Method for forming three-dimensional wood grain on board surface, generated board and use
Patent Information
- Application Number
- MYPI2025005942
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-01
- Publication Date
- 2024-09-30
AI Technical Summary
When the existing technology forms three-dimensional wood grain on the surface of the board, it cannot achieve a texture similar to that of natural wood, especially in terms of visual and tactile authenticity, and there are problems of reduced texture clarity and inconsistent depth.
After forming a wood grain bottom layer on the surface of the board, and then creating a three-dimensional wood grain layer on it, we use the combined technology of multi-layer resin liquid and embossing liquid to control the curing of the resin liquid and the penetration of the embossing liquid to ensure that the wood The adhesion between the bottom layer of the grain and the three-dimensional wood grain layer and the accuracy of the pattern are improved, and the three-dimensional sense and clarity are improved by adjusting the composition and density of the resin liquid and embossing liquid.
The visual and tactile effect of the board surface is closer to that of natural wood, which improves the stability and service life of the texture, reduces the defective rate, and improves the depth and clarity of the three-dimensional wood grain layer.
Smart Images

Figure PI2025005942_DRAWING_001 
Figure PI2025005942_DRAWING_002 
Figure PI2025005942_DRAWING_003
Abstract
Description
Method for forming three-dimensional wood grain on board surface, resulting board and application Technical Field
[0001] The present invention relates to the field of surface structure preparation, and in particular to a method for forming three-dimensional wood grain on a board surface, a board containing the three-dimensional wood grain, a method for forming the board, and applications of the board. Background Art
[0002] At present, in order to obtain a texture similar to natural wood on the surface of artificial boards or non-wood boards, a layer of imitation wood two-dimensional flat image is usually formed on the surface of the board by printing or imitation, thereby visually satisfying people's visual needs for wood materials.
[0003] For example, patent publication number CN 101659073 B discloses a wood grain treatment process for waterproof flooring substrates. This process involves printing simulated wood grain on the surface of a wood-plastic flooring substrate and then adding a wear-resistant layer over the simulated wood grain. This protects the wood grain pattern and maintains the wood grain texture over time. However, this type of board, which is simply printed with a two-dimensional graphic, no longer meets people's demand for a more realistic visual and tactile experience.
[0004] Therefore, forming three-dimensional wood grain on the surface of a board material that corresponds to a two-dimensional plane image and has a touch that is more similar to wood is currently a common concern in the art.
[0005] In the prior art, a variety of different technical solutions have been proposed to form a three-dimensional structure on the surface of a substrate. Conventional methods generally include an upward stacking method and a downward indentation method.
[0006] Taking the upward stacking method as an example, the related technology can be referred to the following patents:
[0007] Patent publication number CN 112455110 A discloses a process for producing wood flooring using inkjet printing. This patent allows for the formation of convex three-dimensional wood grain by continuously printing additive ink on the surface of a printed pattern. However, actual testing revealed that the ink exhibits a certain degree of fluidity before curing, resulting in a limited molding height. Furthermore, as the resin flows, the texture angles of the three-dimensional wood grain produced through this upward stacking method become more rounded than those of natural wood grain, resulting in a significant difference in the actual effect from natural wood grain, making it difficult to achieve the visual effect and tactile feel of natural solid wood.
[0008] Taking the downward inward method as an example, the related technology can be referred to the following patents:
[0009] Patent publication number CN 110177691 B discloses a method and apparatus for producing embossing patterns on a substrate using digital printing technology. This method involves applying an embossing liquid to a non-polymeric resin layer, then UV curing the resin for subsequent polymerization. The embossing liquid is then removed to form a three-dimensional surface. The three-dimensional wood grain produced using this method offers improved visual quality and tactile feel compared to the stacking method. However, actual testing revealed that the clarity of the three-dimensional wood grain produced using this method decreased significantly after forming it on the surface of an ink layer with a wood grain pattern. This was manifested by a whitish appearance and significant color difference.
[0010] Patent publication number CN 112996649 A discloses a method for fabricating a three-dimensional structure on the surface of a flat substrate, the resulting substrate, and an apparatus for producing the substrate according to this method. The method involves pre-applying a material for forming a grain joint onto the substrate surface. A curable resin is then applied to the areas of the substrate surface not covered by the grain joint material. After the resin is cured, the grain joint material is removed, thereby forming grain joints within the cured resin. However, the depth of the grain joints is always the distance between the top surface of the cured resin and the substrate surface; in other words, the depth of each grain joint is consistent. However, the depth of cracks on the surface of real wood panels can vary. Therefore, the depth of the grain joints produced by this method differs significantly from the actual depth, resulting in an unrealistic appearance.
[0011] In summary, in order to measure the similarity between three-dimensional wood grain and natural wood grain, the dimensions that need to be considered include: (1) the similarity between the width and depth of the three-dimensional wood grain and the natural wood grain; (2) the correspondence between the three-dimensional wood grain and the bottom two-dimensional plane structure; (3) the color visual effect presented by the combination of the three-dimensional wood grain and the bottom two-dimensional plane. Currently, in the process of forming three-dimensional wood grain, existing public technologies often focus more on the combination of dimension (1) and dimension (2).
[0012] Among them: Regarding dimension (1), the width and depth of the three-dimensional wood grain can be determined by controlling the amount and position of the material during the formation of the three-dimensional wood grain. For example, the width of the wood grain can be determined by the width of the stacked structure or the breadth during the downward excavation process or the area of the corrosive liquid. The depth of the three-dimensional wood grain can be determined by the height of the upward stacking and the force of the downward excavation. The more obvious the difference in the width and depth of the three-dimensional wood grain, the more three-dimensional the structure it presents, and the closer the effect it can present from the visual and tactile senses to natural wood grain.
[0013] Regarding dimension (2), the degree of correspondence between the three-dimensional wood grain and the two-dimensional planar structure at the bottom can be controlled by controlling the printing accuracy, for example, involving the control of the computer program and the coordination and regulation between the computer and the molding equipment. It also involves various physical and chemical properties of the material itself, such as its own viscosity, surface energy, and the diffusion coefficient between different materials. The higher the degree of correspondence between the three-dimensional wood grain and the two-dimensional planar structure at the bottom, the closer the three-dimensional structure can be to the surface wood grain structure of real solid wood.
[0014] Regarding dimension (3), there is currently no literature or technology that discloses the relationship between three-dimensional structure and visual effects. The few technologies that exist only include matte or glossy effects such as three-dimensional wood grain, while the technology required to truly achieve the visual effect of real wood grain has not yet appeared.
[0015] Therefore, there is no precedent in the currently disclosed technologies for simultaneously taking into account dimension (3) while achieving dimension (1) and dimension (2). Therefore, how to simultaneously take into account these three dimensions is the key to obtaining a texture similar to that of natural wood on the surface of artificial boards or non-wood boards. Summary of the Invention
[0016] The present invention aims to overcome the defect that the existing method of forming three-dimensional wood grain on the surface of a board cannot obtain a texture close to that of natural wood, and provides a method for forming three-dimensional wood grain on the surface of a board, the resulting board and its application.
[0017] To achieve the above-mentioned purpose, the present invention is implemented through the following technical solutions:
[0018] In the first aspect, the present invention first provides a
[0019] The method for forming three-dimensional wood grain on the surface of a board comprises at least the following steps:
[0020] (S.1) covering at least a portion of the surface of the board with ink, thereby forming an ink layer having a wood grain pattern;
[0021] (S.2) a step of covering at least a portion of the surface of the ink layer with a resin liquid;
[0022] (S.3) solidifying at least a portion of the resin liquid on the surface of the ink layer to form a wood grain base layer;
[0023] (S.4) covering at least a portion of the surface of the wood grain base layer with at least one layer of resin liquid;
[0024] (S.5) applying embossing liquid to at least a portion of the surface of the resin liquid on the wood grain base layer along the wood grain pattern of the ink layer, thereby forming an embossing layer with the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid;
[0025] (S.6) a step of solidifying the resin liquid except for the embossed layer formed in the previous step;
[0026] (S.7) A step of removing the embossed layer to form a three-dimensional wood grain layer on the surface of the wood grain base layer.
