, such as 1.0% to 1.28%.
[0048] Furthermore, in the coated ultra-high strength steel of the present invention, if surface cracks are generated at the weld spots during spot welding, the maximum depth of the surface cracks at the weld spots is less than 5% of the plate thickness.
[0049] Furthermore, in the coated ultra-high strength steel described in the present invention, the mechanical properties of the coated ultra-high strength steel meet the following requirements: yield strength of 600MPa to 850MPa, tensile strength of 980MPa to 1150MPa, uniform elongation of not less than 13%, and elongation at break of not less than 15%.
[0050] Furthermore, in the coated ultra-high strength steel described in the present invention, the mechanical properties of the coated ultra-high strength steel meet the following requirements: yield strength ≥ 750 MPa, tensile strength ≥ 1000 MPa, uniform elongation ≥ 14.5%, and elongation at break ≥ 22%.
[0051] Furthermore, in the coated ultra-high strength steel of the present invention, the coating is a pure zinc coating, a zinc-iron alloy coating, a zinc-aluminum-magnesium coating, or an aluminum-zinc coating, wherein the pure zinc coating can be a hot-dip galvanized layer or an electroplated galvanized layer.
[0052] Accordingly, another object of the present invention is to provide a method for manufacturing coated ultra-high strength steel, which is simple to produce and the resulting high-strength steel has significantly improved spot welding performance, especially the ability to resist surface cracks in weld spots, under the same mechanical property conditions.
[0053] In order to achieve the above object, the present invention proposes a method for manufacturing coated ultra-high strength steel, which specifically comprises the following steps:
[0054] (1) Smelting and continuous casting to form steel billets;
[0055] (2) heating;
[0056] (3) Hot rolling: the thickness of the oxide scale on the surface of the steel strip after hot rolling is controlled to be ≤4 μm, and the mass percentage of FeO+Fe3O4 in the oxide scale on the surface of the steel strip after hot rolling is controlled to be ≤50 wt%;
[0057] (4) pickling, or pickling + cold rolling;
[0058] (5) Continuous annealing: anneal at 800-920°C, then slowly cool to 700-770°C at a cooling rate of 3-10°C / s; then quickly cool to 200-300°C at a cooling rate of 50-500°C / s; then heat to 360-460°C, keep warm for 50-600s; finally cool to room temperature;
[0059] (6) Coating with zinc coating.
[0060] The manufacturing method of the present invention can produce coated ultra-high-strength steel with low spot welding crack sensitivity. The coated ultra-high-strength steel produced by this manufacturing method can be welded using conventional spot welding processes used in automotive plants, and the maximum depth of surface cracks at the weld points is less than 5% of the plate thickness, demonstrating very low spot welding crack sensitivity.
[0061] In step (2), controlling the thickness of the oxide scale on the surface of the hot-rolled steel strip to be ≤4 μm and the content of (FeO+Fe3O4) in the oxide scale on the surface of the hot-rolled steel strip to be ≤50 wt% is beneficial to the subsequent steps and has an important influence on the performance of the steel plate obtained after continuous annealing. This is because: in the technical solution described in the present invention, FeO and Fe3O4 are more difficult to pickle than Fe2O3, and controlling the thickness of the oxide scale on the surface of the hot-rolled steel strip prepared by the present invention and the content of (FeO+Fe3O4) in the oxide scale on the surface of the hot-rolled steel strip to be ≤50 wt% can effectively improve the pickling effect and obtain a pickled plate surface that can be used for direct continuous annealing. Since the pickled plate can be directly annealed continuously, the deformation of the hot-rolled structure is small, and the steel plate structure is mainly pearlite and ferrite. Therefore, under the same continuous annealing conditions, the material strength can be reduced, the structure can be made more uniform, and excellent ductility can be obtained.
[0062] The present invention optimizes the continuous annealing process. By controlling the annealing temperature at 800-920°C for annealing, a homogenized austenite structure or austenite + ferrite structure can be formed. Then, the annealing temperature is slowly cooled to 700-770°C at a cooling rate of 3-10°C / s to further adjust the ferrite content in the structure and obtain a certain proportion of ferrite, thereby improving the plasticity of the material. Then, the annealing temperature is slowly cooled to 200-300°C (i.e., between M and S) at a cooling rate of 50-500°C / s. s (starting temperature of martensitic transformation) and M f (martensitic transformation end temperature), at this time, the austenite is partially transformed into martensite, which can ensure that the steel obtains higher strength; then, it is heated to 360-460℃ and kept warm for 50-600s, which can partition carbon in martensite and austenite, forming a certain amount of carbon-rich retained austenite, which is stable to room temperature. Due to the TRIP effect, the work hardening ability and formability of the steel can be significantly improved, and a high-strength steel plate with excellent ductility can be obtained.
