Hot-dip plated steel material
Patent Information
- Application Number
- MYPI2025006167
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional Zn-Al-Mg-based plating layers have insufficient research on how to adjust the ionization tendency of the plating layer to effectively suppress white rust at the initial stage of corrosion, which affects the appearance and corrosion resistance of hot-dip plated steel materials.
A hot-dip plated steel material with a specific chemical composition and microstructural configuration, including a Zn-Al-Mg alloy layer and an Al-Fe interfacial alloy layer, where Cu and Ag are incorporated to enhance the corrosion potential of the Zn-Al(β) phase, reducing the potential difference and thereby minimizing white rust formation.
The solution effectively suppresses white rust at the initial stage of corrosion, improving the appearance and corrosion resistance of the steel material by increasing the corrosion potential of the Zn-Al(β) phase and reducing the area fraction of white rust, ensuring a high-quality metallic luster and enhanced durability.
Smart Images

Figure PI2025006167_DRAWING_001
Abstract
Description
Hot-dip galvanized steel
[0001] This application claims priority to Japanese Patent Application No. 2023-067061, filed on April 17, 2023, the contents of which are incorporated herein by reference.
[0002] When steel materials are used for a long period of time, it is preferable to apply some kind of rust prevention treatment to the steel materials to make them resistant to corrosion. Hot-dip Zn plating is used as a means of inexpensively preventing rust on steel materials in various fields where rust prevention of steel materials is required, such as civil engineering, construction, and automotive fields.
[0003] From the viewpoint of corrosion prevention of the plating layer, suppressing the amount of white rust generated is an important issue. When a Zn-based plating layer corrodes, it reacts with oxygen in the atmosphere to produce corrosion products. Since white rust in the plating layer easily leads to deterioration of the appearance, it is preferable to prevent its generation as much as possible. Furthermore, once a corroded area is corroded, the surface area of the corrosion increases, and the corroded area becomes a starting point for further corrosion, accelerating the subsequent corrosion progression. Generally, Zn-based plating layers have a sacrificial corrosion protection effect, so even if scratches reaching the base steel or corrosion of the plating layer occur to a certain extent, this does not pose a major problem for the material. However, as mentioned above, the problem of deterioration of appearance due to white rust has been confirmed.
[0004] On the other hand, compared to such Zn-based plating layers, plating layers containing elements with a higher ionization tendency than Fe, such as Sn, Ni, and Cr, are called barrier-type coatings. Because they do not have a sacrificial corrosion protection effect against Fe, scratches or other defects are likely to result in fatal material defects. However, such barrier-type coatings can maintain a metallic luster for a long period of time, even for a certain period after production, allowing for a high-quality appearance that gives a minimal feeling of use. Therefore, it is believed that by adjusting the ionization tendency of Zn-based plating layers to bring them closer to the potential of Fe, it is possible to reduce the amount of white rust generated and improve the corrosion appearance.
[0005] For example, Patent Documents 1 and 2 describe Zn—Al—Mg-based plating layers that have been used in recent years as highly corrosion-resistant plating layers. These Zn—Al—Mg-based plating layers have improved designability and corrosion resistance through structural control, and further disclose techniques for improving corrosion resistance by adding elements to the plating layer or actively forming corrosion products.
[0006] International Publication No. WO 2019 / 230894 International Publication No. WO 2018 / 139619
[0007] However, in the conventional Zn—Al—Mg-based plating layers described in Patent Documents 1 and 2, the method of adding elements to the final plating layer and the method of controlling the ionization tendency have not been fully investigated, and the suppression of white rust that occurs in the early stages of corrosion has been insufficient from the viewpoints of improving appearance and suppressing the initiation of corrosion.
[0008] An object of one embodiment of the present invention is to provide a hot-dip plated steel material that can suppress the formation of white rust in the early stages of corrosion.
[0009] In order to solve the above problems, each aspect of the present invention employs the following configuration. [1] A hot-dip galvanized steel material according to one aspect of the present invention is a hot-dip galvanized steel material having a steel material and a coating layer disposed on a surface of the steel material, wherein the coating layer contains, in mass %, Al: more than 10.0% and less than 45.0%, Mg: 4.0% to 15.0%, Si: 0.01% to 2.0%, at least one of Cu: 0.03% to 5.0% and Ag: 0.03% to 6.0%, and further contains Sn: 0% to 0.7%, Bi: 0% to 0.3%, In: 0% to 0.3%, Ca: 0% to 0.6%, Y: 0% to 0.3%, La: 0% to 0.3%, Ce: 0% to 0.3%, Sr: 0% to 0.3%, Li: 0% or more, 0.3% or less, Ni: 0% or more, 1.0% or less, Cr: 0% or more, 0.5% or less, Mo: 0% or more, 0.3% or less, Sb: 0% or more, 0.25% or less, Pb: 0% or more, 0.25% or less, B: 0% or more, 0.5% or less, P: 0% or more, 0.5% or less, Ti: 0% or more, 0.25% or less, Co: 0% or more, 0.25% or less, V: 0% or more, 0.25% or less, Nb: 0% or more, 0.25% or less, Mn: 0% or more, 0.25% or less, Zr: 0% or more, 0.25% or less, W: 0% or more, 0.25% or less, Fe: 0% or more, 5.0% or less, the balance being Zn and impurities, The plating layer has a chemical composition in which the total content of Cu and Ag satisfies 0.03% or more and 6.0% or less, and in an element distribution profile obtained by quantitatively analyzing the plating layer from the surface toward the steel material by glow discharge optical emission spectrometry, when the thickness of the plating layer is t and the ratio of the total concentration of Cu concentration and Ag concentration to the Zn concentration in an internal region between a 1 / 3t position and a 2 / 3t position with respect to the surface of the plating layer is defined as CAZ, the maximum value CAZ of the CAZ max and the minimum value CAZ of the CAZ min satisfies the following formulas (1) to (3): max / CAZ min ≦1.20 … (1) 0.0005≦CAZ min …(2) CAZ max≦0.1000 ... (3) [2] The hot-dip plated steel material according to the above [1] may have an area ratio of β phase of 3% or more in a cross section along the thickness direction of the coating layer, and the concentrations of Al, Zn, Cu and Ag in the β phase may satisfy the following formula (4): 0.85≦[Al] / ([Zn]+[Cu]+[Ag])≦1.15 ... (4) where [Al], [Zn], [Cu] and [Ag] in formula (4) are respectively quantitative analysis values (at %) in the β phase by energy dispersive X-ray analysis. [3] The hot-dip plated steel material according to the above [1] or [2] may have an area ratio of β phase of 3% or more in a cross section along the thickness direction of the coating layer, and the concentrations of Al, Zn, Cu and Ag in the β phase may satisfy the following formula (4): 0.85≦[Al] / ([Zn]+[Cu]+[Ag])≦1.15 ... (4) 2 Within this range, 10 or more (Zn+Al)-(Cu+Ag) compounds having an average crystal grain size of 1 μm or more may be contained as intermetallic compound particles.
[0010] According to one embodiment of the present invention, it is possible to provide a plated steel material that is capable of suppressing the occurrence of white rust in the early stages of corrosion.
