Hexagonal boron nitride powder and production method therefor

MYPI2025005913A0Undetermined Publication Date: 2024-09-27TOKUYAMA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005913
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-02-29
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

Conventional hexagonal boron nitride powders struggle to achieve both a fluffy and moist feel in cosmetics, often resulting in either poor packing properties or insufficient fluffy texture due to high adhesion and low tap bulk density, which limits their application in products like loose foundations that require both qualities.

Method used

The hexagonal boron nitride powder is characterized by a tap bulk density of 0.08 g/cm³ and a shear adhesion force of 3.5 kPa or more, with hexagonal boron nitride primary particles having an elongation degree of 0.80 or more aggregated in a proportion of 13% or more, and specific particle size and aspect ratio ranges, allowing for improved spreadability and moisturizing properties.

Benefits of technology

This formulation enables cosmetics to provide a balanced fluffy and moist feel, enhancing the design freedom for products like loose foundations by maintaining moisture while suppressing bulkiness and glare, and improving the overall sensory experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025005913_DRAWING_001
    Figure PI2025005913_DRAWING_001
Patent Text Reader

Abstract

Provided is hexagonal boron nitride powder that makes it possible to easily provide a cosmetic providing both airy, light texture and moist feel sensed in spreading thereof. Hexagonal boron nitride powder having a tap bulk density of not more than 0.08 g / cm3 and a shearing cohesion of not less than 3.5 kPa can attain the object, the shearing cohesion being calculated from a powder yield locus obtained through a powder bed shear stress analyzing test. The hexagonal boron nitride powder can be easily produced by a method for producing hexagonal boron nitride powder including a heating step of filling, with raw material powder containing coarse hexagonal boron nitride powder, a heating container so that a bulk density thereof becomes 0.16 g / cm3 to 0.23 g / cm3 and heating the raw material powder at a maximum temperature of 1700°C to 2100°C for not less than 3 hours under a nitrogen atmosphere, the coarse hexagonal boron nitride powder having a specific surface area of 12 m2 / g to 30 m2 / g and an eluted boron content of 1% to 15%.
Need to check novelty before this filing date? Find Prior Art

Description

Hexagonal boron nitride powder and its manufacturing method

[0001] The present invention relates to a hexagonal boron nitride powder suitable for use in cosmetics and a method for producing the same.

[0002] Hexagonal boron nitride powder is a white pigment with a hexagonal layer structure. Because of its excellent lubricity, spreadability, covering power, and chemical stability, it has been used as a raw material for various cosmetics. Therefore, attempts to further improve the properties required of hexagonal boron nitride powder as a raw material for cosmetics have been reported. For example, Patent Document 1 describes that the spreadability and hiding power are improved by adjusting the aspect ratio, average particle size, specific surface area, graphitization index, and tapped density (tapped bulk density) of hexagonal boron nitride powder to fall within certain ranges.

[0003] Meanwhile, among the various required properties, a "moist feeling" has recently begun to attract attention. Non-Patent Document 1 describes that the difference between static friction force and kinetic friction force contributes to the moist feeling. Furthermore, Patent Document 2 describes a hexagonal boron nitride powder that has an average particle size of 2.5 to 7.0 μm and a content of agglomerated particles having a particle size of 36 μm or more of 10.0 vol % or less, thereby maintaining a moderate lubricity while enhancing the moist feeling.

[0004] Japanese Patent Application Laid-Open No. 2018-108970 International Publication No. 2019 / 172440

[0005] Bulletin of the Chemical Society of Japan, 2020, 93, 399-405

[0006] As described above, conventional hexagonal boron nitride powders have been shown to have a certain degree of effect in enhancing the moist feeling, a required characteristic for a cosmetic raw material. However, there are still issues to be resolved in terms of achieving both a high moist feeling and other required characteristics. For example, hexagonal boron nitride powders with a high moist feeling have strong adhesion to the skin and high packing properties as a powder, whereas, as described in paragraph 0026 of Patent Document 1, fluffy hexagonal boron nitride powders contain a large amount of air and have low tapped bulk density values, resulting in low packing properties, making it difficult to achieve both a moist feeling and a fluffy feeling in cosmetics using hexagonal boron nitride powders. The hexagonal boron nitride powder described in Patent Document 2 has a content of agglomerated particles limited to 10.0% by volume or less, which increases the packing of the particles and provides an excellent moist feeling, but the fluffy feeling is insufficient. In order to achieve both a fluffy and light feel and a moist feeling when spread on a cosmetic product such as loose foundation, it was necessary to adjust the blend of ingredients other than the hexagonal boron nitride powder in the cosmetic product.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a hexagonal boron nitride powder that can easily provide a cosmetic that has both a fluffy, light feel and a moist feel when spread.

[0008] As a result of extensive research, the present inventors have discovered that a cosmetic composition containing a hexagonal boron nitride powder in which the tap bulk density and the shear adhesive strength calculated from the powder layer fracture envelope obtained from a powder bed shear force measurement test have been adjusted to specific values ​​has both a good moist feeling and a good fluffy feeling, leading to the completion of the present invention.

