Media for biological treatment
Patent Information
- Application Number
- MYPI2025006283
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-28
AI Technical Summary
Existing biological treatment carriers, such as those made from synthetic fibers and polyolefin resins, fail to effectively immobilize sludge and purify wastewater due to insufficient adsorption capabilities.
A biological treatment carrier composed of nylon fibers with specific polymer properties, including a high number of amino terminal groups, a molar fraction of amino terminal groups of 0.45 or more, and a relative viscosity of 2.5 or more, which enhances sludge adhesion and zeta potential, combined with a cationic surfactant for improved sludge attraction and wastewater purification.
The nylon fiber carrier effectively attracts and adheres sludge with negative potential, achieving high wastewater purification efficiency and stable sludge adhesion, as demonstrated by increased zeta potential and sludge adhesion rates in biological treatment tests.
Abstract
Description
Biological treatment carriers
[0001] The present invention relates to a biological treatment carrier, and more particularly to a biological treatment carrier used for biologically treating wastewater containing organic components.
[0002] It is known to use synthetic fibers as biological treatment carriers, for example, polyester fibers as biological treatment carriers for fixed-bed biological treatment tanks (Patent Document 1).It is also known to use polyolefin resins kneaded with hydrophilic polymers such as starch and nonionic surfactants as biological treatment carriers (Patent Document 2).
[0003] Since the sludge in the biological treatment tank when the biological treatment carrier is in use has a negative potential on its surface, it has been proposed to introduce cationic polar groups into the polyolefin resin in order to improve the adsorption of sludge onto the biological treatment carrier (Patent Document 3).
[0004] These techniques aim to improve the ability to immobilize sludge on the surface of biological treatment carriers, but have not yet achieved sufficient results.
[0005] Patent Document 4 shows that polyamide fibers are superior in immobilizing sludge.
[0006] Non-Patent Document 1 describes a method for producing polyamide, a raw material for polyamide fibers.
[0007] Nylon is hydrophilic and has an isoelectric point due to the presence of amino and carboxyl terminal groups, allowing it to assume various surface potentials relative to the pH of the solution. In the present invention, the inventors have discovered that by utilizing this property of nylon, it is possible to provide a biological treatment carrier that is easy for sludge to adhere to and has a high ability to purify wastewater.
[0008] An object of the present invention is to provide a biological treatment carrier to which sludge easily adheres and which has a high capacity to purify wastewater.
[0009] That is, the present invention relates to a biological treatment carrier made of nylon fibers, characterized in that the polymer properties of the nylon fibers include a number of amino terminal groups of 40 μeq / g or more and an amino terminal group molar fraction FA of 0.45 or more, and the relative viscosity ηr of the nylon fiber polymer is 2.5 or more.
[0010] According to the present invention, it is possible to provide a biological treatment carrier to which sludge easily adheres and which has a high capacity to purify wastewater.
[0011] The present invention will be described in detail below.
[0012] [Nylon Fiber] In the present invention, nylon fiber is used as the biological treatment carrier. As the polymer for nylon fiber, nylon 66 or nylon 6 is preferably used because of its high polarity and good processability.
[0013] Nylon fiber polymers have an amino end group at one end of the polymer chain and a carboxyl end group at the other end. The zeta potential of nylon fibers depends on the number of amino end groups, the number of carboxyl end groups, and the balance between them. Depending on the pH of the water solvent, the zeta potential shifts from the basic (high pH) region to the acidic (low pH) region in the positive (+) direction, and the isoelectric point also shifts. In nylon polymers immediately after polymerization, the number of amino end groups is equivalent to the number of carboxyl end groups.
[0014] As the relative viscosity ηr of the polymer constituting nylon fiber increases, the number of amino terminal groups and the number of carboxyl terminal groups decrease, the isoelectric point of the nylon fiber shifts to a lower pH side, and the zeta potential at the same pH shifts in the negative (negative) direction.
[0015] In the present invention, it is important that the number of amino terminal groups is 40 μeq / g or more, preferably 43 μeq / g or more, as a polymer characteristic of nylon fiber, which shifts the isoelectric point of the nylon fiber to a higher pH side and shifts the zeta potential at the same pH in the + (plus) direction.