[0011] FIG. 1 is a graph showing an example of an element distribution profile, illustrating the results of a GDS analysis performed on a coating layer of a hot-dip coated steel material according to an embodiment of the present invention.
[0012] Hereinafter, a hot-dip plated steel material according to one embodiment of the present invention will be described. In this specification, the "%" used to indicate the content of each element in the chemical composition of the plating layer means "mass %" unless otherwise specified. Furthermore, a numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the lower and upper limits. Furthermore, when "greater than" or "less than" is added to the numerical values written before and after "to", the numerical range does not include these numerical values as the lower or upper limit.
[0013] In this specification, "corrosion resistance" refers to the property of the plating layer itself that makes it difficult for the plating layer to corrode. Zn-based plating layers have a sacrificial corrosion protection effect on steel materials. Therefore, in the process of corrosion of plated steel sheets, the plating layer corrodes and turns into white rust first before the steel material corrodes, and the white-rusted plating layer disappears, and then the steel material corrodes and red rust appears. In addition, in this specification, "sacrificial corrosion protection" refers to the property of suppressing corrosion of the steel material at exposed portions of the steel material (for example, at cut end surfaces of plated steel material or at portions where the steel material is exposed due to cracks in the hot-dip plating layer during processing).
[0014] First, the results of the inventors' investigation into means for suppressing the formation of white rust will be described. Specifically, the inventors have conducted extensive investigations into means for suppressing the formation of white rust in the early stages of corrosion on Zn-Al-Mg plated steel materials.
[0015] First, the corrosion morphology of the Zn-Al-Mg-based plating layer was investigated. As a result, it was found that corrosion of the Zn-Al-Mg-based plating layer progresses from the Zn-Al(β) phase. Furthermore, it was found that the reason for this is that this Zn-Al(β) phase exhibits the electrochemically most base corrosion potential (-1.3 V vs. Ag / AgCl in a 1M NaCl aqueous solution) in the plating layer.
[0016] Furthermore, when corrosion progresses in the Zn-Al-Mg based plating layer, the Zn-Al (β) phase is followed by the MgZn phase. 2 It was confirmed that the MgZn phase corrodes. 2 The corrosion potential of the Zn-Al(β) phase was -1.1 V vs. Ag / AgCl in a 1 M NaCl aqueous solution. The β phase is distributed throughout the entire plating layer, and increasing the potential of this corrosion-prone region, the Zn-Al(β) phase, is effective in improving appearance and corrosion resistance.
[0017] To increase the potential of the β-phase, it is preferable that an electrochemically noble element be contained in the Zn-Al(β) phase. Elements effective in increasing the potential of the β-phase include Cu and Ag. This is because Cu and Ag have atomic radii similar to those of Al and Zn, respectively, and exhibit substitutional solid solutions, making them easily miscible with each other.
[0018] An example of a suitable method for incorporating Cu or Ag into the Zn-Al(β) phase in the plating layer is the following two-stage plating method.
[0019] The base sheet is first electroplated with Zn, and then electroplated with Cu or Ag. The Cu or Ag may be an alloy of these. The base sheet plated with Zn and Cu or Ag is then heated to diffuse Cu and / or Ag into the Zn plating layer, resulting in a base sheet for plating. The base sheet for plating is then immersed in a Zn-Al-Mg hot-dip plating bath (which may contain Cu and Ag) to form a hot-dip plating layer. In this specification, this method of forming a predetermined pre-plating layer on the base sheet for plating and then sequentially applying Zn-Al-Mg hot-dip plating is referred to as a "two-stage plating method."
[0020] During the solidification of the plating, the Zn—Al(β) phase is formed and grows in a specific temperature range. Therefore, by reducing the cooling rate in this temperature range, the Zn—Al(β) phase is sufficiently formed, and the Zn—Cu phase formed on the surface of the plating substrate is dissolved and incorporated into the Zn—Al(β) phase.
[0021] In the plating layer containing Cu and Ag thus formed, the Zn atoms and the Cu and Ag atoms are located at approximately the same positions, and these atoms are distributed in a different manner from the Al component distribution in the plating layer.
[0022] In addition, in the plating layer according to this embodiment, Cu and Ag, which efficiently exhibit a noble potential, are contained in the Zn-Al (β) phase, which is the most susceptible portion to corrosion, and therefore the corrosion potential of the β phase increases. As a result, the potential distribution of the entire plating layer becomes MgZn. 2 The resulting layer is almost uniform with the plated steel. As a result, the potential difference at specific locations is reduced, reducing the amount of white rust that forms in the early stages of corrosion on plated steel. Furthermore, even if white rust does form, it forms uniformly, making it less noticeable.
[0023] [Hot-dip plated steel material] Hereinafter, the hot-dip plated steel material according to this embodiment will be described in detail. The hot-dip plated steel material according to this embodiment is a hot-dip plated steel material having a steel material and a plating layer disposed on the surface of the steel material. The average chemical composition of the plating layer is, in mass%, Al: more than 10.0% and less than 45.0%, Mg: 4.0% to 15.0%, Si: 0.01% to 2.0%, at least one of Cu: 0.03% to 5.0% and Ag: 0.03% to 6.0%, and further contains Sn: 0% to 0.7%, Bi: 0% to 0.3%, In: 0% to 0.3%, Ca: 0% to 0.6%, Y: 0% to 0.3%, La: 0% to 0.3%, Ce: 0% to 0.3%, Sr: 0% to 0.3%, Li: 0% to 0.3%, Ni: 0% to 1.0%, Cr: 0% or more, 0.5% or less, Mo: 0% or more, 0.3% or less, Sb: 0% or more, 0.25% or less, Pb: 0% or more, 0.25% or less, B: 0% or more, 0.5% or less, P: 0% or more, 0.5% or less, Ti: 0% or more, 0.25% or less, Co: 0% or more, 0.25% or less, V: 0% or more, 0.25% or less, Nb: 0% or more, 0.25% or less, Mn: 0% or more, 0.25% or less, Zr: 0% or more, 0.25% or less, W: 0% or more, 0.25% or less, Fe: 0% or more, 5.0% or less, the balance being Zn and impurities, and the total content of Cu and Ag is 0.03% or more, 6.0% or less.
[0024] (Steel Material) First, the steel material (original sheet) to be plated will be described. The steel material is, for example, mainly a steel plate, but its size is not particularly limited. The steel plate may be any steel plate that can be applied to a normal hot-dip galvanizing process. Specifically, this applies to steel plates that can be applied to a process in which the steel plate is immersed in molten metal and solidified, such as a continuous hot-dip galvanizing line (CGL). The size of the steel plate that can be applied is, for example, a plate thickness of 10 mm or less and a plate width of 2000 mm or less, but the size of the steel plate is not limited to this.
