Temporary protection film for semiconductor device manufacturing and method for manufacturing semiconductor device
Patent Information
- Application Number
- MYPI2025006215
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-23
- Filing Date
- 2024-08-06
- Publication Date
- 2025-02-23
Smart Images

Figure PI2025006215_DRAWING_001 
Figure PI2025006215_DRAWING_002 
Figure PI2025006215_DRAWING_003
Abstract
Description
Temporary protective film for semiconductor device manufacturing and semiconductor device manufacturing method
[0001] The present disclosure relates to a temporary protective film for use in manufacturing a semiconductor device and a method for manufacturing a semiconductor device.
[0002] Semiconductor packages often have a structure in which an encapsulating layer is formed only on the semiconductor element side of the lead frame, leaving the back surface of the lead frame exposed. In manufacturing semiconductor packages with this structure, there is a risk that the encapsulating material will get onto the back surface of the lead frame when the encapsulating layer is formed. To prevent this, a method is known in which a temporary protective film is attached to the back surface of the lead frame (see Patent Document 1). The temporary protective film is peeled off from the lead frame after the encapsulating layer is formed.
[0003] WO 2001 / 035460
[0004] It is desirable that the temporary protective film has adhesive strength that allows it to be attached to an adherend such as a lead frame at room temperature (25°C), while being easily peelable from the adherend after sealing. Therefore, one aspect of the present invention aims to provide a temporary protective film that can be easily peeled off after sealing without losing adhesive strength after attachment at room temperature.
[0005] According to the inventors' research, when a polymer containing alkyl (meth)acrylate and (meth)acryloyl morpholine as monomer units is used in the adhesive layer of a temporary protective film, it has traditionally been common to use a crosslinking agent in combination. However, it has been found that by not using a crosslinking agent, the temporary protective film can be easily peeled off after sealing without compromising its adhesive strength after application at room temperature.
[0006] The present invention includes the following aspects. [1] A temporary protective film for manufacturing a semiconductor device, comprising a support film and an adhesive layer provided on the support film, wherein the adhesive layer contains a polymer containing alkyl (meth)acrylate and (meth)acryloyl morpholine as monomer units, and does not contain a crosslinking agent. [2] The temporary protective film according to [1], wherein the polymer further contains a monomer having an acidic group as a monomer unit. [3] The temporary protective film according to [1] or [2], wherein the adhesive layer has a thickness of 3 μm or less, and the temporary protective film has a storage modulus at 200° C. of 5 MPa or more. [4] A method for manufacturing a semiconductor device, comprising the steps of: attaching a temporary protective film to one side of a substrate; mounting a semiconductor element on the side of the substrate opposite the temporary protective film; encapsulating the semiconductor element; and peeling the temporary protective film from the substrate, in this order; wherein the temporary protective film comprises a support film and an adhesive layer provided on the support film, and the adhesive layer contains a polymer containing alkyl (meth)acrylate and (meth)acryloyl morpholine as monomer units, and does not contain a crosslinking agent. [5] The manufacturing method according to [4], wherein the polymer further contains a monomer having an acidic group as a monomer unit. [6] The manufacturing method according to [4] or [5], wherein the thickness of the adhesive layer is 3 μm or less, and the storage modulus of the temporary protective film at 200° C. is 5 MPa or more.
[0007] According to one aspect of the present invention, it is possible to provide a temporary protective film that can be easily peeled off after sealing without losing adhesive strength after application at room temperature.
[0008] Fig. 1 is a cross-sectional view showing an embodiment of a temporary protective film; Fig. 2 is a cross-sectional view illustrating an embodiment of a method for manufacturing a semiconductor device; Fig. 3 is a cross-sectional view illustrating an embodiment of a method for manufacturing a semiconductor device; Fig. 4 is a cross-sectional view showing an embodiment of a semiconductor device; Fig. 5 is a perspective view showing an embodiment of a reel body;
[0009] Hereinafter, an embodiment of the present invention will be described. FIG. 1 is a cross-sectional view showing a temporary protective film according to one embodiment. As shown in FIG. 1, a temporary protective film 10 according to one embodiment includes a support film 1 and an adhesive layer 2 provided on the support film 1. The temporary protective film 10 can be used as a temporary protective film for manufacturing a semiconductor device. More specifically, the temporary protective film 10 can be attached to the back surface of a lead frame (the surface opposite to the surface on which the semiconductor element is mounted) during the encapsulation molding process to form an encapsulation layer that encapsulates a semiconductor element mounted on a die pad of the lead frame, thereby being used as a temporary protective film for semiconductor encapsulation molding to temporarily protect the lead frame during encapsulation molding.