[0027] Preferably, the amount of the resin liquid covering the surface of the wood grain bottom layer in the step (S.4) is greater than or equal to 150 g / m 2 .
[0028] Preferably, in the step (S.4), at least a portion of the surface of the wood grain bottom layer is covered with at least two layers of resin liquid.
[0029] Preferably, in the process of covering at least a portion of the surface of the wood grain bottom layer with any two adjacent layers of resin liquid, the process also includes a transition treatment step of stopping the application of force to the resin liquid after the wood grain bottom layer is covered by the previous layer of resin liquid, and covering with the next layer of resin liquid after the transition treatment step is completed.
[0030] Preferably, in the process of covering at least a portion of the surface of the wood grain bottom layer with any two adjacent layers of resin liquid, the directions of the forces applied to the any two adjacent layers of resin liquid are opposite.
[0031] Preferably, the plate completes steps (S.1) to (S.6) in sequence while being transported along a fixed direction.
[0032] Preferably, in the step (S.5), the embossing liquid is applied to the surface of the resin liquid and / or penetrates downward into the interior of the resin liquid.
[0033] Preferably, the curing method of the covering resin liquid in steps (S.2) and (S.4) includes any one of light curing, thermal curing or electron beam curing.
[0034] Preferably, the resin liquid includes at least a photo-crosslinking resin and a photoinitiator.
[0035] Preferably, the photo-crosslinking resin includes any one or more combinations of unsaturated polyester, epoxy resin, acrylic resin, acrylic modified polyurethane resin, acrylic modified silicone resin, acrylic modified epoxy resin, water-based epoxy acrylate, water-based polyurethane acrylate, and water-based polyester acrylate.
[0036] Preferably, the photoinitiator includes any one of a free radical polymerization initiator, a cationic polymerization initiator, an energy transfer initiator, and an ion reaction initiator.
[0037] Preferably, the embossing liquid in the step (S.5) contains at least a polymerization inhibitor for preventing polymerization of the resin liquid.
[0038] In this preferred embodiment, a polymerization inhibitor is added to the embossing liquid, which can quench the free radicals generated by the decomposition of the photoinitiator under light, thereby effectively preventing the polymerization of the resin liquid containing the polymerization inhibitor, thereby obtaining an embossing layer that is easy to remove.
[0039] Preferably, the resin liquid at least includes a thermosetting resin.
[0040] Preferably, the thermosetting resin includes one or more combinations of epoxy resin, phenolic resin, melamine formaldehyde resin, furan resin, unsaturated polyester resin, silicone resin, and polybutadiene resin.
[0041] Preferably, the resin liquid further includes a curing agent.
[0042] Preferably, the step (S.4) further comprises a step for providing kinetic energy for the embossing liquid to penetrate downward into the resin liquid.
[0043] Preferably, the embossing liquid contains a curable resin.
[0044] Preferably, the curable resin contained in the embossing liquid has a surface energy lower than the surface energy of the three-dimensional wood grain layer after curing.
[0045] Preferably, the curable resin contained in the embossing liquid has a surface energy lower than 100 mN / m after curing.
[0046] Preferably, the curable resin contained in the embossing liquid includes any one of fluorocarbon resin, fluorosilicone resin or silicone resin.
[0047] Preferably, the density of the embossing liquid is greater than the density of the resin liquid.
[0048] Preferably, the embossing liquid further comprises a density regulator for adjusting the density of the embossing liquid.
[0049] Preferably, the density regulator is an inorganic solid additive.
[0050] Preferably, the density regulator is nano-calcium carbonate, nano-silicon dioxide, etc.
[0051] Preferably, the embossing liquid comprises at least two embossing liquids with different surface tensions.
[0052] Preferably, the following are arranged in sequence between the board and the wood grain bottom layer:
[0053] A primer layer used to improve the bonding properties of the board surface;
[0054] A color paint layer provided on the surface of the primer layer to cover the color of the substrate;
[0055] An ink layer located on the surface of the paint layer to form a wood grain pattern.
[0056] Preferably, the outer surface of the three-dimensional wood grain layer is further covered with a topcoat layer, and at least a portion of the topcoat layer is lower than the upper surface of the three-dimensional wood grain layer.
[0057] In a third aspect, the present invention further provides a method for preparing the board having three-dimensional wood grain.
[0058] The method at least comprises the steps of preparing a wood grain base layer and a three-dimensional wood grain layer according to the method described above.
[0059] As an advantage, the method further comprises the following steps:
[0060] A step of covering at least a portion of the surface of the plate with a primer and curing the primer layer;
[0061] The step of covering at least a portion of the surface of the primer layer with a color paint and curing the primer layer to obtain a color paint layer;
[0062] The step of covering at least a portion of the surface of the color paint layer with ink having a wood grain pattern and curing the ink layer;
[0063] The step of making at least a portion of the surface of the ink layer cover the wood grain base layer and the three-dimensional wood grain layer prepared according to the method described above;
[0064] The step of covering at least a portion of the surface of the three-dimensional wood grain layer with a topcoat and curing the topcoat layer.
[0065] Preferably, the coverage of the primer is 10-15 g / m 2 ;
[0066] The coverage of the paint is 15-20 g / m 2 ;
[0067] The coverage of the ink is 6-8 g / m 2 ;
[0068] The coverage of the topcoat is 20-30 g / m 2 .
[0069] Preferably, the paint layer is white.
[0070] Preferably, the paint contains at least a photo-crosslinking resin, a photoinitiator and white pigment powder.
[0071] In a fourth aspect, the present invention further provides the use of the board with three-dimensional wood grain in floors, decorative wall panels or ceiling panels.
[0072] Therefore, the present invention has the following beneficial effects:
[0073] (1) The process of the present invention can produce a three-dimensional wood grain on the surface of the board that is closer to the real wood grain in terms of visual and tactile sense, thereby meeting people's demand for a more realistic combination of visual and tactile senses;
[0074] (2) The preparation process of the present invention can effectively improve the stability of the color and pattern of the plate;
[0075] (3) The plate prepared by the preparation process of the present invention has a longer service life and a lower defective rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] Figure 1 is a schematic representation of steps (S.1)-(S.7) of the method of the present invention.
[0077] Figure 2 is a schematic reproduction diagram of steps (S.6)-(S.8) in Example 1 of the present invention.
[0078] FIG3 is a schematic diagram of the three-dimensional structure of the three-dimensional wood grain prepared in Example 1 of the present invention.
[0079] FIG4 is a schematic top view of the three-dimensional wood grain structure prepared in Example 1 of the present invention.
[0080] FIG5 is a schematic diagram of the three-dimensional structure of the three-dimensional wood grain prepared in Comparative Example 1 of the present invention.
[0081] FIG6 is a schematic top view of the three-dimensional wood grain structure prepared in Comparative Example 2 of the present invention.
[0082] FIG7 is a schematic diagram of the three-dimensional structure of the three-dimensional wood grain prepared in Comparative Example 3 of the present invention.
[0083] Figure 8 is a schematic reproduction diagram of steps (S.6)-(S.8) in Example 2 of the present invention.
[0084] FIG. 9 is a schematic reproduction diagram of the method of coating the resin liquid on the surface of the wood grain base layer in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0085] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only a portion of the embodiments of the present invention, rather than all of the embodiments. Therefore, all other embodiments derived by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.