[0025] The steel material is not particularly limited, and examples of applicable steel materials include various steel plates such as general steel, pre-plated steel thinly plated with various metals, Al-killed steel, ultra-low carbon steel, high carbon steel, various high-tensile steels, some high alloy steels (steels containing elements that strengthen corrosion resistance such as Ni and Cr), steel for bolts, and steel wire rods for bridge cables. More specifically, the steel material may be, for example, a hot-rolled steel plate defined in JIS G 3131 (2018), a cold-rolled steel plate defined in JIS G 3141 (2017), a material included in the general structural rolled steel material corresponding to the so-called SS material, a so-called general steel included in the hot-rolled steel plate defined in JIS G 3193 (2019), a pre-plated steel thinly plated with various metals described in JIS H 8641 (2021), JIS G 3302 (2019), 3303 (2017), 3313 (2017), 3314 (2019), 3315 (2017), 3317 (2019), and 3321 (2019), a rolled steel material for building structures described in JIS G 3136 (2012), a pre-plated steel thinly plated with various metals described in JIS G Applicable steels include Al-killed steels, ultra-low carbon steels, and high carbon steels described in JIS G 3126 (2015), various high-tensile steels described in JIS G 3113 (2018), 3134 (2018), and 3135 (2018), and some high alloy steels (steels containing elements that strengthen corrosion resistance, such as Ni and Cr, etc.).
[0026] Furthermore, the manufacturing process of steel materials includes common processes such as pig iron and steel making processes using blast furnaces or electric furnaces, hot rolling processes, pickling processes, cold rolling processes, and heat treatment processes.
[0027] (Plating Layer) Next, the plating layer provided on the steel material will be described. The plating layer according to this embodiment includes a Zn-Al-Mg alloy layer. When alloy elements such as Al and Mg are contained in the Zn phase, corrosion resistance is improved. Therefore, in the case of a plating layer including such a Zn phase, even a thin film (for example, about half the thickness of a normal Zn plating layer) can exhibit corrosion resistance equivalent to that of a normal Zn plating layer. Similarly, even when the plating layer according to this embodiment is thin, corrosion resistance equivalent to or greater than that of a conventional Zn plating layer is ensured.
[0028] The Zn—Al—Mg alloy layer is made of a Zn—Al—Mg alloy, which means a ternary alloy containing Zn, Al, and Mg.
[0029] The plating layer may also include an Al-Fe-based interfacial alloy layer (however, the thickness thereof is less than 5 μm). The Al-Fe-based interfacial alloy layer is an interfacial alloy layer between the steel material and the Zn-Al-Mg-based alloy layer, and is in contact with the surface of the steel material. That is, the plating layer of this embodiment may have a single-layer structure composed of a Zn-Al-Mg-based alloy layer, or may have a laminated structure including a Zn-Al-Mg-based alloy layer and an Al-Fe-based interfacial alloy layer. In the case of a laminated structure, it is preferable that the Zn-Al-Mg-based alloy layer be a layer that constitutes the surface of the plating layer.
[0030] Although the Al-Fe-based interface alloy layer does not significantly affect corrosion resistance, it does affect the adhesion of the plating layer and workability (presence or absence of cracks) during processing of hot-dip galvanized steel. In particular, the Al-Fe-based interface alloy layer may affect powdering resistance, which indicates the degree of peeling of the plating layer during processing. Typically, a thinner Al-Fe-based interface alloy layer reduces the number of crack initiation points in the plating layer during processing, thereby further improving powdering resistance. Therefore, in hot-dip galvanized steel materials that may be subjected to high processing when used as components, etc., it is preferable that the thickness of the Al-Fe-based interface alloy layer be as thin as possible. Specifically, the thickness of the intermetallic compound constituting the Al-Fe-based interface alloy layer is less than 5 μm. This thickness is preferably 2 μm or less, more preferably 1 μm or less, and even more preferably 0.5 μm or less. It may even be 0.3 μm or less. This suppresses cracking during processing and further improves powdering resistance. Furthermore, the ratio of the thickness of the Al-Fe interfacial alloy layer to the thickness of the plating layer is less than 10% on average, and more preferably less than 5%.
[0031] The Al-Fe interfacial alloy layer is formed on the surface of the steel material, specifically, between the steel material and the Zn-Al-Mg alloy layer. 5 Fe 2The Al-Fe interfacial alloy layer is formed by mutual atomic diffusion between the base steel (steel sheet) and the coating bath. When a continuous hot-dip coating method is used as the manufacturing method, an Al-Fe interfacial alloy layer is likely to be formed in a coating layer containing Al element. In this embodiment, since the coating bath contains Al at a certain concentration or more, the Al-Fe interfacial alloy layer contains Al. 5 Fe 2 However, because atomic diffusion takes time, the Fe concentration in the Al-Fe system interface alloy layer is not uniform, and the Fe concentration may be higher in the area closer to the base steel. Therefore, the Al-Fe system interface alloy layer is partially composed of an AlFe phase, an Al 3 Fe phase, Al 5 Fe 2 In some cases, the Al-Fe-based interfacial alloy layer contains a small amount of Zn, because the plating bath contains a certain concentration of Zn. In addition, the Al-Fe-based interfacial alloy layer may contain a small amount of Si, which tends to accumulate at the interface.
[0032] In this embodiment, Si is contained in the plating layer. A portion of the Si is incorporated into the Al-Fe-based interfacial alloy layer to form an Al-Fe-Si intermetallic compound phase. The identified intermetallic compound phase is the AlFeSi phase. Isomers of the AlFeSi phase include the α phase, β phase, q1 phase, and q2 phase. Therefore, these AlFeSi phases and the like may be detected in the Al-Fe-based interfacial alloy layer. An Al-Fe-based interfacial alloy layer containing these AlFeSi phases and the like is also referred to as an Al-Fe-Si alloy layer.
[0033] The upper and lower limits of the thickness of the entire coating layer are not particularly limited. Furthermore, the thickness is affected by the withdrawal speed of the steel material from the coating bath and the wiping conditions. That is, in the case of a continuous hot-dip coating method, the thickness of the entire coating layer is affected by the viscosity and specific gravity of the coating bath. The maximum thickness of the coating layer formed by a continuous hot-dip coating method is often 100 μm or less. Therefore, the coating thickness of the hot-dip coated steel material of this embodiment may be, for example, 100 μm or less.
[0034] Next, the average chemical composition of the plating layer will be described. When the plating layer has a single-layer structure of a Zn-Al-Mg alloy layer, the average chemical composition of the entire plating layer is the average chemical composition of the Zn-Al-Mg alloy layer. When the plating layer has a multilayer structure composed of an Al-Fe interfacial alloy layer and a Zn-Al-Mg alloy layer, the average chemical composition is the combined average chemical composition of the Al-Fe interfacial alloy layer and the Zn-Al-Mg alloy layer.
[0035] In the plating layer of this embodiment, the thickness of the Al-Fe-based interface alloy layer is preferably 10% or less of the total thickness of the plating layer. When the thickness of the Al-Fe-based interface alloy layer is sufficiently small relative to the total thickness of the plating layer, the Fe concentration of the plating layer is often within 5%. Therefore, the average chemical composition of the plating layer is generally similar to the components of the Zn-Al-Mg-based alloy layer. Furthermore, traces of the original plating material are unlikely to remain as chemical components of the plating layer. Therefore, the average chemical composition of the plating layer is nearly identical to the components of the plating bath used in its production.