[0010] The support film 1 may be, for example, a film of at least one polymer selected from the group consisting of polyimide, polyamide, polyamideimide, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherketone, polyarylate, polyetheretherketone, and polyethylene naphthalate, and is preferably a polyimide film. The polyimide may be an aromatic polyimide. The support film 1 may also be a film of copper, aluminum, stainless steel, or nickel. When the support film 1 is a polymer film, its surface may be surface-treated by a method such as a chemical treatment, an alkali treatment, a silane coupling treatment, or the like, a physical treatment, such as a sand mat treatment, a plasma treatment, or a corona treatment.
[0011] The thickness of the support film 1 may be, for example, 5 μm or more, 10 μm or more, 15 μm or more, or 20 μm or more, and may be 100 μm or less, 50 μm or less, or 30 μm or less. 1 Thickness T of adhesive layer 2 2 The ratio T 2 / T 1 may be 0.05 or more, 0.08 or more, or 0.1 or more, and may be 0.5 or less, 0.3 or less, or 0.2 or less.
[0012] The adhesive layer 2 contains a polymer containing alkyl (meth)acrylate and (meth)acryloylmorpholine as monomer units (hereinafter also referred to as "acrylic polymer").
[0013] The alkyl group in the alkyl(meth)acrylate (the alkyl group portion other than the (meth)acryloyl group) may be linear or branched. The number of carbon atoms in the alkyl group may be 2 or more or 3 or more, and may be 30 or less, 20 or less, 10 or less, 7 or less, 5 or less, or 4 or less, or may be 2 or 4.
[0014] Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, and decyl (meth)acrylate.
[0015] The content of alkyl (meth)acrylate may be 70% by mass or more, 75% by mass or more, or 80% by mass or more, and may be 92% by mass or less, 90% by mass or less, or 88% by mass or less, based on the total amount of monomer units in the acrylic polymer.
[0016] The content of (meth)acryloylmorpholine may be 7% by mass or more, 7.5% by mass or more, 8% by mass or more, 8.5% by mass or more, or 9.0% by mass or more, based on the total amount of monomer units in the acrylic polymer, and may be 20% by mass or less, 18% by mass or less, 17% by mass or less, 16.5% by mass or less, or 16% by mass or less.
[0017] The mass ratio of the (meth)acryloylmorpholine content to the alkyl(meth)acrylate content ((meth)acryloylmorpholine / alkyl(meth)acrylate) may be 0.08 / 1 or more, 0.09 / 1 or more, or 0.1 / 1 or more, and may be 0.3 / 1 or less, 0.25 / 1 or less, 0.23 / 1 or less, 0.21 / 1 or less, or 0.2 / 1 or less.
[0018] The acrylic polymer may further contain other monomers as monomer units in addition to the alkyl (meth)acrylate and (meth)acryloyl morpholine. The other monomers have polymerizable groups copolymerizable with the alkyl (meth)acrylate and (meth)acryloyl morpholine. The polymerizable groups may be, for example, ethylenically unsaturated groups.
[0019] The other monomer may be a monomer having an acidic group in addition to a polymerizable group. The acidic group may be, for example, a carboxyl group or a sulfo group, and is preferably a carboxyl group. Examples of crosslinkable monomers having a carboxyl group include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, monohydroxyethyl phthalate acrylate, and 2-acryloyloxyethyl succinate.
[0020] The other monomer may be a monomer having a hydroxyl group in addition to a polymerizable group. Examples of this monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate; and hydroxyalkyl cycloalkane (meth)acrylates such as (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.
[0021] The content of the other monomers may be 0.1% by mass or more, 0.5% by mass or more, or 1% by mass or more, and may be 5% by mass or less, 4% by mass or less, or 3% by mass or less, based on the total amount of monomer units in the acrylic polymer.
[0022] The weight average molecular weight (Mw) of the acrylic polymer may be 550,000 or more or 600,000 or more, and from the viewpoint of easier peeling of the temporary protective film after sealing, is preferably 650,000 or more, more preferably 750,000 or more, even more preferably 850,000 or more, and particularly preferably 950,000 or more. The Mw of the acrylic polymer may be 2,000,000 or less, 1,800,000 or less, 1,600,000 or less, 1,400,000 or less, 1,200,000 or less, or 1,100,000 or less.