[0063] In addition, in view of the inventor's understanding of the influence of carbon, silicon, manganese and chromium on the surface cracks of welds, especially the understanding that silicon and manganese are easily enriched in the shallow surface layer of the steel plate and significantly increase the sensitivity of weld surface cracks, while controlling the content of carbon, silicon, manganese and chromium when designing the steel composition, compared with steels of the same strength level, the content of carbon, silicon and manganese elements is also reduced, and chromium is added to increase the hardenability of the steel, ensuring that the designed proportion of martensite and austenite and the carbon distribution are achieved in the continuous annealing step, while ensuring that the zinc-coated plate has low sensitivity to weld surface cracks, and the maximum depth of the weld surface cracks is less than 5% of the plate thickness.
[0064] It should be noted that, when the zinc-containing coating is plated in step (6), the zinc-containing coating can be produced by, but is not limited to, hot-dip, electroplating, or vacuum plating techniques.
[0065] Because the coated ultra-high-strength steel of the present invention utilizes carbon, silicon, manganese, and chromium, and refines the ferrite grains, during continuous annealing, the number of nucleation sites for reverse austenite transformation increases, further reducing the size. The average grain size of retained austenite stable at room temperature can be ≤2μm, and the average carbon content in the retained austenite is ≥1.0%.
[0066] Furthermore, in the method for manufacturing coated ultra-high strength steel of the present invention, in step (2), the slab is heated to 1200-1300°C.
[0067] Furthermore, in the method for manufacturing coated ultra-high strength steel of the present invention, in step (3), the finishing rolling temperature is controlled to be 860-930°C, and the coiling temperature is controlled to be 450-600°C.
[0068] Furthermore, in the method for manufacturing coated ultra-high strength steel of the present invention, in step (4), when pickling + cold rolling is adopted, the cold rolling deformation is controlled to be 40% to 60%.
[0069] Furthermore, in the method for manufacturing coated ultra-high strength steel according to the present invention, the annealing process parameters of step (5) satisfy at least one of the following:
[0070] Annealing temperature is 820~870℃;
[0071] Slowly cool to 700-730°C at a cooling rate of 3-10°C / s;
[0072] Rapid cooling to 250-300℃;
[0073] After rapid cooling, heat to 400-430°C and keep warm for 180-300 seconds;
[0074] The volume content of hydrogen in the reducing atmosphere in the continuous annealing furnace is controlled to be 10-15%.
[0075] The coated ultra-high strength steel and the manufacturing method thereof of the present invention have the following advantages and beneficial effects:
[0076] The ultra-high-strength steel with coating described in the present invention is based on carbon, silicon, manganese and chromium in its composition design. By optimizing the carbon, silicon, manganese and chromium ratio without adding expensive alloying elements, ultra-high-strength cold-rolled steel with coating and excellent spot welding performance is obtained.
[0077] The coated ultra-high strength steel described in the present invention has very excellent quality and performance. While meeting the user's requirements for the performance of coated high-strength steel and the mechanical properties of spot welding joints, it also has low spot welding crack sensitivity.
[0078] The coated ultra-high-strength steel produced using this technical solution includes a steel substrate and a zinc-containing coating on the surface of the steel substrate. Its mechanical properties meet the following requirements: a yield strength of 600 MPa to 850 MPa, a tensile strength of 980 MPa to 1150 MPa, a uniform elongation of no less than 13%, and an elongation at break of no less than 15%. Furthermore, if surface cracks occur at the weld point during spot welding, the maximum depth of the cracks is less than 5% of the plate thickness.
[0079] The manufacturing method designed in the present invention has a simple production process, and the obtained high-strength steel has significantly improved resistance to spot welding cracks under the same mechanical property conditions, and will have good application prospects in the production of safety structural parts for downstream users. BRIEF DESCRIPTION OF THE DRAWINGS
[0080] FIG1 schematically shows a schematic diagram of a spot weld crack of ultra-high strength steel with a zinc coating. DETAILED DESCRIPTION
[0081] The following will further explain and illustrate the coated ultra-high strength steel with excellent spot welding performance and the manufacturing method thereof described in the present invention in conjunction with specific embodiments. However, such explanation and illustration do not constitute an undue limitation to the technical solution of the present invention.
