Hardened body of hydraulic composition

MYPI2025006307A0Undetermined Publication Date: 2024-10-28KURARAY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025006307
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-25
Publication Date
2024-10-28

AI Technical Summary

Technical Problem

Current hydraulic compositions used in building materials lack high impact resistance, dimensional stability, and low water absorption while maintaining high bending strength, which are essential for advanced building applications.

Method used

A cured product of a hydraulic composition containing alkali-resistant fibers, calcium silicate, and calcium aluminate, with a specific pore size distribution and content of calcium oxide, calcium hydroxide, and calcium carbonate, is developed, utilizing a hydration reaction and pozzolanic reaction between cement, slag, and slaked lime to create a dense and strong matrix.

Benefits of technology

The resulting product exhibits high impact resistance, dimensional stability, low water absorption, and high bending strength, making it suitable for various building material boards such as interior and exterior wall materials, roofing, and flooring.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a hardened body of a hydraulic composition, the hardened body comprising: an alkali-resistant fiber; calcium silicate; and calcium aluminate, wherein a ratio of a pore volume in a range of from 11 to 300,000 nm to a pore volume in a range of from 6 to 10 nm in a pore size distribution of the hardened body determined by a mercury intrusion method is 14 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Cured product of hydraulic composition

[0001] This patent application claims priority under the Paris Convention of Japanese Patent Application No. 2023-74534 (filed April 28, 2023), the entire contents of which are incorporated herein by reference. The present invention relates to a cured product of a hydraulic composition and a building board comprising the cured product.

[0002] Although hydraulic compositions containing cement are highly versatile materials, the cement manufacturing process generates large amounts of carbon dioxide. Therefore, in order to reduce the impact on climate change, efforts are being made to reduce the amount of cement used in the civil engineering and construction sectors.

[0003] For example, Patent Document 1 describes a cement-free hardening composition that uses a cement-free binder consisting of ground granulated blast furnace slag, slaked lime, and optionally fly ash or silica fume. This binder is blended with a high-performance air-entraining water-reducing agent such as a polycarboxylic acid, and optionally a water-soluble admixture primarily composed of multiple inorganic compounds such as calcium ions, magnesium ions, sodium ions, and alkali metal ions, and fresh water. Patent Document 2 describes an inorganic board that is a hardened mat formed by dehydrating a slurry containing blast furnace slag, gypsum, an alkaline material, reinforcing fibers, and an inorganic admixture. This inorganic board has a cement content of 0 to 11% by mass and is suitable for use as a building board. Patent Document 3 also describes a laminated molded board that includes two or more molded boards formed from a hardenable composition containing a specific amount of a specific blast furnace slag as an aluminosilicate source, an alkaline metal hydroxide, cellulose-based fibers, and alkali-resistant fibers. Furthermore, Patent Document 4 describes a hardened body of a hardenable composition containing a specific amount of blast furnace slag as an aluminosilicate source, an alkali activator, and an alkali-resistant fiber, the hardened body having a specific moisture content.

[0004] JP 2012-171855 JP 2013-216534 WO 2022 / 004640 WO 2022 / 004643

[0005] However, there is still a demand for a cured product having higher flexural strength and impact resistance while maintaining dimensional stability and low water absorption. Therefore, an object of the present invention is to provide a cured product of a hydraulic composition having high impact resistance, high dimensional stability, low water absorption, and high flexural strength.

[0006] The present inventors have conducted extensive research to solve the above-mentioned problems, and have completed the present invention. Specifically, the present invention encompasses the following preferred embodiments. [1] A hardened product of a hydraulic composition, the hardened product comprising alkali-resistant fibers, calcium silicate, and calcium aluminate, wherein the ratio of the volume of pores in the range of 11 to 300,000 nm to the volume of pores in the range of 6 to 10 nm in the pore size distribution of the hardened product determined by mercury intrusion porosimetry is 14 or less. [2] The hardened product according to [1], wherein the total content of calcium oxide, calcium hydroxide, and calcium carbonate crystals measured by powder X-ray diffraction is 15 mass% or less, based on the mass of the hardened product excluding the fiber component. [3] The hardened product according to [1] or [2], wherein the average fiber diameter of the alkali-resistant fibers is 3 to 900 μm. [4] The hardened product according to any of [1] to [3], wherein the aspect ratio of the alkali-resistant fibers is 30 to 2,500. [5] The hardened product according to any one of [1] to [4], wherein the alkali-resistant fiber has a tensile strength of 5 cN / dtex or more. [6] The hardened product according to any one of [1] to [5], wherein the alkali-resistant fiber is one or more fibers selected from the group consisting of polyvinyl alcohol-based fibers, polypropylene fibers, and polyethylene fibers. [7] The hardened product according to any one of [1] to [6], wherein the hydraulic composition comprises, relative to the total solid content of the hydraulic composition, 8 to 72 mass% cement, 72 to 18 mass% slag, 0.5 to 12 mass% slaked lime, and 0.1 to 5 mass% alkali-resistant fiber. [8] The hardened product according to [7], wherein the average particle size of the slaked lime is 3 to 600 μm. [9] The hardened product according to any one of [1] to [8], further comprising 0.1 to 10 mass% pulp relative to the mass of the hardened product.