[0009] That is, the present invention is a method for producing a pulp having a tapped bulk density of 0.08 g / cm 3The following is a hexagonal boron nitride powder characterized by having a shear adhesion of 3.5 kPa or more as calculated from a powder bed fracture envelope obtained by a powder bed shear force measurement test. The hexagonal boron nitride powder preferably has a proportion of 13% or more of aggregated structures of hexagonal boron nitride primary particles having an elongation of 0.80 or more in a powder sieved through a 25 μm mesh. The hexagonal boron nitride powder preferably has a particle size D50 of 15 to 30 μm, an average aspect ratio of 15 to 20, and a particle size D90 of 37 to 52 μm.

[0010] The hexagonal boron nitride powder is preferably used in cosmetics. Another aspect of the present invention is a cosmetic, particularly a loose foundation, containing the hexagonal boron nitride powder.

[0011] Furthermore, one embodiment of the present invention is a method for producing a granular material having a specific surface area of ​​12 to 30 m 2 / g, and the amount of eluted boron is 1 to 15%. 3 The mixture is packed into a heating vessel so that the temperature becomes equal to or higher than 1700 to 2100°C, and heated in a nitrogen atmosphere for 3 hours or more.

[0012] The hexagonal boron nitride powder of the present invention makes it easy to provide cosmetics that are both fluffy and light to the touch during use and have a moist feel when spread. As a result, for example, while conventional cosmetics that have a low oil content and a fluffy feel, such as loose foundation, tend to lack moistness and feel dry, by using the hexagonal boron nitride powder of the present invention, it is easy to suppress dryness while maintaining a fluffy feel, thereby increasing the freedom of cosmetic design.

[0013] 1 is an example of a structure formed by agglomeration of hexagonal boron nitride primary particles having an elongation of 0.80 or more contained in the hexagonal boron nitride powder of Example 1 of the present invention. The figure shows the major axis diameter a and the minor axis diameter b of the structure formed by agglomeration of hexagonal boron nitride primary particles of the present invention.

[0014] <Hexagonal boron nitride powder> The hexagonal boron nitride powder of the present invention has a tapped bulk density of 0.08 g / cm3 Hereinafter, the powder bed shear strength measurement test is characterized in that the shear adhesive strength calculated from the powder bed fracture envelope obtained by the powder bed shear strength measurement test is 3.5 kPa or more.

[0015] The tapped bulk density indicates the mass per unit volume of the hexagonal boron nitride powder and is an index of the degree of packing between particles. In other words, the tapped bulk density can also be seen as an index of the amount of voids contained within the powder, and the lower the value, the greater the amount of voids contained within the powder. The greater the amount of voids contained within the powder, the more fluffy the powder feels to the touch. When the tapped bulk density is 0.08 g / cm 3 By setting the tap bulk density to 0.06 g / cm or less, it becomes easy to obtain a cosmetic product that has a light and fluffy feel. 3 On the other hand, from the viewpoint of handling, the tap bulk density is preferably 0.01 g / cm or less. 3 The tapped bulk density is preferably 0.01 g / cm or more. 3 By doing so, it becomes easier to process and mix into cosmetics and the like.

[0016] The shear adhesive strength is calculated from the powder bed failure envelope, which shows the relationship between the shear stress and normal stress generated when a powder layer made of hexagonal boron nitride powder is sheared under normal stress, and refers to the shear stress when no normal stress is applied. In other words, it can be considered an index of the adhesive strength between particles within the hexagonal boron nitride powder, which is not affected by the force used to apply the hexagonal boron nitride powder or the surface condition of the target. When applying the powder to skin, the higher the shear adhesive strength of the powder, the easier it is to impart a moist feeling to the cosmetic. While the reason for this is unclear, the inventors believe as follows: When applying the powder to skin, the user potentially senses the adhesive strength between the powder particles in addition to the adhesive strength between the skin and the powder, and this is thought to be important for achieving a moist feeling. Conventional hexagonal boron nitride powders with a high moist feeling contain trace amounts of water, which provides high wettability to the skin and improved adhesion, leading to a high moist feeling felt by the user. Such conventional hexagonal boron nitride powders with a high moist feeling do not change significantly in appearance, but the fluidity of the particles is slightly reduced due to moisture bonding between the particles. Although the shear adhesion is high, the particles are bonded by traces of moisture, making it impossible to increase the amount of voids. As a result, the tapped bulk density is high, and a fluffy feel cannot be achieved. On the other hand, the hexagonal boron nitride powder of the present invention has a low tapped bulk density, which provides a fluffy feel when applied to the skin. However, when the user spreads the powder on the skin after application, the high interparticle adhesion slightly reduces the fluidity of the particles, resulting in a feel similar to that of a powder containing a trace amount of moisture. As a result, it is presumed that users perceive the hexagonal boron nitride powder of the present invention as having high wettability, resulting in a high moist feeling.

[0017] The hexagonal boron nitride powder according to one embodiment of the present invention has a shear adhesion of 3.5 kPa or more, preferably 3.7 kPa or more, and more preferably 4.0 kPa or more. By setting the shear adhesion of 3.5 kPa or more, a moist feel can be obtained when applied to the skin. There is no particular upper limit to the shear adhesion, but it may usually be 6.0 kPa or less, and particularly 5.0 kPa or less.

