Chlorosulfonated polyolefin latex

MYPI2025005983A0Undetermined Publication Date: 2024-09-30SUMITOMO SEIKA CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025005983
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-25
Publication Date
2024-09-30

AI Technical Summary

Technical Problem

Conventional chlorosulfonated polyolefin latexes do not coagulate with common coagulants, making it difficult to form films suitable for applications like gloves.

Method used

A chlorosulfonated polyolefin latex is formulated with an aqueous dispersion medium, chlorosulfonated polyolefin, and specific emulsifiers such as alkylbenzene sulfonate, polyoxyalkylene disulfonate, and taurine salt, which enables coagulation and stability, allowing for the production of dip-molded articles without organic solvents.

Benefits of technology

The formulation allows for efficient production of stable chlorosulfonated polyolefin latex that can be coagulated using common coagulants, enabling the creation of dip-molded articles like gloves while avoiding the use of organic solvents, thus addressing environmental concerns.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a method that allows even a chlorosulfonated polyolefin latex to be coagulated using a common coagulant. Specifically, provided is a chlorosulfonated polyolefin latex comprising: an aqueous dispersion medium; a chlorosulfonated polyolefin; at least one compound (first agent) selected from the group consisting of an alkylbenzene sulfonic acid salt, a polyoxyalkylene disulfonic acid salt, and a taurine salt; and a fatty acid salt (second agent).
Need to check novelty before this filing date? Find Prior Art

Description

Chlorosulfonated polyolefin latex

[0001] The present disclosure relates to a chlorosulfonated polyolefin latex and its uses, etc. More specifically, the present disclosure relates to a coagulable chlorosulfonated polyolefin latex, a dip-molding composition using the latex, and a dip-molded article.

[0002] Chlorosulfonated polyolefins have excellent heat resistance, weather resistance, ozone resistance, chemical resistance, abrasion resistance, and the like, and are used in the form of latex as coating materials and adhesive materials. Patent Document 1 discloses that in a transmission belt made of a composite of an ethylene-propylene-diene rubber matrix and polyester fibers, a resorcinol-formalin-latex adhesive (RFL adhesive) using chlorosulfonated polyethylene latex as a latex component is used to bond the matrix rubber and the fibers. Furthermore, because chlorosulfonated polyolefins have excellent resistance to strong acids and strong alkalis, they are also used as a material for protective gloves for work involving the heavy use of highly hazardous chemicals, such as plating processes, semiconductor manufacturing processes, and dyeing processes. Gloves made of chlorosulfonated polyolefins are generally manufactured by immersing a hand mold corresponding to the three-dimensional shape of the glove in an organic solvent solution of rubber, followed by drying and vulcanization (see, for example, Patent Document 2). However, from the viewpoint of environmental protection, organic solvent solutions are not preferable, and therefore, a method for producing gloves using chlorosulfonated polyolefin latex, which does not require the use of organic solvents, is desired.

[0003] Generally, the coagulation dipping method is widely used as a method for manufacturing rubber gloves from latex. For example, Patent Document 3 discloses a method for manufacturing gloves by preparing a mold corresponding to the three-dimensional shape of the glove, treating the surface of the mold with a coagulant such as a calcium nitrate aqueous solution, and then immersing the treated mold in a dip solution containing nitrile rubber latex to adhere rubber particles to the surface of the mold, followed by drying and crosslinking. Also, Patent Document 4 discloses a method for manufacturing gloves by heat-sensitizing chlorosulfonated polyethylene latex and using a heat-sensitive coagulation method.

[0004] JP 2001-003991 A JP 05-230702 A International Publication No. 2015 / 146974 JP 2011-032590 A

[0005] As described in Patent Document 4 (particularly, paragraphs 0008 to 0009, etc.), conventional chlorosulfonated polyolefin latex does not coagulate even when a general coagulant (e.g., calcium salt) is applied, and therefore it has been difficult to form a film useful for gloves.

[0006] Therefore, the present inventors have conducted studies to provide a method that enables coagulation of even chlorosulfonated polyolefin latex using a general coagulant.

[0007] The present disclosure includes, for example, the subject matter described in the following items. <Item 1> A chlorosulfonated polyolefin latex comprising: an aqueous dispersion medium; a chlorosulfonated polyolefin; at least one compound (first agent) selected from the group consisting of alkylbenzene sulfonate, polyoxyalkylene disulfonate, and taurine salt; and a fatty acid salt (second agent). <Item 2-1> A chlorosulfonated polyolefin latex comprising: a chlorosulfonated polyolefin latex comprising: a chlorosulfonated polyolefin latex; a chlorosulfonated polyolefin latex; and a fatty acid salt (second agent). <Item 2-2> A chlorosulfonated polyolefin latex comprising: a chlorosulfonated polyolefin latex; ... and a chlorosulfonated polyolefin latex; wherein the taurine salt is a compound represented by the 3 )-(CH 2 ) 2 -SO 3 M (wherein R represents a cocoyl group or an acyl group having 8 to 18 carbon atoms, and M represents an alkali metal (preferably sodium or potassium), ammonium (NH), or triethanolammonium (NH(CH) 2 CH 2 OH) 3) ). The latex according to item 1, wherein the alkylbenzenesulfonate is a C8-18 alkylbenzenesulfonate. <Item 2-3> The latex according to item 1, 2-1, or 2-2, wherein the polyoxyalkylene disulfonate is a salt of an ester in which hydroxy groups at both ends of a polyalkylene glycol are sulfated, and the polyalkylene glycol is formed by polymerizing C2-4 alkylene glycol. <Item 3> The latex according to any of items 1 and 2-1 to 2-3, wherein the mass ratio of the first part to the second part is 0.5 to 5. <Item 4> The latex according to any of items 1, 2-1 to 2-3, and 3, wherein the total amount of the first part and the second part is 3 to 8 parts by mass per 100 parts by mass of chlorosulfonated polyolefin. <Item 5> The latex according to any one of Items 1, 2-1 to 2-3, and 3 to 4, wherein the second agent is at least one selected from the group consisting of laurates, myristates, and oleates. <Item 6> A method for producing a chlorosulfonated polyolefin latex, comprising: an emulsification step of dispersing a chlorosulfonated polyolefin dissolved in an organic solvent in an aqueous dispersion medium in the presence of at least one compound (first agent) selected from the group consisting of alkylbenzenesulfonates, polyoxyalkylene disulfonates, and taurates, and a fatty acid salt (second agent), to prepare an emulsion; and a desolvation step of removing the organic solvent from the emulsion. <Item 7> A chlorosulfonated polyolefin emulsification composition comprising at least one compound selected from the group consisting of alkylbenzenesulfonates, polyoxyalkylene disulfonates, and taurates, and a fatty acid salt. <Item 8> A dip-forming composition comprising the chlorosulfonated polyolefin latex according to any one of Items 1, 2-1 to 2-3, and 3 to 5. <Item 9> A dip-molded article obtained by dip-molding the dip-molding composition according to Item 8.

[0008] The chlorosulfonated polyolefin latex obtained has excellent stability and can be applied to a general coagulation dipping method. Furthermore, by using the latex, a dip-molded article can be efficiently produced.

[0009] Each embodiment included in the present disclosure will be described in more detail below. The present disclosure preferably includes, but is not limited to, a chlorosulfonated polyolefin latex containing a specific emulsifier, its uses, and a production method, etc. The present disclosure includes all that is disclosed in the present specification and that can be recognized by a person skilled in the art.

