Solder alloy, solder ball, solder preform, solder joint, and circuit

MYPI2025005910A0Undetermined Publication Date: 2024-10-28SENJU METAL IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005910
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-19
Publication Date
2024-10-28

AI Technical Summary

Technical Problem

Conventional solder alloys used in BGA packages face issues with void formation, shear strength, drop impact resistance, and wettability due to repeated reflow soldering, leading to bonding defects and irregularly shaped solder bumps, which compromise the reliability and performance of electronic components.

Method used

A solder alloy composition with specific ranges of Ag (0.10-3.00%), Cu (0.80-6.00%), Ni (0.08-0.60%), and Ge (0.0010-0.0150%) is developed, along with optional elements like Bi, Sb, and rare earth metals, to enhance wettability, shear strength, and drop impact resistance, while controlling intermetallic compound growth and bump shape.

Benefits of technology

The optimized solder alloy composition achieves excellent wettability, shear strength, appropriate fracture mode, and improved drop impact resistance, suppressing intermetallic compound growth and ensuring regular bump shape, even after multiple reflows, thus enhancing the reliability of solder joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005910_DRAWING_001
    Figure PI2025005910_DRAWING_001
Patent Text Reader

Abstract

ABSTRACT SOLDER ALLOY, SOLDER BALL, SOLDER PREFORM, SOLDER JOINT, AND CIRCUIT Provided are a solder alloy, a solder ball, a solder preform, a solder joint, and a circuit which have excellent wettability and shear strength, as well as an appropriate fracture mode, suppressed growth of an intermetallic compound at a joint interface even after reflowing is performed a plurality of times, excellent drop impact resistance, and an appropriate bump shape. The solder alloy has an alloy composition consisting of, by mass%, Ag: 0.10 to 3.00%, Cu: 0.80 to 6.00%, Ni: 0.08 to 0.60%, Ge: 0.0010 to 0.0150%, with the balance being Sn. Preferably, the alloy composition further contains at least one of Bi, Sb, In, Zn, Ga, Mn, Cr, Co, Si, Ti, and rare earth elements: 0.1% or less in total. FIG. 1
Need to check novelty before this filing date? Find Prior Art

Description

Solder alloys, solder balls, solder preforms, solder joints, and circuits

[0001] The present invention relates to solder alloys, solder balls, solder preforms, solder joints, and circuits.

[0002] In recent years, there has been a demand for electronic devices to be highly integrated and lighter, thinner, and smaller. The electronic components mounted on these electronic devices are also being required to be smaller and thinner. The mainstream semiconductor package that meets these demands is the area array surface mount package, the BGA (Ball Grid Array). A BGA has external electrode terminals in which solder balls are arranged in a grid pattern at equal intervals on the mounting substrate of the package. After the solder balls are placed on the electrodes, they are heated together with the mounting substrate in a reflow furnace, where they melt and form solder bumps.

[0003] To meet the increasing demands for higher integration and lighter, thinner, shorter, and smaller electronic devices, electronic components are often connected to both sides of a substrate. To connect electronic components to both sides of a substrate, a first reflow soldering is performed on one side, followed by a second reflow soldering on the other side. Furthermore, in the case of power semiconductor substrates, a third reflow soldering is performed to connect a heat sink. When multiple reflow soldering processes are performed, the solder alloy used in the first or second soldering cycle is repeatedly melted and solidified.

[0004] Conventional BGAs have used Sn-Ag-Cu solder alloys, such as Sn-3.0Ag-0.5Cu. However, repeated reflow soldering can cause voids to form at the interface between the solder alloy and the electrodes that make up the solder joint. The growth of these voids can lead to poor shear strength and drop impact resistance. Furthermore, repeated melting and solidification of the solder alloy can cause oxidation of the solder alloy, resulting in poor wettability.

[0005] Therefore, Patent Document 1 discloses Sn alloys containing 1 to 9% Cu and various optional elements in order to suppress deterioration of solder joint reliability due to multiple reflow soldering. Specifically, Sn—Cu—Ni solder alloys and Sn—Cu—Ni—Ge solder alloys are disclosed. These solder alloys further contain P and other elements. It is also disclosed that Ag may be contained as an optional element. In this document, die tilt, void growth, and shear strength after multiple reflow soldering are evaluated.

[0006] Patent Document 2 discloses a Sn—Ag—Cu—Ni solder alloy that improves drop impact resistance by reducing the hardness of the solder alloy. The invention described in this document also describes the inclusion of P and Ge as elements that suppress discoloration of the solder alloy.