[0018] In the hexagonal boron nitride powder according to one embodiment of the present invention, it is preferable that the powder passing through a 25 μm sieve contains 13% or more of structures formed by agglomeration of hexagonal boron nitride primary particles having an elongation of 0.80 or more. When the relatively large particle group that did not pass through the 25 μm sieve contains 13% or more of structures formed by agglomeration of hexagonal boron nitride primary particles having an elongation of 0.80 or more, the tapped bulk density is 0.08 g / cm. 3 Hereinafter, it becomes easy to obtain a hexagonal boron nitride powder having a shear adhesive strength of 3.5 kPa or more as calculated from the powder bed fracture envelope obtained from the powder bed shear strength measurement test. The reason for this is not clear, but the present inventors believe it to be as follows.

[0019] That is, if a relatively large particle group that did not pass through a 25 μm mesh sieve contains a large number of structures with a relatively high degree of elongation, the structures will penetrate between the agglomerated particles and between the agglomerated particles and the single particles, resulting in many voids, making it easier to adjust the tap bulk density low. Furthermore, it is presumed that the high degree of elongation of the structures causes the structures to interlock with each other when the powder is spread, generating a large frictional force instantaneously, thereby increasing the shear adhesion force and providing a highly moist feeling. Furthermore, it is presumed that the structures are destroyed when the powder is spread, causing a decrease in frictional force, and that this fluctuation in frictional force also contributes to increasing the shear adhesion force.

[0020] In the present invention, the elongation of the structure is an index representing the slenderness of the structure, with a higher elongation indicating a more slender structure. As shown in Figure 2, the longest-spaced line among the lines connecting the edges of the structure is defined as the major axis, and the longest-spaced line among the lines connecting the edges of the structure perpendicular to the major axis is defined as the minor axis. The elongation of the structure is calculated from the length of the major axis (major axis diameter a) and the length of the minor axis (minor axis diameter b) using the following formula. The major axis diameter a and the minor axis diameter b can be measured from an image captured by a scanning electron microscope.

[0021]

[0022] The proportion of structures formed by agglomeration of hexagonal boron nitride primary particles having an elongation of 0.80 or more in the powder on the 25 μm sieve is preferably 13% or more, more preferably 16% or more. There is no particular upper limit to this proportion, and all of the powder on the 25 μm sieve may be structures formed by agglomeration of hexagonal boron nitride primary particles having an elongation of 0.80 or more, but it may usually be 25% or less, particularly 20% or less.

[0023] The hexagonal boron nitride powder according to one embodiment of the present invention preferably has a particle size D50 of 15.0 μm or more, and more preferably 20.0 μm or more. By setting the particle size D50 to 15.0 μm or more, the adhesive force between individual particles becomes appropriate, and it becomes easy to obtain high spreadability and a fluffy feel in a cosmetic preparation containing the hexagonal boron nitride powder according to one embodiment of the present invention. Furthermore, the particle size D50 is preferably 40.0 μm or less, more preferably 35.0 μm or less, even more preferably 30.0 μm or less, and particularly preferably 25.0 μm or less. By setting the particle size D50 to 40.0 μm or less, it becomes easy to impart smoothness and suppress the occurrence of glare in a cosmetic preparation containing the hexagonal boron nitride powder according to one embodiment of the present invention.

[0024] The hexagonal boron nitride powder according to one embodiment of the present invention preferably has a particle size D90 of 37.0 to 52.0 μm, more preferably 37.0 to 45.0 μm, and even more preferably 38.0 to 42.0 μm. When the particle size D90 is within the above range, it becomes easy to enhance the moist feeling and fluffy feeling while suppressing roughness in a cosmetic containing the hexagonal boron nitride powder according to one embodiment of the present invention.

[0025] In one embodiment of the present invention, the particle size D50 and particle size D90 of the hexagonal boron nitride powder refer to the volume-based cumulative 50% value (particle size D50) and cumulative 90% value (particle size D90) on a particle size distribution curve, respectively.

[0026] In the hexagonal boron nitride powder according to one embodiment of the present invention, the proportion of powder that has passed through a 25 μm sieve is preferably 40% by mass or more, more preferably 50% by mass or more. The upper limit of the proportion of powder that has passed through a 25 μm sieve is not particularly limited, but is usually 70% by mass or less, particularly 60% by mass or less. The proportion of powder that has passed through a 25 μm sieve can be calculated by passing all or a portion of the hexagonal boron nitride powder through a 25 μm sieve and calculating the mass of the powder that has passed through the sieve and the mass of the powder that has passed through the sieve.

[0027] The aspect ratio of the primary particles of the hexagonal boron nitride powder according to one embodiment of the present invention is preferably 15.0 to 20.0, and more preferably 17.0 to 18.0. Having an aspect ratio of the primary particles within the above range facilitates good spreadability while suppressing glare when applied to the skin. If the aspect ratio of the primary particles is less than 15.0, a cosmetic containing the hexagonal boron nitride powder according to one embodiment of the present invention may experience resistance upon application and may have reduced spreadability. Furthermore, if the aspect ratio of the primary particles exceeds 20.0, a cosmetic containing the hexagonal boron nitride powder according to one embodiment of the present invention may experience glare after application to the skin.