[0010] The chlorosulfonated polyolefin latex encompassed by the present disclosure comprises an aqueous dispersion medium, a chlorosulfonated polyolefin, at least one compound selected from the group consisting of alkylbenzene sulfonates, polyoxyalkylene disulfonates, and taurates, and a fatty acid salt. The chlorosulfonated polyolefin latex encompassed by the present disclosure may be referred to as the "latex of the present disclosure." The at least one compound selected from the group consisting of alkylbenzene sulfonates, polyoxyalkylene disulfonates, and taurates may be referred to as the "first agent," and the fatty acid salt may be referred to as the "second agent." Both the first agent and the second agent are compounds that can function as emulsifiers, and their combined use can produce a good chlorosulfonated polyolefin latex.

[0011] Chlorosulfonated polyolefins can be obtained by chlorinating and chlorosulfonating polyolefins, including polymers or copolymers of α-olefins and copolymers of α-olefins with other polymerizable components.

[0012] Examples of α-olefins include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, etc. Other polymerizable components include chain dienes such as isoprene, 1,3-butadiene, 1,4-hexadiene, 1,6-octadiene, and 2-methyl-1,5-hexadiene; cyclic dienes such as 1,4-cyclohexadiene, dicyclopentadiene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, and 6-chloromethyl-5-isopropenyl-2-norbornene; and vinyl compounds such as vinyl acetate, vinyl chloride, acrylonitrile, styrene, methyl acrylate, and methyl methacrylate.

[0013] The chlorosulfonated polyolefin is preferably a chlorosulfonated α-olefin polymer. In the chlorosulfonated α-olefin polymer, one α-olefin may be used alone or two or more α-olefins may be used. When two or more α-olefins are used, one of them is preferably ethylene.

[0014] More specific examples of chlorosulfonated polyolefins include chlorosulfonated polyethylene, chlorosulfonated ethylene-α-olefin copolymers, and chlorosulfonated α-olefin polymers. Note that the "α-olefin" in chlorosulfonated ethylene-α-olefin copolymers and chlorosulfonated α-olefin polymers refers to α-olefins other than ethylene. A preferred example of the α-olefin other than ethylene here is propylene. That is, a preferred example of the chlorosulfonated ethylene-α-olefin copolymer is chlorosulfonated ethylene-propylene copolymer, and a preferred example of the chlorosulfonated α-olefin polymer is chlorosulfonated propylene polymer.

[0015] The chlorosulfonated polyolefins may be used alone or in combination of two or more.

[0016] The sulfur content in the chlorosulfonated polyolefin is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, preferably 2.0% by mass or less, more preferably 1.5% by mass or less, and preferably 0.5 to 2.0% by mass, more preferably 0.8 to 1.5% by mass.

[0017] The chlorine content in the chlorosulfonated polyolefin of the present disclosure is not particularly limited, but is preferably 10% by mass or more, more preferably 20% by mass or more. It is also preferably 50% by mass or less, more preferably 40% by mass or less. It is also preferably 10 to 50% by mass, more preferably 20 to 40% by mass.

[0018] The sulfur content and chlorine content of the chlorosulfonated polyolefin are the contents of sulfur atoms and chlorine atoms contained in the chlorosulfonated polyolefin, respectively, and can be measured by the oxygen flask combustion method.

[0019] Methods for chlorinating and chlorosulfonating polyolefins include a solution method in which the polyolefin is dissolved in an organic solvent and the reaction is carried out in a homogeneous system, a suspension method in which the polyolefin is suspended in a solvent and the reaction is carried out, a melt method in which the polyolefin is reacted in a molten state, and a gas-phase method in which the polyolefin is suspended in a gas phase and the reaction is carried out. Among these, the solution method is preferred from the viewpoint of uniform chlorination and chlorosulfonation. Examples of the chlorinating agent and chlorosulfonating agent that can be used include a combination of chlorine gas and sulfurous acid gas, a combination of chlorine gas and sulfuryl chloride, and sulfuryl chloride alone. The chlorosulfonation reaction can be carried out by using a chlorinating agent, a chlorosulfonating agent, a radical generator, and, if necessary, a co-catalyst such as pyridine.

[0020] Commercially available chlorosulfonated polyolefins may be used, examples of which include those available from Tosoh Corporation under the trade names "TOSO-CSM" and "extos" (chlorosulfonated polyethylene).

[0021] The content of the chlorosulfonated polyolefin in the latex of the present disclosure is not particularly limited, but is, for example, preferably about 20 to 60 mass%, more preferably about 25 to 55 mass% or about 30 to 50 mass%, and even more preferably about 35 to 45 mass%.

[0022] As described above, the latex of the present disclosure contains at least one compound (first agent) selected from the group consisting of alkylbenzene sulfonate, polyoxyalkylene disulfonate, and taurine salt.

[0023] The alkylbenzenesulfonate is preferably a C8-18 alkylbenzenesulfonate. In other words, the alkyl group of the alkylbenzenesulfonate is preferably a C8-18 (C8, 9, 10, 11, 12, 13, 14, 15, 16, 17, or 18) alkyl group. The alkyl group may be linear or branched, with linear being preferred. Furthermore, preferred salts of alkylbenzenesulfonates include alkali metal salts (more specifically, sodium salts and potassium salts), ammonium salts, and triethanolammonium salts, with sodium salts being particularly preferred. More specific examples of alkylbenzenesulfonates include sodium dodecylbenzenesulfonate, potassium dodecylbenzenesulfonate, ammonium dodecylbenzenesulfonate, triethanolammonium dodecylbenzenesulfonate, sodium decylbenzenesulfonate, sodium tetradecylbenzenesulfonate, sodium hexadecylbenzenesulfonate, and sodium octadecylbenzenesulfonate. Among these, sodium dodecylbenzenesulfonate is preferred from the viewpoint of facilitating the production of a latex having a small particle size.

[0024] Alkylbenzene sulfonates can be prepared by sulfonating alkylbenzene and neutralizing the resulting alkylbenzene sulfonic acid with a basic compound. The alkylbenzene used as a raw material can be prepared by the Friedel-Crafts reaction of an alkyl halide with benzene or by reacting an olefin with benzene using hydrogen fluoride, zeolite, or the like. The resulting alkylbenzene can be reacted with a sulfonating agent to prepare alkylbenzene sulfonic acid. Examples of sulfonating agents include concentrated sulfuric acid, fuming sulfuric acid, chlorosulfuric acid, sulfur trioxide, and sulfur trioxide-Lewis base complexes. The resulting alkylbenzene sulfonic acid is neutralized with a basic compound. Examples of basic compounds include alkali metal salts such as sodium hydroxide, potassium hydroxide, and sodium carbonate, as well as ammonia and triethanolamine.

[0025] Commercially available alkylbenzene sulfonates may be used, and examples thereof include those available under the trade name "Neopelex G-25" from Kao Corporation, those available under the trade name "Lipon LS-250" from Lion Specialty Chemical Co., Ltd., those available under the trade name "Lunox S-40TD" from Toho Chemical Industry Co., Ltd., those available under the trade names "Newcoal 210" and "Newcoal 220-L" from Nippon Nyukazai Co., Ltd., those available under the trade names "Newex R" from NOF Corporation, those available under the trade names "Neogen RK" and "Neogen S-20F" from Dai-ichi Kogyo Seiyaku Co., Ltd., and those available under the trade names "Takesurf A-41-B" and "Takesurf A-41-S" from Takemoto Yushi Co., Ltd.