[0023] The molecular weight distribution (Mw / Mn) of the acrylic polymer may be 2.0 or less, 1.9 or less, 1.8 or less, or 1.7 or less, or may be 1.0 or more, 1.2 or more, 1.4 or more, or 1.6 or more.
[0024] The Mw and Mw / Mn of an acrylic polymer are measured by the following procedure. They were determined by gel permeation chromatography (GPC) using a high-performance liquid chromatograph (Tosoh Corporation, Model HLC-8320GPC). Two TSKgel Super Multipore HZ-H (Tosoh Corporation) columns were used, a tetrahydrofuran solution was used as the mobile phase, and a differential refractometer was used as the detector. The measurement conditions were a column temperature of 40°C, a sample concentration of 10 mg / mL, a sample injection volume of 10 μm, and a flow rate of 0.2 mL / min. A calibration curve was created using polystyrene (molecular weights: 1,090,000, 775,000, 427,000, 289,000, 190,000, 96,400, 37,900, 10,200, 2,630, and 440) as a standard substance, and the weight-average molecular weight (Mw) and number-average molecular weight (Mn) were measured. The molecular weight distribution (Mw / Mn) was calculated from these measurements.
[0025] The acid value of the acrylic polymer may be 10 mgKOH / g or more or 20 mgKOH / g or more, and 40 mgKOH / g or less or 30 mgKOH / g or less. The hydroxyl value of the acrylic polymer may be 1 mgKOH / g or more or 2 mgKOH / g or more, and 10 mgKOH / g or less or 5 mgKOH / g or less. The acid value and hydroxyl value of the acrylic polymer are measured in accordance with the method described in JIS K0070.
[0026] The content of the acrylic polymer may be 80% by mass or more, 85% by mass or more, or 90% by mass or more, and may be 99.5% by mass or less, or 99% by mass or less, based on the total amount of the adhesive layer 2.
[0027] The adhesive layer 2 does not contain a crosslinking agent. Since the adhesive layer 2 does not contain a crosslinking agent, the adhesive strength of the temporary protective film after application at room temperature is not impaired, and the temporary protective film can be easily peeled off after sealing. Furthermore, in one embodiment, when the adhesive layer 2 does not contain a crosslinking agent, thickening of the varnish used to form the adhesive layer 2 can also be suppressed.
[0028] The adhesive layer 2 may further contain other components in addition to the acrylic polymer. Examples of the other components include a polymer other than the acrylic polymer and a coupling agent.
[0029] The thickness of the adhesive layer 2 may be 1 μm or more, or 2 μm or more, and may be 20 μm or less, 15 μm or less, 10 μm or less, 5 μm or less, 4 μm or less, or 3 μm or less.
[0030] The storage modulus of the temporary protective film 10 at 200°C may be 0.5 MPa or more or 1 MPa or more, preferably 2 MPa or more, 3 MPa or more, 4 MPa or more, or 5 MPa or more, for example, 10 MPa or less. The storage modulus of the temporary protective film at 200°C is measured by the method described in the examples.
[0031] The temporary protective film 10 exhibits a high storage modulus even when the adhesive layer 2 is thin. Specifically, in one embodiment, even when the thickness of the adhesive layer 2 is 3 μm or less, the storage modulus of the temporary protective film 10 at 200° C. can be within the above-mentioned range (particularly, preferably 2 MPa or more, 3 MPa or more, 4 MPa or more, or 5 MPa or more). When the temporary protective film 10 exhibits such a high modulus, wire bonding can be performed neatly.
[0032] In another embodiment, the temporary protective film may further include a cover film provided on the surface of the adhesive layer opposite the support film. That is, the temporary protective film may include a support film, an adhesive layer, and a cover film in this order. The cover film may be a polyethylene terephthalate film. The thickness of the cover film may be 10 μm or more and 100 μm or less.
[0033] In another embodiment, the temporary protective film may further include a non-adhesive layer provided on the side of the support film opposite the adhesive layer. The non-adhesive layer may be a resin layer that has substantially no adhesiveness to an adherend at 0 to 270°C. The non-adhesive layer may contain a thermoplastic resin, a thermosetting resin (cured product), or a resin that is a combination thereof. The non-adhesive layer may further contain a filler (e.g., ceramic powder, glass powder, silver powder, copper powder, resin particles, rubber particles), a coupling agent, etc. The thickness of the non-adhesive layer may be 1 μm or more and 10 μm or less.