[0028] The amount of eluted boron from the hexagonal boron nitride powder according to one embodiment of the present invention is preferably 20 ppm or less. By keeping the amount of eluted boron at 20 ppm or less, it is possible to reduce the burden on the skin when a cosmetic containing the hexagonal boron nitride powder according to one embodiment of the present invention is applied to the skin.

[0029] <Method for producing hexagonal boron nitride powder> The hexagonal boron nitride powder according to one embodiment of the present invention is not particularly limited, but can be easily obtained by heat-treating a coarse hexagonal boron nitride powder obtained under specific conditions under specific conditions. Specifically, a raw material powder containing the coarse hexagonal boron nitride powder is heated under specific conditions to a bulk density of 0.16 to 0.23 g / cm. 3 and heating the powder in a nitrogen atmosphere at 1700°C to 2100°C for 3 hours or more, wherein the coarse hexagonal boron nitride powder has a specific surface area of ​​12 to 30 m 2 / g and the amount of eluted boron is 1 to 15%.

[0030] (Method for producing coarse hexagonal boron nitride powder) The coarse hexagonal boron nitride powder has a specific surface area of ​​12 to 30 m 2 / g and the amount of eluted boron is 1 to 15%, any known boron compound can be used without particular limitation. For example, the boron compound can be produced by the melamine method in which a raw material mixture containing an oxygen-containing boron compound and a nitrogen-containing organic compound is heated under a nitrogen atmosphere.

[0031] Examples of the oxygen-containing boron oxide include diboron trioxide (boron oxide), diboron dioxide, tetraboron trioxide, metaboric acid, perboric acid, and orthoboric acid. Generally, boric acid and boron oxide, which are readily available, are preferably used. The average particle size of the oxygen-containing boron compound is not particularly limited, but from the viewpoints of operability and reactivity, it is preferably 30 to 800 μm, and more preferably 100 to 500 μm. An average particle size of more than 30 μm reduces hygroscopicity and facilitates handling. An average particle size of 800 μm or less reduces uneven distribution of raw material components, making it easier to control the reaction.

[0032] Examples of the nitrogen-containing organic compound include cyandiamide, ammeline, melamine, urea, etc. Generally, melamine is preferably used because it is easy to handle.

[0033] In the raw material mixture for producing crude hexagonal boron nitride powder, the boron / nitrogen element ratio (B / N) is preferably 0.2 to 1.0, more preferably 0.25 to 0.75. The raw material mixture can be obtained by measuring and mixing predetermined amounts of the oxygen-containing boron compound and nitrogen-containing organic compound described above. The mixing method is not particularly limited as long as it can uniformly disperse the components, and can be carried out using a general mixer such as a vibration mill, bead mill, ball mill, or mixer.

[0034] Nitride powder can be obtained by heating the above-mentioned raw material mixture in a nitrogen atmosphere to cause a reaction. The heating temperature is not particularly limited as long as it is 1600°C or higher, but it is preferable to gradually increase the temperature to the maximum temperature in each temperature range for the reaction process and the firing process, and then maintain the temperature. In the reaction process, a range of 700 to 1200°C is preferred, and 800 to 1100°C is more preferred. By setting the heating temperature in this range in the reaction process, the reaction can be efficiently carried out while suppressing volatilization of the raw material mixture.

[0035] The maximum temperature in the firing process is preferably 1600 to 2000°C, more preferably 1700 to 1800°C. By setting the maximum temperature to 1600°C or higher, the nitriding reaction of the oxygen-containing boron compound can be completed efficiently and in a short time. Furthermore, by setting the maximum temperature to 2000°C or lower, yellowing and loss of transparency due to nitrogen defects can be prevented, the specific surface area can be prevented from becoming too small, and efficient grain growth can be facilitated during the heat treatment described below.

[0036] The retention time during the reaction process is preferably 1 to 5 hours, more preferably 2 to 4 hours. If the retention time during the reaction process is too short, there is a risk that unreacted raw materials will remain, and if it is too long, productivity will decrease. The retention time during the firing process is preferably 1 to 6 hours, more preferably 2 to 5 hours. If the retention time during the firing process is too short, particle growth will be insufficient, resulting in a decrease in crystallinity and making particle size control difficult, and if it is too long, productivity will decrease.

[0037] Since the nitride powder obtained by the nitriding reaction generally contains coagulated bodies of several hundred μm or more, it is preferable to crush the coagulated bodies with a force sufficient to pulverize the coagulated bodies. Crushing the coagulated bodies also makes it possible to obtain an appropriate specific surface area for the coarse hexagonal boron nitride powder. Crushing the coagulated bodies also makes it possible to efficiently carry out the washing and classification steps described below. As long as the coagulated bodies can be crushed, the crushing method is not particularly limited, and can be suitably carried out using a stone mill, ball mill, dry jet mill, mortar, roll crusher, wet rotary disk mill, or the like.