[0026] Polyoxyalkylene disulfonates are salts of esters in which hydroxy groups at both ends of a polyalkylene glycol are sulfated. The polyalkylene glycol is preferably a polymer of C2-4 alkylene glycol, more specifically, polypropylene glycol, poly-1,2-butylene glycol, poly-1,3-butylene glycol, poly-1,4-butylene glycol, polyethylene glycol-propylene glycol copolymer, polyethylene glycol-1,2-butylene glycol copolymer, polypropylene glycol-1,2-butylene glycol copolymer, etc. In the case of a copolymer with ethylene glycol, it is preferable that the molar ratio E / A of the ethylene glycol units (E) to the other glycol units (A) is less than 1, i.e., the amount of ethylene glycol units is less than the amount of the other glycol units. The copolymer may be a random copolymer or a block copolymer. The number of repeating units of the polyalkylene glycol is preferably 1 to 50, more preferably 5 to 40, and particularly preferably 10 to 30. It can also be said that the polyoxyalkylene disulfonate is preferably a polyoxy C2-4 alkylene disulfonate, and the number of polyoxyalkylene repeats is preferably 1-50, more preferably 5-40, and particularly preferably 10-30.

[0027] As the salt of the polyoxyalkylene disulfonate, alkali metal salts (for example, sodium salt, potassium salt) and ammonium salt are preferred.

[0028] More specific examples of the polyoxyalkylene disulfonate include sodium polypropylene glycol disulfonate, potassium polypropylene glycol disulfonate, ammonium polypropylene glycol disulfonate, sodium polyethylene glycol-propylene glycol disulfonate, sodium poly 1,2-butylene glycol disulfonate, etc. Among these, sodium polypropylene glycol disulfonate is preferred from the viewpoint of easily obtaining a latex having a small particle size.

[0029] Polyoxyalkylene disulfonates can be prepared by, for example, sulfate esterification of the hydroxy groups at both ends of a polyalkylene glycol, neutralizing the resulting sulfate ester with a basic compound, and forming a salt thereof. Methods for preparing the polyalkylene glycol used as a raw material include ring-opening polymerization of a cyclic ether compound and dehydration condensation polymerization of glycols. As described above, examples of polyalkylene glycols include polypropylene glycol, poly-1,2-butylene glycol, poly-1,3-butylene glycol, poly-1,4-butylene glycol, polyethylene glycol-propylene glycol copolymer, polyethylene glycol-1,2-butylene glycol copolymer, and polypropylene glycol-1,2-butylene glycol copolymer. In the case of copolymers with ethylene glycol, the molar ratio E / A of the ethylene glycol units (E) to the other glycol units (A) is preferably less than 1, i.e., the amount of ethylene glycol units is less than the amount of the other glycol units. The copolymer may be a random copolymer or a block copolymer. The number of repeating units of the polyalkylene glycol is preferably 1 to 50, more preferably 5 to 40, and particularly preferably 10 to 30. The sulfation method involves dissolving the polyalkylene glycol in an organic solvent and carrying out a reaction under conditions where the amount of sulfating agent used is at least twice the molar amount of the polyalkylene glycol. Examples of sulfating agents include concentrated sulfuric acid, fuming sulfuric acid, chlorosulfuric acid, sulfur trioxide, and sulfur trioxide-Lewis base complexes. After the sulfation, the solution is neutralized with a suitable basic compound. Examples of basic compounds include alkali metal salts such as sodium hydroxide, potassium hydroxide, and sodium carbonate, as well as ammonia and triethanolamine.

[0030] The polyoxyalkylene disulfonate may be a commercially available product, for example, "Newcol 240" manufactured by Nippon Nyukazai Co., Ltd.

[0031] The taurine salt is preferably one obtained by amidating an N-alkyl taurine salt, and examples of the salt include alkali metal salts (e.g., sodium salt, potassium salt), ammonium salt, and triethanolammonium salt.

[0032] Such taurine salts include those represented by the formula: R—N(CH 3 )-(CH 2 ) 2 -SO 3 M

[0033] (wherein R represents a cocoyl group or an acyl group having 8 to 18 carbon atoms, M represents an alkali metal (preferably sodium or potassium), ammonium (NH 4 ), or triethanolammonium (NH(CH 2 CH 2 OH) 3 ) is preferably mentioned.

[0034] Specific examples of the acyl group having 8 to 18 carbon atoms (8, 9, 10, 11, 12, 13, 14, 15, 16, 17, or 18) include a lauroyl group, a myristoyl group, a palmitoyl group, a stearoyl group, and an oleoyl group.

[0035] More specific examples of the taurine salt include N-acylmethyl taurine sodium salts such as sodium N-cocoyl methyl taurate, sodium N-lauroyl methyl taurate, sodium N-myristoyl methyl taurate, sodium N-palmitoyl methyl taurate, sodium N-stearoyl methyl taurate, and sodium N-oleoyl methyl taurate, as well as potassium N-cocoyl methyl taurate, ammonium N-cocoyl methyl taurate, ammonium N-cocoyl methyl taurate triethanol, and sodium N-cocoyl ethyl taurate. Among these, sodium N-acyl methyl taurate is preferred from the viewpoint that a latex having a small particle size can be easily obtained.

[0036] Such taurine salts can be prepared, for example, by amidating an N-alkyl taurine salt. N-Alkyl taurine salts can be prepared by reacting chloroethyl sulfate, bromoethyl sulfate, isethionate, vinyl sulfonate, or the like with an alkylamine. Examples of amidation of an N-alkyl taurine salt include a method of reacting the obtained N-alkyl taurine salt with acyl chloride in the presence of a base, a method of dehydrating and condensing an N-alkyl taurine salt with a fatty acid, and a method of reacting an N-alkyl taurine salt with a fatty acid isopropenyl ester.

[0037] Commercially available taurine salts may be used, and examples thereof include products sold by Nikko Chemicals Co., Ltd. under the trade names "NIKKOL CMT-30," "NIKKOL LMT-30," "NIKKOL MMT," "NIKKOL PMT," and "NIKKOL SMT," products sold by Toho Chemical Industry Co., Ltd. under the trade names "NEOSCOPE CN-30" and "NEOSCOPE CTS-25," products sold by NOF Corporation under the trade names "DIAPON S," "DIAPON LM," and "DIAPON K."

[0038] The latex of the present disclosure contains a fatty acid salt (second agent). The fatty acid constituting the fatty acid salt may be either a saturated fatty acid or an unsaturated fatty acid. As the unsaturated fatty acid, for example, those having 1, 2, 3, or 4 carbon double bonds are preferred, and those having 1 bond are more preferred. The unsaturated fatty acid may be either linear or branched. Fatty acids having 8 to 24 carbon atoms (8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, or 24) are preferred, and fatty acids having 12 to 22 carbon atoms are more preferred. More specifically, examples of the fatty acid salt include saturated fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, and behenic acid, and unsaturated fatty acids such as myristoleic acid, palmitoleic acid, sapienic acid, oleic acid, elaidic acid, ricinoleic acid, linoleic acid, linolenic acid, gadoleic acid, arachidonic acid, cetoleic acid, erucic acid, and brassidic acid. Examples of the fatty acid salt include alkali metal salts (e.g., sodium salts and potassium salts), ammonium salts, and amine salts (e.g., triethanolamine salts), with the salts of the specific fatty acids mentioned above being particularly preferred.

[0039] Among these fatty acid salts, from the viewpoint of obtaining a more excellent latex stability, it is preferable to use a laurate, a myristate, or an oleate, it is more preferable to use a laurate or an oleate, and it is further preferable to use potassium laurate or potassium oleate.

[0040] The fatty acid salts can be used singly or in combination of two or more.

[0041] The fatty acid salt may be added as a fatty acid salt, or may be prepared by neutralizing the fatty acid with an alkali in the latex production system. When prepared in the system, the fatty acid is not completely neutralized, and unreacted fatty acid may also be present in the system, or an alkali equivalent to or greater than the fatty acid may be added to contain excess alkali in the system. The neutralization rate of the fatty acid is not particularly limited, but is preferably, for example, 60 to 400 mol%, more preferably 90 to 300 mol%, and even more preferably 100 to 200 mol%. Here, a "neutralization rate of 400 mol%" means that the fatty acid has been neutralized with 4 equivalents of alkali.