[0016] For the purpose of improving the stability in the polymer remelting process such as the spinning process and the stability of the quality of the nylon fiber, it is preferable to add an end-group blocking agent to block the end groups of the polymer of this nylon fiber.
[0017] Benzoic acid is preferably used as the blocking agent for these end groups. This end blocking results in a state in which the number of amino end groups and the number of carboxyl end groups are not necessarily equivalent. That is, the molar fraction of amino end groups, FA, is not 0.5. In this case, as the molar fraction of amino end groups, FA, decreases from 0.5, the isoelectric point of the nylon fiber shifts toward a lower pH, and the zeta potential at the same pH shifts toward the negative (negative) direction.
[0018] Here, the molar fraction FA of amino terminal groups is defined by the following formula: Molar fraction FA of amino terminal groups = Number of amino terminal groups / (Number of amino terminal groups + Number of carboxyl terminal groups) Generally, the molar fraction FA of amino terminal groups as a polymer characteristic of nylon fiber is about 0.44 to 0.41. However, in the present invention, it is important that the molar fraction FA of amino terminal groups as a polymer characteristic of nylon fiber is 0.45 or more, and preferably 0.46 or more.
[0019] In the present invention, by having the number of amino terminal groups of 40 μeq / g or more and the molar fraction FA of amino terminal groups of 0.45 or more, the isoelectric point of the nylon fiber polymer is shifted to the higher pH side, and the zeta potential of the nylon fiber is increased at the pH during wastewater treatment. Therefore, the biological treatment carrier of the present invention made of nylon fiber can attract and adhere negatively charged sludge to its surface.
[0020] In the present invention, the relative viscosity ηr of nylon fibers as a polymer characteristic is 2.5 or more, preferably 2.5 to 3.0. If the relative viscosity ηr is less than 2.5, the strength of the nylon fibers is insufficient. On the other hand, if the relative viscosity ηr exceeds 3.0, the isoelectric point of the nylon fibers shifts toward a lower pH, and the zeta potential at the same pH shifts toward the negative (-) side, making it difficult to attract and adhere sludge, which is undesirable.
[0021] The nylon fiber is preferably a filament, i.e., a continuous long fiber, and may be an aggregate of multiple monofilaments or a single filament. The monofilament fineness is preferably 3 to 35 dtex. If the monofilament fineness is less than 3 dtex, the resistance from the adhering sludge may cause single fiber breakage, which is undesirable. On the other hand, if the monofilament fineness exceeds 35 dtex, the surface area of the nylon fiber becomes small, the sludge adhesion rate decreases, and the treatment effect is hindered, which is undesirable.
[0022] The cross-sectional shape of the nylon fiber may be a perfect circle or an irregular shape, but is preferably an irregular shape. Among irregular shapes, a trilobal shape is preferably used as the cross-sectional shape from the viewpoint of increasing the surface area per unit weight of the nylon fiber. The degree of irregularity of the trilobal shape is expressed using the deformation ratio, which is the ratio of the radius of the circle inscribed in the cross section to the radius of the circle circumscribed in the cross section.
[0023] The deformation ratio is the radius of the inscribed circle r 1 circumscribed circle radius r 2 The ratio (r 2 / r 1 )
[0024] In the present invention, from the viewpoint of ensuring sufficient adhesion of sludge, a trilobal cross-sectional shape with a deformation ratio of 2.5 or more is preferably used.
[0025] The total surface area per apparent unit volume of the nylon fiber is preferably 1,000 m from the viewpoint of ensuring sufficient adhesion of sludge. 2 / m 3 More preferably, 4,000 m 2 / m 3 The total surface area per apparent unit volume is the surface area per unit weight measured by the BET method using a nitrogen gas adsorption mechanism, converted into bulk density.
[0026] The nylon fiber is preferably a crimped fiber, and the crimp rate is preferably 30% or more from the viewpoint of sludge adhesion.
[0027] [Cationic Surfactant] The present invention preferably further comprises a cationic surfactant adhered to the surface of the nylon fiber. That is, a preferred embodiment of the present invention further comprises a cationic surfactant adhered to the surface of the nylon fiber, and the adhesion of the cationic surfactant to the nylon fiber changes the zeta potential of the surface of the nylon fiber by +10 to +30 mV in the pH range of 6 to 8.
[0028] This cationic surfactant can change the zeta potential of the surface of nylon fibers by +10 to +30 mV in the pH range of 6 to 8 by adhering to the nylon fibers.