[0034] The temporary protective film can be produced, for example, by a method including the steps of applying a varnish containing an acrylic polymer and a crosslinking agent onto a support film and removing the solvent from the coating to form an adhesive layer.
[0035] Next, a method for manufacturing a semiconductor device using the above-mentioned temporary protective film will be described. The method for manufacturing a semiconductor device according to one embodiment includes, in this order, a step S1 of attaching a temporary protective film to one side of a substrate, a step S2 of mounting a semiconductor element on the surface of the substrate opposite the temporary protective film, a step S3 of encapsulating the semiconductor element, and a step S4 of peeling the temporary protective film from the substrate. Hereinafter, as an example, a method for manufacturing a semiconductor device (semiconductor device package) in which the substrate is a lead frame will be described in more detail.
[0036] 2 is a cross-sectional view illustrating one embodiment (step S1) of a method for manufacturing a semiconductor device. In step S1, as shown in FIG. 2, a temporary protective film 10 is attached to the back surface, which is one surface of a lead frame 11 having a die pad 11a and inner leads 11b. The temporary protective film 10 is attached in a direction such that the adhesive layer of the temporary protective film 10 contacts the lead frame 11.
[0037] The lead frame 11 may be made of, for example, an iron-based alloy such as alloy 42, copper, or a copper-based alloy. The lead frame 11 may have a molded body made of copper or a copper-based alloy and a coating layer of palladium, gold, silver, or the like that coats the surface of the molded body.
[0038] The temporary protective film 10 has excellent adhesive strength at room temperature (e.g., 25°C), and can be attached to the lead frame 11 at room temperature. The temporary protective film 10 may be attached to the lead frame 11 while being heated and pressed. In this case, the heating temperature may be 150°C or higher and 400°C or lower. The pressure may be 0.5 MPa or higher and 30 MPa or lower. The heating and pressing time may be 1 second or longer and 60 seconds or shorter.
[0039] 3 is a cross-sectional view illustrating one embodiment of a method for manufacturing a semiconductor device (steps S2 and S3). In step S2, as shown in FIG. 3, a semiconductor element 14 is mounted on the surface of the die pad 11a opposite the temporary protective film 10. The semiconductor element 14 is bonded to the die pad 11a via an adhesive (e.g., silver paste). After bonding the semiconductor element 14 to the die pad 11a, reflow connection (CuClip connection, etc.) may be performed at a maximum temperature of 250 to 440°C or 250 to 400°C for 1 to 30 minutes.
[0040] Next, the semiconductor element 14 is connected to the inner leads 11b using wires 12. The wires 12 may be, for example, gold wires, copper wires, or palladium-coated copper wires. The wires 12 may be bonded to the semiconductor element 14 and the inner leads 11b using ultrasonic waves and pressure while being heated at, for example, 200 to 350°C.
[0041] 3, an encapsulating layer 13 is formed to encapsulate the semiconductor element 14 and the wires 12. This results in a temporarily protected encapsulated molded body 20 having the lead frame 11, the semiconductor element 14, and the encapsulating layer 13.
[0042] The sealing layer 13 is formed by sealing molding using a sealing material. By the sealing molding, it is possible to obtain an encapsulated molded body 20 having a plurality of semiconductor elements 14 and the sealing layer 13 that encapsulates them collectively. During the sealing molding, the temporary protective film 10 is provided, thereby preventing the sealing material from creeping around to the back side of the lead frame 11.
[0043] The temperature during the formation of the sealing layer 13 (temperature of the sealing material) may be 140 to 200° C., or 160 to 180° C. The pressure during the formation of the sealing layer may be 6 to 15 MPa, or 7 to 10 MPa. The time for sealing molding may be 1 to 5 minutes, or 2 to 3 minutes.
[0044] The encapsulant may contain, for example, an epoxy resin such as cresol novolac epoxy resin, phenol novolac epoxy resin, biphenyl diepoxy resin, naphthol novolac epoxy resin, etc. The encapsulant may also contain a filler, a flame retardant substance such as a bromine compound, a wax component, etc.