[0038] The crushed powder obtained in the crushing step may be washed with pure water or the like for the purposes of removing impurities and adjusting the amount of boron eluted from the crude hexagonal boron nitride powder. The washing method and the amount of pure water or the like used for washing are not particularly limited, and known methods can be used without limitation. The method for drying the crushed powder after washing is not particularly limited, and known methods can be used without limitation. Examples of drying devices that can be used include tray dryers, fluidized bed dryers, spray dryers, rotary dryers, and belt dryers. Note that if the amount of boron eluted from the crude hexagonal boron nitride powder becomes too low due to excessive washing, for example, an oxygen-containing boron compound such as boron oxide may be added to adjust the amount of boron eluted from the crude hexagonal boron nitride powder.

[0039] Classification may be performed to remove any coagulated material remaining in the crushed powder obtained in the crushing step. The classification method is not particularly limited, and known methods can be used without limitation. Specific examples include a vibrating sieve, a wet sieve, an air classifier, a cyclone, and a liquid cyclone. The sieve opening is preferably 25 to 90 μm, and more preferably 25 to 45 μm. By setting the opening to 90 μm or less, the proportion of single particles in the powder can be increased, allowing for efficient generation of structures in the heating step described below. Furthermore, if the opening is less than 25 μm, the time required for processing becomes longer, so a sieve opening of 25 μm or more is preferred.

[0040] (Method for producing hexagonal boron nitride powder) The hexagonal boron nitride powder according to one embodiment of the present invention has a specific surface area of ​​12 to 30 m 2 A raw material powder containing the crude hexagonal boron nitride powder having a bulk density of 0.16 to 0.23 g / cm3 and an eluted boron amount of 1% to 15% is mixed with the raw material powder. 3 The mixture is packed into a heating vessel so that the temperature becomes 1700° C. to 2100° C., and heated in a nitrogen atmosphere for 3 hours or more.

[0041] Although the reason why the hexagonal boron nitride powder of the present invention is obtained in this way is not clear, the inventors believe as follows: Namely, by heating crude hexagonal boron nitride powder with 1 to 15% eluted boron in a nitrogen atmosphere, the powder is heated in a state in which a small amount of boric acid is present on the particle surface, and the nitriding reaction proceeds again on the particle surface, causing the particles to grow and some of the primary particles to bond together, thereby producing the above-mentioned structure. 3 By setting the range to 0.08 g / cm, it is possible to achieve slight orientation while leaving a moderate gap between the particles. Although bonding occurs at the ends of the a-planes, which are likely to come into contact due to the orientation, the presence of voids prevents bonding between the structures in the c-axis direction, resulting in a structure with an elongation of 0.80 or more. As a result, a tapped bulk density of 0.08 g / cm is obtained. 3 Hereinafter, it is assumed that a hexagonal boron nitride powder having a shear adhesive strength of 3.5 kPa or more calculated from the powder bed fracture envelope obtained by the powder bed shear strength measurement test can be easily obtained.

[0042] The specific surface area of ​​the coarse hexagonal boron nitride powder is 12 to 30 m 2 / g, and 15 to 28 m 2 / g, and 20 to 25m 2 / g is more preferable. Furthermore, the amount of eluted boron from the crude hexagonal boron nitride powder is 1 to 15%, preferably 2 to 10%, and more preferably 3 to 5%. By setting the specific surface area and amount of eluted boron of the crude hexagonal boron nitride powder within the above ranges, efficient grain growth and the formation of a structure can be achieved by heat treatment. That is, a specific surface area within the above range allows nitrogen to circulate within the powder while providing sufficient reaction sites on the primary particles of the crude hexagonal boron nitride powder. Furthermore, it is presumed that a boron source amount within the above range facilitates grain growth and facilitates the formation of a structure with a high degree of elongation. Furthermore, by setting the amount of eluted boron from the crude hexagonal boron nitride powder to 15% or less, it becomes easy to suppress the amount of eluted boron from the hexagonal boron nitride powder to 20 ppm or less.

[0043] The raw material powder may contain the coarse hexagonal boron nitride powder, and may consist solely of the coarse hexagonal boron nitride powder, or may contain other components within limits that do not impair the effects of the present invention. However, it is preferable that the raw material powder consist solely of the coarse hexagonal boron nitride powder, as this makes it easier to omit the washing operation after heating, which will be described later, and to simplify the classification operation.

[0044] The heating temperature is preferably 1700°C to 2100°C, more preferably 1750°C to 2000°C, and even more preferably 1800°C to 1950°C. By heating the crude hexagonal boron nitride powder to a temperature of 1700°C or higher, it becomes easy to form structures while efficiently growing particles and increase shear adhesion. By setting the heating temperature to 2100°C or lower, it becomes easy to prevent yellowing due to nitrogen defects and to obtain hexagonal boron nitride powder with a color tone appropriate for cosmetic use. Furthermore, the particle size of the hexagonal boron nitride powder can be adjusted by the heating temperature, and by setting the heating temperature within the above range, it becomes easy to adjust the particle size of the resulting hexagonal boron nitride powder to a range appropriate for cosmetic use.