[0029] Cationic surfactants that satisfy this condition include amine salt-based and quaternary ammonium salt-based cationic surfactants. Because amine salt-based cationic surfactants exhibit pH dependency, quaternary ammonium salt-based cationic surfactants are preferably used.
[0030] Examples of the quaternary ammonium salt cationic surfactant include benzalkonium salt type, dialkyldimethylammonium salt type, monoalkyltrimethylammonium salt type, trialkylmonomethylammonium salt type, and tetraalkylammonium salt type quaternary ammonium salt cationic surfactants.
[0031] Cationic surfactants are thought to significantly inhibit the physiological action of microbial proteins, like disinfectants, when adsorbed to microorganisms. Therefore, among the above cationic surfactants, it is preferable to use a monoalkyltrimethylammonium salt type quaternary ammonium salt, as these do not strongly adsorb microorganisms and do not significantly shift the zeta potential of the fiber surface upward.
[0032] Examples of this monoalkyltrimethylammonium salt type quaternary ammonium salt include decyltrimonium chloride, decyltrimonium bromide, cocotrimonium chloride, steartrimonium chloride, steartrimonium bromide, cetrimonium chloride, cetrimonium bromide, behentrimonium chloride, behentrimonium bromide, lauryltrimonium chloride, and lauryltrimonium bromide.
[0033] The cationic surfactant is preferably attached to the surface of the nylon fiber and has durability in the attached state, meaning that the cationic surfactant does not peel off from the nylon fiber after the nylon fiber is laid in a biological treatment tank as a biological treatment carrier until sludge adheres to the nylon fiber.
[0034] To achieve this durability, the cationic surfactant is preferably used in combination with a nonionic surfactant, which is a hydrophilic, non-ionic surfactant.
[0035] Nonionic surfactants are composed of hydrophilic and hydrophobic (lipophilic) groups, but the hydrophilic groups strongly adsorb to the highly hydrophilic nylon surface, while the hydrophobic groups strongly interact with the hydrophobic groups of cationic surfactants. These interactions give the surfactants durability when attached to the surface of nylon fibers.
[0036] [Production Method] Nylon fibers having polymer properties in which the number of amino terminal groups is 40 μeq / g or more and the molar fraction of amino terminal groups FA is 0.45 or more, and the relative viscosity ηr of the polymer of the nylon fiber is 2.5 or more, can be produced by known methods.
[0037] When the polymer of the nylon fiber is nylon 6, it can be produced by the following steps of melt polymerization, extraction (refining) of monomers and oligomers, and drying.
[0038] In melt polymerization, caprolactam crystals are melted in a melter, mixed with water and an end-capping agent in an adjusting tank, and this adjusted raw material is retained in an atmospheric pressure polymerization tower heated to about 260°C for about 10 hours to obtain nylon 6 polymer.
[0039] The polymer that reaches polymerization equilibrium in this atmospheric polymerization contains about 0.2% by weight of water, about 10% by weight of caprolactam, and 2-3% by weight of cyclic oligomers, which are extracted and removed in a hot water extraction tower. The pellets fed to the top of the extraction tower are countercurrently extracted with hot water fed from the bottom of the tower, and then continuously removed from the bottom of the tower. This process is called refining.
[0040] The pellets continuously removed from the bottom of the tower contain 10% or more by weight of water and must be dried to a water content below the condensation equilibrium water content. Because nylon 6 is susceptible to thermal oxidative degradation, drying is carried out in a vacuum or in an inert gas atmosphere at around 100°C (drying).
[0041] Nylon 6 polymers polymerized under the conditions shown above can have various relative viscosities, numbers of amino end groups, numbers of carboxyl end groups, and molar fractions of amino end groups.
[0042] Among these, the polymer that can be used as the polymer for nylon 6 fiber in the present invention is a nylon 6 polymer having an amino terminal group number of 40 μeq / g or more, preferably 45 μeq / g or more, an amino terminal group molar fraction FA of 0.45 or more, more preferably 0.46 or more, and particularly preferably 0.47 or more, and a relative viscosity ηr of 2.5 or more, preferably 2.7 or more.