[0042] The fatty acid salt may be a commercially available product, for example, products sold under the trade names "NnS Soap," "SS-40N," "OS Soap," and "KS Soap" by Kao Corporation; products sold under the trade names "NIKKOL Potassium Laurate LK-120," "NIKKOL Potassium Myristate MK-140," and "Taisoap MNK-40" by Nikko Chemicals Co., Ltd.; and products sold under the trade names "NonSal PK-1," "NonSal SK-1," and "NonSal MK-1" by NOF Corporation. When a fatty acid is used to prepare a fatty acid salt, the fatty acid may be a commercially available product, for example, products sold under the trade names "NAA-142," "NAA-160," "NAA-35," and "Extra Olein" by NOF Corporation; products sold under the trade names "Palmitic Acid 60," "Stearic Acid 65," and "PM200" by Miyoshi Oil & Fats Co., Ltd.; and products sold under the trade names "Lunac L-55A," "Lunac BA," and "Lunac O-V" by Kao Corporation.

[0043] The latex of the present disclosure may contain an emulsifier other than the first and second agents, as long as the effects of the invention according to the present disclosure are not impaired. Examples of such emulsifiers include anionic emulsifiers such as alkyl sulfate ester salts and alkyl phosphate ester salts; nonionic emulsifiers such as polyoxyethylene alkyl ethers and glycerin fatty acid esters; and amphoteric emulsifiers such as alkyl betaine salts, sulfobetaine salts, and N-acylamino acid salts. The latex of the present disclosure preferably does not contain any emulsifiers other than the first and second agents. (In other words, it is preferable that the only emulsifiers contained in the latex of the present disclosure are the first and second agents.)

[0044] In the latex of the present disclosure, the first agent is preferably contained in an amount of 1 to 15 parts by mass relative to 100 parts by mass of the chlorosulfonated polyolefin latex. The upper or lower limit of this range may be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, or 14 parts by mass. For example, the range is more preferably 1 to 10 parts by mass, and even more preferably 2 to 5 parts by mass. If the amount of the first agent used is within this range, a latex with a small particle size is more likely to be obtained, which is preferable.

[0045] In the latex of the present disclosure, the second agent is preferably contained in an amount of 0.1 to 10 parts by mass per 100 parts by mass of the chlorosulfonated polyolefin latex. The upper or lower limit of this range may be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, or 9 parts by mass. For example, the range is more preferably 0.2 to 7 parts by mass, and even more preferably 0.5 to 5 parts by mass. Using the second agent in this range in amount is preferred because it makes it easier to obtain a latex with excellent stability.

[0046] The ratio of the first agent to the second agent is not particularly limited, but the mass ratio of the amount of the first agent to the amount of the second agent is preferably 0.5 to 5. The upper or lower limit of this range may be, for example, 1, 1.5, 2, 2.5, 3, 3.5, 4, or 4.5. For example, the range is more preferably 2 to 4. It is more preferable that the above content ratio of the first agent to 100 parts by mass of the chlorosulfonated polyolefin latex and / or the above content ratio of the second agent to 100 parts by mass of the chlorosulfonated polyolefin latex are satisfied, and that the above usage ratio of the first agent to the second agent is also satisfied.

[0047] In addition, in the latex of the present disclosure, the conditions for the content ratio of the first agent and the second agent are satisfied, and the total amount of the first agent and the second agent is preferably 3 to 8 parts by mass, and particularly preferably 4 to 6 parts by mass, per 100 parts by mass of chlorosulfonated polyolefin.

[0048] The aqueous dispersion medium is preferably one that is commonly used for latex, such as water, which is not particularly limited and includes, for example, tap water, deionized water, and distilled water.

[0049] The content of the aqueous dispersion medium in the latex of the present disclosure is not particularly limited and can be appropriately adjusted depending on the amount of other components contained. For example, in the latex of the present disclosure, the aqueous dispersion medium can be contained preferably in an amount of 60% by mass or more, more preferably 65% ​​by mass or more or 70% by mass or more. It is also possible to use the aqueous dispersion medium as the balance of the components other than the aqueous dispersion medium, and adjust the content ratio of each component while making the total latex 100% by mass.

[0050] In the latex of the present disclosure, the average particle size of the chlorosulfonated polyolefin is preferably 0.1 to 10 μm, more preferably 0.3 to 5.0 μm, and even more preferably 0.5 to 2.0 μm. When the average particle size of the chlorosulfonated polyolefin is 10 μm or less, the particles do not settle too quickly, and static stability is more preferable. When the average particle size is 0.1 μm or more, the viscosity of the latex can be prevented from becoming too high, making it easier to handle. Note that the average particle size in the present disclosure is the volume-based median particle size measured with a laser diffraction particle size distribution system.

[0051] The latex of the present disclosure can be produced, for example, through an emulsification step of preparing an emulsion by dispersing a chlorosulfonated polyolefin dissolved in an organic solvent in an aqueous dispersion medium in the presence of a first agent and a second agent, and a desolvation step of removing the organic solvent from the emulsion.

[0052] In the emulsification step, the organic solvent for dissolving the chlorosulfonated polyolefin is not particularly limited as long as it is capable of dissolving the chlorosulfonated polyolefin, and examples thereof include aliphatic hydrocarbon organic solvents such as hexane, heptane, octane, etc.; alicyclic hydrocarbon organic solvents such as cyclohexane, methylcyclohexane, decalin, etc.; aromatic hydrocarbon organic solvents such as benzene, toluene, xylene, etc.; halogenated hydrocarbon organic solvents such as chloroform, 1,2-dichloroethane, chlorobenzene, etc. These organic solvents may be used alone or in combination of two or more.

[0053] The amount of the organic solvent used is preferably set so that the concentration of the chlorosulfonated polyolefin becomes, for example, 3 to 20 mass %, more preferably 10 to 16 mass %. When the concentration of the chlorosulfonated polyolefin is in this range, the solution is easy to handle and a latex having a small particle size is easily obtained, which is preferable.

[0054] The temperature when dissolving the chlorosulfonated polyolefin in the organic solvent is preferably, for example, about 20 to 100° C. From the viewpoint of suppressing hydrolysis of the chlorosulfonated polyolefin (hydrolysis of the chlorosulfonic acid group), 40 to 80° C. is more preferable.

[0055] The emulsification step can be carried out, for example, in the following two forms.

[0056] For example, an emulsion can be prepared by dissolving or dispersing the first and second agents in an aqueous dispersion medium, and then adding and dispersing a chlorosulfonated polyolefin solution to the aqueous dispersion medium (this emulsification process is sometimes referred to as the first form). The first and second agents used in this form act as emulsifiers. The first and second agents may be added separately to the aqueous dispersion medium, or the first and second agents may be mixed and then added to the aqueous dispersion medium.

[0057] Alternatively, for example, an emulsion can be prepared by adding a fatty acid to a chlorosulfonated polyolefin solution, mixing, dissolving or dispersing the fatty acid, and then adding and dispersing this mixed solution to an aqueous dispersion medium in which the first agent and a neutralizer for the fatty acid have been dissolved (this emulsification process is sometimes referred to as the second form). The fatty acid used is the same as described above and is used as a precursor for the second agent. The neutralizer used may be any agent that can react with the fatty acid to form a fatty acid salt, and preferred examples include sodium hydroxide, sodium methoxide, potassium hydroxide, potassium tert-butoxide, ammonia, and triethanolamine.

