Metal fiber structure

MYPI2025006092A0Undetermined Publication Date: 2024-10-05TOMOEGAWA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025006092
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-05
Filing Date
2024-04-04
Publication Date
2024-10-05

AI Technical Summary

Technical Problem

Conventional metal fiber structures lack flexibility and balanced physical properties, as they are typically sintered together using solid core portions, limiting their application in materials requiring both flexibility and strength.

Method used

A metal fiber structure where multiple metal fibers are bound together using a porous metal body, with a space factor between 20% to 80% and an average fiber diameter of 10 μm to 3000 μm, allowing for enhanced flexibility and specific resistance, and Young's modulus of 150 to 450 GPa, enabling improved stress relaxation and strength.

Benefits of technology

The metal fiber structure exhibits excellent flexibility, specific resistance, and strength, making it suitable for various applications such as filters, heat-resistant materials, conductive materials, and electrostatic shielding, while maintaining a balanced range of physical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025006092_DRAWING_001
    Figure PI2025006092_DRAWING_001
  • Figure PI2025006092_DRAWING_002
    Figure PI2025006092_DRAWING_002
Patent Text Reader

Abstract

Provided is a metal fiber structure (1) in which a plurality of metal fibers (2) are bonded to each other, the metal fiber structure (1) including a porous metal body (3) that is in contact with the plurality of metal fibers (2) to connect the plurality of metal fibers (2). Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Metal fiber structure

[0001] The present invention relates to a metal fiber structure.

[0002] Various metal fiber sheets have been known in the past. For example, Japanese Patent Laid-Open Publication No. 7-258706 (JPH7-258706A) discloses a method for producing a sintered metal fiber sheet used as a filter material, a heat-resistant material, a conductive material, a static electricity shielding material, etc.

[0003] In the method for producing a sintered metal fiber sheet disclosed in Japanese Patent Laid-Open Publication No. 7-258706, a slurry consisting only of metal fibers is formed using a specific wire mesh, and porous flexible ceramic sheets are provided on both sides of the wire mesh to form a three-layer structure. The resulting structure is then dried and sintered in an argon gas or hydrogen gas atmosphere at a temperature below the melting point of the metal fibers to produce a sintered metal fiber sheet. In this case, the solid cores of the metal fibers are sintered together. However, a new metal fiber structure that differs from this structure is desired.

[0004] The present invention has been made in consideration of the above points, and has an object to provide a metal fiber structure with a new structure.

[0005] The metal fiber structure of the present disclosure is a metal fiber structure in which a plurality of metal fibers are bonded together, and includes a metal porous body that contacts the plurality of metal fibers to connect the plurality of metal fibers.

[0006] In the metal fiber structure of the present disclosure, the metal porous body may be disposed between the metal fibers.

[0007] The metal fiber structure of the present disclosure may have a structure in which the metal fibers are covered with the metal porous body.

[0008] In the metal fiber structure of the present disclosure, the metal space factor in the cross section of the porous metal body may be within a range of 20% to 80%.

[0009] In the metal fiber structure of the present disclosure, the space factor of the metal in the cross section of the metal fiber structure may be within a range of 30% to 80%.

[0010] In the metal fiber structure of the present disclosure, the metal fibers may have an average fiber diameter in the range of 10 μm to 3000 μm.

[0011] The metal fiber structure of the present disclosure may have a thickness in the range of 0.01 mm to 50.0 mm.

[0012] In the metal fiber structure of the present disclosure, the material of the metal porous body has a specific resistance of 1.5×10 at 20° C. -8 Ω m to 3.0 x 10 -8 It may contain a metal with a resistivity of Ω·m.

[0013] In the metal fiber structure of the present disclosure, the material of the metal fiber has a specific resistance of 1.5×10 at 20° C. -8 Ω m to 3.0 x 10 -8 It may contain a metal with a resistivity of Ω·m.

[0014] In the metal fiber structure of the present disclosure, the material of the metal porous body may contain a metal having a Young's modulus of 150 to 450 GPa.