[0043] Next, the nylon 6 polymer is used as a raw polymer, and is melt-kneaded in an extruder at 230°C to 260°C, and then fed to a spinning machine, where it is extruded as a thread through a spinneret heated to 240°C to 260°C and having 50 to 250 Y-shaped holes.
[0044] The extruded filaments are cooled and solidified by cold air at 20°C or less, and then a spinning oil is applied thereto, followed by drawing at a take-up speed of 400 to 600 m / min on the first roller and 1000 to 2000 m / min on the final roller.
[0045] The drawn yarn is subsequently crimped in a crimping device using heated air at 160 to 180°C and 0.7 to 1.0 MPa, and then sprayed onto a rotary transfer device for cooling. The yarn is then stretched between rollers to loosen clumps, entangled, and wound into a cheese-like shape to obtain nylon 6 fiber.
[0046] The spinning oil may contain additives such as surfactants, lubricants, sizing agents, and friction modifiers. Furthermore, the spinning oil may be applied to the nylon 6 fiber before it is wound using a slitting device or the like.
[0047] When the biological treatment carrier is composed of nylon fibers and a cationic surfactant attached to the surface thereof, a spinning oil containing the cationic surfactant is used. The obtained nylon 6 fibers may be twisted or air-entangled to obtain the required fineness.
[0048] By the above method, a fiber bundle of nylon 6 fibers can be obtained in which the polymer properties of the nylon 6 fibers are such that the number of amino terminal groups is 40 μeq / g or more, the molar fraction of amino terminal groups FA is 0.45 or more, and the relative viscosity ηr of the nylon fiber polymer is 2.5 or more.
[0049] The present invention will be described in detail below with reference to examples. Measurements and evaluations were performed using the following methods. (1) Number of Amino End Groups, Number of Carboxyl End Groups, and Molar Fraction of Amino End Groups (FA) 1) Number of Amino End Groups (μeq / g) 1 g of deoiled fiber was dissolved in a mixed solvent of phenol and methanol (volume ratio 9:1) and titrated with 0.01 mol / L hydrochloric acid using thymol blue as an indicator. "eq" stands for "equivalent." 2) Number of Carboxyl End Groups (μeq / g) 1 g of deoiled fiber was dissolved in benzyl alcohol at 180°C under a nitrogen stream and titrated with 0.01 mol / L potassium hydroxide using phenolphthalein as an indicator. 3) Molar Fraction of Amino End Groups (FA) The molar fraction of amino end groups (FA) was calculated using the following formula 1: Molar fraction of amino terminal groups FA = number of amino terminal groups / (number of amino terminal groups + number of carboxyl terminal groups) (1)
[0050] (2) Relative Viscosity (ηr): Pre-deoiled fibers were dissolved in 96 wt% sulfuric acid to a concentration of 1 wt%, and the viscosity was measured in accordance with JIS K-6920-2:2009, Appendix JA (Regulations), Method for Determining Relative Viscosity, JA.2, sulfuric acid solution method. The fibers were deoiled using n-hexane as the solvent and a Soxhlet extractor. (3) Zeta Potential of the Fiber Surface: The fiber sample was densely packed in a measurement column between perforated plates at both ends to prevent the fiber sample from moving, and the streaming potential ΔV generated by applying a constant pressure from one direction was measured at each pH, and the zeta potential was calculated using Equation 2 below. In this case, the pH was adjusted by adding hydrochloric acid diluted with pure water to decrease the pH, or by adding potassium hydroxide diluted with pure water to increase the pH. Zeta potential = -ΔV × η × k / (ε × ΔP) (2) ΔV: streaming potential η: viscosity of the measured solution k: electrical conductivity of the measured solution ε: dielectric constant of the measured solution ΔP: pressure loss between the perforated plates at both ends (4) Deformation rate The radius r of the inscribed circle in the shape of the fiber cross section 1 circumscribed circle radius r 2 The ratio (r 2 / r 1 (5) Crimping ratio (TC): A 1 m crimped yarn was taken out and subjected to a load of 0.09 cN / dtex for 1 minute. 0 The sample was then treated in boiling water in a free state for 30 minutes to induce crimping, and then dehydrated and air-dried under standard conditions for 24 hours. After that, a load of 0.09 cN / dtex was applied to the sample, and the length L after 1 minute was measured. 1 Then, after leaving it free for 3 minutes, the length L after 1 minute under a load of 0.0018 cN / dtex was measured. 2 The crimp rate was calculated from these measured values using the following formula: TC (%) = {(L 1 -L 2 ) / L 0} x 100