[0045] After the formation of the sealing layer 13 (sealing molding), the temporary protective film 10 is peeled off from the lead frame 11 and the sealing layer 13 of the obtained sealed molded body 20. When the sealing layer 13 is cured, the temporary protective film 10 may be peeled off either before or after the sealing layer 13 is cured.
[0046] The temperature at which the temporary protective film 10 is peeled off is not particularly limited, but may be room temperature (e.g., 5 to 35°C) or higher than the glass transition temperature (Tg) of the adhesive layer. In this case, the temporary protective film 10 is more easily peeled off from the lead frame 11 and the encapsulant. If the Tg of the acrylic polymer in the adhesive layer is, for example, 5°C or lower or 0°C or lower, the Tg of the adhesive layer becomes equal to or lower than room temperature, and the temporary protective film is more easily peeled off at room temperature.
[0047] When the lead frame 11 includes a plurality of patterns having die pads 11 a and inner leads 11 b, the encapsulated body 20 can be divided as necessary to obtain a plurality of semiconductor devices (semiconductor packages) 100 shown in Fig. 4, each having one semiconductor element. That is, when the lead frame 11 has a plurality of die pads 11 a and a semiconductor element 14 is mounted on each of the plurality of die pads 11 a, the manufacturing method according to one embodiment may further include a step of peeling the temporary protective film 10 from the encapsulated body 20 and then dividing the encapsulated body 20 to obtain semiconductor devices (semiconductor packages) 100 having one die pad 11 a and one semiconductor element 14.
[0048] The temporary protective film may be long and may be used in the form of a reel wound around a core. In this case, the temporary protective film is attached to the adherend while being unwound from the reel.
[0049] Fig. 5 is a perspective view showing one embodiment of a reel body. As shown in Fig. 5, a reel body 30 according to one embodiment includes a winding core 31, a temporary protective film 10 wound around the winding core 31, and side plates 32. The widths of the winding core 31 and the temporary protective film 10 (the length in the direction perpendicular to the winding direction) may be 1 mm or more, 5 mm or more, or 10 mm or more, and may be 1000 mm or less, 800 mm or less, or 500 mm or less. In another embodiment, the reel body may not include side plates.
[0050] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0051] Example 1 Acrylic polymer A-1 (weight average molecular weight (Mw): 600,000, molecular weight distribution (Mw / Mn): 1.7) containing, as monomer units, 80% by mass of butyl acrylate, 16% by mass of acryloylmorpholine, 3% by mass of acrylic acid, and 1% by mass of other monomers (monomers having a hydroxyl group) was dissolved in cyclohexanone to obtain a varnish for forming an adhesive layer. A polyimide film (thickness: 25 μm, manufactured by DuPont-Toray Co., Ltd., product name: Kapton 100EN) was prepared as a support film. The obtained varnish was applied to one side of the support film. The coating on the support film was dried by heating at 90°C for 1.5 minutes and then at 260°C for 1.5 minutes to form a 2 μm-thick adhesive layer. This obtained a temporary protective film.
[0052] Examples 2 and 3 Temporary protective films were obtained in the same manner as in Example 1, except that the thickness of the adhesive layer was changed as shown in Table 1.
[0053] Comparative Example 1: A compound having the following formula: A temporary protective film was obtained in the same manner as in Example 1, except that a varnish was prepared by adding 7 parts by mass of a crosslinking agent represented by the formula: and the thickness of the adhesive layer was changed as shown in Table 1.
[0054] Example 4 A temporary protective film was obtained in the same manner as in Example 2, except that instead of the acrylic polymer A-1, an acrylic polymer A-2 (weight average molecular weight (Mw): 1,000,000, molecular weight distribution (Mw / Mn): 1.9) containing, as monomer units, 90.5% by mass of butyl acrylate, 5.5% by mass of acryloylmorpholine, 3% by mass of acrylic acid, and 1% by mass of other monomers (monomers having a hydroxyl group) was used.
[0055] Example 5 A temporary protective film was obtained in the same manner as in Example 4, except that the thickness of the adhesive layer was changed as shown in Table 1.
[0056] (Evaluation of Varnish Thickening) The varnish for forming the adhesive layer used in producing each temporary protective film was evaluated for thickening. Specifically, 1.1 mL of varnish was used, and the viscosity of the varnish at 25°C on the day the varnish was produced and one month after the production date was measured using a viscosity measuring instrument L (manufactured by). The thickening of the varnish was evaluated according to the following criteria. A: The increase in viscosity of the varnish one month after the production date relative to the viscosity of the varnish on the day the varnish was produced is less than 30%. B: The increase is 30% or more, or the varnish one month after the production date has gelled and lost fluidity.