[0007] Patent Document 3 discloses a Sn-Ag-Cu-Ni-Ge solder alloy as an inexpensive 5-element solder alloy with good bondability. The invention described in this document is evaluated for the rate of void generation and elongation at break. The document also describes a method for reducing void generation and increasing Cu content. 3 It is described that the elongation at break is improved by reducing the thickness of the Sn film. Furthermore, the same document discloses that the reason for adding Ge is to suppress oxidation.

[0008] Patent Document 4 discloses a solder alloy containing a predetermined amount of at least one of La, Ce, Pr, Nd, Sm, and Yb, or Y, Gd, and Dy, in a Sn—Ag—Cu solder alloy to improve joint strength while reducing the Ag content. This document also discloses that the solder alloy may further contain Ni and / or Fe to refine the crystals in the solidification structure of the solder alloy and improve its mechanical strength. This document also discloses that the solder alloy may contain P, Ga, and Ge as highly oxidizable elements to suppress the generation of dross due to oxidation of La, Ce, Pr, Nd, Sm, and Yb, or Y, Gd, and Dy, and Ni and Fe.

[0009] International Publication No. 2020 / 135932 International Publication No. 2007 / 102588 Japanese Patent Application Laid-Open No. 2008-93701 Japanese Patent Application Laid-Open No. 2013-049073

[0010] In Patent Document 1, various evaluations were performed on alloy compositions containing Sn and Cu. However, the evaluations were performed using alloy compositions with different constituent elements depending on the evaluation item. For example, in the evaluation of die tilt, a solder alloy with constituent elements exhibiting a melting point such that the solder does not melt during the second reflow or maintains a high viscosity even after melting was used. Similarly, evaluations of void growth and shear strength after multiple reflow soldering were performed using solder alloys with different constituent elements.

[0011] As described above, although various evaluations are performed in the invention described in Patent Document 1, the constituent elements other than Sn and Cu vary depending on each evaluation item. Therefore, Patent Document 1 does not disclose an alloy composition that satisfies all of the evaluation items disclosed therein. Furthermore, as mentioned above, Patent Document 1 discloses that Ag may be contained. However, not a single alloy composition containing Ag has been evaluated. Therefore, the effect of adding Ag has not been proven in the invention described in Patent Document 1.

[0012] In the inventions described in Patent Documents 2 and 3, the Ni content is reduced to improve the properties of the bonded interface, thereby improving drop impact resistance, etc. In the invention described in Patent Document 4, an expensive rare metal is used to refine the bonded interface.

[0013] As described above, Patent Documents 1 to 4 all examine the joint interface of a solder joint. Naturally, improving the properties of the joint interface of a solder joint is an important objective of solder alloys. However, even if the load on the solder joint increases, the fracture mode must not be one in which the fracture occurs at the joint interface. In a solder joint, physical and electrical loads are mainly applied to the joint interface, so it is desirable for the joint interface to be firmly joined.

[0014] In this way, evaluation of solder joints under extreme conditions is an important indicator for confirming that good solder joints have been formed. However, because Patent Documents 1 to 4 do not consider the fracture mode, it is unclear whether solder joints with good bonding interfaces have been formed.

[0015] Furthermore, the evaluation items discussed in Patent Documents 1 to 4 are all for the conditions after a solder joint has been formed. Excellent wettability of the molten solder is also an important property of the solder alloy before a solder joint is formed. Although Patent Documents 1 to 4 mention wettability, they do not evaluate specific alloy compositions.

[0016] Furthermore, when bonding to a substrate such as a BGA, the solder bumps must have an appropriate shape before the solder joint is formed. This is because irregularly shaped solder bumps are likely to cause problems during soldering. However, Patent Documents 1 to 4 do not consider at all the shape of the solder bumps used to form the solder joint.

[0017] Solder bumps are formed when a solder ball melts on an electrode, solidifies, and then bonds to the electrode. Therefore, it is considered preferable for the surface to have a roughly elliptical shape. However, solder bumps can have holes, resulting in surface irregularities, needle-like intermetallic compounds protruding from the surface, or irregular shapes that deviate significantly from a roughly elliptical shape. Such solder bumps are prone to poor bonding and short circuits between electronic components and substrates. In recent years, due to the miniaturization and thinning of electronic components, bonding defects caused by irregularly shaped bumps have been increasing year by year, and urgent improvements are needed.

[0018] Therefore, an object of the present invention is to provide a solder alloy, a solder ball, a solder preform, a solder joint, and a circuit that have excellent wettability and shear strength, an appropriate fracture mode, suppression of growth of intermetallic compounds at the bonding interface even after multiple reflows, excellent drop impact resistance, and an appropriate bump shape.