[0058] The amount of aqueous dispersion medium used in the emulsification step is preferably set so that the total concentration of the first agent and the second agent relative to the aqueous dispersion medium is 0.1 to 50% by mass in the case of the first embodiment, and in the case of the second embodiment, the total concentration of the first agent contained in the aqueous dispersion medium, the fatty acid salt formed by the fatty acid in the organic solvent solution and the neutralizer for the aqueous dispersion medium is 0.1 to 50% by mass relative to the aqueous dispersion medium.

[0059] In the first embodiment, the amounts of the first agent and the second agent used are preferably set to 2 to 5 parts by mass and 0.5 to 4 parts by mass, respectively, per 100 parts by mass of chlorosulfonated polyolefin dissolved in an organic solvent. On the other hand, in the second embodiment, the amount of the first agent used is preferably set to the same as in the first embodiment. The amounts of the fatty acid and neutralizing agent used are preferably set so that the amount of fatty acid salt formed by adding the organic solvent solution to the aqueous dispersion medium is the same as in the first embodiment.

[0060] In preparing the emulsion in the emulsification step, a method of stirring and mixing using an emulsifier having an appropriate shear force, for example, a batch-type emulsifier such as a homomixer, homodisper, homogenizer, or colloid mill; a method of stirring and mixing using a continuous emulsifier such as an in-line homomixer or in-line homogenizer; or a method of dispersing using an ultrasonic disperser or the like can be used. These methods may be used alone or in combination of two or more. The temperature in the emulsification step is not particularly limited, but is preferably set to 5 to 70°C, more preferably 25 to 60°C. The average particle size of the chlorosulfonated polyolefin in the target chlorosulfonated polyolefin latex can also be adjusted by controlling the intensity of stirring and mixing, the ultrasonic frequency, the treatment time, the treatment temperature, etc. during the preparation of the emulsion.

[0061] In the solvent removal step, examples of a method for removing the organic solvent from the emulsion obtained in the emulsification step include a method for distilling the emulsion under normal pressure, reduced pressure, or increased pressure, a method for blowing steam or the like into the emulsion to volatilize and remove the organic solvent, a method for removing the organic solvent using a membrane that selectively allows only the organic solvent to permeate, etc. These methods may be carried out alone or in combination of two or more thereof.

[0062] In the desolvation step, an antifoaming agent may be used to suppress foaming of the emulsion. Examples of antifoaming agents include mineral oil-based antifoaming agents, silicone-based antifoaming agents, acetylene-based antifoaming agents, metal soap-based antifoaming agents, acrylic antifoaming agents, and fluorine-based antifoaming agents. Among these, acetylene-based antifoaming agents are preferred. These may be used alone or in combination of two or more types. The amount of antifoaming agent used depends on the amount of emulsifier used, but is preferably 100 to 2000 ppmwt per 100 parts by mass of chlorosulfonated polyolefin. The antifoaming agent may be added to the emulsion before the desolvation step, or may be added appropriately during the desolvation step. Methods of addition that can be used include adding all at once, adding dropwise, spraying, and the like.

[0063] Furthermore, the emulsion after removing the organic solvent can be concentrated to a desired solid content concentration, if necessary. Examples of the concentration method include heat concentration, centrifugation, filtration, and wet separation. Among them, the method of concentration using a filtration membrane is preferred, and the method of concentration using an ultrafiltration membrane is more preferred, because it does not require much heat or stress to be applied to the emulsion and is less likely to impair the stability of the emulsion.

[0064] The solid content concentration of the target chlorosulfonated polyolefin latex obtained through the solvent removal step is preferably 20 to 60% by mass.

[0065] In the above-mentioned production method, a neutralizing agent may be added to the obtained chlorosulfonated polyolefin latex to adjust the pH. As the neutralizing agent, for example, a common neutralizing agent such as sodium hydroxide, potassium hydroxide, sodium carbonate, ammonia, monoethanolamine, etc. may be used. The neutralizing agent may be added before the solvent removal step, may be added while the solvent is being removed, or may be added after the solvent removal step.

[0066] To enhance the stability of the latex of the present disclosure, additives such as dispersion stabilizers such as polyvinyl alcohol, polyvinylpyrrolidone, and hydroxyethyl cellulose, and stabilizers such as dibutylhydroxytoluene, 2,5-di-tert-butylhydroquinone, and bisphenol A epoxy resin may be added within a range that does not impair the effects of the present disclosure. Such additives may be added to the chlorosulfonated polyolefin latex after preparation, or, depending on the type of additive, may be added to the organic solvent solution or aqueous dispersion medium used in the emulsification step during the preparation of the chlorosulfonated polyolefin latex. These additives are typically preferably added individually or as a mixture in the form of an aqueous solution or dispersion. When additives are added, a total amount of about 0.1 to 10 parts by mass per 100 parts by mass of the chlorosulfonated polyolefin is preferred.

[0067] The present disclosure also encompasses a chlorosulfonated polyolefin emulsion composition comprising a first agent and a second agent. This chlorosulfonated polyolefin emulsion composition may be referred to as the emulsification composition of the present disclosure. Because the emulsification composition of the present disclosure comprises the first agent and the second agent, a highly stable, coagulable chlorosulfonated polyolefin latex can be produced by emulsifying a chlorosulfonated polyolefin with the emulsification composition of the present disclosure. The emulsification composition of the present disclosure can be preferably used to produce the chlorosulfonated polyolefin latex of the present disclosure.

[0068] With regard to the emulsification composition of the present disclosure, the above descriptions apply as they are with respect to the chlorosulfonated polyolefin to be emulsified, the types and mass ratios of the first and second agents contained therein, and further, the preferred amounts when applied to the chlorosulfonated polyolefin.

[0069] The latex of the present disclosure can be particularly preferably used as a dip-molding composition.

[0070] The latex of the present disclosure may further contain known additives such as a rheology modifier, an antioxidant, an antifoaming agent, a pH adjuster, a chelating agent, a vulcanizing agent, a vulcanization accelerator, a vulcanization accelerator aid, an acid acceptor, a film-forming aid, a plasticizer, a filler, a pigment, etc., within a range that does not impair the effects of the present disclosure. Such additives can be preferably used particularly when the latex of the present disclosure is used as a dip-molding composition.

[0071] Examples of rheology modifiers include polysaccharides such as cellulose, cellulose nanofiber, cellulose nanocrystal, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropylmethyl cellulose, carboxymethyl cellulose, chitin, chitosan, guar gum, and xanthan gum; water-soluble vinyl polymers such as polyacrylic acid, sodium polyacrylate, crosslinked polyacrylic acid, polyacrylamide, polyvinyl alcohol, polyvinyl methyl ether, and polyvinylpyrrolidone; and clay minerals such as montmorillonite, nontronite, saponite, beidellite, and hectorite.

[0072] Examples of the antioxidant include phenol-based antioxidants such as dibutylhydroxytoluene, 2,2′-methylenebis(4-ethyl-6-tert-butylphenol), and 2,5-di-tert-butylhydroquinone; amine-based antioxidants such as N-phenyl-1-naphthylamine and di(4-octylphenyl)amine; phosphorus-based antioxidants such as tris(nonylphenyl)phosphite; sulfur-based antioxidants such as dilauryl thiodipropionate, 2-mercaptobenzimidazole, and nickel dibutyldithiocarbamate; and bisphenol A-type epoxy resins.

[0073] Examples of the defoaming agent include oil-based defoaming agents, mineral oil-based defoaming agents, silicone-based defoaming agents, and polyether-based defoaming agents.

[0074] Examples of pH adjusters include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, ammonia, trimethylamine, triethanolamine, hydrochloric acid, sulfuric acid, phosphoric acid, citric acid, and acetic acid.