[0086] As shown in FIG1 , in a first embodiment of the present invention, the present invention first provides a method for forming three-dimensional wood grain on a surface of a board, comprising at least the following steps:
[0087] (S.1) covering at least a portion of the surface of the board with ink, thereby forming an ink layer having a wood grain pattern;
[0088] (S.2) a step of covering at least a portion of the surface of the ink layer with a resin liquid;
[0089] (S.3) solidifying at least a portion of the resin liquid on the surface of the ink layer to form a wood grain base layer;
[0090] (S.4) covering at least a portion of the surface of the wood grain base layer with at least one layer of resin liquid;
[0091] (S.5) applying embossing liquid to at least a portion of the surface of the resin liquid on the wood grain base layer along the wood grain pattern of the ink layer, thereby forming an embossing layer with the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid;
[0092] (S.6) a step of solidifying the resin liquid except for the sacrificial layer formed in the previous step;
[0093] (S.7) A step of removing the embossed layer to form a three-dimensional wood grain layer on the surface of the wood grain base layer.
[0094] The principle of the three-dimensional wood grain formed on the surface of the board material in the present invention is the same as the downward indentation method described in the background art. Compared with the upward stacking method, the width of the texture formed is controllable and the depth is longer, so the three-dimensional effect is stronger. At the same time, there will be no deformation of the wood grain during the printing process, so the printing accuracy is higher. However, in the process of conventionally forming three-dimensional wood grain using the downward indentation method, a portion of the ink layer will be exposed during the process of removing the embossed layer to obtain the three-dimensional wood grain layer. This exposed ink layer is easily worn or even peeled off by external forces. Therefore, in the process of using a machine to remove the embossed layer, the depth of the downward removal needs to be considered to prevent the wear of the ink layer, which makes it difficult to increase the depth of the three-dimensional wood grain layer.
[0095] During the process of creating a three-dimensional structure, the ink layer is first covered with a wood-grain base layer formed by solidifying a resin liquid. A three-dimensional wood-grain layer is then formed on the surface of the wood-grain base layer. Due to the presence of the wood-grain base layer, the ink layer remains covered during the removal of the embossed layer and the formation of the three-dimensional wood-grain layer. This prevents the ink layer from being worn or peeled off by external forces. Consequently, the embossed layer can be mechanically removed to the maximum depth, effectively increasing the depth of the three-dimensional wood-grain layer.
[0096] In addition, in order to make the board containing three-dimensional wood grain prepared by the present invention obtain a texture similar to that of natural wood, in addition to considering the wear of the ink layer and the depth of the three-dimensional wood grain layer, it is also necessary to consider the correspondence between the bottom ink layer and the upper three-dimensional wood grain layer, that is, the problem of alignment between the two. Regarding the problem of alignment, the applicant found that the following factors can cause the ink layer and the upper three-dimensional wood grain layer to have a misalignment defect: (1) During the preparation of the upper three-dimensional wood grain layer, the three-dimensional wood grain layer or the ink layer is deformed due to the shrinkage of the resin material itself during the curing process; (2) During the preparation of the three-dimensional wood grain layer, the compatibility between the embossing liquid and the resin liquid is insufficient, resulting in the depth, width and edge shape of the three-dimensional wood grain layer not being consistent with expectations. The applicant found that only after considering the above two factors at the same time can a texture similar to that of natural wood be truly obtained.
[0097] Regarding the influencing factor (1), the applicant found that during the curing process of the resin layer, since the energy (UV or heat) used to cure the resin liquid is usually input from the top of the resin liquid, the resin liquid at the top will cure first, while the resin liquid at the bottom will cure later. Since the resin liquid often shrinks in volume during the curing process, it will generate a certain amount of internal stress. These internal stresses will be superimposed downward, thus reaching a maximum value at the bottom of the resin liquid. If the resin liquid is in direct contact with the ink layer at this time, once the maximum internal stress is greater than the bonding force between the ink layer and the surface of the board, it will cause the ink layer and the surface of the board to slip, and then make it difficult for the ink layer at the bottom to correspond to the three-dimensional wood grain at the top, resulting in the problem of misalignment, which seriously affects the visual effect of the board. In addition, when the amount of resin liquid applied above the ink layer is large, the ink layer and the surface of the board may even peel off, which seriously reduces the product yield.
[0098] Therefore, in order to overcome the above problems, the present invention first covers at least a portion of the surface of the ink layer with resin liquid and solidifies this portion of the resin liquid to form a wood grain base layer. Since the amount of this portion of the resin liquid is small at this time, the internal stress generated after solidification is weak and will not affect the ink layer and the surface of the board.
[0099] Because the three-dimensional wood grain layer is formed by coating the wood grain base layer with a resin liquid and then curing it to form the three-dimensional wood grain layer, the affinity and adhesion between the wood grain base layer and the three-dimensional wood grain layer are strong, so slippage and peeling between the two will not occur. Furthermore, because the wood grain base layer has high mechanical strength after curing, the internal stress generated by the three-dimensional wood grain layer during curing is not sufficient to cause deformation of the wood grain base layer, and thus the internal stress generated by the three-dimensional wood grain layer during curing will not be transmitted to the ink layer located below the wood grain base layer. Therefore, by adding step (S.3), the problem of misalignment between the three-dimensional wood grain layer and the ink layer in subsequent steps (S.4) to (S.7) can be prevented to a certain extent.
[0100] As for the influencing factor (2), we need to further improve the compatibility between the embossing liquid and the resin liquid to improve the morphological stability of the embossing layer formed after the embossing liquid enters the resin liquid. In this regard, the prior art has adopted the step of adding embossing liquid to the incompletely cured resin layer. However, from the actual test results, due to the high viscosity of the incompletely cured resin layer itself, it is difficult for the embossing liquid to enter the resin layer. This brings the following problems: (1) The depth of the embossing liquid entering the resin layer is low, resulting in a low depth of the final wood grain, making the three-dimensional effect of the overall three-dimensional wood grain layer poor; (2) Due to the high viscosity of the incompletely cured resin layer, the embossing liquid is more likely to accumulate on the surface of the incompletely cured resin layer after application, making it easier for the embossing liquid to diffuse on the surface of the resin layer, making it difficult for the shape and width of the final wood grain to match the ink layer below, thereby causing the problem of misalignment; (3) The incompletely cured resin layer has weak fluidity, so it is difficult to blend with the embossing liquid in a short time, resulting in the formation of three-dimensional wood grain. The edges of the three-dimensional wood grain layer are more blurred and not sharp, which is obviously different from the structure of natural wood grain; (4) Since the viscosity of the incompletely cured resin layer is relatively high, even after it is mixed with the embossing liquid, the viscosity of the embossed layer obtained is relatively high. Although the embossed layer cannot be completely cured in the subsequent curing process, its viscosity can still be improved to a certain extent. Therefore, these high-viscosity embossed layers are difficult to be removed in the subsequent mechanical removal process, so there will often be a certain amount of residue, which further leads to the problem of unclear and blurred wood grain texture, which further widens the gap between its texture and the actual natural wood material.
[0101] Therefore, in addition to adding step (S.3) in the preparation process, the present invention also adopts the technical solution of applying the embossing liquid directly to the surface of the uncured resin liquid during the preparation process (i.e., step (S.5)). Compared with applying the embossing liquid to the semi-cured resin layer, by changing this step, it can bring the following beneficial effects: (1) Since the uncured resin liquid itself has a low viscosity, it has good fluidity. After being applied to the resin liquid, the embossing liquid can smoothly penetrate downward into the resin liquid, thereby greatly improving the depth of the prepared wood grain and effectively improving the three-dimensional effect of the three-dimensional wood grain layer. (2) At the same time, since the embossing liquid can penetrate into the resin liquid, it avoids the embossing liquid from diffusing on the surface of the uncured resin liquid, so that the shape and width of the wood grain finally formed can match the ink layer below, thereby effectively improving the accuracy of the pattern. (3) Since the resin liquid and the embossing liquid have a good mixing effect, the edges of the embossing liquid or the embossing layer obtained by mixing the embossing liquid and the resin liquid are more neat and sharp, so the prepared three-dimensional wood grain layer is closer to the natural wood grain. (4) Since the embossing liquid or the embossing layer obtained by mixing the embossing liquid with the resin liquid still has a low viscosity after curing, it is easier to remove after curing, and no residue will be left after removing the embossing layer, so the wood grain formed is cleaner and the edges are sharper.