[0019] The present inventors have investigated various alloy compositions for the solder alloys disclosed in Patent Documents 2 to 4 in order to solve the problems of the present invention. Specifically, evaluation was carried out using a Sn-1.0Ag-1.0Cu-0.1Ni solder alloy containing no Ge, which is the alloy composition of Example 10 in Patent Document 2. As a result, it was discovered that abnormalities occur in the solder bumps.

[0020] Therefore, the inventors evaluated a Sn-1.0Ag-1.0Cu-0.1Ni-0.02Ge solder alloy, which is a Sn-1.0Ag-1.0Cu-0.1Ni solder alloy with Ge added. As a result, abnormalities were observed in the solder bumps, and it was found that the wettability was poor.

[0021] Next, a study was conducted focusing on the Ni content. Paragraphs 0072 and 0139 of Patent Document 2 explain that if the Ni content exceeds 0.07%, the solder alloy before reflow becomes hard, to the extent that there is no practical problem, and thus the drop impact resistance is deteriorated. On the other hand, paragraph 0063 of the same document explains that Ni is a (Cu, Ni) alloy in which part of Cu is substituted with Ni. 6 Sn 5 Intermetallic compounds and adjacent Cu 3 In view of these facts, it is presumed that the Sn-Ag-Cu-Ni-Ge solder alloy disclosed in this document only has an alloy composition with a Ni content of 0.05%, which is close to 0.07%.

[0022] 3 and 4 of Patent Document 3 disclose that the generation of voids cannot be suppressed if the Ni content exceeds 0.05%. Furthermore, Figure 5 of the same document discloses that an alloy composition containing 0.03% Ni has a similar fracture elongation to an alloy composition containing 0.07% Ni, and that it is not necessary to include more than 0.05% Ni.

[0023] In light of these findings, the present inventors evaluated an alloy composition in which the Ni content was reduced to 0.05% in a Sn—Ag—Cu—Ni—Ge solder alloy, and found that, similar to an alloy composition with a Ni content of 0.07%, the shear strength was poor and abnormalities occurred in the solder bumps.

[0024] Furthermore, since Patent Document 4 describes reducing the Ag content, an Sn—Ag—Cu—Ni—Ge solder alloy with an Ag content reduced to 0.05% was evaluated. As a result, it was found that although the abnormalities in the solder bumps were reduced, the wettability and shear strength were inferior.

[0025] In light of these findings, it is believed that it would be difficult to solve the problem of the present invention with a Sn-Ag-Cu-Ni-Ge solder alloy, even if the trends in conventional alloy compositions and effects are taken into consideration. Therefore, in order to obtain a Sn-Ag-Cu-Ni-Ge solder alloy that simultaneously satisfies all of the effects listed as the problem of the present invention, the inventors decided to take a different approach from conventional methods and study an alloy composition in which the Ni content is increased to 0.08% or more. Furthermore, they also studied detailed adjustments of the Ag, Cu, and Ge contents.

[0026] As described in paragraphs 0072 and 0139 of Patent Document 2, even if the characteristics are somewhat deteriorated, the characteristics are still at a level that does not pose a problem in practical use. Therefore, it is considered that it is not necessary to achieve all of the objects set forth in the objects of the present invention at a level higher than necessary. For this reason, the above study was carried out so that the effects that do not pose a problem in practical use can be exhibited.

[0027] As a result, it was discovered that when the Ni content is increased and each constituent element is within a predetermined range, the wettability and shear strength are excellent, the fracture mode is appropriate, the growth of intermetallic compounds at the bonding interface is suppressed even after multiple reflows, and the drop impact resistance is excellent, and furthermore, no abnormalities are observed in the bump shape, and the present invention was completed. The present invention, which was obtained based on these findings, is as follows.

[0028] (0) A solder alloy characterized by having, in mass %, an alloy composition consisting of 0.10 to 3.00% Ag, 0.80 to 6.00% Cu, 0.08 to 0.60% Ni, 0.0010 to 0.0150% Ge, and the balance being Sn and unavoidable impurities. (1) A solder alloy characterized by having, in mass %, an alloy composition consisting of 0.10 to 3.00% Ag, 0.80 to 6.00% Cu, 0.08 to 0.60% Ni, 0.0010 to 0.0150% Ge, and the balance being Sn.

[0029] (2) The solder alloy according to (0) or (1) above, wherein the alloy composition further contains 0.1% or less in total of at least one of Bi, Sb, In, Zn, Ga, Mn, Cr, Co, Si, Ti, and rare earth elements.