[0015] In the metal fiber structure of the present disclosure, the material of the metal fibers may contain a metal having a Young's modulus of 150 to 450 GPa.

[0016] Fig. 1 is a conceptual diagram of a metal fiber structure according to an embodiment of the present disclosure. Fig. 2 is another conceptual diagram of a metal fiber structure according to an embodiment of the present disclosure. Fig. 3 is an exemplary micrograph of a metal fiber structure according to an embodiment of the present disclosure. Fig. 4 is a micrograph showing a cross section of a metal fiber structure of Example 1. Fig. 5 is a micrograph showing a cross section of a metal fiber structure of Comparative Example 1.

[0017] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. Figures 1 and 2 are conceptual diagrams of a metal fiber structure according to an embodiment of the present disclosure. Figure 3 is an exemplary micrograph of a metal fiber structure according to an embodiment of the present disclosure (scanning electron microscope manufactured by JEOL Ltd., 1000x magnification).

[0018] 1 and 2 , the metal fiber structure 1 according to the present embodiment includes a plurality of metal fibers 2 and a metal porous body 3 in contact with the metal fibers 2, and the metal fibers 2 are connected and bound together by the metal porous body 3. In this specification, the phrase "bound" between metal fibers refers to a state in which the metal fibers are physically fixed together, and the portions where the metal fibers are physically fixed are also referred to as "bonded portions." In the metal fiber structure 1, the metal fibers 2 are indirectly fixed together via the metal porous body 3 (i.e., bonded portions) ( FIG. 1 , etc.).

[0019] As will be described later, compared to when no metal porous body is present (for example, when the metal fibers are connected to each other via a solid material), the metal porous body 3 is in contact with the metal fibers 2, allowing the metal fiber structure 1 as a whole to exhibit excellent flexibility (stress relaxation, pliability, bendability), etc.

[0020] In the metal fiber structure 1, the structure in which the metal porous body 3 is connected to the metal fibers 2 is not particularly limited, and the metal fibers 2 may be covered with the metal porous body 3 (FIGS. 1 and 2), or the metal porous body 3 may be disposed partially between the metal fibers 2. In other words, the space factor of the entire metal fiber structure 1 can take various values ​​depending on the relative position of the metal porous body 3 with respect to the metal fibers 2.

[0021] Specifically, the space factor of the metal (metal of the metal fibers 2 and the metal porous body 3) in the cross section of the metal fiber structure 1 is preferably in the range of 30% to 80%, and more preferably in the range of 40% to 70%. The lower the space factor of the metal fiber structure 1, the better the flexibility tends to be, and the higher the space factor of the metal fiber structure 1, the better the other physical properties such as resistivity or strength tend to be. Within the above ranges, both flexibility and other physical properties can be achieved.

[0022] The term "space factor" refers to the proportion of solid portions (metal fibers, metal particles, etc.) present relative to a certain area of ​​the metal fiber structure 1. The metal fiber structure 1 is cut vertically, and the cross section obtained is examined using a scanning electron microscope (SEM) and known image analysis software, and the average value of the values ​​obtained can be determined by the following formula: Space factor (%) = Area occupied by metal in metal fiber structure 1 / (Area occupied by metal in metal fiber structure 1 + Area occupied by non-metal in metal fiber structure 1) × 100

[0023] The dimensions of the metal fiber structure 1 are not particularly limited as they are adjusted appropriately depending on the application, but the thickness of the metal fiber structure 1 is preferably within the range of 0.01 mm to 50.0 mm, and more preferably within the range of 0.01 mm to 20.0 mm. Within these ranges, flexibility and other physical properties such as resistivity and strength can be achieved at the same time. Note that the surface of the metal fiber structure 1 may be uneven (surface roughness) due to individual differences, arrangement, or manufacturing process of the metal fibers 2, which are components of the metal fiber structure 1.

[0024] (Metal Fibers 2) The metal fibers 2 are fibrous metal members. The metal fibers 2 are preferably sintered. By sintering the metal fibers 2, the thermal conductivity and homogeneity of the metal fiber structure 1 tend to be stable.