[0102] Therefore, the present invention adopts the method of combining step (S.3) and step (S.5) to connect the functions and characteristics of the wood grain base layer, resin liquid and embossing liquid in series, thereby effectively overcoming the problem in the prior art that the morphology structure of the three-dimensional wood grain layer is too different from the natural wood grain, and there is misalignment between the three-dimensional wood grain layer and the ink layer below.
[0103] Furthermore, generally speaking, covering the ink layer with a transparent resin layer will cause the board's surface clarity to decrease visually, and this decrease in clarity increases with the thickness or number of resin layers above the ink layer. However, the applicant unexpectedly discovered that, through the method of the present invention, adding a wood grain base layer to the bottom of the three-dimensional wood grain layer can actually improve the clarity issue.
[0104] After conducting research, the applicant discovered that forming a three-dimensional wood grain layer on the surface of the ink layer visually creates a miniature "lens" effect, magnifying the underlying pattern. However, when the three-dimensional wood grain layer is directly attached to the ink layer, its focal length causes a certain degree of blurriness, resulting in poor clarity. The present application first provides a wood grain base layer below the three-dimensional wood grain layer, which adjusts the focal length of the three-dimensional wood grain layer, effectively improving the clarity of the wood grain.
[0105] Therefore, in summary, the method in this application can produce a board with three-dimensional wood grain that has a stronger three-dimensional effect, is more accurately aligned with the ink layer, and has a texture closer to that of actual natural wood materials.
[0106] In another preferred embodiment of the present invention, the amount of the resin liquid covering the surface of the wood grain bottom layer in step (S.2) is 40-50 g / m 2 .
[0107] In another preferred embodiment of the present invention, the amount of the resin liquid covering the surface of the wood grain bottom layer in the step (S.4) is greater than or equal to 150 g / m 2 .
[0108] The applicant discovered in actual practice that in order to make the three-dimensional wood grain on the surface of the board closer to the feel of natural wood, it is necessary to control the amount of resin liquid applied to form the three-dimensional wood grain. After testing, it was found that the total amount of resin liquid applied only on the wood grain base layer and the three-dimensional wood grain layer was greater than 200g / m 2 When the coating is more than 200g / m 2 After the above resin liquid is applied, it will cause the bottom of the wear-resistant layer to be difficult to solidify instantly, resulting in poor bonding between the three-dimensional wood grain and the ink layer on the surface of the board, and easy peeling between the three-dimensional wood grain and the substrate.
[0109] In order to achieve smooth curing of a large amount of resin liquid and enhance the bonding strength between the three-dimensional wood grain and the board, it is necessary to increase the curing power used during curing. However, the provision of high power will generate more waste heat during the curing process. This waste heat will cause deformation of the board and yellowing or aging of the resin liquid. Therefore, this method of increasing the curing power is not practical.
[0110] After studying the three-dimensional wood grain after solidification, the applicant found that the three-dimensional wood grain actually contains two functional areas in the longitudinal direction, including: (1) a bonding area for bonding with the board, namely the wood grain bottom layer in this application; (2) a functional area for forming a three-dimensional structure, namely the three-dimensional wood grain layer in this application. The wood grain bottom layer does not require much resin, while the applicant has calculated that the amount of resin required for the three-dimensional wood grain layer is 150g / m 2 Only when the above is achieved can the feel of natural wood and better wear resistance be achieved.
[0111] Therefore, the present invention applies a first layer of resin liquid on the surface of the board, which is then cured to form a wood grain base layer. Since the amount of resin liquid used to form the wood grain base layer is small, it can be completely cured under normal curing power, effectively improving the bonding strength between the wood grain base layer and the board, and preventing peeling during use. Subsequently, the resin coating amount on the surface of the wood grain base layer is increased to 150g / m 2 The above ensures the three-dimensional sense of the three-dimensional wood grain.
[0112] In another preferred embodiment of the present invention, in step (S.4), at least a portion of the surface of the wood grain base layer is covered with at least two layers of resin liquid.
[0113] In another preferred embodiment of the present invention, in the process of covering at least a portion of the surface of the wood grain base layer with any two adjacent layers of resin liquid, it also includes a transition treatment step of stopping the application of force to the resin liquid after the wood grain base layer is covered by the previous layer of resin liquid, and covering with the next layer of resin liquid after the transition treatment step is completed.
[0114] As mentioned above, in order to ensure the three-dimensional effect of the wood grain in this application, at least 150g / m2 of coating is required on the surface of the wood grain bottom layer. 2 Therefore, the focus of this application is shifted to how to form a resin coating amount of 150g / m on the surface of the wood grain bottom layer. 2 The above three-dimensional wood grain layer.
[0115] The most common way to apply the resin liquid is to use a roller coater. The applicant has tried to apply up to 150g / m2 of resin liquid at one time on the wood grain bottom layer. 2 However, the applicant found that this one-time coating method requires too much resin liquid to be loaded on a single roller. If a conventional roller is used, the resin liquid will flow down if it is too thick, making it impossible to complete normal production.
[0116] Therefore, in order to solve the above problems, the present invention adopts a two-roller distributed coating method, so that each roller coats a layer of resin liquid, so that the total amount of resin in the two layers of resin liquid is greater than 150g / m 2 This approach not only achieves the coating of a large amount of resin, but also reduces the resin load pressure of each roller.
[0117] To achieve multi-pass coating, conventional roller coaters typically employ two rollers in parallel. These rollers typically employ a combination of one forward-moving roller and one counter-moving roller. As the first roller applies the resin liquid to the sheet surface and pushes the substrate forward, it exerts a force on the sheet and the uncured resin layer adhering to it in the direction of transport. This force, combined with the bristle structure on the roller surface, causes deformation of the resin surface. Before the first layer of resin has evened out, the second roller, already receiving the sheet coated with uncured resin liquid, exerts a force in the opposite direction of transport on the uncured resin liquid. This force also causes deformation of the second layer of resin liquid in the opposite direction. Furthermore, due to the speed difference between the second roller and the first, the deformations of the first and second layers cannot be offset. Instead, the deformations of the two layers are superimposed, further exacerbating the appearance of marks on the resin liquid. These marks become permanent after curing, severely impacting the visual quality of the final product. The production of this mark will cause obvious defects in the appearance of the finished product, especially the finished product with shallow texture. That is, when viewed from a distance, a blockage can be found in the middle of the part coated with resin liquid.
[0118] Therefore, based on the existing roller coating machine, the present application adds a transition treatment step of stopping the application of force to the resin liquid during the process of covering at least a portion of the surface of the wood grain bottom layer with any two adjacent layers of resin liquid. In this way, when the board passes through the first roller, after the first roller finishes applying force to the board as a whole, before being conveyed to the second roller, since no force is applied to the entire board, and then after a longer distance, it is conducive to the leveling of the first layer of resin liquid. At this time, the board is coated from beginning to end by the second roller again. At this time, since the deformation of the second layer of resin liquid is smaller, it can be quickly leveled before curing, thereby eliminating the influence of the force and speed difference between the two rollers on the resin liquid on the surface morphology.
[0119] In another preferred embodiment of the present invention, during the process of covering at least a portion of the surface of the wood grain bottom layer with any two adjacent layers of resin liquid, the directions of the forces applied to the any two adjacent layers of resin liquid are opposite.