[0045] The hexagonal boron nitride powder obtained by heat-treating the crude hexagonal boron nitride powder by the above-mentioned method may be washed after the heating in order to remove impurities. Washing can be carried out using, for example, pure water, and the washing method and the amount of pure water used for washing are not particularly limited, and any known method can be used without limitation.

[0046] The hexagonal boron nitride powder obtained by heat-treating the crude hexagonal boron nitride powder using the above-described method may be classified for the purposes of removing impurities and controlling the particle size D90. The classification method is not particularly limited, and known methods can be used without limitation. Specific examples include a vibrating sieve, a wet sieve, an air classifier, a cyclone, and a liquid cyclone. The sieve opening is preferably 40 to 90 μm, and more preferably 45 to 63 μm. By setting the opening to 90 μm or less, the roughness of the hexagonal boron nitride powder can be suppressed. Furthermore, if the opening is too small, the time required for processing increases.

[0047] <Cosmetics> While the use of the hexagonal boron nitride powder of the present invention is not particularly limited, its use in cosmetics is preferred, and it is particularly well suited to solid or powdered cosmetics. Another aspect of the present invention is a cosmetic containing the hexagonal boron nitride powder, particularly a solid or powdered cosmetic. By incorporating the hexagonal boron nitride powder of the present invention into a cosmetic, it is possible to easily achieve both a moist and fluffy feel. While previously it was not possible to achieve both a moist and fluffy feel, or it was necessary to achieve both by adjusting the blending of other ingredients as needed, the use of the hexagonal boron nitride powder of the present invention makes it easier than ever to achieve both a moist and fluffy feel, thereby increasing the flexibility of cosmetic design. Examples of cosmetics include loose foundation and face powder. The content of the hexagonal boron nitride powder in the entire cosmetic is not particularly limited, but a content of 0.1% to 50% by mass is preferred. By blending the present invention into cosmetics within the above ranges, the moist feeling and fluffy feeling of the cosmetics can be improved more easily.

[0048] <Summary> As described above, the hexagonal boron nitride powder according to aspect 1 of the present invention has a tapped bulk density of 0.08 g / cm 3 The shear adhesive strength calculated from the powder bed fracture envelope obtained by the powder bed shear force measurement test is 3.5 kPa or more.

[0049] The hexagonal boron nitride powder according to Aspect 2 of the present invention may be the same as Aspect 1, wherein the proportion of structures formed by agglomeration of hexagonal boron nitride primary particles having an elongation of 0.80 or more in the powder passing through a 25 μm mesh sieve is 13% or more.

[0050] The hexagonal boron nitride powder according to Aspect 3 of the present invention may be the same as Aspect 1 or 2, in which the particle size D50 is 15 to 30 μm and the average aspect ratio is 15 to 20.

[0051] The hexagonal boron nitride powder according to Aspect 4 of the present invention may be the powder of any one of Aspects 1 to 3, and have a particle size D90 of 37 to 52 μm.

[0052] The hexagonal boron nitride powder according to Aspect 5 of the present invention may be for use in cosmetics in any one of Aspects 1 to 4.

[0053] A cosmetic according to a sixth aspect of the present invention comprises the hexagonal boron nitride powder according to any one of the first to fifth aspects.

[0054] A loose foundation according to a seventh aspect of the present invention comprises the hexagonal boron nitride powder according to any one of the first to fifth aspects.

[0055] A method for producing a hexagonal boron nitride powder according to an eighth aspect of the present invention comprises: mixing a raw material powder containing a coarse hexagonal boron nitride powder with a bulk density of 0.16 to 0.23 / cm 3 and heating the powder in a nitrogen atmosphere at a maximum temperature of 1700°C to 2100°C for 3 hours or more, wherein the coarse hexagonal boron nitride powder has a specific surface area of ​​12 to 30 m 2 / g, and the amount of eluted boron is 1 to 15%.

[0056] Examples will be described below to specifically explain the present invention, but the present invention is not limited to these examples. The measurements of the various items in the examples and comparative examples were performed by the following methods.

[0057] (1) Tapped bulk density of hexagonal boron nitride powder The tapped bulk density (g / cm) was measured using a tapped densityr KYT-5000 (manufactured by Seishin Enterprises). 3 Specifically, 100 mL of hexagonal boron nitride powder was filled into a 100 mL sample cell, and tapped 500 times at a tapping speed of 120 times / min, at a tapping height of 5 cm, and then the weight was measured to calculate the tapped bulk density.

[0058] (2) Shear Adhesion of Hexagonal Boron Nitride Powder Measurements were performed in accordance with JIS Z8835:2016 using a powder bed shear force measuring device NS-S500 (manufactured by Nano Seeds Corporation). Specifically, hexagonal boron nitride powder was filled into a shear cell, the top surface of the powder bed was flattened, and then lateral sliding was initiated with a target indentation load of 160 N. The normal stress and shear stress were measured over time to measure the powder bed failure envelope. The shear adhesion was then calculated from the intersection of the powder bed failure envelope and the shear stress axis.