[0057] (Measurement of storage modulus of temporary protective film) Each temporary protective film was cut into a size of 5 mm x 8 mm to prepare a test specimen. The test specimen was heated at 180°C for 1 hour, and then heated at 200°C for 1 hour, and then the storage modulus of the test specimen at 200°C was measured using a dynamic viscoelasticity measuring device (UBM Corporation, Rheogel-E4000). The test specimen was fixed using a shear modulus measuring jig with a tightening torque of 7 cN m. The measurement conditions were as follows: measurement mode: frequency dependent, measurement frequency: 20 Hz to 600 Hz, load: constant control.
[0058] (Measurement of Adhesion Strength After Room-Temperature Application) A CDA194 palladium-plated plate (PPF, manufactured by Shinko Electric Industries, Ltd.) was prepared as a lead frame. Each temporary protective film cut into a size of 10 mm x 50 mm was attached to this lead frame with the adhesive layer facing the lead frame using a hand roller at 25°C and a load of 20 N. Next, using a force gauge, each temporary protective film was peeled off at 25°C in a direction 90 degrees relative to the main surface of the lead frame at a rate of 50 mm / min. The maximum load (N / m) per 10 mm width of the adhesive layer at this time was measured as the adhesive strength (90-degree peel strength) after room-temperature application. The results are shown in Table 1. If the adhesive strength after room-temperature application is 20 N / m or more, it can be said that the adhesive strength is not impaired.
[0059] (Measurement of peel strength after sealing) Using a mold molding machine (manufactured by Apic Yamada Co., Ltd.), a sealing layer was formed on the surface of the lead frame opposite the temporary protective film to which the temporary protective film had been attached in the same manner as in the above "Measurement of adhesive strength after room temperature application" using a sealing material (trade name: GE-300, manufactured by Resonac Co., Ltd.). The sealing conditions were 175 ° C., 6.8 MPa, and 2 minutes. Thereafter, at 25 ° C., each temporary protective film was peeled off at a rate of 50 mm / min in a direction 180 degrees relative to the main surface of the lead frame, and the peel strength at that time was measured with a force gauge. At this time, the peel strength from the portion with a large adhesive area between the temporary protective film and the lead frame was taken as the peel strength on the lead frame, and the peel strength from the portion with a large adhesive area between the temporary protective film and the sealing layer was taken as the peel strength on the sealing layer. The smaller the peel strength after sealing, the easier it is to peel off the temporary protective film after sealing.
[0060]
[0061] 1...support film, 2...adhesive layer, 10...temporary protective film, 11...lead frame, 11a...die pad, 11b...inner lead, 12...wire, 13...encapsulating layer, 14...semiconductor element, 20...encapsulated molded body, 100...semiconductor device.
Claims
1. A temporary protective film for use in the manufacture of semiconductor device, comprising: a support film; and an adhesive layer provided on the support film, wherein the adhesive layer contains a polymer having alkyl (meth)acrylate and (meth)acryloylmorpholine as monomer units, and does not contain a crosslinking agent.
2. The temporary protective film according to claim 1, wherein the polymer further comprises a monomer having an acidic group as a monomer unit.
3. A temporary protective film as described in claim 1 or 2, wherein the adhesive layer has a thickness of 3 μm or less, and the temporary protective film has a storage modulus at 200° C. of 5 MPa or more.
4. A method for manufacturing a semiconductor device comprising the steps of: attaching a temporary protective film to one side of a substrate; mounting a semiconductor element on the surface of the substrate opposite the temporary protective film; encapsulating the semiconductor element; and peeling the temporary protective film from the substrate, in this order; wherein the temporary protective film comprises a support film and an adhesive layer provided on the support film, and the adhesive layer contains a polymer having alkyl (meth)acrylate and (meth)acryloylmorpholine as monomer units, and does not contain a crosslinking agent.
5. The method according to claim 4, wherein the polymer further comprises a monomer having an acidic group as a monomer unit.
6. The manufacturing method described in claim 4 or 5, wherein the adhesive layer has a thickness of 3 μm or less, and the temporary protective film has a storage modulus of 5 MPa or more at 200° C.