[0030] (3) A solder alloy according to any one of (0) to (2) above, wherein the alloy composition satisfies the following formulas (1) and (2): 0.00043≦Cu×Ni×Ge≦0.00149 (1) 0.09≦Ag×Cu×Ni≦0.11 (2) In formulas (1) and (2), Ag, Cu, Ni, and Ge represent the contents (mass %) of the alloy composition.

[0031] (4) A solder ball made of the solder alloy according to any one of (0) to (3) above.

[0032] (5) A solder preform made of the solder alloy according to any one of (0) to (3) above.

[0033] (6) A soldered joint comprising the solder alloy according to any one of (0) to (3) above.

[0034] (7) A circuit having the solder joint described in (6) above.

[0035] Fig. 1 is a surface SEM photograph of an intermetallic compound formed at the joint interface of a soldered joint produced using the solder alloy of Example 3. Fig. 2 is a surface SEM photograph of an intermetallic compound formed at the joint interface of a soldered joint produced using the solder alloy of Comparative Example 4.

[0036] The present invention will be described in more detail below. In this specification, "%" relating to the solder alloy composition is "% by mass" unless otherwise specified.

[0037] 1. Solder alloy (1) Ag: 0.10 to 3.00% Ag contributes to improving wettability. 3 The precipitation of Sn can improve the shear strength. If the Ag content is less than 0.10%, the wettability decreases, and the shear strength decreases due to poor bonding between the solder alloy and the electrode. The lower limit of the Ag content is 0.10% or more, preferably 0.50% or more, and more preferably 0.90% or more.

[0038] On the other hand, when the Ag content exceeds 3.00%, coarse Ag 3 The precipitation of Sn reduces the shear strength, and after multiple reflows, the drop impact resistance decreases. The upper limit of the Ag content is 3.00% or less, preferably 2.50% or less, more preferably 2.00% or less, even more preferably 1.50% or less, particularly preferably 1.10% or less, and most preferably 1.00% or less.

[0039] (2) Cu: 0.80 to 6.00%. Cu contributes to improving shear strength by controlling the growth of intermetallic compounds that precipitate at the joint interface. Furthermore, although thin, brittle compounds are formed on the molten solder surface together with Ge, which will be described later, these compounds are easily destroyed by convection in the molten solder, cleaning the surface of the molten solder. This improves the surface tension of the molten solder, thereby preventing deformation of the solder bumps. Furthermore, Cu improves drop impact resistance and wettability, and optimizes the fracture mode.

[0040] If the Cu content is less than 0.80%, the effect of suppressing the growth of intermetallic compounds at the bonding interface is not exerted, resulting in a decrease in shear strength. In addition, thin compounds of Ge and Cu are not formed on the surface of the molten solder, resulting in irregularly shaped solder bumps. The lower limit of the Cu content is 0.80% or more, preferably 0.95% or more.

[0041] On the other hand, if the Cu content exceeds 6.00%, the liquidus temperature rises excessively, resulting in poor wettability. Furthermore, coarse intermetallic compounds precipitate at the bonding interface, resulting in poor drop impact resistance and shear strength, and an inappropriate fracture mode. Furthermore, a large amount of thick Ge and Cu compounds precipitates on the molten solder surface, reducing the surface tension of the molten solder and causing the solder bump to become irregular. The upper limit of the Cu content is 6.00% or less, preferably 5.00% or less, more preferably 4.00% or less, even more preferably 3.00% or less, even more preferably 2.00% or less, particularly preferably 1.20% or less, and most preferably 1.05% or less, and may even be 1.00% or less.

[0042] (3) Ni: 0.08-0.60% Like Cu, Ni contributes to improving shear strength and suppressing deformation of solder bumps. Furthermore, Ni improves drop impact resistance and wettability, and can optimize the fracture mode. If the Ni content is less than 0.08%, the effect of suppressing the growth of intermetallic compounds at the bonding interface is not exerted, and shear strength decreases. Furthermore, thin compounds of Ge and Ni are not formed on the surface of the molten solder, causing the solder bumps to become deformed. The lower limit of the Ni content is 0.08% or more, and preferably 0.09% or more.

[0043] On the other hand, if the Ni content exceeds 0.60%, the wettability deteriorates as with Cu, and coarse intermetallic compounds precipitate at the bonding interface, resulting in poor drop impact resistance and shear strength, and an inappropriate fracture mode. Furthermore, a large amount of Ge and Ni compounds precipitates on the molten solder surface, causing the solder bump to become irregular. The upper limit of the Ni content is 0.60% or less, preferably 0.50% or less, more preferably 0.40% or less, even more preferably 0.30% or less, even more preferably 0.20% or less, particularly preferably 0.12% or less, and most preferably 0.11% or less, and may be 0.10% or less.