[0051] (6) Biological Treatment Test (BOD, CODcr, s-CODcr, SS) Measurements were performed using the following procedure. 1) A 7.5 L biological treatment test tank, a substrate frame to be installed in the tank, a blower, aeration stones, and tubing connecting the blower and aeration stones were prepared. 2) A 5850 dtex fiber bundle, consisting of three 1950 dtex fibers twisted together and weighed in advance, was attached to a substrate frame measuring 140 mm x 132 mm x 320 mm high. The number of fiber bundles was adjusted so that the fiber bundle filling volume between the upper and lower substrate frames was the same at each level. 3) The substrate frame with the fiber bundle attached was installed in the biological treatment test tank. 4) Aeration stones connected to the blower by tubing were installed in the biological treatment test tank, and aeration was initiated. 5) 7.5 L of seed sludge was added to the biological treatment test tank. The MLSS of the seed sludge to be added was set at 2,000 to 8,000 mg / L. 6) The aeration rate was adjusted to 1.0 L / min. 7) 24 hours after the seed sludge was added, artificial sewage adjusted to glucose 388 mg / L, ammonium chloride 230 mg / L, sodium dihydrogen phosphate (dihydrate) 48 mg / L, sodium bicarbonate 365 mg / L, magnesium nitrate (heptahydrate) 37 mg / L, and calcium chloride 59 mg / L was started to be passed as raw water. The raw water flow rate was set at 0.2 kg-BOD / m when the BOD volume load of the raw water was 0.2 kg-BOD / m 3 / d. 8) Treated water and raw water were sampled 1 day, 3 days, 8 days, and 10 days after the start of raw water flow, and BOD, CODcr, s-CODcr, and SS were measured in accordance with JIS K-0102. 9) After sampling 10 days after the start of raw water flow, the raw water flow pump and blower were stopped, the carrier frame was removed from the biological treatment test tank, and the fiber bundle with sludge attached was removed and dried at 110°C overnight. 10) The total amount of sludge attached was calculated from the fiber bundle weight after drying and the fiber bundle weight before the test using the following equation 3, and the amount of sludge attached per 1 g of carrier (fiber bundle weight) (g / g) was calculated using the following equation 4. Total sludge adhesion amount (g) = Weight of fiber bundle after drying (g) - Weight of fiber bundle before test (g) (3) Sludge adhesion amount per 1 g of carrier (weight of fiber bundle) (g / g) = Total sludge adhesion amount (g) / Weight of fiber bundle before test (g) (4)
[0052] (7) Evaluation of BOD and CODcr The BOD and CODcr determined in (6) above were evaluated according to the following criteria: 1) The start-up ability was evaluated from the analytical values 3 days after the start of raw water flow.
[0053] Reduction rate (%) from initial value = (analysis value after 3 days - initial value) / initial value x 100 The reduction rate from the initial value is 75% or more AA The reduction rate from the initial value is 60% or more but less than 75% A The reduction rate from the initial value is 45% or more but less than 60% B The reduction rate from the initial value is less than 45% C 2) The overall water treatment capacity was evaluated from the analysis values 8 or 10 days after the start of raw water flow. Reduction rate (%) relative to the initial value = (analysis value after 8 or 10 days - initial value) / initial value x 100 The reduction rate relative to the initial value is 85% or more AA The reduction rate relative to the initial value is 80% or more and less than 85% A The reduction rate relative to the initial value is 75% or more and less than 80% B The reduction rate relative to the initial value is less than 75% C (8) Adhesion rate of surfactant After drying overnight at 105°C, it was measured by the methanol extraction method in accordance with JIS L-1013 2010, Section 8.27 (c).
[0054] Example 1 Caprolactam crystals were melted in a melter, and in an adjusting tank, 2.65 mol (=47.7 g) of water per 1 kg of caprolactam and 6.3 mmol (=0.77 g) of benzoic acid as an end-capping agent were mixed with 1 kg of caprolactam. This adjusted raw material was retained for 7 hours in an atmospheric pressure polymerization tower heated to 255°C, and when the raw material reached polymerization equilibrium, it was discharged in the form of a strand from the bottom of the tower into a water tank and pelletized.