[0036] Al: more than 10.0% and less than 45.0% Al is an element that mainly constitutes the coating layer. If the Al content is 10% or less, a sufficient amount of Zn-Al phase may not be secured. Therefore, the Al content is more than 10%. On the other hand, if the Al content is 45.0% or more, the Al-Zn(α) phase becomes the main component in the coating layer, and the Al-Zn(β) phase does not form. Therefore, the upper limit of the Al content is less than 45%.
[0037] Mg: 4.0% or more, 15.0% or less Like Zn, Mg is an element that mainly constitutes the coating layer. In the coated steel sheet according to this embodiment, Mg is an important element for improving sacrificial corrosion protection. If the Mg content in the coating layer is less than 4.0%, the effect of improving sacrificial corrosion protection is not as clear as when no Mg is contained. Therefore, the Mg content is set to 4.0% or more. On the other hand, if excessive Mg is added to a Zn-Al-Mg-based coating bath, a rapid oxidation reaction occurs at the surface of the coating bath, making stable plating impossible. Therefore, to ensure stable plating and good manufacturability, the Mg content in the coating layer is set to 15% or less.
[0038] Si: 0.01% or more, 2.0% or less. Si inhibits the Al-Fe reaction, thereby inhibiting the formation of an Al-Fe-based interfacial alloy layer. Furthermore, Si is incorporated into a portion of the Al-Fe-based interfacial alloy layer to form an Al-Fe-Si compound. Without Si, the Al-Fe reaction becomes active, resulting in an increased thickness of the Al-Fe alloy layer, which can lead to powdering during processing and significantly impair corrosion resistance. On the other hand, if the Si content is 0.01% or more, the growth rate of the interfacial alloy layer becomes slow. However, if the Si content is 2.0% or more, Si bonds with Mg to form a large amount of an intermetallic compound having the composition Mg2Si, which significantly increases the viscosity of the coating bath, reducing the amount of molten metal adhering to the steel when the steel is removed from the coating bath and resulting in an extremely thin coating layer. Furthermore, the coating appearance is significantly impaired. For these reasons, the upper limit of the Si content is set to 2.0% or less. The preferred range is 0.10 to 0.40%, and more preferably 0.20 to 0.30%. If the Si content is 2.0% or less, almost no Mg2Si is formed.
[0039] Because Cu and Ag have atomic radii similar to those of Zn and Al, they readily substitute for and intermix with these elements in the plating layer. The inclusion of Cu or Ag in the plating layer increases the potential of the Zn-Al (β) phase, improving corrosion resistance. Cu and Ag have nearly identical effects. To change the potential and alter the initial white rust formation behavior, it is effective to include 0.03% or more of at least one of Cu and Ag in the plating layer. Preferably, the total concentration of Cu and Ag in the plating layer is 0.4% or more. On the other hand, excessive Cu and Ag contents may generate electrically noble portions due to the Cu and Ag that cannot be contained in the β phase, accelerating corrosion. Therefore, the upper limit of the Cu content is set to 5.0% or less, and the upper limit of the Ag content is set to 6.0% or less. Furthermore, when both Cu and Ag are contained, the upper limit of the total Cu and Ag content is set to 6%. This is because when the total content of Cu and Ag reaches 6.0%, electrically noble portions are generated by Cu and Ag that cannot be contained in the β phase, which promotes corrosion.
[0040] Sn: 0% or more, 0.7% or less Bi: 0% or more, 0.3% or less In: 0% or more, 0.3% or less Sn, Bi, and In are elements that promote softening of the plating layer when contained in the plating layer. Since Sn, Bi, and In are elements that can be contained optionally, the content of each is 0% or more. When Sn is contained, Mg 9 Sn 5 Bi tends to form Mg 3 Bi 2 , In is Mg 3 In and other elements are also formed. 2 These elements are softer than the tin phase and have good workability, and their inclusion in the plating layer clearly improves workability. Furthermore, these elements exhibit very base electrochemical properties, providing a high level of sacrificial corrosion protection. By incorporating at least one of Sn, Bi, and In, the corrosion resistance of the processed portion can be improved.
[0041] Ca: 0% or more, 0.6% or less Y: 0% or more, 0.3% or less La: 0% or more, 0.3% or less Ce: 0% or more, 0.3% or less Sr: 0% or more, 0.3% or less Li: 0% or more, 0.3% or less Ni: 0% or more, 1.0% or less Cr: 0% or more, 0.5% or less Mo: 0% or more, 0.3% or less Sb: 0% or more, 0.25% or less Pb: 0% or more, 0.25% or less B: 0% or more, 0.5% or less P: 0% or more, 0.5% or less Ti: 0% or more, 0.25% or less Co: 0% or more, 0.25% or less V: 0% or more, 0.25% or less Nb: 0% or more, 0.25% or less Mn: 0% or more, 0.25% or less Zr: 0% or more, 0.25% or less W: 0% or more, 0.25% or less Ca, Y, La, Ce, Sr, Li, Ni, Cr, Mo, Sb, Pb, B, P, Ti, Co, V, Nb, Mn, Zr, and W all form intermetallic compounds with Si, Zn, Al, etc. However, if the contents of these elements are within the above ranges, they do not affect the initial corrosion of the plating layer. On the other hand, if these elements are contained in excess, a potential difference may occur in the plating layer, causing a large amount of initial white rust to occur. Therefore, if these elements are contained, it is preferable to keep them within the above ranges.
[0042] Fe: 0% or more, 5.0% or less. The hot-dip plated steel material of this embodiment is produced by a continuous hot-dip plating method, so Fe may diffuse from the base material to be plated into the plated layer during production. As described above, in this embodiment, the Al concentration of the plated layer is high, and an Al-Fe-based interfacial alloy layer may be formed, but its thickness is thin. As a result, the plated layer may contain up to 5.0% Fe, but as long as the Fe concentration is limited to 5.0% or less, there is no effect on the frequency of cracks in the plated layer, etc. Therefore, the Fe content is set to 0 to 5.0%. The Fe content may be greater than 0%.
[0043] The balance is preferably Zn and impurities. The balance preferably contains Zn. Since the hot-dip plated steel material of this embodiment is a highly versatile Zn-based plated steel material, the element constituting the main phase of the plated layer is Zn.
[0044] Impurities refer to components contained in raw materials or components mixed in during the manufacturing process, but not intentionally included. For example, trace amounts of components other than Fe may be mixed into the plating layer as impurities due to atomic diffusion between the steel material (base steel) and the plating bath. Furthermore, since metals with 3N purity are typically used to manufacture plating alloys, the total concentration of impurities may be approximately 0.03% or less.
[0045] To identify the average chemical composition of the plating layer, the plating layer is stripped and dissolved using an acid containing an inhibitor that suppresses corrosion of the base steel (steel material) to obtain an acid solution. The resulting acid solution is then measured using ICP atomic emission spectroscopy or ICP-MS to obtain the chemical composition. There are no particular restrictions on the type of acid, as long as it is an acid that can dissolve the plating layer. By measuring the area and weight before and after stripping, the plating adhesion amount (g / m 2 ) can also be obtained at the same time.