[0059] (3) Elongation and Content of Hexagonal Boron Nitride Powder Structures 15 g of hexagonal boron nitride powder was sieved through a 25 μm mesh sieve, and the hexagonal boron nitride powder that did not pass through (powder on the 25 μm mesh sieve) was collected and weighed. A portion of the powder on the 25 μm mesh sieve was observed with a scanning electron microscope (SEM). From the SEM images obtained, the length of the longest line (major axis) connecting the ends of each structure was measured as the major axis diameter a, and the length of the longest line (minor axis) intersecting the major axis at a right angle as the minor axis diameter b, and the elongation of each structure was calculated. Thereafter, the area of ​​the structures having an elongation of 0.80 or more and the area of ​​the other particles were determined, and the area ratio of the structures having an elongation of 0.80 or more to the area of ​​all particles (the sum of the area of ​​the structures having an elongation of 0.80 or more and the area of ​​the other particles) was determined, and this was taken as the ratio of structures formed by agglomeration of hexagonal boron nitride primary particles having an elongation of 0.80 or more.

[0060] (4) Aspect Ratio of Primary Particles of Hexagonal Boron Nitride Powder 10 parts by mass of hexagonal boron nitride powder was dispersed in 100 parts by mass of epoxy resin (EA E-30CL, manufactured by Henkel). The resulting resin composition was degassed under reduced pressure, poured into a 10 mm square, 1 mm thick mold, and cured at a temperature of 70 ° C. The cured resin composition was then removed from the mold and polished to achieve equilibrium on both sides. Furthermore, the center of one of the surfaces perpendicular to the thickness direction of the resin composition was subjected to cross-sectional milling, and an image of the processed surface was taken using an SEM at a magnification of 2500x. 100 boron nitride primary particles were randomly selected from the obtained image, and the long side (major axis) and short side (thickness) of the particles were measured. The average values ​​were defined as the average major axis (μm) and average thickness (μm), respectively. The value obtained by dividing the average major axis by the average thickness was defined as the aspect ratio (average major axis / average thickness).

[0061] (5) Particle size (D50) and (D90) of hexagonal boron nitride powder: Measurement was performed by laser diffraction using a laser diffraction / scattering particle size analyzer MT3000 (manufactured by Microtrac Bell Co., Ltd.) Specifically, 0.1 g of hexagonal boron nitride powder was placed in a mixing vessel attached to the analyzer filled with 50 cc of ethanol, and the powder was ultrasonically dispersed for 20 seconds at an output of 40 W. The resulting sample was used for measurement, and the particle size (D50) and (D90) on a volume basis were calculated.

[0062] (6) Specific Surface Area of ​​Crude Hexagonal Boron Nitride Powder A gas adsorption test was carried out using a Flowsorb III 2310 (manufactured by Micromeritics) with nitrogen gas as the adsorbent, and the nitrogen adsorption isotherm was measured. Specifically, the crude hexagonal boron nitride powder was pretreated by vacuum drying and degassing at 200°C for 10 minutes, and the nitrogen adsorption isotherm was measured at a gas flow rate of 15 cm. 3 The adsorption / desorption isotherm of nitrogen gas was measured using a continuous flow method under the condition of 1000 kJ / min, and the adsorption / desorption isotherm was calculated by the BET method.

[0063] (7) Amount of Boron Dissolved from Crude Hexagonal Boron Nitride Powder and Hexagonal Boron Nitride Powder 50 g of a 0.5 mol / L aqueous sulfuric acid solution and 2 g of crude hexagonal boron nitride powder or hexagonal boron nitride powder were added to a 50 mL Eye-Boy, and the solution was shaken and stirred for 1 minute while the temperature of the solution was adjusted to 25° C. After allowing to stand for 120 minutes, the amount of boron in the resulting solution was analyzed using an ICP optical emission spectrometer (iCAP6500 manufactured by THERMO FISHER), and the measurement result was divided by the mass of the crude hexagonal boron nitride powder or hexagonal boron nitride powder used in the test to determine the amount of boron dissolved per unit mass (ppm).

[0064] (Example 1) Boron oxide (B 2 O 3120 g of hexagonal boron nitride powder and 100 g of melamine (boron / nitrogen element ratio (B / N) 0.72) were mixed in a mixer and stirred, and then filled into a lidded carbon container. The mixture was then heated at 1000°C for 4 hours in a nitrogen gas atmosphere using a graphite Tammann furnace (reaction process). The temperature was then increased to 1750°C and maintained at that temperature for 4 hours (sintering process), thereby obtaining nitride powder. The obtained nitride powder was then crushed in a millstone grinder, washed with pure water, and dried at 200°C. The powder was then classified using a sieve with 45 μm openings to obtain a crude hexagonal boron nitride powder with an eluted boron content of 4%. The obtained crude hexagonal boron nitride powder was used as a raw material powder and placed in a lidded carbon container surface-coated with boron nitride. A bulk density of 0.19 g / cm was obtained. 3 The mixture was packed so that the powder was filled into a molten metal powder, and heated in a graphite Tammann furnace under a nitrogen gas atmosphere at 1950°C for 6 hours. The mixture was then classified using a sieve with 45 µm openings to obtain hexagonal boron nitride powder. The production conditions and the evaluation results of the obtained hexagonal boron nitride powder are shown in Table 1.