[0044] (4) Ge: 0.0010 to 0.0150%. Ge forms compounds with Cu and Ni, which migrate to the surface of the molten solder. However, convection in the molten solder destroys these compounds, cleaning the surface of the molten solder and preventing the solder bumps from becoming misshapen. If the Ge content is less than 0.0010%, the compounds with Cu and Ni are not sufficiently precipitated on the surface of the molten solder, resulting in misshapen solder bumps. The lower limit of the Ge content is 0.0010% or more, preferably 0.0020% or more, more preferably 0.0050% or more, and even more preferably 0.0060% or more.

[0045] On the other hand, if the Ge content exceeds 0.0150%, the molten solder surface will have a thick layer of compounds with Cu and Ni, and these compounds will remain on the surface of the solder alloy during solidification, resulting in irregularly shaped solder bumps. This will also result in reduced wettability. The upper limit of the Ge content is 0.0150%, preferably 0.0120%, more preferably 0.0100%, and particularly preferably 0.0080%.

[0046] (5) 0.1% or less total content of at least one of Bi, Sb, In, Zn, Ga, Mn, Cr, Co, Si, Ti, and rare earth elements. The solder alloy according to the present invention may contain at least one of Bi, Sb, In, Zn, Ga, Mn, Cr, Co, Si, Ti, and rare earth elements in a total content of 0.1% or less as optional elements, provided that the effects of the present invention are not adversely affected. In the present invention, rare earth elements refer to 17 elements, including Sc and Y, which belong to Group 3 of the periodic table, and 15 elements of the lanthanum group corresponding to atomic numbers 57 to 71. The upper limit of the content of the optional elements is not particularly limited, but is preferably 0.1% or less, and more preferably 0.01% or less. The lower limit is also not particularly limited, but is preferably 0.001% or more.

[0047] (6) Formulas (1) and (2) 0.00043≦Cu×Ni×Ge≦0.00149 (1) 0.09≦Ag×Cu×Ni≦0.11 (2) In formulas (1) and (2), Ag, Cu, Ni, and Ge represent the contents (mass %) of the alloy composition.

[0048] The solder alloy according to the present invention preferably satisfies formulas (1) and (2). When these formulas are satisfied, the fracture mode is more optimized, shear strength is further improved, drop impact resistance is further improved even after multiple reflows, the intermetallic compounds precipitated at the bonding interface become finer, and deformation of the solder bump is suppressed. Formula (1) is a formula composed of Cu, Ni, and Ge, which are elements that suppress deformation of the solder bump. Although the Ge content is less than the Cu and Ni contents, Ge forms compounds with Cu and Ni and significantly affects the behavior of the alloy structure during the solidification process, so even a small amount of Ge contributes significantly to the properties of the solder alloy. Therefore, the content of each constituent element can be expressed as a formula directly without multiplying Ge by a coefficient.

[0049] Formula (2) is a formula consisting of Ag, Cu, and Ni, which contribute to improving wettability and shear strength. A solder joint must not fracture at the joint interface, but the strength of the solder alloy itself must not be too weak. In this regard, Ag is a precipitation-strengthening element, and by satisfying formula (2), the strength of the solder alloy itself can be improved to a certain extent, to the extent that the fracture mode is not inappropriate. Furthermore, Cu and Ni contribute to the formation of fine intermetallic compounds at the joint interface and the liquidus temperature, and therefore, together with Ag, affect the overall characteristics of the solder joint.

[0050] These formulas are obtained by the interdependence of each constituent element. This is because an alloy is a single entity formed by combining all constituent elements, and each constituent element influences the other. Thus, the solder alloy according to the present invention, which adjusts the content of each constituent element to the optimum content and further satisfies formulas (1) and (2), is set within a range that fully takes into account the interdependence of each constituent element. Therefore, an alloy composition in which each constituent element is within the above-mentioned range and satisfies formulas (1) and (2) exhibits excellent drop impact resistance even after multiple soldering cycles, and suppresses coarsening of intermetallic compounds precipitated at the joint interface. At the same time, it also exhibits excellent wettability and shear strength, an appropriate fracture mode, and high levels of suppression of solder bump deformation.