[0046] Next, the distribution of the components of the plating layer in the depth direction will be described. Glow discharge optical emission spectroscopy (GDS) is used to understand the component distribution in the depth direction of the plating layer. On the other hand, GDS is effective for understanding components over a relatively wide range of several mm or more in diameter, and the interface position varies depending on the sputtering rate, etc., depending on the definition. In this embodiment, the surface of the plating layer is taken as the starting point (zero point), and the interface position of the plating layer is defined as the position where the Fe concentration shows a quantitative analysis value of 5 mass% according to the Fe concentration distribution. Details of the GDS analysis conditions will be described later.
[0047] Although FeAl-based compounds may occur in the interface alloy layer, in this case the interface is located on the interface alloy layer. The above definition allows us to understand the components focusing only on the plating layer portion of the Zn-Al-Mg alloy layer, excluding the interface alloy layer. Furthermore, if the thickness of the plating layer is t, the center of the plating layer can be considered to be 1 / 3t to 2 / 3t of the thickness t. In other words, the range from 1 / 3t to 2 / 3t is the main part of the plating layer. An overview is shown in Figure 1.
[0048] In the plating layer of this embodiment, the Cu and Ag elements mostly bond with or substitute for Zn, so that they have similar distributions in the depth direction. On the other hand, for example, in the case of a plating layer formed by adding Cu and Ag elements to a plating bath, the distributions of the Cu and Ag elements are close to that of Al, and there is a case where no correlation with Zn is observed.
[0049] The corrosion potential of the plating layer increases when electrochemically noble Cu or Ag occupies the electrochemically less noble Zn site. That is, the inventors have discovered that when Cu or Ag occupies the same site as Zn, it can be considered that Cu or Ag is contained in the Zn—Al(β) phase or has substituted for Zn in the Zn—Al(β) phase, and that the more the proportion (degree) of inclusion or substitution is constant, the higher the potential of the entire plating layer.
[0050] The degree of substitution of Zn with Cu and / or Ag (CAZ) can be expressed by the following formula (5) in the component analysis of GDS.
[0051] CAZ=[Cu+Ag] / [Zn] (5) In the formula (5), [Cu], [Ag], and [Zn] are quantitative component analysis values (mass%) in the depth direction in GDS.
[0052] "CAZ" is the ratio of the total concentration of Cu and Ag to the Zn concentration in the internal region between the 1 / 3t position and the 2 / 3t position on the surface of the plating layer. The larger this CAZ value, the more the substitution progresses.
[0053] In addition, in the plating layer, the maximum value of CAZ max and the minimum value of CAZ min When the following formula (1) is satisfied, the corrosion potential of the plating layer increases throughout the entire plating layer, and the amount of white rust generated on the plated steel sheet tends to be reduced. This is because Cu and / or Ag are uniformly distributed in the plating layer. max / CAZ min is preferably 1.1 or less.
[0054] CAZ max / CAZ min ≦1.20 … (1)
[0055] In order to sufficiently increase the corrosion potential, it is necessary to satisfy the following formula (2). On the other hand, an excessive increase in corrosion potential will accelerate corrosion. max It is necessary to satisfy the following formula (3). More preferably, 0.01≦CAZ min , C.A.Z. max ≦0.08. This allows the corrosion potential to be reduced by 100%. 2 This allows the potential to be approximately the same as that of the phase, reducing the occurrence of white rust due to corrosion and improving the appearance.
[0056] 0.0005≦CAZ min …(2) CAZ max ≦0.1000 ... (3)
[0057] Increasing the potential of the Zn-Al phase (β phase) is effective in preventing appearance deterioration due to the formation of white rust in the plating layer. Furthermore, increasing the potential to reduce the potential difference with the surrounding intermetallic compounds and metallic phases, as well as increasing the electrical resistance of the β phase itself, can slow the progression of corrosion and improve corrosion resistance. This tendency can be evaluated by corrosion current density and achieved by maintaining a constant substitution rate for Al and Zn in the β phase. Because the β phase has a size of approximately 5 μm or more in the plating layer, its presence can be easily confirmed using SEM. Quantitative analysis of the area can also be obtained using EDS, EPMA, etc.
[0058] The ratio of Zn to Al (Zn:Al) in the β phase is approximately 1:1, and within this range, the β phase can exist as a phase with excellent corrosion resistance. Furthermore, it is preferable that the following formula (4) be satisfied at any point or any region within the β phase. By satisfying the following formula (4), the electrical resistance of the β phase increases, and corrosion resistance can be further improved.
[0059] 0.85≦[Al] / ([Zn]+[Cu]+[Ag])≦1.15 (4) Here, [Al], [Zn], [Cu], and [Ag] in formula (4) are quantitative analysis values (at %) in the β phase determined by energy dispersive X-ray analysis.
[0060] Furthermore, the corrosion current density depends on the area fraction of the β phase. Therefore, it is preferable that the area fraction of the β phase is 3% or more in any SEM cross section of the plating layer. The area fraction of the β phase in the plating layer can be controlled by the manufacturing method. The area fraction of the β phase is more preferably 5% or more, and even more preferably, the Cu+Ag concentration in the plating layer is 0.4% or more and the area fraction of the β phase is 10% or more. Here, the "β phase" referred to in this specification can also be said to be an intermetallic compound region composed of at least one of an Al-Zn-Cu compound, an Al-Zn-Ag compound, and an Al-Zn-Cu-Ag compound.
[0061] To properly supply Cu and / or Ag to the β phase in the plating layer, it is preferable to provide them from a pre-plating layer formed on the base sheet by the method described below. The Zn, Cu, and Ag in the pre-plating layer are thermally diffused during pre-annealing to form a Cu-Ag-Zn diffusion plating layer (an aggregate of Cu, Ag-Zn intermetallic compounds). However, this Cu-Ag-Zn diffusion plating layer disappears during hot-dip plating. However, if a small amount of (Zn + Al)-(Cu + Ag) compounds is ultimately present in the plating layer, the potential of the plating layer can be increased.
[0062] The (Zn + Al)-(Cu + Ag) compound is a compound in which Cu, Ag, and Al are dissolved in small amounts in Zn, and has a potential of -1.2 V (vs. Ag / AgCl 1M NaCl). Therefore, by leaving the (Zn + Al)-(Cu + Ag) compound in the final plating layer, the potential of the plating layer can be further increased. The (Zn + Al)-(Cu + Ag) compound can be confirmed in the plating layer using SEM, and quantitative analysis values can be confirmed using point analysis as described above.
[0063] In order to obtain a (Zn+Al)-(Cu+Ag) compound that exhibits an appropriate potential, it is preferable that the component ratio be Zn+Al:Cu+Ag=4:1 to 9:1. In addition, the (Zn+Al)-(Cu+Ag) compound has an equivalent circle diameter of 1 μm or more in any cross section along the thickness direction of the plating layer, and the number of such compounds is 10,000 μm or more. 2 It is preferable that the number of (Zn+Al)-(Cu+Ag) compounds is 10 or more, and more preferably 20 or more, per unit area. The number of (Zn+Al)-(Cu+Ag) compounds tends to depend on the adhesion amounts of Cu, Ag, and Zn in the base sheet, i.e., the adhesion amount of the pre-plated layer.
[0064] Next, an example of a method for analyzing a plating layer will be shown.