[0025] The average fiber diameter of the metal fibers 2 is preferably in the range of 10 μm to 3000 μm, more preferably in the range of 10 μm to 200 μm, and even more preferably in the range of 10 μm to 50 μm. The smaller the average fiber diameter of the metal fibers 2, the better the flexibility of the resulting metal fiber structure 1 tends to be. The larger the average fiber diameter of the metal fibers 2, the better the resistivity or strength of the resulting metal fiber structure 1 tends to be. Within the above ranges, both flexibility and other physical properties can be achieved. Note that the "average fiber diameter" in this specification refers to the average area diameter (e.g., the average value of 20 fibers) calculated by calculating the cross-sectional area of ​​the metal fibers 2 in any cross section perpendicular to the longitudinal direction of the metal fibers 2 imaged with a microscope (e.g., using known software) and calculating the diameter of a circle having the same area as the cross-sectional area. Furthermore, the metal fibers 2 may become rounded due to sintering. In this case, the average fiber diameter of the metal fibers 2 is calculated in the same manner.

[0026] The average fiber length of the metal fibers 2 is not particularly limited, but is preferably in the range of 1 mm to 50 mm, and more preferably in the range of 1 mm to 20 mm. For example, when the metal fiber structure 1 is used as a metal fiber nonwoven fabric, a shorter average fiber length of the metal fibers 2 is preferable because this makes it easier to improve the homogeneity of the metal fiber nonwoven fabric. In this specification, the "average fiber length" refers to the average value obtained by measuring 20 fibers under a microscope.

[0027] The material of the metal fiber 2 has a specific resistance of 1.5 × 10 at 20 ° C. -8 Ω m to 3.0 x 10 -8 The metal fiber structure 1 may contain metal fibers 2 made of two or more of these metals.

[0028] The material of the metal fibers 2 may also contain a metal having a Young's modulus (23°C) of 150 to 450 GPa. Examples of such metals include iron, nickel, chromium, beryllium, tungsten, molybdenum, and alloys thereof. The metal fiber structure 1 may contain two or more of such metals as the metal fibers 2.

[0029] (Metal Porous Body 3) As described above, in the metal fiber structure 1, the metal porous body 3 is a binding portion that binds the metal fibers 2 together.

[0030] The space factor of the metal in the cross section of the metal porous body 3 is preferably in the range of 20% to 80%, and more preferably in the range of 30% to 70%. The lower the space factor of the metal porous body 3, the better the flexibility of the resulting metal fiber structure 1 tends to be, and the higher the space factor of the metal porous body 3, the better the resistivity or strength of the resulting metal fiber structure 1 tends to be. Within the above ranges, flexibility and other physical properties can be achieved at the same time.

[0031] The space factor of the metal porous body 3 can also be determined as an area ratio using an electron microscope (SEM) and known image analysis software. Specifically, the space factor of the metal porous body 3 can be determined by averaging values ​​obtained from cross-sectional samples (e.g., 20 samples) of the metal porous body 3 in the SEM image using the following formula: Space factor (%) = Area occupied by the metal in the metal porous body 3 / (Area occupied by the metal in the metal porous body 3 + Area occupied by parts other than the metal porous body 3) × 100

[0032] The material of the metal porous body 3 is a metal having a specific resistance of 1.5×10 at 20° C. -8 Ω m to 3.0 x 10 -8 Examples of such metals are given above.

[0033] Furthermore, the material of the metal porous body 3 may contain a metal having a Young's modulus (23° C.) of 150 to 450 GPa. Examples of such metals are as described above.

[0034] The metal fibers 2 and the metal porous body 3 are preferably made of copper, silver, or aluminum, since the resulting metal fiber structure 1 will exhibit excellent flexibility and resistivity. The metal fibers 2 and the metal porous body 3 are preferably made of stainless steel, tungsten, nickel, or iron, since the resulting metal fiber structure 1 will exhibit excellent flexibility and strength. The materials of the metal porous body 3 and the metal fibers 2 may be the same or different.