[0051] The lower limit of formula (1) is preferably 0.00043 or more, more preferably 0.00060 or more, even more preferably 0.00064 or more, particularly preferably 0.00072 or more, and most preferably 0.00076 or more. The upper limit of formula (1) is preferably 0.00149 or less, more preferably 0.00120 or less, even more preferably 0.00100 or less, still more preferably 0.00096 or less, particularly preferably 0.00088 or less, most preferably 0.00086 or less, and may be 0.00084 or less, or 0.00080 or less.

[0052] The lower limit of the formula (2) is preferably 0.09 or more, more preferably 0.095 or more, and the upper limit of the formula (2) is preferably 0.11 or less, more preferably 0.105 or less, and even more preferably 0.10 or less.

[0053] (7) Balance: Sn The balance of the solder alloy according to the present invention is Sn. In addition to the above elements, unavoidable impurities may be contained. The balance of the solder alloy according to the present invention may consist of Sn and unavoidable impurities. Even if unavoidable impurities are contained, the above-mentioned effects are not affected. P forms compounds with Cu, Ni, and Ge on the surface of the molten solder, resulting in poor wettability and bump deformation, so it is preferable not to include it in the solder alloy according to the present invention. Fe forms an oxide film that is difficult to remove with flux, etc., resulting in poor wettability and bump deformation, so it is preferable not to include it in the solder alloy according to the present invention. Ce increases the melting point of the solder alloy, forms oxide films and compounds, and forms coarse intermetallic compounds at the bonding interface, preventing the effects of the present invention from being achieved, so it is preferable not to include it in the solder alloy according to the present invention.

[0054] 2. Solder Balls The solder alloy according to the present invention can be used as solder balls. The solder balls according to the present invention are used to form electrodes of semiconductor packages such as BGA (ball grid array) and bumps on substrates. The diameter of the solder balls according to the present invention is preferably within the range of 1 to 1000 μm. The solder balls can be manufactured by a general solder ball manufacturing method.

[0055] 3. Solder Preform The shape of the solder preform according to the present invention is not particularly limited, and it can be used in shapes such as a plate, ring, cylinder, ribbon, square, disk, washer, chip, wire, etc. The solder preform may contain high-melting-point metal particles (e.g., Ni particles or Cu particles, and alloy powder mainly composed of Ni or Cu) therein, which have a higher melting point than the solder alloy and are easily wetted by molten solder.

[0056] 4. Solder Joint The solder joint according to the present invention is suitable for use in joining at least two or more members to be joined. The members to be joined are not particularly limited, as long as they are electrically connected using the solder alloy according to the present invention, and include, for example, elements, substrates, electronic components, printed circuit boards, insulating substrates, heat sinks, lead frames, semiconductors using electrode terminals, power modules, inverter products, etc.

[0057] The joining method using the solder alloy of the present invention may be carried out in a conventional manner, for example, using a reflow method. The melting temperature of the solder alloy when performing flow soldering may be approximately 20°C higher than the liquidus temperature. Furthermore, when joining using the solder alloy of the present invention, consideration of the cooling rate during solidification can further refine the alloy structure. For example, the solder joint is cooled at a cooling rate of 2 to 3°C / s or more. Other joining conditions can be adjusted as appropriate depending on the alloy composition of the solder alloy.

[0058] 5. Circuit The circuit according to the present invention is an electric circuit, and since it includes the solder joints described above, it is preferably an in-vehicle electronic circuit that requires high reliability, particularly a hybrid semiconductor circuit. The present invention, including the solder alloy, can also be used in a power module.

[0059] 6. Others The solder alloy according to the present invention can be manufactured using low alpha radiation materials as its raw materials. When such low alpha radiation alloys are used to form solder bumps around memory, they can suppress soft errors.

[0060] The present invention will be described with reference to the following examples, but is not limited to these examples. To demonstrate the effects of the present invention, the solder alloys listed in Table 1 were used to evaluate (1) wettability, (2) shear strength, (3) fracture mode, (4) drop impact, (5) IMC grain size, and (6) irregular-shaped bumps.

[0061] (1) Wettability Solder balls with a diameter of 0.3 mm were prepared from the solder alloys listed in Tables 1 and 2 below. Flux (WF-6317, manufactured by Senju Metal Industry Co., Ltd.) was applied to a substrate (S / F: Cu-OSP), and the resulting solder balls were then mounted. Next, reflow soldering (heating temperature: 220°C or higher, holding time: 40 seconds, peak temperature: 245°C) was performed using a reflow device (SNR-615, manufactured by Senju Metal Industry Co., Ltd.). After reflow, the maximum wetting spread length, which is the distance between two parallel lines sandwiching the projected image of the wetted and spread flat shape, was measured using a digital microscope (VHX-7000, manufactured by Keyence Corporation). The substrate material used was a 1.2 mm thick glass epoxy substrate (FR-4). When the wet spreading length was 900 μm or more, it was evaluated as "◎", when the wet spreading length was 800 μm or more but less than 900 μm, it was evaluated as "◯", and when the wet spreading length was less than 800 μm, it was evaluated as "×". In this example, "◯" and "◎" were evaluation results that were acceptable for practical use.