[0065] A glow discharge optical emission spectrometer (GDS) is preferably used to analyze the components in the depth direction within the plating layer. The inventors used a LECO Japan 850A glow discharge optical emission spectrometer, but the measurement device is not limited to this. When performing depth direction analysis, analysis is preferably performed while Ar sputtering is performed, under the following analysis conditions: argon pressure: 0.27 MPa, output power: 30 W, output voltage: 1000 V, and discharge area: a circular area with a diameter of 4 mm. Measurement is performed from the surface of the plating layer toward the depth direction until the Fe concentration reaches 100% (reaching the base steel). Therefore, the analysis range of depth direction analysis using GDS is from the plating surface to the Zn-Al-Mg plating layer, the interface alloy layer (Al-Fe alloy layer), and a portion of the steel material. After GDS analysis, the sputter depth of the cross section is measured using a Surfcom 130A manufactured by Tokyo Seimitsu Co., Ltd. GDS analysis provides an element distribution profile in the depth direction of the plating layer. The element distribution profile shows the distribution of the content of each element in the depth direction, assuming that the total amount of the detected elements is 100%.
[0066] Cross-sectional observation using an SEM can be performed using the following procedure. First, an observation sample measuring approximately 20 x 20 mm is cut from the plated steel sheet so that the cross section of the plating layer is exposed, and this sample is embedded in resin. Next, the observation surface is mirror-polished, and the cross-sectional observation of the plating layer is performed. Note that cross-sectional observation should be performed after Au is vapor-deposited onto the cross section of the plating layer. To eliminate bias in the selection of the field of view of the plating layer, at least three observation samples are taken from one plated steel sheet, and at least 30 locations are observed randomly so that the field of view is approximately 500 to 2000 times larger, and each phase is identified and its area fraction is measured.
[0067] When determining the area fraction of the β phase, the field of view is first specified, and then the field of view is specified to include an area where the β phase component range is close to 0.85≦[Al] / ([Zn]+[Cu]+[Ag])≦1.15 using point analysis by EDS. If β phase is found, a quantitative analysis element mapping image of the entire plating layer is taken. The same component range is identified from the Zn and Al in the captured mapping image using the image analysis software "ImageJ" and then binarization is performed. The area fraction of the β phase in the plating layer is measured from the obtained binarized area.
[0068] Similarly, for Zn-Cu compounds, the Zn, Cu, and equivalent circle diameter are measured. The distribution of the number of (Zn + Al)-(Cu + Ag) compounds can be determined using functions attached to known image analysis software such as ImageJ. After observing each field of view, the total area of the plating layer (equivalent to the number of pixels) is measured to be 10,000 μm 2 The number distribution is checked for each sample until it reaches the value of 0. It is preferable to check the number of (Zn+Al)-(Cu+Ag) compounds from at least three samples.
[0069] [Method for manufacturing hot-dip plated steel material] Next, a preferred method for manufacturing the hot-dip plated steel material of this embodiment will be described. In the manufacturing method according to this embodiment, Cu and Ag behave in almost the same way, and therefore, hereinafter, no distinction will be made between them and Cu will be used as a representative. In other words, the description of Cu below may be read as "Ag" or "Cu and Ag."
[0070] A simple method for forming the above-mentioned plating layer is to add Cu directly to a Zn-Al-Mg plating bath. 2 There is a concern that the formation of intermetallic compounds such as Cu and a reaction between the base steel and Cu may make it difficult to efficiently incorporate Cu into the β phase. Therefore, as an example of a suitable method for producing the hot-dip plated steel material of this embodiment, a method in which Cu is supplied to the plated layer from a pre-plated layer provided on a base sheet for plating will be described below.
[0071] First, a base steel sheet such as a cold-rolled steel sheet or a hot-rolled steel sheet is electroplated with Zn to form a pre-Zn-plated layer (hereinafter simply referred to as a Zn-plated layer or a Zn layer). The amount of Zn deposited on the base steel sheet is preferably equal to or greater than the amount of Cu in the final plating layer. The pre-plating method may be electroplating, displacement plating, vapor deposition, or the like.
[0072] There are no particular restrictions on the Zn plating on Fe, provided that it is carried out under conditions that allow for normal zinc plating, such as in a cyanide bath, zincate bath, zinc chloride bath, or zinc sulfate bath.
[0073] Then, Cu is plated on the Zn layer to form a pre-Cu plating layer. In this embodiment, it is effective to form a pre-Cu plating layer on the pre-Zn plating layer after forming the pre-Cu plating layer. If the pre-Cu plating layer and the pre-Zn plating layer are formed in this order, the Cu in the pre-Cu plating layer may diffuse toward the base sheet, making it impossible to obtain the desired plating layer. Therefore, it is preferable to form the pre-Zn plating layer and the pre-Cu plating layer in this order. For Cu plating, copper sulfate, copper cyanide, copper pyrophosphate, alkanol baths, etc. can be used, and there are no particular restrictions on the plating bath. Silver cyanide is used for Ag, and electroless plating of Cu is also possible.
[0074] In order to increase the number of (Zn+Al)-(Cu+Ag) compounds, it is preferable that the coating weight of the pre-Cu plating layer exceeds 1 / 1000 of the final plating coating weight.
[0075] Next, the plated original sheet is heated to 450 to 600°C. This heating may also serve as annealing of the original sheet (hereinafter, this heating may be referred to as pre-annealing). This heating causes Zn to melt and react with Cu to form an alloy, thereby forming a Zn-Cu plated diffusion layer. If the heating temperature is less than 450°C, Cu may not be efficiently diffused into the plated layer. On the other hand, if the heating temperature exceeds 600°C, this is not preferable because it may cause the pre-Zn plated layer to evaporate or form a reaction layer between Fe and Zn. The pre-annealing temperature range is preferably 450 to 600°C.
[0076] Next, the base sheet with the Zn—Cu plating diffusion layer formed thereon is immersed in a Zn—Al—Mg-based plating bath and then pulled out. At this time, the bath temperature of the Zn—Al—Mg-based plating bath is preferably 450 to 600°C. When the base sheet with the Zn—Cu plating diffusion layer formed thereon is immersed in the Zn—Al—Mg-based plating bath and pulled out, a higher bath temperature facilitates dissolution of the Zn—Cu plating layer and facilitates fine dispersion of Cu in the plating layer. Therefore, the bath temperature is preferably 450°C or higher. More preferably, it is 470°C or higher, even more preferably, 500°C or higher, and even more preferably, 550°C or higher. On the other hand, if the bath temperature is excessively high, Zn in the plating bath evaporates, easily disrupting the bath balance. Therefore, the bath temperature is preferably 600°C or lower. More preferably, it is 580°C or lower. In this embodiment, it is preferable to control the temperature when pulling out the plated base sheet. That is, by performing appropriate temperature control and cooling control after immersion, Cu is finely dispersed in the plating bath, and Cu is contained in the Zn—Al(β) phase during the solidification process of the plating layer.
[0077] The Zn-Al (β) phase is formed after the Al (α) phase precipitates and grows from the molten state of the plating. After the Al (α) phase has grown sufficiently, the Zn-Al (β) phase precipitates and grows to surround it. Since the Zn-Cu fine compounds taken in from the original plate do not dissolve in the solid Al (α) phase, many of the Zn-Cu fine compounds can remain.