[0055] The pellets were then fed to the top of the extraction tower, and the monomers and oligomers were countercurrently extracted with hot water fed from the bottom of the tower and continuously removed from the bottom of the tower. The hot-water-extracted pellets were dried in an inert gas atmosphere at 100°C to obtain nylon 6 polymer.
[0056] The resulting nylon 6 polymer had an amino terminal group count of 47.0 μeq / g, a carboxyl terminal group count of 52.9 μeq / g, an amino terminal group molar fraction FA of 0.470, and a relative viscosity ηr of 2.81. This nylon 6 polymer was used as a raw polymer and was melt-kneaded at 245°C in a single-screw extruder, and then fed to a spinning machine.
[0057] A yarn was extruded from a spinning machine through a spinneret with 150 Y-shaped holes and heated to 250° C. The extruded yarn was cooled and solidified with cold air at 15° C., and then an oil containing an anionic surfactant was applied thereto, followed by drawing at a take-up speed of 500 m / min on the first roller and 1850 m / min on the final roller.
[0058] The drawn yarn was subsequently crimped in a crimping device with heated air at 170°C and 0.8 MPa, and then sprayed onto a rotary transfer device for cooling. The yarn was then stretched between rollers to loosen clumps, entangled, and wound into a cheese shape to produce a nylon 6 fiber with a total fineness of 1950 dtex, 150 monofilaments constituting the yarn, a monofilament fineness of 13 dtex, a trilobal cross-sectional shape of the monofilaments with a deformation ratio of 3.15, and a crimp ratio of 42%.
[0059] The polymer properties of this nylon 6 fiber were as follows: the number of amino terminal groups was 43.0 μeq / g, the number of carboxyl terminal groups was 50.0 μeq / g, the molar fraction of amino terminal groups FA was 0.462, and the relative viscosity ηr was 2.75. The adhesion rate of the oil solution containing an anionic surfactant to the obtained nylon 6 fiber was 0.5 wt%.
[0060] The obtained nylon 6 fiber was deoiled in a Soxhlet extractor using ethanol as a solvent, and the zeta potential was measured before and after deoiling at pH = 6, 7, and 8. The zeta potentials of the obtained nylon 6 fiber measured at pH = 6, 7, and 8 are shown in Table 1.
[0061]
[0062] A biological treatment test was conducted using this nylon 6 fiber as a biological treatment carrier, and the results are shown in Table 2. The raw water used in the biological treatment test had a BOD of 2,298 mg / L and a CODcr of 2,580 mg / L.
[0063]
[0064] The amount of sludge adhered per gram of carrier (weight of fiber bundle) after 10 days was 0.691 g. The evaluation results of BOD and CODcr of the biological treatment carrier after 3 days, 8 days, and 10 days from the start of raw water flow were as shown in Table 3.
[0065]
[0066] Comparative Example 1 A nylon 6 fiber having a total fineness of 1950 dtex, 150 filaments, a monofilament fineness of 13 dtex, a trilobal cross-sectional shape of the monofilament with a deformation rate of 1.7, and a crimp rate of 34%, was produced in the same manner as in Example 1, except that a nylon 6 raw polymer (manufacturer: Bestory Advanced Materials Co. Ltd., product number: BE3280-3) having the number of amino terminal groups of 43.0 μeq / g, the number of carboxyl terminal groups of 54.0 μeq / g, an amino terminal group molar fraction FA of 0.443, and a relative viscosity ηr of 2.75 was used, and an oil solution containing an anionic surfactant was used during production.
[0067] The polymer properties of this nylon 6 fiber were as follows: the number of amino terminal groups was 40.0 μeq / g, the number of carboxyl terminal groups was 50.0 μeq / g, the molar fraction of amino terminal groups was FA 0.444, and the relative viscosity ηr was 2.70. The adhesion rate of the oil solution containing an anionic surfactant to the obtained nylon 6 fiber was 0.5 wt%.
[0068] The obtained nylon 6 fiber was deoiled in a Soxhlet extractor using ethanol as a solvent, and the zeta potential was measured before and after deoiling at pH = 6, 7, and 8. The zeta potentials of the obtained nylon 6 fiber measured at pH = 6, 7, and 8 are shown in Table 4.