[0062] (2) Shear Strength Solder balls with a diameter of 0.3 mm were prepared from the solder alloys listed in Tables 1 and 2 below. These solder balls were placed on a substrate with a thickness of 1.2 mm and electrodes with a diameter of 0.5 mm (Cu-OSP), and soldering was performed. Ten solder balls were soldered. The soldering conditions were as follows: flux (WF-6400 manufactured by Senju Metal Industry Co., Ltd.) was applied to the electrodes, and the reflow profile was a heating temperature of 220°C or higher, a holding time of 40 seconds, a peak temperature of 245°C, and a cooling rate of 2°C / s. Soldering was performed using a reflow machine (SNR-615 manufactured by Senju Metal Industry Co., Ltd.). The prepared substrates were subjected to a shear strength test using a shear strength measuring device (SERIES4000HS manufactured by Nordson Dage) at a shear rate of 1000 mm / s. When the average bonding strength of the 10 pieces was 5.5 N or more, it was marked with "◎", when it was 4.6 N or more but less than 5.5 N, it was marked with "◯", and when it was less than 4.6 N, it was marked with "×". In this example, "◯" and "◎" were evaluation results that were acceptable for practical use.

[0063] (3) Breakdown mode After the shear strength test, the samples were observed using a digital microscope (Keyence Corporation: VHX-7000) to check for breakage in the bulk or at the bonding interface. If all 10 samples were broken in the solder alloy (bulk), it was marked with "◎", if 9 out of 10 samples were broken in the solder alloy (bulk), it was marked with "○", and if 8 or less out of 10 samples were broken in the solder alloy (bulk), it was marked with "×". In this example, "◯" and "◎" were evaluation results that were acceptable for practical use.

[0064] (4) Drop Impact Solder balls with a diameter of 0.3 mm were prepared from the solder alloys listed in Tables 1 and 2 below. These solder balls were soldered to a 12 x 12 mm CSP module substrate using flux WF-6317 manufactured by Senju Metal Industry Co., Ltd., to prepare CSPs using the solder alloys of each composition as electrodes. An electrode pattern was printed on a 30 x 120 mm, 0.8 mm thick glass epoxy substrate (FR-4) using solder paste. The prepared CSP was then mounted on the substrate and soldered using a reflow machine (SNR-615 manufactured by Senju Metal Industry Co., Ltd.) with a reflow profile of a heating temperature of 220°C or higher, a holding time of 40 seconds, and a peak temperature of 245°C, to prepare an evaluation board.

[0065] A drop impact test was carried out on the fabricated evaluation board under the following conditions. The test method involved fixing both ends of the evaluation board using a dedicated jig at a position 10 mm above the base. In accordance with the JEDEC standard, an impact of 1500 G acceleration was repeatedly applied, and the point at which the resistance increased 1.5 times from the initial resistance value was considered to be a break, and the number of drops was recorded. A break count of 210 or more was evaluated as "◎", 150 to 209 was evaluated as "◯", and 149 or less was evaluated as "×". In this example, "◯" and "◎" were evaluation results that were acceptable for practical use.

[0066] (5) IMC Crystal Grain Size After the fracture mode observation, the remaining solder bulk on the substrate surface was removed using a metal stripper to expose the crystal grains of the intermetallic compound. The exposed intermetallic compound was then photographed at 3000x magnification using a scanning electron microscope (JEOL Ltd.: JSM-7000F). The image analysis software (EMSIS GmbH: Scandium) attached to the scanning electron microscope was then used to calculate the total area of ​​each crystal grain from the photographed image, and the average area (S) of the crystal grains was calculated by dividing the total area by the number of crystal grains. The square root of (4S / π) was calculated from this average area (S) to determine the crystal grain size. When the IMC grain size was 3 μm or less, it was evaluated as "◎", when it was greater than 3 μm and less than 6 μm, it was evaluated as "◯", and when it was greater than 6 μm, it was evaluated as "×". In this example, "◯" and "◎" were evaluation results that were acceptable for practical use.