[0075] Examples of the chelating agent include ethylenediaminetetraacetic acid, nitrilotriacetic acid, trans-1,2-diaminocyclohexanetetraacetic acid, diethylenetriaminepentaacetic acid, bis(aminoethyl)glycol ether-N,N,N',N'-tetraacetic acid, N-(2-hydroxyethyl)ethylenediamine-N,N',N'-triacetic acid, dihydroxyethylglycine, 1-hydroxyethane-1,1-diphosphonic acid, gluconic acid, citric acid, malic acid, and tartaric acid.

[0076] Examples of the vulcanizing agent include sulfur such as powdered sulfur, sulfur flowers, precipitated sulfur, and colloidal sulfur; organic peroxides such as di-tert-butyl peroxide and dicumyl peroxide; maleimide compounds such as N,N'-m-phenylene bismaleimide; quinoid compounds such as p-quinone dioxime and p,p'-dibenzoylquinone dioxime; metal compounds such as magnesium oxide and lead oxide; and polyhydric alcohol compounds such as pentaerythritol, dipentaerythritol, sorbitol, and trimethylolpropane.

[0077] Examples of the vulcanization accelerator include diethyldithiocarbamic acid, dibutyldithiocarbamic acid, diphenyldithiocarbamic acid, sodium diethyldithiocarbamate, sodium dibutyldithiocarbamate, sodium diphenyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, zinc diphenyldithiocarbamate, 2-mercaptobenzothiazole, zinc 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-(4'-morpholino) dithio)benzothiazole, trimethylthiourea, N,N'-diethylthiourea, 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, N-cyclohexyl-2-benzothiazolylsulfenamide, N-oxydiethylene-2-benzothiazolylsulfenamide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetramethylthiuram monosulfide, dipentamethylenethiuram tetrasulfide, zinc isopropyl xanthogenate, and the like.

[0078] Examples of the vulcanization accelerator include metal oxides such as zinc oxide and magnesium oxide, and fatty acids such as stearic acid and palmitic acid.

[0079] Examples of the acid acceptor include metal oxides such as lead oxide, magnesium oxide, zinc oxide, and calcium oxide; metal hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide; clay minerals such as hydrotalcite; and epoxy compounds such as phenyl glycidyl ether, bisphenol A diglycidyl ether, epoxidized soybean oil, epoxidized linseed oil, epoxidized polybutadiene, and polyglycidyl methacrylate.

[0080] Examples of the film-forming aid include propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol monoiso-butyl ether, ethylene glycol mono-tert-butyl ether, ethylene glycol monophenyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoiso-butyl ether, diethylene glycol mono-tert-butyl ether, diethylene glycol monophenyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, triethylene glycol monobutyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dipropylene glycol mono-n-butyl ether, dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, and 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate.

[0081] Examples of the plasticizer include phthalate esters, adipic acid esters, glycerin fatty acid esters, polyether polyols, and polyester polyols.

[0082] Examples of fillers include carbon fiber, cellulose fiber, carbon black, silica, talc, clay, calcium carbonate, titanium oxide, and barium sulfate.

[0083] Examples of pigments include carbon black, titanium oxide, chromium oxide, iron blue, amber, nickel titanium yellow, viridian, cobalt blue, phthalocyanine blue, phthalocyanine green, molybdenum orange, chrome yellow, anthraquinone, and quinacridone.

[0084] When an additive is contained, the amount of the additive contained in the latex of the present disclosure is not particularly limited, but is preferably 5 to 30 parts by mass per 100 parts by mass of the solid content in the latex composition (i.e., chlorosulfonated polyolefin).

[0085] Furthermore, when the latex of the present disclosure is used as a dip-molding composition, it may contain other rubber latexes as long as the effects are not impaired. Examples of such other latexes include natural rubber latex, isoprene rubber latex, butadiene rubber latex, chloroprene rubber latex, butyl rubber latex, styrene-butadiene rubber latex, acrylic rubber latex, acrylonitrile-butadiene rubber latex, silicone rubber latex, fluororubber latex, epichlorohydrin rubber latex, and olefin rubber latex. When these various rubber latexes are used in combination with the latex of the present disclosure as a dip-molding composition, the content of the other rubber is preferably less than the content of the chlorosulfonated polyolefin. For example, the content of the other rubber is preferably 50 parts by mass or less, 40 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less per 100 parts by mass of the chlorosulfonated polyolefin.

[0086] The method for preparing such a dip-molding composition is not particularly limited, and examples thereof include a method of mixing various additives with the chlorosulfonated polyolefin latex using a dispersing machine such as a ball mill, a bead mill, a kneader, or a disper; a method of previously preparing an aqueous dispersion of desired additives using a dispersing machine, and then mixing the aqueous dispersion with the chlorosulfonated polyolefin latex; and a method of mixing some additives with the chlorosulfonated polyolefin latex, and then mixing it with an aqueous dispersion of other additives.

[0087] The pH of the latex of the present disclosure is preferably 5 or higher (particularly when used as a dip-forming composition), and more preferably 7 to 12.

[0088] When the latex of the present disclosure is used as a dip-molding composition, it may be aged (also referred to as pre-vulcanization) before being subjected to dip molding. The aging time cannot be determined in general because it depends on the type of additives and the aging temperature, but is preferably 1 to 7 days, more preferably 1 to 3 days. The aging temperature is preferably 10 to 50°C, more preferably 20 to 40°C. After aging, it is preferably stored at a temperature of 30°C or less until it is subjected to dip molding.

[0089] The present disclosure also encompasses a dip-molded article obtained by using the latex of the present disclosure as a dip-molded article composition.

[0090] Dip molding is a method in which a mold (molding mold) is immersed in a dip-molding composition, the composition is deposited on the surface of the mold, the mold is then lifted from the composition, and the composition deposited on the surface of the mold is then dried. Below, methods that can be used to prepare the dip-molded article of the present disclosure are described in more detail.

[0091] The mold used for dip molding can be a mold that corresponds to the desired three-dimensional shape and is integrally formed from ceramic, metal, glass, plastic, etc. The surface of the mold may be finished with a matte finish or may be provided with other materials such as fibers or other types of rubber coatings, depending on the purpose of the dip-molded article. In addition, the mold may be preheated before being immersed in the dip-molding composition.

[0092] Before immersing the mold in the dip-molding composition or after removing the mold from the dip-molding composition, a coagulant is preferably used to aggregate the solid component (hereinafter sometimes simply referred to as the rubber component) mainly composed of chlorosulfonated polyolefin. Examples of methods for using the coagulant include immersing the mold before immersion in the dip-molding composition in a coagulant solution (hereinafter also referred to as the coagulant liquid) to adhere the coagulant to the mold, and immersing the mold on which the dip-molding composition has been deposited in the coagulant liquid. From the viewpoint of obtaining a dip-molded article with minimal thickness unevenness, a method of immersing the mold before immersion in the dip-molding composition in a coagulant solution to adhere the coagulant to the mold is preferred.

[0093] Examples of coagulants include metal salts, with water-soluble metal salts being more preferred. Among metal salts, polyvalent metal salts that generate polyvalent metal ions are preferred from the viewpoint of high coagulation power, with water-soluble polyvalent metal salts being more preferred. Examples of water-soluble metal salts include metal halides such as sodium chloride, potassium chloride, barium chloride, calcium chloride, magnesium chloride, zinc chloride, and aluminum chloride; metal nitrates such as sodium nitrate, potassium nitrate, barium nitrate, calcium nitrate, zinc nitrate, and aluminum nitrate; metal acetates such as sodium acetate, potassium acetate, barium acetate, calcium acetate, zinc acetate, and aluminum acetate; and metal sulfates such as sodium sulfate, potassium sulfate, calcium sulfate, magnesium sulfate, and aluminum sulfate. As the polyvalent metal, alkaline earth metals are preferred, with calcium, barium, and magnesium being more preferred, and calcium being particularly preferred. Furthermore, as the coagulant, calcium chloride and calcium nitrate are particularly preferred from the viewpoint of high solubility in water. These coagulants may be used alone or in combination of two or more.