[0069]
[0070] A biological treatment test was conducted using the obtained nylon 6 fiber as a biological treatment carrier, and the results are shown in Table 5 below. The raw water used in the biological treatment test had the following characteristics: BOD = 2,054 mg / L, CODcr = 2,555 mg / L.
[0071]
[0072] The amount of sludge adhered per gram of carrier (weight of fiber bundle) after 10 days was 0.537 g. The evaluation results of BOD and CODcr of the biological treatment carrier after 3 days, 8 days, and 10 days from the start of raw water flow were as shown in Table 6.
[0073]
[0074] Example 2 Caprolactam crystals were melted in a melter, and in an adjusting tank, 2.65 mol (=47.7 g) of water per 1 kg of caprolactam and 6.3 mmol (=0.77 g) of benzoic acid as an end-capping agent were mixed with 1 kg of caprolactam. This adjusted raw material was retained for 7 hours in an atmospheric pressure polymerization tower heated to 255°C. When the raw material reached polymerization equilibrium, it was discharged in the form of a strand from the bottom of the tower into a water tank and pelletized.
[0075] The pellets were then fed to the top of the extraction tower, and the monomers and oligomers were countercurrently extracted with hot water fed from the bottom of the tower and continuously removed from the bottom of the tower. The hot-water-extracted pellets were dried in an inert gas atmosphere at about 100°C to obtain nylon 6 polymer.
[0076] The resulting nylon 6 polymer had the number of amino terminal groups of 47.0 μeq / g, the number of carboxyl terminal groups of 52.9 μeq / g, an amino terminal group molar fraction FA of 0.470, and a relative viscosity ηr of 2.81. Using this as a raw polymer, a nylon 6 fiber was produced in the same manner as in Example 1, except that NF-20443C oil solution manufactured by GTI, Inc. of the United States, which contains a cationic surfactant, was used as the oil solution to be used after spinning and cooling and solidifying, with the result that the total fineness was 1950 dtex, the number of filaments was 150, and the monofilament fineness was 13 dtex, the monofilament deformation rate was 3.15, and the crimp rate was 42%.
[0077] The polymer properties of this nylon 6 fiber were as follows: the number of amino terminal groups was 43.0 μeq / g, the number of carboxyl terminal groups was 50.0 μeq / g, the molar fraction of amino terminal groups FA was 0.462, and the relative viscosity ηr was 2.75. The adhesion rate of the oil agent containing a cationic surfactant to the obtained nylon 6 fiber was 0.5 wt%.
[0078] The obtained nylon 6 fiber was deoiled in a Soxhlet extractor using ethanol as a solvent, and the zeta potential was measured before and after deoiling at pH = 6, 7, and 8. The zeta potentials of the obtained nylon 6 fiber measured at pH = 6, 7, and 8 are shown in Table 7.
[0079]
[0080] A biological treatment test was conducted using the obtained fibers as a biological treatment carrier, and the results were as shown in Table 8. The raw water used in the biological treatment test had a BOD of 2,200 mg / L and a CODcr of 2,700 mg / L.
[0081]
[0082] The amount of sludge attached per 1 g of carrier (weight of fiber bundle) after 10 days was 0.700 g. The evaluation results of BOD and CODcr of the biological treatment carrier 3 days, 8 days, and 10 days after the start of raw water flow were as shown in Table 9.
[0083]
[0084] The biological treatment carrier of the present invention can be used for the biological treatment of wastewater and sewage in sewage plants, food factories, beverage factories, chemical factories, cosmetics factories, dye factories, pharmaceutical factories, car seat factories, automobile factories, etc.
Claims
1. A biological treatment carrier made of nylon fiber, characterized in that the polymer characteristics of the nylon fiber include an amino terminal group count of 40 μeq / g or more and an amino terminal group molar fraction FA of 0.45 or more, and the relative viscosity ηr of the nylon fiber polymer is 2.5 or more.
2. The carrier for biological treatment according to claim 1, further comprising a cationic surfactant attached to the surface of the nylon fiber, and the attachment of the cationic surfactant to the nylon fiber changes the zeta potential of the surface of the nylon fiber by +10 to +30 mV in the pH range of 6 to 8.
3. A carrier for biological treatment according to claim 1 or 2, wherein the nylon fiber is composed of one or more monofilaments, and the fineness of said monofilaments is 3 to 35 dtex.