[0067] (6) Irregular Bumps Solder balls with a diameter of 0.3 mm were prepared from the solder alloys listed in Tables 1 and 2 below. These solder balls were placed on a substrate with a thickness of 1.2 mm and electrodes with a diameter of 0.5 mm (Cu-OSP), and soldered. Thirty balls were soldered. The soldering conditions were as follows: flux (WF-6400, manufactured by Senju Metal Industry Co., Ltd.) was applied to the electrodes, and the reflow profile was as follows: heating temperature: 220°C or higher, holding time: 40 seconds, peak temperature: 245°C, cooling rate: 2°C / s. Soldering was performed using a reflow machine (SNR-615, manufactured by Senju Metal Industry Co., Ltd.). After soldering, the bumps were observed using a scanning electron microscope (JSM-7000F, manufactured by JEOL Ltd.). A score of "◎" was given for zero irregular bumps out of 30, "◯" for one to two irregular bumps, and "×" for three or more irregular bumps. In this example, the evaluation results of "good" and "good" were those that presented no practical problems. The evaluation results are shown in Tables 1 and 2.

[0068]

[0069]

[0070] As is clear from Tables 1 and 2, all of Examples 1 to 40 had appropriate contents of Ag, Cu, Ni, and Ge, and therefore were rated "◯" or "◎" for all evaluation items. Furthermore, Examples 2 to 4, 8, 9, 17, 18, 26, 27, and 29 to 40, which satisfied formulas (1) and (2), were rated "◎" for the evaluation items of solder joints: fracture mode, shear strength, drop impact, and irregular bumps, demonstrating excellent effects.

[0071] On the other hand, Comparative Example 1 had poor wettability and shear strength due to a low Ag content. Comparative Example 2 had poor shear strength and drop impact resistance due to a high Ag content. Comparative Example 3 had poor shear strength and many irregularly shaped bumps due to a low Cu content. Comparative Example 4 had poor results in all evaluations due to a high Cu content.

[0072] Comparative Example 5 did not contain Ni, resulting in an inappropriate fracture mode and poor shear strength. Comparative Examples 6 and 7 contained a low Ni content, resulting in poor shear strength and numerous irregularly shaped bumps. Comparative Example 8 contained a high Ni content, resulting in poor evaluations in all categories. Comparative Examples 9 and 10 contained a low Ge content, resulting in numerous irregularly shaped bumps. Comparative Example 11 contained a high Ge content, resulting in poor wettability and numerous irregularly shaped bumps. Comparative Examples 12 and 13 contained P and Fe, resulting in poor wettability and numerous irregularly shaped bumps. Comparative Examples 14 to 16 contained Ce, resulting in poor evaluations in all categories.

[0073] FIG. 1 is a SEM photograph of the surface of an intermetallic compound formed at the joint interface of a solder joint fabricated using the solder alloy of Example 3. FIG. 2 is a SEM photograph of the surface of an intermetallic compound formed at the joint interface of a solder joint fabricated using the solder alloy of Comparative Example 4. The particles shown in FIGS. 1 and 2 are IMCs (intermetallic compounds), and these are SEM images taken in the above-mentioned "(5) IMC grain size." As is clear from FIGS. 1 and 2, the IMC of Example 3 was finer than the IMC of Comparative Example 4. Furthermore, compared with the IMC of Comparative Example 4, the crystal grain shape of the IMC of Example 3 was more rounded, and the IMC surface irregularities were smaller. Therefore, Example 3 exhibited an appropriate fracture mode, high shear strength, and excellent drop impact resistance. This was also true for the other Examples, with particularly excellent results being observed in Examples 2, 4, 8, 9, 17, 18, 26, 27, and 29-40.

Claims

1. A solder alloy having an alloy composition consisting of, in mass%, 0.10-3.00% Ag, 0.80-6.00% Cu, 0.08-0.60% Ni, 0.0010-0.0150% Ge, and the balance being Sn.

2. The solder alloy of claim 1, wherein the alloy composition further contains 0.1% or less in total of at least one of Bi, Sb, In, Zn, Ga, Mn, Cr, Si, Ti, and rare earth elements.

3. The solder alloy according to claim 1 or 2, wherein the alloy composition satisfies the following formulas (1) and (2): 0.00043≦Cu×Ni×Ge≦0.00149 (1) 0.09≦Ag×Cu×Ni≦0.11 (2) In the above formulas (1) and (2), Ag, Cu, Ni, and Ge represent the contents (mass%) of the alloy composition.

4. A solder ball made of the solder alloy according to claim 1 or 2.

5. A solder preform made of the solder alloy according to claim 1 or 2.

6. A solder joint comprising the solder alloy according to claim 1 or 2.

7. A circuit having the solder joint of claim 6.