[0065] (Examples 2 to 5, Comparative Examples 2 to 4) Hexagonal boron nitride powder was obtained in the same manner as in Example 1, except that the production conditions were changed as shown in Table 1. The amount of boron eluted from the crude hexagonal boron nitride powder was adjusted by the washing conditions. The production conditions and the evaluation results of the obtained hexagonal boron nitride powder are shown in Table 1.

[0066] Comparative Example 1 The physical properties of the crude hexagonal boron nitride powder obtained in Example 1 were evaluated. Table 1 shows the production conditions and the evaluation results of the obtained hexagonal boron nitride powder.

[0067] Furthermore, loose foundations were produced using the hexagonal boron nitride powders obtained in Examples 1 to 5 and Comparative Examples 1 to 4, according to the following compositions.

[0068] Hexagonal boron nitride powder 20.0 mass% Mica 32.0 mass% Synthetic phlogopite 12.0 mass% (Vinyl dimethicone / methicone silsesquioxane) crosspolymer 5.0 mass% (Diphenyl dimethicone / vinyl diphenyl dimethicone / silsesquioxane) crosspolymer 5.0 mass% Nylon 12 3.0 mass% Silica 3.0 mass% Talc 3.0 mass% Zinc oxide 3.0 mass% Polymethyl methacrylate polymer 3.0 mass% Ethylhexyl methoxycinnamate 2.0 mass% Perfluorooctyltriethoxysilane 1.0 mass% Silicone-treated red iron oxide (red iron oxide) 1.0 mass% Silicone-treated yellow iron oxide 0.6 mass% Silicone-treated black iron oxide 0.4 mass% Silicone-treated titanium oxide 6.0 mass% The loose foundation obtained with the above formulation was subjected to a sensory evaluation by 20 expert panelists regarding the fluffy feel and moist feel. If less than 30% of the panelists felt it was good, it was rated as "bad," if it was 30% or more but less than 60%, it was rated as "average," if it was 60% or more but less than 80%, it was rated as "good," and if it was 80% or more, it was rated as "very good." The evaluation results are shown in Table 1.

[0069]

[0070] In the evaluation results, raw material powder containing coarse hexagonal boron nitride powder with an eluted boron amount of 1 to 15% was used in a powder having a bulk density of 0.16 to 0.23 g / cm 3 The mixture was packed into a heating vessel so that the tapped bulk density was 0.08 g / cm and heated in a nitrogen atmosphere at 1750°C to 2100°C for 4 hours or more to obtain hexagonal boron nitride powder. In Examples 1 to 5, all of the obtained hexagonal boron nitride powders had a tapped bulk density of 0.08 g / cm. 3The powder shear adhesive strength was 3.5 kPa or more. The loose foundations containing these hexagonal boron nitride powders showed good results in terms of both fluffy feel and moist feel in the sensory evaluation.

[0071] On the other hand, the tapped bulk density of Comparative Example 1, in which a coarse hexagonal boron nitride powder was evaluated without heat treatment, and the hexagonal boron nitride powder of Comparative Example 2, which was produced by heating a coarse hexagonal boron nitride powder with an eluted boron amount of less than 1%, was 0.08 g / cm 3 The shear adhesive strength exceeded 3.5 kPa, and the fluffy and moist feel was not obtained.

[0072] In addition, when the coarse hexagonal boron nitride powder is heat-treated, the bulk density is 0.16 g / cm 3 In Comparative Example 3, in which the powder was packed into a heating vessel so that the bulk density was less than 0.23 g / cm, the resulting hexagonal boron nitride powder had a shear adhesion strength of less than 3.5 kPa and did not have a moist feel. 3 In Comparative Example 4, in which the powder was produced by filling the heating vessel with the powder so that the tapped bulk density exceeded 0.08 g / cm. 3 This exceeded the limit, and it was not possible to obtain a satisfactory fluffy feel.

Claims

1. Tapped bulk density is 0.08 g / cm 3 and a shear adhesion strength calculated from a powder bed fracture envelope obtained by a powder bed shear strength measurement test is 3.5 kPa or more.

2. The hexagonal boron nitride powder according to claim 1, in which the proportion of structures in which hexagonal boron nitride primary particles having an elongation of 0.80 or more are aggregated in the powder passing through a 25 μm mesh sieve is 13% or more.

3. The hexagonal boron nitride powder according to claim 1, having a particle size D50 of 15-30 μm and an average aspect ratio of 15-20.

4. The hexagonal boron nitride powder according to claim 1, having a particle size D90 of 37 to 52 μm.

5. The hexagonal boron nitride powder according to any one of claims 1 to 4, which is for use in cosmetics.

6. A cosmetic comprising the hexagonal boron nitride powder according to claim 5.

7. A loose foundation comprising the hexagonal boron nitride powder according to claim 5.

8. The raw material powder containing the coarse hexagonal boron nitride powder is mixed with a powder having a bulk density of 0.16 to 0.23 / cm 3 and heating the powder in a nitrogen atmosphere for 3 hours or more at a maximum temperature of 1700° C. to 2100° C., 2 / g and the amount of eluted boron is 1 to 15%.