[0120] As discussed above, a roller coater exerts a certain force on the resin liquid during coating. Since the resin liquid typically contains a high molecular weight polymer or prepolymer with relatively long molecular chains, it will experience a certain amount of elastic deformation and orientation force under the action of external forces. Since the overall process time from coating to curing of the resin liquid is relatively short, the molecular chains of the high molecular weight polymer in the resin liquid often solidify before returning to their initial state, resulting in a large internal stress in the middle of the cured three-dimensional wood grain layer, which in turn makes it prone to cracking in the middle of the cured three-dimensional wood grain layer. Therefore, in order to reduce the generation of internal stress in the middle of the three-dimensional wood grain layer, the present invention specifically adjusts the force applied by the two rollers to any two adjacent layers of resin liquid in opposite directions during the process of coating at least a portion of the surface of the wood grain base layer with any two adjacent layers of resin liquid. This allows the second roller to apply a force opposite to the internal stress of the uncured second wear-resistant layer during operation, thereby reducing or offsetting the internal stress originally present in the three-dimensional wood grain layer, thereby reducing the probability of cracking in the middle of the cured three-dimensional wood grain layer.
[0121] In another preferred embodiment of the present invention, the plate material sequentially completes steps (S.1) to (S.6) during the process of being transported along a fixed direction.
[0122] In another preferred embodiment of the present invention, in the step (S.5), the embossing liquid is applied to the surface of the resin liquid and / or penetrates downward into the interior of the resin liquid.
[0123] In the present application, there are various principles for forming the embossing layer by adding embossing liquid on the surface of the resin liquid, including but not limited to ultraviolet covering method, free radical absorption method or volume occupation method.
[0124] Among them, the UV covering method is suitable for UV-curable resin liquid. Its principle is to cover the surface of the uncured resin liquid with a layer of embossing liquid that can prevent ultraviolet light from penetrating, so that the resin liquid below the embossing liquid can remain in a liquid and uncured state. This part of the uncured resin liquid forms an embossing layer, which can be removed by mechanical cleaning or solution washing in the subsequent processing process to obtain a three-dimensional wood grain layer with a simulated wood grain structure.
[0125] The free radical absorption law is applicable to resin liquid based on the free radical polymerization principle. The principle is that the free radicals used to polymerize the resin liquid and undergo free radical polymerization and solidification can be absorbed by the free radical absorption law. As a result, the resin liquid in the part containing the embossing liquid can remain in a liquid and unsolidified state. This part of the unsolidified resin liquid forms an embossing layer, which can be removed by mechanical cleaning or solution washing in the subsequent processing process to obtain a three-dimensional wood grain layer with a wood grain structure.
[0126] The volume occupation rule means that when the embossing liquid penetrates downward into the uncured resin liquid, it squeezes out the uncured resin liquid, so that the occupied volume only contains the embossing liquid. The embossing liquid can be polymerizable or non-polymerizable. Finally, the embossing liquid is cleaned and removed through the principle of mechanical or solvent cleaning to obtain a three-dimensional wood grain layer with a simulated wood grain structure.
[0127] In another preferred embodiment of the present invention, the curing method of the covering resin liquid in steps (S.2) and (S.4) includes any one of light curing, thermal curing or electron beam curing.
[0128] In another preferred embodiment of the present invention, the resin solution at least includes a photo-crosslinking resin and a photoinitiator.
[0129] In another preferred embodiment of the present invention, the photo-crosslinking resin includes any one or more combinations of unsaturated polyester, epoxy resin, acrylic resin, acrylic modified polyurethane resin, acrylic modified silicone resin, acrylic modified epoxy resin, water-based epoxy acrylate, water-based polyurethane acrylate, and water-based polyester acrylate.
[0130] In another preferred embodiment of the present invention, the photoinitiator includes any one of a free radical polymerization initiator, a cationic polymerization initiator, an energy transfer initiator, and an ion reaction initiator.
[0131] In another preferred embodiment of the present invention, the embossing liquid in step (S.5) at least contains a polymerization inhibitor for preventing polymerization of the resin liquid.
[0132] In this preferred embodiment, an inhibitor is added to the embossing liquid, which can quench the free radicals generated by the decomposition of the photoinitiator under light, thereby effectively preventing the polymerization of the resin liquid containing the inhibitor or reducing the curing speed of the resin liquid containing the inhibitor, so that after the end of step (S.6), the resin liquid containing the inhibitor can still remain in a liquid or semi-solid state, making the embossing layer easier to remove.
[0133] In another preferred embodiment of the present invention, the resin liquid at least includes a thermosetting resin.
[0134] In another preferred embodiment of the present invention, the thermosetting resin includes one or more combinations of epoxy resin, phenolic resin, melamine formaldehyde resin, furan resin, unsaturated polyester resin, silicone resin, and polybutadiene resin.
[0135] In another preferred embodiment of the present invention, the resin solution further includes a curing agent.
[0136] In another preferred embodiment of the present invention, the step (S.4) further comprises a step for providing kinetic energy for the embossing liquid to penetrate downward into the resin liquid.
[0137] After being applied to the surface of uncured resin, the embossing liquid may not quickly penetrate into the interior of the uncured resin, resulting in insufficient depth of the three-dimensional wood grain in some embodiments. Therefore, to enhance the three-dimensional wood grain, the applicant proposed solving this technical problem by increasing the penetration rate of the embossing liquid. The applicant discovered that applying kinetic energy to the embossing liquid allows it to penetrate the interior of the uncured resin at a faster speed, thereby increasing the depth of the three-dimensional wood grain.
[0138] In another preferred embodiment of the present invention, the embossing liquid contains a curable resin.
[0139] The curable resin contained in the embossing liquid includes acrylic resin, epoxy resin or other curable resins.
[0140] In another preferred embodiment of the present invention, the surface energy of the curable resin contained in the embossing liquid after curing is lower than the surface energy of the three-dimensional wood grain layer.
[0141] In some preferred embodiments of the present application, the embossing liquid contains a resin having a surface energy lower than that of the three-dimensional wood grain layer, so that the embossing liquid has a weaker adhesion to the three-dimensional wood grain layer after curing, thereby allowing the embossing liquid to be easily removed through mechanical or solvent cleaning steps after curing.
[0142] In another preferred embodiment of the present invention, the curable resin contained in the embossing liquid has a surface energy lower than 100 mN / m after curing.
[0143] In another preferred embodiment of the present invention, the curable resin contained in the embossing liquid includes any one of fluorocarbon resin, fluorosilicone resin or organosilicon resin.
[0144] In another preferred embodiment of the present invention, the density of the embossing liquid is greater than the density of the resin liquid.
[0145] In addition to actively providing kinetic energy to the embossing liquid as described above, the applicant also proposes that in some preferred embodiments of the present application, the kinetic energy of the embossing liquid can be passively increased to further increase the speed at which the embossing liquid penetrates into the uncured resin liquid. For example, the density of the embossing liquid can be adjusted so that the density of the embossing liquid is greater than that of the resin liquid. This allows the embossing liquid to have a higher mass after applying the same volume of embossing liquid to at least a portion of the surface of the uncured resin liquid, thereby exerting greater kinetic energy upon entering the uncured resin liquid, thereby resulting in a deeper three-dimensional wood grain layer. Furthermore, after the high-density embossing liquid enters the resin liquid, it is more likely to quickly penetrate downward into the uncured resin liquid due to its own gravity.
[0146] In another preferred embodiment of the present invention, the embossing liquid further comprises a density regulator for adjusting the density of the embossing liquid.
[0147] In another preferred embodiment of the present invention, the density regulator is an inorganic solid powder additive.
[0148] In another preferred embodiment of the present invention, the density regulator may be an inorganic solid additive, such as calcium carbonate, silicon dioxide, and the like.
[0149] In another preferred embodiment of the present invention, the embossing liquid comprises at least two embossing liquids with different surface tensions.
[0150] As mentioned in the background, in order to achieve a three-dimensional structure with a feel similar to that of actual wood, in addition to the depth mentioned above, another key factor is how to control the width of the three-dimensional structure. Currently, the width of the three-dimensional structure is primarily controlled by the amount of embossing fluid sprayed. Generally, the larger the amount of embossing fluid sprayed or the individual droplets of embossing fluid, the wider the wood grain gaps, while the smaller the amount of embossing fluid sprayed or the droplets of embossing fluid, the smaller the width of the resulting wood grain gaps.