[0035] (Method and Use of Metal Fiber Structure 1) In a method for producing the metal fiber structure 1, for example, first, a slurry solution containing metal particles or metal fibers that will become the metal porous body 3 is prepared. Next, this solution is applied to metal fibers 2 prepared as a substrate, and dried at a predetermined temperature. Here, it is necessary to adjust the drying heating temperature according to the melting point of the metal used so that the metal porous body 3 formed on the metal fibers 2 does not melt (liquefy). From the structures obtained in this way, the metal fiber structure 1 according to the present disclosure can be obtained by appropriately separating and selecting based on the structure in which the metal porous body 3 is connected to the metal fibers 2 and the above-mentioned characteristics (space factor, diameter, thickness, etc.). The metal particle diameter and the diameter of the metal fibers are preferably 0.001 μm to 10.0 μm.

[0036] Due to its flexibility, the metal fiber structure 1 is a structure that can be molded into a plate, sheet, or other shape. Depending on the application, the metal fiber structure 1 may be further coated with a resin film. The thickness of the resin film may be 1 to 1000 times the thickness of the metal fiber structure 1, and the resin film may be made of a known resin material that is insulating and flexible. Examples of the resin film include acrylic resin, polyvinylpyrrolidone resin, polyester resin, polypropylene resin, fluororesin, polyimide resin, and silicone resin. Furthermore, the metal fiber structure 1 can be used as a filter material, heat-resistant material, conductive material, heat-dissipating material, heat-transfer material, or static electricity-shielding material, depending on the material (properties) of the metal fibers 2.

[0037] The metal fiber structure 1 of the present embodiment having the above-described configuration is a metal fiber structure 1 in which a plurality of metal fibers 2 are bonded together, and includes a metal porous body 3 that contacts the plurality of metal fibers 2 to connect the plurality of metal fibers 2. Unlike the conventional technology in which the entangled portions of solid metal fibers are melted by sintering to join the metal fibers, such a metal fiber structure 1 allows the plurality of metal fibers 2 to be connected via the metal porous body 3, as described above, and therefore allows the metal fiber structure 1 as a whole to exhibit excellent flexibility, etc.

[0038] Furthermore, in the metal fiber structure 1 of the present embodiment, as described above, the metal porous body 3 may be disposed between the metal fibers 2. Alternatively, the metal fiber structure 1 may have a structure in which the metal fibers 2 are covered with the metal porous body 3.

[0039] In the metal fiber structure 1 of this embodiment, the space factor of the metal in the cross section of the metal porous body 3 may be in the range of 20% to 80%. In this way, the flexibility and other physical properties of the metal fiber structure 1 can be more suitably achieved at the same time.

[0040] Furthermore, in the metal fiber structure 1 of this embodiment, the space factor of the metal in the cross section of the metal fiber structure 1 may be in the range of 30% to 80%. In this way, it is possible to more suitably achieve both flexibility and other physical properties of the metal fiber structure 1.

[0041] In the metal fiber structure 1 of the present embodiment, the average fiber diameter of the metal fibers 2 may be in the range of 10 μm to 3000 μm. In this way, the flexibility of the metal fiber structure 1 can be suitably achieved while also achieving other physical properties.

[0042] The thickness of the metal fiber structure 1 of this embodiment may be in the range of 0.01 mm to 50.0 mm, so that the flexibility of the metal fiber structure 1 and other physical properties can be suitably achieved at the same time.

[0043] In the metal fiber structure 1 of the present embodiment, the material of the metal porous body 3 has a specific resistance of 1.5×10 at 20° C. -8 Ω m to 3.0 x 10 -8The metal fiber structure 1 may contain a metal having a resistivity of Ω·m. In this way, it is possible to obtain a metal fiber structure 1 having excellent flexibility and resistivity.