[0082] Examples 1-28 and Comparative Examples 1-4
[0083] The coated ultra-high strength steels of Examples 1-28 of the present invention and the comparative steels of Comparative Examples 1-4 were prepared by the following steps:
[0084] (1) Smelt and continuously cast steel billets according to the chemical composition ratios designed in Table 1.
[0085] (2) Heating: Heat the slab to 1200-1300°C.
[0086] (3) Hot rolling: The thickness of the oxide scale on the surface of the strip after hot rolling is controlled to be ≤4μm, and the (FeO+Fe3O4) in the oxide scale on the surface of the strip after hot rolling is ≤50wt%. The finishing temperature is controlled to be 860-930℃, and the coiling temperature is controlled to be 450-600℃.
[0087] (4) Pickling, or pickling + cold rolling. When pickling + cold rolling is used, the cold rolling deformation is controlled to be 40% to 60%. When galvanizing or zinc alloy is directly plated after pickling, the cold rolling deformation in Table 2-2 is 0.
[0088] (5) Continuous annealing: Control the volume content of hydrogen in the reducing atmosphere in the continuous annealing furnace to be 10-15%; anneal at 800-920°C, preferably the annealing temperature can be controlled to be 820-870°C, then slowly cool to 700-770°C at a cooling rate of 3-10°C / s to obtain a certain proportion of ferrite, and the slow cooling final cooling temperature can be preferably controlled between 700-730°C; then quickly cool to 200-300°C at a cooling rate of 50-500°C / s to partially transform austenite into martensite, and the rapid cooling final cooling temperature can be preferably controlled between 250-300°C; then quickly cool and then heat to 360-460°C, preferably 400-430°C, and keep warm for 50-600s, preferably 180-300s; finally cool to room temperature.
[0089] (6) Coating with zinc or zinc alloy, wherein the coating can be specifically selected from pure zinc coating, zinc-iron alloy coating, zinc-aluminum-magnesium coating or aluminum-zinc coating.
[0090] It should be noted that the chemical composition designs and related manufacturing processes used in the coated ultra-high-strength steels of Examples 1-28 of the present invention all meet the specifications of the present invention. Accordingly, the chemical composition designs and related manufacturing processes used in the comparative steels of Comparative Examples 1-4 all contain process parameters that do not meet the design requirements of the present invention.
[0091] The coatings of the steels in Examples 1-28 and Comparative Examples 1-4 were all hot-dip pure zinc.
[0092] Table 1 lists the mass percentages of the chemical elements in the steel substrates of the coated ultra-high strength steels of Examples 1-28 and the comparative steels of Comparative Examples 1-4.
[0093] Table 1. (wt%, the balance is Fe and other inevitable impurities except P, S, and N)
[0094] Table 2-1 and Table 2-2 list the specific process parameters of the coated ultra-high strength steels of Examples 1-28 and the comparative steels of Comparative Examples 1-4.
[0095] In Table 2-1, the mass percentage of FeO and Fe3O4 in the oxide scale on the surface of the hot-rolled strip (i.e., the proportion of (FeO+Fe3O4)) is determined by X-ray diffraction (XRD).
[0096] Table 2-1.
[0097] Note: In the above Table 2-1, "(FeO+Fe3O4) ratio" means the mass percentage of FeO and Fe3O4 in the oxide scale on the surface of the strip after hot rolling.
[0098] Table 2-2.
[0099] Note: In the above Table 2-2, a cold rolling deformation of 0 means that no cold rolling was used, but only pickling was used.
[0100] Before performing the plating process in step (6), the inventors sampled the coated ultra-high strength steel substrates of Examples 1-28 and the comparative steel substrates of Comparative Examples 1-4 obtained after the continuous annealing process in step (5), and observed the microstructures of the substrates of each example and comparative example. The microstructure observation results of the substrates of each example and comparative example are listed in Table 3 below.
[0101] Table 3 lists the microstructure observation results of the coated ultra-high strength steel substrates of Examples 1-28 and the comparative steel substrates of Comparative Examples 1-4.