[0151] However, the above solution has the following two problems:
[0152] (1) In order to form a wider three-dimensional wood grain, more embossing liquid needs to be added. Since the embossing liquid needs to be removed in the final step, adding more embossing liquid will result in more waste of embossing liquid.
[0153] (2) In order to form a three-dimensional wood grain with a smaller width, a smaller amount of embossing liquid needs to be added. However, doing so will result in the depth of the three-dimensional wood grain being too small. At the same time, the accuracy of the three-dimensional wood grain may be insufficient, resulting in unnatural defects in the three-dimensional wood grain.
[0154] In response to the above problem, this application proposes a solution, that is, the embossing liquid used to form the three-dimensional wood grain with a larger width and the embossing liquid used to form the three-dimensional wood grain with a smaller width are made of materials with different tensions.
[0155] When using embossing liquid with smaller tension, it is easier to spread on the surface of the wear-resistant layer. In this case, the contact angle between the embossing liquid with small tension and the wear-resistant layer is smaller because it can spread over a larger area under the same volume, which is equivalent to using less embossing liquid to achieve a wider three-dimensional wood grain.
[0156] When using embossing liquid with greater tension, it is not easy to spread on the surface of the wear-resistant layer. In this case, the contact angle between the embossing liquid with greater tension and the wear-resistant layer is greater. Therefore, under the condition of the same volume, the height of the droplets is higher. Therefore, when using a smaller amount of embossing liquid with greater tension, it can obtain finer and deeper three-dimensional wood grain.
[0157] In another preferred embodiment of the present invention, the coverage of the ink on the surface of the plate in step (S.1) is 6-8 g / m 2 .
[0158] In another preferred embodiment of the present invention, the amount of the resin liquid covering the surface of the wood grain bottom layer in step (S.2) is 30-50 g / m 2 .
[0159] In a second aspect, in another preferred embodiment of the present invention, the present invention further provides a board having three-dimensional wood grain, comprising a board;
[0160] The surface of the board comprises a wood grain base layer and a three-dimensional wood grain layer prepared by the method described above.
[0161] In another preferred embodiment of the present invention, the following are further provided in sequence between the board and the wood grain bottom layer:
[0162] A primer layer used to improve the bonding properties of the board surface;
[0163] A color paint layer provided on the surface of the primer layer to cover the color of the substrate;
[0164] An ink layer located on the surface of the paint layer to form a wood grain pattern.
[0165] In another preferred embodiment of the present invention, the outer surface of the three-dimensional wood grain layer is further covered with a topcoat layer, and at least a portion of the topcoat layer is lower than the upper surface of the three-dimensional wood grain layer.
[0166] In a third aspect, in another preferred embodiment of the present invention, the present invention further provides a method for preparing the board having three-dimensional wood grain.
[0167] The method at least comprises the steps of preparing a wood grain base layer and a three-dimensional wood grain layer according to the method described above.
[0168] In another preferred embodiment of the present invention, the following steps are also included:
[0169] A step of covering at least a portion of the surface of the plate with a primer and curing the primer layer;
[0170] The step of covering at least a portion of the surface of the primer layer with a color paint and curing the primer layer to obtain a color paint layer;
[0171] The step of covering at least a portion of the surface of the color paint layer with ink having a wood grain pattern and curing the ink layer;
[0172] The step of making at least a portion of the surface of the ink layer cover the wood grain base layer and the three-dimensional wood grain layer prepared according to the method described above;
[0173] The step of covering at least a portion of the surface of the three-dimensional wood grain layer with a topcoat and curing the topcoat layer.
[0174] In another preferred embodiment of the present invention,
[0175] The coverage of the primer is 10-15 g / m 2 ;
[0176] The coverage of the paint is 15-20 g / m 2 ;
[0177] The coverage of the topcoat is 20-30 g / m 2 .
[0178] In another preferred embodiment of the present invention, the color paint layer is white.
[0179] In another preferred embodiment of the present invention, the paint contains at least a photo-crosslinking resin, a photoinitiator and white pigment powder.
[0180] In a fourth aspect, the present invention further provides the use of the board with three-dimensional wood grain in floors, decorative wall panels or ceiling panels.
[0181] The following examples are provided only to illustrate the present invention and are not intended to limit the scope of protection defined by the appended claims.
[0182] Example 1
[0183] The method for forming three-dimensional wood grain on the surface of a board comprises the following steps:
[0184] (S.1) Place an SPC sheet with a length, width and thickness of 1260mm*970mm*4.85mm on the surface of a conveyor moving in a fixed direction;
[0185] (S.2) During the transportation process, the SPC sheet first passes through the first roller coater. The coating roller of the roller coater is adhered with a light-curable primer (the primer contains: 90% light-curing varnish HYS01-1, 5% photoinitiator 184, 0.5% photoinitiator TPO, 4.5% diluent hydroxyethyl acrylate). When the SPC sheet contacts the coating roller, 12g / m 2 The primer is applied to the surface of the SPC board with a 395nm and 8W / cm 2 The primer is cured by a UV lamp to form a primer layer;
[0186] (S.3) The SPC sheet obtained in the previous step is passed through a second roller coater. The coating roller of the roller coater is coated with a light-curable white paint (the white paint contains: 50% light-curing epoxy HYS01-1, 30% titanium dioxide, 5% photoinitiator 184, 0.5% photoinitiator TPO, 14.5% diluent hydroxyethyl acrylate). When the SPC sheet is in contact with the coating roller, 18g / m 2 The white paint is applied on the surface of the primer, and the 2 After curing with UV lamp, a white paint layer is obtained;
[0187] (S.4) The SPC sheet obtained in the previous step is conveyed to the first inkjet printer, so that the surface of the color paint layer is sprayed with 6-8 g / m 2 The ink is cured to form an ink layer having a wood grain pattern on the surface of the primer layer;
[0188] (S.5) The SPC sheet obtained in the previous step is conveyed to the third roller coater and a 45g / m2 roller is applied on the surface of the ink layer. 2 The photocurable resin liquid (resin liquid contains: 90% Dow Corning 65 Additive, 5% photoinitiator 184, 0.5% photoinitiator TPO, 4.5% diluent hydroxyethyl acrylate) was sequentially subjected to 395nm and 8W / cm 2 UV lamp and 160w / cm 2 After being irradiated and cured by Hg lamp, a wood grain bottom layer is formed;
[0189] (S.6) The SPC sheet obtained in the previous step is conveyed to the fourth roller coater, so that the coating roller of the fourth roller coater is rolled along the conveying direction of the SPC sheet (the roller rotates clockwise) to coat 80g / m 2 Resin solution (resin solution contains: 90% Dow Corning 65 Additive, 5% photoinitiator 184, 0.5% photoinitiator TPO, 4.5% diluent hydroxyethyl acrylate);
[0190] (S.7) After applying the first layer of resin liquid, the SPC sheet is conveyed forward along the surface of the conveying equipment, and it is ensured that the fourth roller coater does not apply any force to the resin liquid before conveying it to the next roller coater;
[0191] (S.8) The SPC sheet obtained in the previous step is conveyed to the fifth roller coater, and the coating roller of the fifth roller coater is rotated in the opposite direction of the SPC sheet conveying (the roller itself rotates in a clockwise direction) to continue to roll coat 75g / m 2 Resin liquid;
[0192] FIG2 shows a schematic diagram of steps (S.6) to (S.8) in this embodiment, so as to better understand these three steps;
[0193] (S.9) The SPC sheet obtained in the previous step is transported to the second inkjet printer so that 6-8 g / m2 of the resin liquid is sprayed on the surface. 2 The embossing liquid (the embossing liquid comprises: 45.5% diacrylate monomer PEG600DA, 20.5% p-hydroxyanisole HQMME, 10% 2-tert-butylhydroquinone MTBHQ, 24% diethylene glycol butyl ether), and the embossing liquid is allowed to penetrate downward into the resin liquid and mix with the resin liquid to form an embossing layer;
[0194] (S.10) The surface of the SPC sheet obtained in the previous step, except for the embossed layer, was subjected to 395nm and 8W / cm 2 UV lamp and 160w / cm 2 Hg lamp irradiation for deep curing;
[0195] (S.11) conveying the SPC sheet obtained in the previous step to a cleaning device including a steel brush, so that the embossed layer is brushed out by the steel brush, thereby forming a three-dimensional wood grain layer;
[0196] (S.12) The SPC sheet obtained in the previous step was passed through the sixth roller coater and 395nm and 8W / cm 2 UV lamp, thereby coating the surface of the three-dimensional wood grain layer with 12g / m 2 a first topcoat, and curing the topcoat to obtain a first topcoat layer;
[0197] (S.13) The SPC sheet obtained in the previous step was passed through the seventh roller coater and 395nm and 8W / cm 2 UV lamp, thereby coating 12g / m on the surface of the first topcoat layer 2 The second topcoat is applied and cured to obtain a second topcoat layer.