[0044] In the metal fiber structure 1 of the present embodiment, the material of the metal porous body 3 may contain a metal having a Young's modulus of 150 to 450 GPa. In this way, a metal fiber structure 1 having excellent flexibility and strength can be obtained.

[0045] In the metal fiber structure 1 of the present embodiment, the material of the metal fibers 2 has a specific resistance of 1.5×10 at 20° C. -8 Ω m to 3.0 x 10 -8 The metal fiber structure 1 may contain a metal having a resistivity of Ω·m. In this way, it is possible to obtain a metal fiber structure 1 having excellent flexibility and resistivity.

[0046] In the metal fiber structure 1 of the present embodiment, the material of the metal fibers 2 may contain a metal having a Young's modulus of 150 to 450 GPa. In this way, a metal fiber structure 1 having excellent flexibility and strength can be obtained.

[0047] The metal fiber structure 1 according to this embodiment is not limited to the above-mentioned aspects and combinations.

[0048] For example, the metal porous body 3 may thinly cover the surface of each metal fiber 2, and more (thicker) metal porous body 3 may be present at the connection points between the metal fibers 2 as binding portions of the metal fibers 2 (FIGS. 2 and 3). In other words, the amount (volume) of the metal porous body 3 in the metal fiber structure 1 may vary depending on the position of the metal fiber 2.

[0049] Furthermore, in the metal fiber structure 1 of this embodiment, if the materials of the metal fibers 2 and the metal porous body 3 contain a metal with high thermal conductivity, it is possible to obtain a metal fiber structure 1 with excellent flexibility and thermal conductivity. Examples of metals with high thermal conductivity include silver, copper, gold, aluminum, and alloys of each of these.

[0050] Furthermore, a component other than metal may be used as part of the metal fiber 2, and such a component may be covered with the above-mentioned metal component.

[0051] The present disclosure will be described in more detail below using examples and comparative examples.

[0052] Examples 1 to 16 Metal fiber structures were produced using the materials shown in Tables 1 and 2. That is, a slurry solution (solid content: 50%, solvent: glycerin) containing copper particles (average primary particle diameter: 25 nm, manufactured by Ioritec Co., Ltd.) was applied to copper fibers used as substrates shown in Tables 1 and 2, and N 2 The metal fiber structure was heated in an atmosphere at 250° C. for 1 hour. FIG. 4 is a photomicrograph (3000x magnification) showing the cross section of the metal fiber structure of Example 1.

[0053] Example 17 A metal fiber structure was produced using the materials shown in Table 2. That is, a slurry solution (solid content: 50%, solvent: glycerin) containing copper particles (average primary particle diameter: 25 nm, manufactured by Ioritec Co., Ltd.) was applied to an aluminum fiber substrate shown in Table 2, and N 2 The mixture was heated in an atmosphere at 250° C. for 1 hour.

[0054] Examples 18 to 33 Metal fiber structures were produced using the materials shown in Tables 3 and 4. That is, a slurry solution (solid content: 50%, solvent: glycerin) containing stainless steel SUS316L particles (average primary particle diameter 70 nm, manufactured by Ioritec Co., Ltd.) was applied to stainless steel fibers (SUS304) used as substrates shown in Tables 3 and 4, and N 2 The mixture was heated in an atmosphere at 250° C. for 1 hour.

[0055] Example 34 A metal fiber structure was produced using the materials shown in Table 4. That is, a slurry solution (solid content: 50%, solvent: glycerin) containing stainless steel SUS316L particles (average primary particle diameter: 70 nm, manufactured by Ioritec Co., Ltd.) was applied to a tungsten fiber substrate shown in Table 4, and N 2 The mixture was heated in an atmosphere at 250° C. for 1 hour.

[0056] <Comparative Examples 1 and 2> For the same metal fibers as the copper fibers or stainless steel fibers used in Examples 1 and 18, N 2The metal fiber structures were subjected to a heat treatment at 250° C. for 1 hour in an atmosphere to obtain metal fiber structures of Comparative Examples 1 and 2. Fig. 5 is a photomicrograph (3000x magnification) showing a cross section of the metal fiber structure of Comparative Example 1.