[0078] The temperature range of 550 to 450°C is a temperature range in which only the α phase is formed, and the β phase is not formed. If the average cooling rate in this temperature range is more than 10°C, the growth of the α phase may be inhibited. If the α phase does not grow sufficiently in the temperature range of 550 to 450°C, the subsequent formation of the β phase may be insufficient. Furthermore, if the average cooling rate in the temperature range of 550 to 450°C is too high, the amount of β phase cannot be sufficiently secured, and therefore Zn-Cu cannot be sufficiently incorporated into the β phase, resulting in the formation of the CAZ. max / CAZ min Therefore, the average cooling rate in the temperature range of 550 to 450°C is set to 10°C / sec or less.
[0079] The average cooling rate in the temperature range of 450 to 350°C is not particularly limited. However, the amount of β phase can be increased by lowering the average cooling rate between 450 and 350°C. Therefore, the average cooling rate between 450 and 350°C is preferably 8°C / second or less.
[0080] The average cooling rate in the temperature range below 350° C. does not affect the formation of the β phase. In addition, the cooling conditions in the temperature range below 350° C. are not particularly limited because they do not affect the potential, corrosion current density, etc.
[0081] Next, a method for evaluating the performance of hot-dip galvanized steel materials will be described.
[0082] (Corrosion Potential) The corrosion potential of the plating layer can be measured using a common device configuration, such as an electrochemical cell, a reference electrode, a salt bridge, and a potentiostat (a constant potential field device). One example of an evaluation method is a method using an Ag / AgCl type reference electrode, a 1 M NaCl aqueous solution as the measurement solution, and performing the measurement under conditions such as degassing and constant room temperature. When the surface of a plated steel sheet is thoroughly cleaned and then immersed in the measurement solution, the corrosion potential immediately after immersion may be significantly negative. However, the potential stabilizes after immersion in the solution for approximately 1,800 seconds. This potential is the corrosion potential of the plating layer surface.
[0083] When the corrosion potential approaches −1.1 V, the variation in the potential of the plating layer becomes smaller, which is preferable, and the amount of white rust generated in the early stage of corrosion can be minimized. The early stage of corrosion refers to the tendency of the white rust area ratio after 24 hours in a salt spray test (SST) specified in JIS Z 2371 (2015).
[0084] <Evaluation criteria> E: Corrosion potential is -1.3V or less, and the white rust area ratio on the surface evaluated in the corrosion test is "25% or more". D: Corrosion potential is -1.3 to -1.25V, and the white rust area ratio on the surface evaluated in the corrosion test is "20 to 25% or more". C: Corrosion potential is -1.25 to -1.2V, and the white rust area ratio on the surface evaluated in the corrosion test is "15 to 20% or more". B: Corrosion potential is -1.25 to -1.2V, and the white rust area ratio on the surface evaluated in the corrosion test is "10 to 15% or more". A: Corrosion potential is -1.2 to -1.1V, and the white rust area ratio on the surface evaluated in the corrosion test is "less than 10%".
[0085] (Corrosion Current Density) A polarization curve is drawn by changing the potential in the positive and negative directions, and the corrosion potential is determined by Tafel extrapolation. The corrosion current density depends on the corrosion rate. This can also be estimated from the corrosion weight loss in a salt spray test. That is, since only the β phase corrodes initially, the corrosion weight loss after 120 hours of SST is measured. The corrosion weight loss can be measured by immersing the steel sheet before and after the corrosion test in 30% chromic acid for 5 minutes, which allows the amount of corrosion of the β phase to be estimated.
[0086] <Evaluation Criteria> E: Corrosion current density log|i| (A / cm 2 ) when the value obtained is -4 or more, and the corrosion weight loss is 25 g / m 2 or more. D: Corrosion current density log |i| (A / cm 2 ) was obtained as -4.5 to -4, and the corrosion weight loss was 20 g / m 2 C: Corrosion current density log |i| (A / cm 2 ) was obtained with a value of -5 to -4.5, and corrosion weight loss of 15 g / m 2 B: Corrosion current density log |i| (A / cm 2 ) was obtained with a value of -5.5 to -5, and corrosion weight loss was 10 g / m 2 A: Corrosion current density log |i| (A / cm 2 ) was obtained with a value of -6 to -5.5, and corrosion weight loss of 5 g / m 2 or more. S: corrosion current density log |i| (A / cm 2 ) when obtained, the value is less than -6, and the corrosion weight loss is 5 g / m 2 If it is less than.
[0087] After the plating layer is formed, various chemical conversion treatments and painting treatments may be carried out.
[0088] In the hot-dip plated steel material of this embodiment, a coating may be formed on the plating layer. One or more layers of the coating may be formed. Examples of the type of coating directly on the plating layer include a chromate coating, a phosphate coating, and a chromate-free coating. These coatings can be formed by known methods such as chromate treatment, phosphate treatment, and chromate-free treatment.
[0089] Chromate treatments include electrolytic chromate treatments that form a chromate film by electrolysis, reactive chromate treatments that form a film by utilizing a reaction with the material and then wash away excess treatment solution, and paint-on chromate treatments that apply a treatment solution to the substrate and dry it without rinsing with water to form a film. Any of these treatments may be used.
[0090] Examples of electrolytic chromate treatments include electrolytic chromate treatments using chromic acid, silica sol, resins (phosphoric acid, acrylic resins, vinyl ester resins, vinyl acetate acrylic emulsions, carboxylated styrene butadiene latex, diisopropanolamine-modified epoxy resins, etc.), and hard silica.
[0091] Examples of the phosphate treatment include zinc phosphate treatment, zinc calcium phosphate treatment, and manganese phosphate treatment.
[0092] Chromate-free treatments are particularly suitable because they do not place a burden on the environment. Chromate-free treatments include electrolytic chromate-free treatments that form a chromate-free film by electrolysis, reactive chromate-free treatments that form a film by utilizing a reaction with the material and then wash away excess treatment liquid, and paint-on chromate-free treatments that apply a treatment liquid to the substrate and dry it without rinsing with water to form a film. Any of these treatments may be used.
[0093] Furthermore, one or more organic resin coatings may be provided on the coating directly on the plating layer. The organic resin is not limited to a specific type, and examples thereof include polyester resins, polyurethane resins, epoxy resins, acrylic resins, polyolefin resins, and modified versions of these resins. Here, the term "modified version" refers to a resin obtained by reacting a reactive functional group contained in the structure of these resins with another compound (such as a monomer or a crosslinking agent) containing a functional group capable of reacting with the functional group.
[0094] Such organic resins may be a mixture of one or more unmodified organic resins, or a mixture of one or more organic resins obtained by modifying at least one other organic resin in the presence of at least one organic resin. The organic resin film may also contain any coloring pigment or anti-rust pigment. Water-based organic resins obtained by dissolving or dispersing them in water may also be used.
[0095] Next, examples of the present invention will be described, but the conditions in the examples are merely examples adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to these examples. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0096] First, a cold-rolled steel sheet (corresponding to SPCC defined in JIS G 3141 (2017)) having a size of 100 mm × 200 mm and a thickness of 0.8 mm was prepared as a base sheet for plating. First, a predetermined amount of Zn was applied to the surface of this cold-rolled steel sheet using a zinc plating bath described below to form a Zn plating layer.