[0198] The plate with a three-dimensional surface structure prepared in Example 1 was analyzed by a laser profilometer to obtain Figures 3 and 4, where Figure 3 is a schematic diagram of the three-dimensional structure of the three-dimensional wood grain, and Figure 4 is a schematic diagram of the top view of the three-dimensional wood grain.
[0199] Comparative Example 1
[0200] Comparative Example 1 follows essentially the same procedures as Example 1, except that step (S.5) is omitted. Consequently, the resulting three-dimensional structure lacks a wood grain base layer. Figures 5 and 6 are schematic diagrams of the three-dimensional wood grain structure and a top-down view of the three-dimensional wood grain structure, respectively, produced in Comparative Example 1. As can be seen from the figures, omitting step (S.5) results in a lower average depth of the resulting wood grain.
[0201] Comparative Example 2
[0202] The steps of Comparative Example 2 are substantially the same as those of Example 1, except that, in step (S.5), the resin liquid is not completely solidified until it is gelled.
[0203] Comparative Example 3
[0204] Comparative Example 3 follows essentially the same procedures as Example 1, except that after step (S.8), the resin liquid is exposed to UV light, resulting in an incompletely cured, gel-like resin layer. Figure 7 is a schematic diagram of the three-dimensional wood grain structure produced in Comparative Example 3 of the present invention. As can be seen from the figure, the three-dimensional wood grain produced in Example 3 has a lower depth and less defined edges.
[0205] Product testing:
[0206] Surface wear resistance test: Tested in accordance with standard GT / T 18102-2020.
[0207] Surface scratch resistance index test: tested in accordance with standard GT / T 18102-2020.
[0208] Clarity test: Tested in accordance with standard JIS K7374.
[0209] Product Qualification Rate Test: 50 panels were produced in batches according to the methods of Example 1, Comparative Example 1, and Comparative Example 2. The panels were observed for cracking and delamination, and their initial warpage and heating warpage were measured. The product qualification rate was calculated, and the results are shown in Table 1. Panels with visually observable quality issues and panels with heating warpage greater than 1 mm / m were deemed unqualified.
[0210] Alignment accuracy test: The alignment accuracy can be observed with the naked eye to check for offset, ghosting, or damage.
[0211] Warpage test: Cut the sheet into 240mm*240mm specimens, place them on the aluminum plate with the wear-resistant layer facing up, and place them at 23±2℃ and 50±5%RH for 24 hours. Measure the average initial warpage of the sheet with a caliper. Adjust the temperature in the constant temperature drying oven to 80℃, place the specimen together with the aluminum plate in the constant temperature drying oven for 6 hours, then take out the specimen together with the aluminum plate, and place them at 23±2℃ and 50±5%RH for 24 hours. Measure the average heating warpage of the sheet with a caliper.
[0212] The test results of the plate properties of Example 1 and Comparative Examples 1 to 3 are shown in Table 1 below:
[0213]
[0214] Example 2
[0215] The steps in Example 2 are essentially the same as those in Example 1, differing in the coating method of the resin liquid in steps (S.6) through (S.8). As shown in Figure 8, in this example, steps (S.6) and (S.8) utilize a spraying method to sequentially apply the resin liquid to the surface of the wood grain base layer. During the spraying process, the nozzle forms a certain angle with the SPC board.
[0216] Among them: in step (S.6), the nozzle forms a certain angle with the direction of SPC sheet conveying (in this embodiment, the nozzle and the direction of SPC sheet conveying form an acute angle of 30°). And in step (S.8), the nozzle forms a certain angle along the direction of SPC sheet conveying (in this embodiment, the nozzle and the direction of SPC sheet conveying form an obtuse angle of 150°).
[0217] Example 3
[0218] The steps of Example 3 are basically the same as those of Example 1, except that the composition of the resin liquid and the curing method are changed in steps (S.5) to (S.8).
[0219] The composition of the resin liquid can choose to use a thermosetting resin system, as follows:
[0220] Resin (bisphenol A epoxy resin E-51) 100 parts;
[0221] Curing agent (methyltetrahydrophthalic anhydride) 30 parts;
[0222] Active diluent (butyl glycidyl ether BGE) 15 parts;
[0223] Accelerator (DMP30) 10 parts.
[0224] After the thermosetting resin system obtained by mixing the above formula is applied to the surface of the SPC board, the ambient temperature of the SPC board is raised to 140° C. by infrared heating, so that the thermosetting resin system can be cured.
[0225] The test results of the plate performance of Example 3 are shown in Table 2 below:
[0226]
[0227] Example 4
[0228] The steps of Example 4 are basically the same as those of Example 1, except that the composition of the embossing liquid in step (S.9) is changed.
[0229] In this embodiment, the embossing liquid is a polytetrafluoroethylene emulsion with a solid content of 60%. After the polytetrafluoroethylene emulsion is coated on the resin liquid, it penetrates downward into the interior of the resin liquid. Since the polytetrafluoroethylene emulsion is water-based, it will not be miscible with the resin liquid after penetrating into the resin liquid. Therefore, after the resin liquid is solidified, a portion of the water in the polytetrafluoroethylene emulsion evaporates due to heat, thereby forming a polytetrafluoroethylene layer. Since the surface energy of the polytetrafluoroethylene layer is lower than 100mN / m, it will not adhere to the solidified resin liquid, and can be removed more easily.
[0230] Example 5
[0231] The steps of Example 5 are basically the same as those of Example 4, except that when the embossing liquid (polytetrafluoroethylene emulsion with a solid content of 60%) is added to the resin liquid, the injection speed of the embossing liquid into the resin liquid is increased to 5 m / s.
[0232] The specific impacts are shown in Table 3 below:
[0233]
[0234] As can be seen from Table 1 above, after increasing the embossing liquid injection speed, the depth of the three-dimensional structure of the final plate surface is significantly improved, with the maximum depth increasing by 17.4%.
[0235] Example 6
[0236] The steps of Example 6 are basically the same as those of Example 4, except that nano-silicon dioxide is added to the embossing liquid (polytetrafluoroethylene emulsion with a solid content of 60%) to increase the density of the embossing liquid from 1.5 g / cm 3 Increased to 2.0 g / cm 3 .
[0237] The specific impacts are shown in Table 4 below:
[0238]
[0239] As can be seen from Table 3 above, after increasing the density of the embossing liquid, the depth of the three-dimensional structure of the surface of the final plate is significantly improved, with the maximum depth increasing by 27.5%.
[0240] Comparative Example 4
[0241] The steps of Comparative Example 4 are basically the same as those of Example 1, except that steps (6) to (8) are combined and coated using a conventional double-roller coater.