[0102] The methods for observing and measuring the microstructure are as follows:
[0103] The volume fractions of ferrite and martensite were determined by metallographic method;
[0104] The size and volume fraction of ferrite grains were determined by metallographic method;
[0105] The average grain size of retained austenite was determined by metallographic method;
[0106] The average carbon content in retained austenite was determined by Castaing electron probe microscopy (EPMA).
[0107] Table 3.
[0108] Note: The volume ratio of retained austenite not listed in Table 3 is the remainder other than ferrite and martensite.
[0109] As shown in Table 3 above, the microstructure of the steel plates of Examples 1-28 of the present invention is: ferrite + martensite + retained austenite. Furthermore, the microstructure of the substrates of each example meets the following criteria: the volume fraction of ferrite is 25% to 45%, and the volume fraction of martensite is 45% to 65%. The volume fraction of ferrite grains 10 μm or smaller is ≥ 85%, and the volume fraction of ferrite grains 5 μm or smaller is ≥ 55%. The average grain size of retained austenite is ≤ 2 μm, and the average carbon content in the retained austenite is ≥ 1.0%.
[0110] In addition, the inventors also tested the mechanical properties of the coated steel sheets of each embodiment and comparative example, and the test results are listed in Table 4 below. When testing the mechanical properties of the coated steel sheets of each embodiment and comparative example, the relevant mechanical properties testing methods are as follows:
[0111] Tensile property test: GB / T228.1-2010 Tensile tests on metallic materials Part 1: Room temperature test method were used to conduct tensile tests to test the yield strength, tensile strength, uniform elongation, and elongation at break of the coated ultra-high strength steels of Examples 1-28 and the comparative steels of Comparative Examples 1-4.
[0112] Table 4.
[0113] It can be seen from Table 4 above that the steel plates of Examples 1-28 designed by the present invention all have very excellent mechanical properties, with yield strength ≥600 MPa, tensile strength ≥980 MPa, uniform elongation ≥13%, and elongation at break ≥15%.
[0114] In addition, in order to verify that the prepared finished products of Examples 1-28 with coated ultra-high strength steel have excellent low spot welding crack sensitivity, the inventors took samples of the finally prepared finished products of Examples 1-28 with coated ultra-high strength steel and the comparative steel plates of Comparative Examples 1-4, and conducted spot welding tests on the finished steel plate samples of each embodiment and comparative example. The relevant spot welding process parameters are shown in Table 5 below.
[0115] Table 5 lists the specific spot welding process parameters of the coated ultra-high strength steels of Examples 1-28 and the comparative steel plates of Comparative Examples 1-4.
[0116] Table 5.
[0117] During spot welding, one tensile shear specimen (TSS), one cross tensile test specimen (CTS), and one metallographic specimen were welded at each welding current. The joint bearing capacity of TSS and CTS was measured using a tensile testing machine according to ISO 14273-2016 and ISO 14272-2016 standards. The results are shown in Table 6.
[0118] For the metallographic specimens, dilute hydrochloric acid was used to remove the coating on the joint surface. The distribution and direction of the cracks on the solder joint surface were observed under a microscope. The cross section passing through the center of the weld nugget and capable of cutting the most surface cracks was selected as the metallographic section of the joint. Wire cutting was used for sampling. The cross section included all the welding characteristic areas of the spot weld joint. The surface of the cut specimens was rinsed to prevent foreign matter from interfering with the test results. The rinsed samples were dried. The dried specimens were mounted, ground and polished, and measured under a metallographic microscope. The maximum crack depths are listed in Table 6.
[0119] Table 6 lists the mechanical properties of the welds and the crack test results of the welds of the coated ultra-high strength steels of Examples 1-28 and Comparative Examples 1-4 after spot welding.
[0120] Table 6.
[0121] As shown in Table 6, for Examples 1-28 of this case, when the welding current was less than the spatter current (referred to as non-spatter welds), the welds produced had no surface cracks. When the welding current was greater than the spatter current, the longest surface crack in the welds produced (referred to as spatter welds) was less than 5% of the plate thickness. In contrast, for Comparative Examples 1-4, regardless of whether the welding current was greater than the spatter current, the welds produced cracks. The surface cracks in the spatter welds were more severe than those in the non-spatter welds, and the ratio of maximum crack length to plate thickness was significantly greater than 5%. This demonstrates that the coated ultra-high-strength steel of each of the examples of this case exhibits excellent low weld surface crack sensitivity while maintaining plate performance.
[0122] It should be noted that the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.