[0094] The coagulant is preferably used in the form of an aqueous solution. This aqueous solution may further contain a water-soluble organic solvent such as methyl alcohol or ethyl alcohol, or a nonionic surfactant. The concentration of the coagulation liquid is not particularly limited, but is preferably 5 to 50% by mass, more preferably 10 to 40% by mass, and particularly preferably 15 to 35% by mass. The immersion time of the casting mold in the coagulation liquid is not particularly limited, but is usually preferably 5 to 300 seconds, and more preferably 10 to 100 seconds.

[0095] After the casting mold is immersed in the coagulation liquid to adhere the coagulation liquid to the surface, the solvent of the coagulation liquid may be removed by drying. The drying temperature can be set appropriately depending on the type of solvent and salt used, and is preferably 60 to 150°C, and more preferably 80 to 120°C. The drying time is not particularly limited, but is preferably 1 to 600 seconds, and more preferably 5 to 300 seconds. Drying the coagulation liquid on the surface of the casting mold makes it easier to create a state in which the salt is uniformly adhered to the surface of the casting mold.

[0096] The time for immersing the mold in the latex (dip-molding composition) of the present disclosure may be appropriately set depending on the desired thickness (film thickness), but is preferably 5 to 600 seconds, more preferably 10 to 300 seconds.

[0097] After the mold is removed from the dip-molding composition, the solidified coating formed on the mold surface is typically dried by heating. The drying method is not particularly limited, and drying can be performed using a hot air heater, infrared heater, microwave heater, high-frequency heater, or the like. The drying temperature is not particularly limited, but is preferably 50 to 160°C, more preferably 60 to 140°C, and particularly preferably 70 to 120°C. The drying time is also not particularly limited, but is preferably 1 to 120 minutes, more preferably 10 to 100 minutes, and particularly preferably 20 to 60 minutes.

[0098] Furthermore, if necessary, further heating may be performed to vulcanize the solidified coating formed on the mold surface. The heating conditions during vulcanization are not particularly limited, but 60 to 200°C is preferred, 80 to 180°C is more preferred, and 100 to 160°C is particularly preferred. By setting the heating temperature within this range, it is possible to achieve an appropriate vulcanization rate and suppress deterioration of the rubber component due to excessive heating. The heating time for vulcanization may be selected appropriately depending on the heating temperature, and is usually 5 to 120 minutes. The heating method can be, for example, the same method as the heating method described above.

[0099] Before or after heating the mold onto which the dip-molding composition has been deposited, it is preferable to wash the mold with water or warm water to remove water-soluble impurities (e.g., excess emulsifier, surfactant, coagulant, uncoagulated latex, etc.). The temperature of the water or warm water used is preferably 20 to 80°C, more preferably 30 to 70°C. The washing time is preferably about 0.5 to 60 minutes.

[0100] The dip-molded article after drying (and further vulcanization, if necessary) is removed from the mold. Removal methods include peeling from the mold by hand, peeling from the mold using a peeling roller, and peeling using water pressure or compressed air pressure. After being removed from the mold, the dip-molded article may be further washed with water. Furthermore, if necessary, to prevent adhesion at the contact surfaces between dip-molded articles and to improve slippage during attachment and detachment, inorganic fine particles such as talc or calcium carbonate or organic fine particles such as cornstarch may be applied to the surface, an elastomer layer containing fine particles may be further formed on the surface, or the surface layer may be chlorinated.

[0101] The thickness of the dip-molded article thus obtained is preferably 0.1 to 2 mm, more preferably 0.2 to 1.5 mm, and particularly preferably 0.3 to 1.0 mm. The thickness can be appropriately set by the immersion time, etc., as described above.

[0102] In this specification, the term "comprising" includes "consisting essentially of" and "consisting of." In addition, the present disclosure includes any and all combinations of the constituent elements described in this specification.

[0103] Furthermore, the various characteristics (properties, structures, functions, etc.) described in each embodiment of the present disclosure above may be combined in any way to identify the subject matter encompassed by the present disclosure, i.e., the present disclosure encompasses all subject matter consisting of any combination of the combinable characteristics described herein.

[0104] The present disclosure will be specifically described below with reference to examples and comparative examples, but the present disclosure is not limited to these examples or the like.

[0105] As the chlorosulfonated polyolefin, chlorosulfonated polyethylene (product name "TOSO-CSM" by Tosoh Corporation, product numbers TS-320, TS-530, or CN-1500) was used. The chlorine and sulfur contents of these chlorosulfonated polyethylenes (CSM rubbers) are as follows: TS-320: chlorine content 23% by mass, sulfur content 1.0% by mass TS-530: chlorine content 35% by mass, sulfur content 1.0% by mass CN-1500: chlorine content 30% by mass, sulfur content 1.4% by mass

[0106] The emulsifiers (including fatty acids as precursors) used in the examples and comparative examples are listed below. A: Sodium alkyl (C10-16) benzenesulfonate (manufactured by NOF Corporation, trade name "Newlex R", solid content concentration 50% by mass) B: Sodium N-acylmethyl taurate (manufactured by NOF Corporation, trade name "Diapon S", solid content concentration 13% by mass) C: Sodium polyoxyalkylene disulfonate (manufactured by Nippon Nyukazai Co., Ltd., trade name "Newcol 240", solid content concentration 30% by mass) D: Sodium N-lauroylmethyl alanine (manufactured by NOF Corporation, trade name "Softilt AS-L", solid content concentration 30% by mass) E: Sodium lauryl sulfate (manufactured by Tokyo Chemical Industry Co., Ltd., reagent, solid content concentration 97% by mass) F: Sodium polyoxyethylene C12,14 alkyl ether sulfate (manufactured by NOF Corporation, trade name "Persoft EF", solid content concentration 25% by mass) G: Lauryl dimethylaminoacetic acid betaine (manufactured by NOF Corporation, trade name "Nissan Anon BL", solid content concentration 35% by mass) H: Oleic acid (manufactured by NOF Corporation, trade name "Extra Olein") I: Myristic acid (manufactured by Kishida Chemical Co., Ltd., reagent, solid content concentration 99% by mass) J: Lauric acid (manufactured by Tokyo Chemical Industry Co., Ltd., reagent, solid content concentration 98% by mass)

[0107] The parts by mass of each emulsifier in the examples and comparative examples are values ​​relative to 100 parts by mass of chlorosulfonated polyolefin (specifically, chlorosulfonated polyethylene) in the chlorosulfonated polyolefin latex. The number of added parts [phr] (per hundred rubber) in Table 1 indicates this value.

[0108] The emulsifier concentrations (solids concentrations) of the above-mentioned emulsifier products vary, and the values ​​in parts by mass of each emulsifier in the examples are calculated based on the amount of emulsifier converted based on the solids concentration. For example, as described below, in Example 1, 3.14 g of a 50% by mass solids alkyl (C10-16) benzenesulfonate product (Newrex®) was used as the first agent for 37.8 g of chlorosulfonated polyethylene. As described above, the solids concentration of Newrex® is 50% by mass, so the phr of the alkyl (C10-16) benzenesulfonate in this case is calculated as 3.14 x 0.5 / 37.8 x 100 = 4.16.

[0109] In addition, in Table 1, the column for second agent contains the notation "+KOH" in addition to emulsifier products H, I, and J. This indicates the fatty acid salt obtained by adding KOH to each of the fatty acids H to J, and phr also indicates the parts by mass of the fatty acid salt relative to 100 parts by mass of chlorosulfonated polyolefin (specifically, chlorosulfonated polyethylene).