[0057] <Evaluation> (Specific resistance (volume resistivity)) The specific resistance (volume resistivity) of the metal fiber structures of Examples 1 to 17 and Comparative Example 1 was measured and evaluated as follows. The specific resistance (volume resistivity) of each metal fiber structure was measured by the four-terminal method using a Loresta GP, a low resistivity meter manufactured by Nitto Seiko Analytech. The measurement samples were cut to a given size according to the measurement range, with a constant thickness. This value was 1.7 × 10 -8 Greater than Ω m, 3.4 x 10 -8 If it is Ω·m or less, it is considered excellent (◎), and if it is 3.4×10 -8 Greater than Ω m, 5.1 x 10 -8 Ω·m or less: Good (○), 5.1×10 -8 Greater than Ω m, 6.8 x 10 -8 Ω·m or less: Acceptable (△), 6.8×10 -8 If it was larger than Ω·m, it was judged as defective (×).

[0058] (Stress Relaxation Property) The stress relaxation property (flexibility) of the metal fiber structures of Examples 1 to 34 and Comparative Examples 1 and 2 was measured and evaluated as follows. Each metal fiber structure except for Examples 15 and 32 was cut into a doughnut shape (outer diameter 50 mmφ, inner diameter 30 mmφ) with a thickness reduced to approximately 1 / 10 of the original size (for example, 1.1 mm in the case of Example 1). A doughnut-shaped alumina plate (outer diameter 55 mmφ, inner diameter 35 mmφ, thickness 0.5 mm) with a purity of 95% was prepared, and a two-component curing epoxy adhesive (1500, manufactured by Cemedine Co., Ltd.) was uniformly applied to one side of the alumina plate to a thickness of 10 μm. The doughnut-shaped metal fiber structure or the doughnut-shaped metal fiber structure of Examples 15 and 32 was then attached to the surface of the alumina plate coated with the two-component curing epoxy adhesive, and the resulting mixture was left standing for 24 hours in an environment of 23°C and 65% RH to obtain a test specimen. The obtained test piece was placed in a thermostatic oven (PV-212, manufactured by Espec Corporation) at 150°C, and the amount of warping of the test piece during heating was measured to evaluate the stress relaxation property. When the amount of warping was less than 0.05 mm, it was rated as excellent (◎), when it was 0.05 mm or more and less than 0.20 mm, it was rated as good (◯), when it was 0.20 mm or more and less than 0.50 mm, it was rated as fair (△), and when it was 0.50 mm or more, it was rated as poor (×).

[0059] (Strength) The strength of the metal fiber structures of Examples 18 to 34 and Comparative Example 2 was measured and evaluated as follows. Each metal fiber structure was cut into a No. 4 test piece in accordance with JIS Z2241, and a tensile test was performed using a tensile tester (Shimadzu Corporation, UH-1000kNI). The obtained Young's modulus (23°C) value was taken as the strength. When the Young's modulus value was 20.0 GPa or more, it was rated as excellent (◎); when it was 15.0 GPa or more and less than 20.0 GPa, it was rated as good (◯); when it was 10.0 GPa or more and less than 15.0 GPa, it was rated as fair (△); and when it was less than 10.0 GPa, it was rated as poor (×).

[0060] The above results and overall evaluation are shown in Tables 1 to 4. In making the overall evaluation, if two individual items were rated as ◎, the overall evaluation was rated as "excellent (◎)." If there was one or more individual items rated as 〇 and no △ or ×, the overall evaluation was rated as "good (○)." If even one individual evaluation was △ and the other evaluations were ◎ or 〇, the overall evaluation was rated as "fair (△)." Furthermore, if even one individual evaluation was ×, the overall evaluation was rated as "poor (×)."