[0123] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therefrom that can be directly derived from or easily conceived by those skilled in the art based on the disclosure of the present invention are intended to fall within the scope of protection of the present invention.
Claims
1. A coated ultra-high strength steel with excellent spot welding performance, comprising a steel substrate and a zinc-containing coating on the surface of the steel substrate, wherein the steel substrate contains Fe and unavoidable impurity elements, characterized in that: The steel substrate further contains the following chemical elements in the following mass percentages: C: 0.10-0.22%; Si: 0.30-0.79%; Mn: 1.00-2.50%; Cr: 0.50-5.00%; Al: 0.03-1.0%.
2. The coated ultra-high strength steel according to claim 1, characterized in that: The mass percentage of each chemical element of the steel substrate is: C: 0.10-0.22%; Si: 0.30-0.79%; Mn: 1.00-2.50%; Cr: 0.50-5.00%; Al: 0.03-1.0%; the remainder is Fe and unavoidable impurity elements.
3. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The mass percentage of each chemical element of the steel substrate satisfies at least one of the following items: C: 0.15-0.20%; Si: 0.30-0.79%; Mn: 1.00-2.00%; Cr: 1.00-3.00%.
4. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The chemical elements of the steel substrate further include at least one of the following: 0<Mo≤0.03%; 0<Nb≤0.03%; 0<Ti≤0.03%; 0<V≤0.03%; 0<B≤0.001%。 5. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The mass percentage of the inevitable impurity elements of the steel substrate meets the following requirements: P≤0.01%, S≤0.01%, and N≤0.003%.
6. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The microstructure of the steel substrate is ferrite+martensite+retained austenite.
7. The coated ultra-high strength steel according to claim 6, characterized in that: The volume proportion of ferrite is 25% to 45%; and / or the volume proportion of martensite is 45% to 65%.
8. The coated ultra-high strength steel according to claim 6, characterized in that: In the ferrite, the volume proportion of grains with a size of less than 10 μm is ≥85%, and the volume proportion of grains with a size of less than 5 μm is ≥55%.
9. The coated ultra-high strength steel according to claim 6, characterized in that: The average grain size of the retained austenite is ≤2 μm; and / or the average C content in the retained austenite is ≥1.0%.
10. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: When spot welding is performed, if cracks occur on the surface of the weld, the maximum depth of the cracks on the surface of the weld is less than 5% of the plate thickness.
11. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The mechanical properties of the coated ultra-high strength steel meet the following requirements: yield strength is 600MPa-850MPa, tensile strength is 980MPa-1150MPa, uniform elongation is not less than 13%, and elongation at break is not less than 15%.
12. The coated ultra-high strength steel according to claim 1 or 2, characterized in that: The coating is pure zinc coating, zinc-iron alloy coating, zinc-aluminum-magnesium coating or aluminum-zinc coating.
13. The method for manufacturing coated ultra-high strength steel according to any one of claims 1 to 12, characterized in that: Includes steps: (1) Smelting and continuous casting; (2) Heating; (3) Hot rolling: the thickness of the oxide scale on the surface of the steel strip after hot rolling is controlled to be ≤4 μm, and the mass percentage of FeO+Fe3O4 in the oxide scale on the surface of the steel strip after hot rolling is controlled to be ≤50wt%; (4) pickling, or pickling + cold rolling; (5) Continuous annealing: anneal at 800-920°C, then slowly cool to 700-770°C at a cooling rate of 3-10°C / s; then quickly cool to 200-300°C at a cooling rate of 50-500°C / s; then heat to 360-460°C, keep warm for 50-600s; finally cool to room temperature; (6) Coating with zinc coating.
14. The manufacturing method according to claim 13, characterized in that: The manufacturing method has one or more of the following characteristics: In step (2), the slab is heated to 1200-1300° C.; In step (3), the final rolling temperature is controlled to be 860-930°C and the coiling temperature is controlled to be 450-600°C; In step (4), when pickling + cold rolling is adopted, the cold rolling deformation is controlled to be 40% to 60%.
15. The manufacturing method according to claim 13, characterized in that: The annealing process parameters of step (5) satisfy at least one of the following: Annealing temperature is 820~870℃; Slowly cool to 700-730°C at a cooling rate of 3-10°C / s; Rapid cooling to 250-300℃; After rapid cooling, heat to 400-430°C and keep warm for 180-300 seconds; The volume content of hydrogen in the reducing atmosphere in the continuous annealing furnace is controlled to be 10-15%.