[0097] Zinc plating conditions: zinc chloride: 50 g / L, ammonium chloride: 200 g / L, pH = 5.5, bath temperature: 30°C, current density: 2 A / dm 2 .
[0098] Next, a Cu plating layer, an Ag plating layer, or a plating layer containing Cu and Ag was formed on the plated original sheet on which the Zn plating layer had been formed, using the following copper plating bath and the following silver plating bath. When forming a plating layer containing Cu and Ag, the plated original sheet was immersed in the copper plating bath and then the silver plating bath. The copper plating bath was subjected to air agitation. The pH of the silver plating bath was adjusted to H 4 P 2 O 7 , and adjusted with KOH.
[0099] Copper plating conditions: copper pyrophosphate: 80 g / L, potassium pyrophosphate: 290 g / L, ammonia water: 3 mg / L, potassium nitrate: 10 g / L, anode: oxygen-free high-purity copper, current density: 3 A / dm 2 .
[0100] Silver plating conditions: KAg(CN)2: 40 g / L (Ag equivalent), K 4 P 2 O 7 : 150 g / L, EDTA (tetrapotassium salt): 5 g / L, smoothing material HS II (selenium, mercapto compound): 0.5 mL / L, pH = 8 to 9, current density: 40 A / dm 2 , Bath temperature: 40°C, Anode: Pt / Ti electrode.
[0101] After forming a Cu plating layer, an Ag plating layer, or a plating layer containing Cu and Ag on the plating base sheet, the plating base sheet was heated for 0.5 to 3 minutes at the pre-annealing temperatures shown in Tables 1A to 1C to form a plating diffusion layer, thereby obtaining a plating substrate. The composition of the plating diffusion layer is shown in Tables 1A to 1C.
[0102] The obtained plating substrate was subjected to hot-dip plating using a hot-dip plating simulator. First, alloys having the plating bath components shown in Tables 1A to 1C were prepared by a vacuum melting method, and the alloys were melted in a completely oxygen-free, nitrogen-substituted atmosphere (O 2 The plating bath was prepared in a state where the concentration was less than 5 ppm. Next, one point on the original plate (the backside of the center of the surface to be evaluated) was spot-welded to a K thermocouple, and the temperature history until the plating solidification was completed was measured. 2 (25%)-N 2 The plating bath temperature was set to 550 to 600°C, and the substrate was immersed in the bath at a rate of 600 mm / sec. After stopping in the bath for 3 seconds, the substrate was pulled up at a rate of 600 mm / sec. 2 Wiping gas: 135 to 140 g / m 2 After that, the deposition amount was adjusted so that 2 Gas was blown onto the steel sheet, followed by air cooling at the average cooling rates shown in Tables 1A to 1C. Through the above steps, plated steel sheets were obtained.
[0103] Next, evaluation samples were cut out from each of the plated steel sheets. Samples for GDS analysis and SEM observation were cut out at 30 mm square positions on the opposite side of the thermocouple position. Corrosion samples measuring 100 × 50 mm were taken from the center of the plated steel sheets.
[0104] Electrochemical tests and corrosion tests (SST) were conducted to evaluate the various cut samples. The Fe content of the plating layer is not shown in the table, but it was in the range of 0 to 5% in all cases. The evaluation results, plating layer composition, GDS analysis results, and each structure in the β-phase region are shown in Tables 2A to 2C. The underlined parts in each table indicate that the results are outside the scope of the present invention, that the manufacturing conditions are not preferable, or that the characteristic values are unfavorable. The (*) symbols in Tables 2A to 2C indicate that the equivalent circle diameter of a (Zn+Al)-(Cu+Ag) compound is 1 μm or more in any cross section along the thickness direction of the plating layer. 2 The number per
[0105]
[0106]
[0107]
[0108]
[0109]
[0110]
[0111] According to the above aspect of the present invention, it is possible to provide a hot-dip plated steel material that can suppress the occurrence of white rust in the early stages of corrosion.
Claims
1. A hot-dip plated steel material having a steel material and a plating layer disposed on a surface of the steel material, the plating layer containing, by mass%, Al: more than 10.0% and less than 45.0%, Mg: 4.0% or more and 15.0% or less, Si: 0.01% or more and 2.0% or less, at least one of Cu: 0.03% or more and 5.0% or less and Ag: 0.03% or more and 6.0% or less, and further containing Sn: 0% or more and 0.7% or less, Bi: 0% or more and 0.3% or less, In: 0% or more and 0.3% or less, Ca: 0% or more and 0.6% or less, Y: 0% or more and 0.3% or less, La: 0% or more and 0.3% or less, Ce: 0% or more and 0.3% or less, Sr: 0% or more and 0.3% or less, Li: 0% or more, 0.3% or less, Ni: 0% or more, 1.0% or less, Cr: 0% or more, 0.5% or less, Mo: 0% or more, 0.3% or less, Sb: 0% or more, 0.25% or less, Pb: 0% or more, 0.25% or less, B: 0% or more, 0.5% or less, P: 0% or more, 0.5% or less, Ti: 0% or more, 0.25% or less, Co: 0% or more, 0.25% or less, V: 0% or more, 0.25% or less, Nb: 0% or more, 0.25% or less, Mn: 0% or more, 0.25% or less, Zr: 0% or more, 0.25% or less, W: 0% or more, 0.25% or less, Fe: 0% or more, 5.0% or less, the balance being Zn and impurities, The plating layer has a chemical composition in which the total content of Cu and Ag satisfies 0.03% or more and 6.0% or less, and in an element distribution profile obtained by quantitatively analyzing the plating layer from the surface toward the steel material by glow discharge optical emission spectrometry, the plating layer has a thickness of t, and in an internal region between a 1 / 3t position and a 2 / 3t position with respect to the surface of the plating layer, the ratio of the total concentration of Cu concentration and Ag concentration to the Zn concentration in the internal region is defined as CAZ, and the maximum value CAZ of the CAZ is max and the minimum value CAZ of the CAZ min The hot-dip coated steel material is characterized in that it satisfies the following formulas (1) to (3). max / C.A.Z. min ≦1.20 ... (1) 0.0005≦C A Z min … (2) C.A.Z. max ≦0.1000 ... (3) 2. The hot-dip plated steel material according to claim 1, characterized in that in a cross section along the thickness direction of the plated layer, the area ratio of the β phase is 3% or more, and the concentrations of Al, Zn, Cu and Al in the β phase satisfy the following formula (4): 0.85≦[Al] / ([Zn]+[Cu]+[Ag])≦1.15 ... (4), where [Al], [Zn], [Cu] and [Ag] in formula (4) are respectively quantitative analysis values (at %) in the β phase by energy dispersive X-ray analysis.
3. 10,000 μm in a cross section along the thickness direction of the plating layer 2 The hot-dip galvanized steel material according to claim 1 or 2, characterized in that, within the range, 10 or more (Zn+Al)-(Cu+Ag) compounds having an average crystal grain size of 1 μm or more are contained as intermetallic compound particles.