[0061]

[0062]

[0063]

[0064]

[0065] As shown in Tables 1 to 4 above, it was confirmed that the metal fiber structures 1 according to Examples 1 to 34 have a (new) structure different from conventional structures (see Figs. 4 and 5), are excellent in flexibility (stress relaxation property), and are also excellent in resistivity and strength compared to the metal fiber structures of Comparative Examples 1 and 2. Unlike Comparative Examples 1 and 2, which were poor in overall evaluation, it was found that all Examples were able to achieve both resistivity or strength and stress relaxation property.

[0066] Furthermore, when comparing Examples 8-9 with Examples 10-11, and Examples 25-26 with Examples 27-28, it was found that when the space factor of the metal porous body 3 was within the range of 20% to 80%, the overall evaluation was even better, and resistivity or strength and stress relaxation properties could be more suitably achieved at the same time.

[0067] Furthermore, compared with Examples 2 and 3, Examples 4 to 7 have an increased lower limit of resistivity and a decreased upper limit, and the upper limit of stress relaxation also decreases, indicating that these properties are exhibited in a more balanced manner. Furthermore, compared with Examples 19 and 20, Examples 21 to 24 have an increased lower limit of strength and a decreased upper limit, and the upper limit of stress relaxation also decreases, indicating that these properties are exhibited in a more balanced manner. Therefore, it was found that when the space factor of the metal fiber structure 1 is within the range of 30% to 80%, it is possible to more suitably achieve both resistivity or strength and stress relaxation.

[0068] Furthermore, when Example 12 is compared with Examples 13 and 14, and Example 29 is compared with Examples 30 and 31, it is found that when the average fiber diameter of the metal fibers 2 is within the range of 10 μm to 3000 μm, the overall evaluation is further improved, and the resistivity or strength and the stress relaxation property can be more suitably achieved at the same time.

[0069] Furthermore, from the results of Examples 15 to 16 and Examples 32 to 33, it can be seen that when the thickness of the metal fiber structure 1 is within the range of 0.01 mm to 50.0 mm, both the individual evaluation and the overall evaluation are "excellent" or "good," and it can be seen that resistivity or strength and stress relaxation can be more suitably balanced.

[0070] As described above, the metal fiber structure of the present disclosure is a metal fiber structure in which a plurality of metal fibers are bonded together, and is provided with a metal porous body that connects the plurality of metal fibers by coming into contact with the plurality of metal fibers, and has excellent physical properties such as flexibility.

Claims

1. A metal fiber structure in which a plurality of metal fibers are bonded together, comprising a metal porous body that contacts the plurality of metal fibers to connect the plurality of metal fibers.

2. The metal fiber structure according to claim 1, wherein the metal porous body is disposed between the metal fibers.

3. The metal fiber structure according to claim 1, wherein the metal fibers are covered with the metal porous body.

4. A metal fiber structure according to any one of claims 1 to 3, wherein the metal space factor in the cross section of the metal porous body is within the range of 20% to 80%.

5. A metal fiber structure according to any one of claims 1 to 4, wherein the metal space factor in the cross section of the metal fiber structure is within the range of 30% to 80%.

6. The metal fiber structure according to any one of claims 1 to 5, wherein the average fiber diameter of the metal fibers is within the range of 10 µm to 3000 µm.

7. The metal fiber structure according to any one of claims 1 to 6, having a thickness in the range of 0.01 mm to 50.0 mm.

8. The material of the metal porous body has a resistivity of 1.5×10 at 20° C. -8 Ω m to 3.0 x 10 -8 The metal fiber structure according to claim 1 , comprising a metal having a modulus of Ω·m.

9. The material of the metal fiber has a resistivity of 1.5 x 10 at 20°C. -8 Ω m to 3.0 x 10 -8 The metal fiber structure according to claim 1 , comprising a metal having a modulus of Ω·m.

10. A metal fiber structure according to any one of claims 1 to 9, wherein the material of the metal porous body contains a metal having a Young's modulus of 150 to 450 GPa.

11. A metal fiber structure according to any one of claims 1 to 10, wherein the material of the metal fibers comprises a metal having a Young's modulus of 150 to 450 GPa.