[0110] <Evaluation Method> The chlorosulfonated polyethylene latex and coating obtained in each Example and Comparative Example were evaluated by the following method. (Mean Particle Size Measurement) The mean particle size of the emulsion and latex was measured using a laser diffraction particle size analyzer (Shimadzu Corporation, trade name "SALD-2300"). The mean particle size here is the volume-based median particle size calculated by assuming that particles to be measured that exhibit the same diffraction and scattering light pattern as a sphere with a diameter of 1 μm are 1 μm regardless of their shape. (Stability Evaluation) During the latex production process and after leaving the latex standing at 25°C for one month, the following criteria were met: ○: Almost no agglomerates were observed visually; △: Agglomerates were observed after leaving the latex standing at 25°C for one month; and ×: A large amount of agglomerates were observed during the production process. (Evaluation of Coagulation) A film thickness of 0.1 mm or more was deemed to have coagulated; ○: A film thickness of less than 0.1 mm was deemed not to have coagulated; ×: A film thickness of less than 0.1 mm was deemed not to have coagulated. (Measurement of film thickness) The dip-formed body was divided into approximately three parts in the longitudinal direction, and the thickness was measured near the center of gravity of three parts (three rectangles) at the top, middle, and bottom, and the average of the entire thicknesses was taken as the thickness of the dip-formed body.

[0111] Example 1 (Latex Production) 37.8 g of chlorosulfonated polyethylene (manufactured by Tosoh Corporation under the trade name "TOSO-CSM," product number TS-320) and 232.2 g of toluene were placed in a 500 mL separable flask and dissolved by stirring at 70°C for 6 hours. 0.39 g of oleic acid (manufactured by NOF Corporation under the trade name "Extra Olein") was added thereto to prepare an organic solvent solution. 3.14 g of sodium alkylbenzenesulfonate (manufactured by NOF Corporation under the trade name "Newlex R") and 0.16 g of potassium hydroxide (manufactured by Kanto Chemical Co., Inc., reagent) were dissolved in 159.45 g of water to prepare an aqueous solution.

[0112] The aqueous solution was added to the organic solvent solution, and the mixture was stirred and mixed for 12 minutes using a homomixer (trade name "TK Homomixer M" manufactured by Primix Corporation) to obtain an emulsion. The rotation speed during stirring and mixing was set to 12,000 rpm. The obtained emulsion was heated to 55°C under a reduced pressure of 20 kPa to distill off toluene, and then concentrated to a solids concentration of 40% using an ultrafilter (ultrafiltration membrane: flat membrane type, molecular weight cutoff 200,000, material: polysulfone) to obtain a chlorosulfonated polyethylene latex. The solids concentration was determined by drying a part of the obtained latex at 130°C for 2 hours to remove water, and then measuring the mass of the residue.

[0113] (Preparation of Dip-Forming Composition) To the chlorosulfonated polyethylene latex, 3 parts by mass, in terms of solid content, of an aqueous sodium dibutyldithiocarbamate solution (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name "Noccela TP") and 10 parts by mass of tripropylene glycol monomethyl ether (manufactured by Nippon Nyukazai Co., Ltd., trade name "Methylpropylene Triglycol") were added, and the mixture was stirred until homogeneous, to obtain a dip-forming composition.

[0114] (Production of Dip-Molded Article) A ceramic mold (boat-shaped, 10 cm long x 1.5 cm wide x 1 cm deep) was immersed in a 35% by mass aqueous solution of calcium nitrate for 5 seconds and dried in a 120°C air dryer for 5 minutes. The ceramic mold was then immersed in the dip-molding composition for 30 seconds to adhere the rubber component to the ceramic mold, and then removed from the dip-molding composition. The ceramic mold was dried in a 100°C air dryer for 20 minutes and then further heated at 160°C for 20 minutes to perform vulcanization. After cooling to room temperature, the coating was peeled off from the ceramic mold, and the film thickness of the resulting dip-molded article was measured.

[0115] Examples 2 to 11, Comparative Examples 1 to 5 The same procedures as in Example 1 were carried out except that the types and amounts of rubbers and emulsifiers shown in Table 1 were used, and the obtained latexes and films were evaluated.

[0116] The results are also shown in Table 1.

[0117]

[0118] Furthermore, an investigation was conducted under the same conditions as in Example 1, except that the emulsifier used as the first agent was changed to each of the following components. As a result, a latex could be prepared (i.e., no coagulation of rubber occurred), and there was no case in which both the stability and the coagulation properties were evaluated as good. The emulsifiers used as the first agent are summarized below by the results.

[0119] [Rubber coagulated and latex could not be obtained] Potassium rosinate Polystyrene / maleic anhydride half ester ammonium Sodium lauryl sulfate Sodium N-lauroylmethylalanine Disodium alkyl sulfosuccinate [Stability evaluation: Poor] Sodium dioctyl sulfosuccinate Sodium allyl alkyl sulfosuccinate Sodium naphthalene sulfonate-formaldehyde condensate Potassium oleate [Stability evaluation: Good, but coagulation evaluation: Poor] Lauryl dimethylaminoacetic acid betaine Sodium polyoxyethylene lauryl sulfate

[0120] According to one aspect of the present disclosure, a chlorosulfonated polyolefin latex can be obtained that is excellent in stability and can be applied to a general coagulation dipping method. By using the latex, dip-molded articles can be efficiently produced. Furthermore, the present disclosure is useful from the viewpoint of environmental protection, since dip-molded articles such as gloves can be obtained without using organic solvents during dip molding.

Claims

1. A chlorosulfonated polyolefin latex comprising: an aqueous dispersion medium; a chlorosulfonated polyolefin; at least one compound (first agent) selected from the group consisting of alkylbenzene sulfonate, polyoxyalkylene disulfonate, and taurine salt; and a fatty acid salt (second agent).

2. The alkylbenzene sulfonate is a C8-18 alkylbenzene sulfonate, the polyoxyalkylene disulfonate is a salt of an ester in which hydroxy groups at both ends of a polyalkylene glycol are sulfated, and the polyalkylene glycol is a polymer of a C2-4 alkylene glycol, and the taurine salt is a compound represented by the formula: R-N(CH 3 )-(CH 2 ) 2 -SO 3 M (wherein R represents a cocoyl group or an acyl group having 8 to 18 carbon atoms, and M represents an alkali metal (preferably sodium or potassium), ammonium (NH 4 ), or triethanolammonium (NH(CH 2 CH 2 O.H. 3 2. The latex according to claim 1 , wherein the compound is represented by the formula:

3. The latex according to claim 1 or 2, wherein the mass ratio of the first agent to the second agent is 0.5 to 5.

4. The latex according to claim 1 or 2, wherein the total amount of the first agent and the second agent is 3 to 8 parts by mass per 100 parts by mass of chlorosulfonated polyolefin.

5. The latex according to claim 1 or 2, wherein the second agent is at least one selected from the group consisting of laurate, myristate, and oleate.

6. A method for producing a chlorosulfonated polyolefin latex, comprising: an emulsification step of preparing an emulsion by dispersing a chlorosulfonated polyolefin dissolved in an organic solvent in an aqueous dispersion medium in the presence of at least one compound (first agent) selected from the group consisting of alkylbenzene sulfonates, polyoxyalkylene disulfonates, and taurine salts, and a fatty acid salt (second agent); and a desolvation step of removing the organic solvent from the emulsion.

7. A chlorosulfonated polyolefin emulsion composition comprising: at least one compound selected from the group consisting of alkylbenzenesulfonates, polyoxyalkylene disulfonates, and taurine salts; and a fatty acid salt.

8. A dip-molding composition comprising the chlorosulfonated polyolefin latex according to claim 1 or 2.