[0242] The schematic diagram of its structure during the roller coating process is shown in FIG8 . When the SPC sheet covered with the wood grain bottom layer is conveyed along the conveying mechanism to the bottom of the double-roller roller coater, the sheet first coats a layer of resin liquid on the surface of the wood grain bottom layer to form resin liquid 1 when passing through the first roller of the double-roller roller coater. Then, when the surface of the wood grain bottom layer is not completely covered by the resin liquid 1, the SPC sheet passes through the second roller of the double-roller roller coater again, thereby continuing to coat a layer of resin liquid on the surface of the resin liquid 1 to form resin liquid 2, until the resin liquids 1 and 2 completely cover the surface of the wood grain bottom layer.
[0243] FIG2 is an image of a plate having a three-dimensional structure on its surface prepared by the method in Comparative Example 4. It can be seen from the figure that the plate prepared by the method in Comparative Example 4 has obvious marks on its surface.
[0244] The performance test results of the board material of Comparative Example 4 are shown in Table 5 below:
[0245] .
Claims
1. A method for forming three-dimensional wood grain on a board surface, characterized in that: At least the following steps are included: (S.1) a step of covering at least a portion of the surface of the board with ink, thereby forming an ink layer having a wood grain pattern; (S.2) a step of covering at least a portion of the surface of the ink layer with a resin liquid; (S.3) a step of solidifying at least a portion of the resin liquid on the surface of the ink layer to form a wood grain bottom layer; (S.4) a step of covering at least a portion of the surface of the wood grain bottom layer with at least one layer of resin liquid; (S.5) a step of applying embossing liquid to at least a portion of the surface of the resin liquid on the wood grain bottom layer along the wood grain pattern of the ink layer, so that the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid forms an embossing layer; (S.6) a step of solidifying the resin liquid except for the embossed layer formed in the previous step; (S.7) A step of removing the embossed layer to form a three-dimensional wood grain layer on the surface of the wood grain base layer.
2. The method according to claim 1, characterized in that The amount of the resin liquid covering the surface of the wood grain bottom layer in the step (S.4) is greater than or equal to 150 g / m 2 .
3. The method according to claim 2, characterized in that In the step (S.4), at least a portion of the surface of the wood grain bottom layer is covered with at least two layers of resin liquid.
4. The method according to claim 3, characterized in that In the process of covering at least a portion of the surface of the wood grain bottom layer with any two adjacent layers of resin liquid, it also includes a transition treatment step of stopping the application of force to the resin liquid after the wood grain bottom layer is covered by any layer of resin liquid, and covering with the next layer of resin liquid after the transition treatment step is completed.
5. The method according to claim 3 or 4, characterized in that In the process of covering at least a part of the surface of the wood grain bottom layer with any two adjacent layers of resin liquid, the directions of the forces applied to the any two adjacent layers of resin liquid are opposite.
6. The method according to claim 1, characterized in that The plate completes steps (S.1) to (S.6) in sequence while being transported along a fixed direction.
7. The method according to claim 1, characterized in that In the step (S.5), the embossing liquid is applied to the surface of the resin liquid and / or penetrates downward into the interior of the resin liquid.
8. The method according to claim 1 or 7, characterized in that The curing method of the covering resin liquid in the steps (S.2) and (S.4) includes any one of light curing, heat curing or electron beam curing.
9. The method according to claim 8, characterized in that The resin solution at least includes a photo-crosslinking resin and a photoinitiator.
10. The method according to claim 9, characterized in that The embossing liquid in the step (S.4) contains at least a polymerization inhibitor for preventing the polymerization of the photo-crosslinking resin.
11. The method according to claim 9, characterized in that The photo-crosslinking resin includes any one or more combinations of unsaturated polyester, epoxy resin, acrylic resin, acrylic modified polyurethane resin, acrylic modified silicone resin, acrylic modified epoxy resin, water-based epoxy acrylate, water-based polyurethane acrylate, and water-based polyester acrylate.
12. The method according to claim 9, characterized in that The photoinitiator includes any one of a free radical polymerization initiator, a cationic polymerization initiator, an energy transfer initiator, and an ion reaction initiator.
13. The method according to claim 8, characterized in that The resin liquid at least includes a thermosetting resin.
14. The method according to claim 13, characterized in that The thermosetting resin includes one or more of epoxy resin, phenolic resin, melamine formaldehyde resin, furan resin, unsaturated polyester resin, silicone resin, and polybutadiene resin.
15. The method according to claim 13, characterized in that The resin solution also includes a curing agent for catalyzing the curing of the thermosetting resin.
16. The method according to claim 7, characterized in that The step (S.4) further includes a step for providing kinetic energy for the embossing liquid to penetrate downward into the resin liquid.
17. The method according to claim 16, characterized in that The embossing liquid contains a curable resin.
18. The method according to claim 17, characterized in that The curable resin contained in the embossing liquid has a surface energy lower than the surface energy of the three-dimensional wood grain layer after curing.
19. The method according to claim 18, characterized in that The curable resin contained in the embossing liquid has a surface energy lower than 100 mN / m after curing.
20. The method according to any one of claims 17 to 19, characterized in that: The curable resin contained in the embossing liquid includes any one of fluorocarbon resin, fluorosilicone resin or organic silicone resin.
21. The method according to any one of claims 1 or 7 or 16 to 19, characterized in that: The density of the embossing liquid is greater than the density of the resin liquid.
22. The method according to claim 21, characterized in that The embossing liquid also includes a density regulator for adjusting the density of the embossing liquid.
23. The method according to claim 22, characterized in that The density regulator is an inorganic solid powder additive.
24. The method according to any one of claims 1 or 7 or 16 to 19, characterized in that: The embossing liquid comprises at least two embossing liquids with different surface tensions.
25. The method according to claim 1, characterized in that The coverage of the ink on the surface of the plate in step (S.1) is 6-8 g / m 2 .
26. The method according to claim 1, characterized in that The amount of the resin solution in step (S.2) is 30-50 g / m 2 .
27. A board with three-dimensional wood grain, characterized in that: Including plates; The surface of the board comprises a wood grain base layer and a three-dimensional wood grain layer prepared by the method according to any one of claims 1 to 26.
28. The board with three-dimensional wood grain according to claim 27, characterized in that: The following are arranged in sequence between the board and the wood grain bottom layer: A primer layer used to improve the bonding performance of the board surface; A color paint layer provided on the surface of the primer layer to cover the color of the substrate; An ink layer located on the surface of the paint layer to form a wood grain pattern.
29. The board with three-dimensional wood grain according to claim 27 or 28, characterized in that: The outer surface of the three-dimensional wood grain layer is also covered with a topcoat layer, and at least a portion of the topcoat layer is lower than the upper surface of the three-dimensional wood grain layer.
30. A method for preparing a board having three-dimensional wood grain as claimed in any one of claims 27 to 29, characterized in that: The method at least comprises the steps of preparing a wood grain base layer and a three-dimensional wood grain layer according to the method as claimed in any one of claims 1 to 26.
31. The method for preparing a board having three-dimensional wood grain according to claim 30, characterized in that: The following steps are involved: A step of covering at least a portion of the surface of the plate with a primer and curing the primer layer; The step of covering at least a portion of the surface of the primer layer with a color paint and curing the primer layer to obtain a color paint layer; The step of making at least a portion of the surface of the color paint layer covered with an ink layer, a wood grain base layer and a three-dimensional wood grain layer prepared by the method according to any one of claims 1 to 26; The step of covering at least a portion of the surface of the three-dimensional wood grain layer with a topcoat and curing the topcoat layer.
32. The method for preparing a board having three-dimensional wood grain according to claim 31, characterized in that: The coverage of the primer is 10-15 g / m 2 ; The coverage of the paint is 15-20 g / m 2 ; The coverage of the topcoat is 20-30 g / m 2 .
33. The method for preparing a board having three-dimensional wood grain according to claim 31 or 32, characterized in that: The color paint layer is white.
34. The method for preparing a board having three-dimensional wood grain according to claim 33, characterized in that: The color paint at least contains a photo-crosslinking resin, a photoinitiator and white pigment powder.