[10] The cured product according to any one of [1] to [8], wherein the cured product does not contain pulp and has a water absorption of 1 to 25% as determined in accordance with JIS A 5430: 2018.

[11] The cured product according to [9], wherein the water absorption of the cured product is 5 to 40% as determined in accordance with JIS A 5430: 2018.

[12] The cured product according to any one of [1] to

[11] , wherein the pore volume in the range of 6 to 10 nm in the pore size distribution of the cured product as determined by mercury intrusion porosimetry is 0.05 mL / g or more.

[13] The cured product according to any one of [1] to

[12] , wherein the pore volume in the range of 11 to 300,000 nm in the pore size distribution of the cured product determined by mercury intrusion porosimetry is 0.3 to 3.0 mL / g.

[14] A building board comprising the cured product according to any one of [1] to

[13] .

[0007] According to the present invention, it is possible to provide a hardened product of a hydraulic composition having high impact resistance, high dimensional stability, low water absorption, and high flexural strength.

[0008] Hereinafter, embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.

[0009] [Hardened Product] The hardened product of the present invention is a hardened product of a hydraulic composition, and the hardened product contains an alkali-resistant fiber, calcium silicate, and calcium aluminate. In the pore size distribution of the hardened product determined by mercury intrusion porosimetry, the ratio (B) / (A) of the volume of pores in the range of 11 to 300,000 nm to the volume of pores in the range of 6 to 10 nm is 14 or less.

[0010] The reasons why the hardened body of the present invention has high impact resistance, high dimensional stability, low water absorption, and high flexural strength are unclear, but the following mechanism of action is presumed. The hardened body of the present invention can be produced, for example, by curing a hydraulic composition containing cement, slag, slaked lime, and alkali-resistant fibers. During the curing process, not only does the cement hydration reaction occur, but the silicon and aluminum contained in the slag also react with the slaked lime. Unlike typical geopolymer-like hardening reactions, this reaction occurs primarily on the surface of the slag, so a relatively small amount of calcium is required. Furthermore, the reaction is relatively slow, resulting in the formation of fine, dense pores. Water penetration into the fine pores is also resistant. Furthermore, the fine pores do not easily impede the adhesion between the fiber and the matrix, so the reinforcing effect of the fibers is less likely to be reduced. As a result, the hardened body exhibits high strength and impact resistance. Furthermore, because the reaction proceeds on the slag surface without the need for large amounts of calcium, the amounts of cement and slaked lime used can be reduced, and the formation of relatively large pores is less likely. As a result, it is presumed that the cured product of the present invention has high impact resistance, high dimensional stability, low water absorption, and high bending strength, although the above is merely presumed and the present invention is not limited to this mechanism of action.

[0011] Calcium silicate and calcium aluminate are produced as the hardening of a hydraulic composition containing cement and slag progresses, and are usually contained in the hardened body as hydrates, i.e., calcium silicate hydrate (calcium silicate hydrate) and calcium aluminate hydrate (calcium aluminate hydrate), respectively.

[0012] The total content of calcium silicate and calcium aluminate contained as crystals in the hardened body is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, based on the mass of the hardened body excluding the fiber component. The upper limit is not particularly limited, but may be 50% by mass or less, 40% by mass or less, 30% by mass or less, or 10% by mass or less. The total content is preferably 1 to 50% by mass, more preferably 2 to 40% by mass, and even more preferably 3 to 10% by mass, based on the mass of the hardened body excluding the fiber component. When the total content is equal to or greater than the lower limit and equal to or less than the upper limit, or within the above range, the hardened body can have higher bending strength. The total content can be adjusted to be equal to or greater than the lower limit and equal to or less than the upper limit, or within the above range, by adjusting the amounts of the pozzolanic reactive material and calcium source, such as cement, slag, and slaked lime, in the hydraulic composition. The total content, the contents of calcium oxide, calcium hydroxide, and calcium carbonate contained as crystals in the hardened body described below, and the total content of calcium oxide, calcium hydroxide, and calcium carbonate contained as crystals in the hardened body described below can be measured using powder X-ray diffraction, for example, by the method described in the Examples described below.

[0013] The alkali-resistant fiber has the effect of increasing the impact resistance and bending strength of the set body, and further has the effect of preventing a decrease in the impact resistance and / or bending strength of the set body by suppressing cracks that may occur during the curing and drying process of the hydraulic composition.

[0014] The alkali-resistant fiber may be inorganic or organic, as long as it has chemical resistance to alkali. Examples of alkali-resistant inorganic fibers include alkali-resistant glass fibers, steel fibers, stainless steel fibers, and carbon fibers. Examples of alkali-resistant organic fibers include various alkali-resistant fibers such as polyvinyl alcohol (hereinafter sometimes referred to as "PVA") fibers, polyolefin fibers (e.g., polyethylene fibers and polypropylene fibers), ultra-high molecular weight polyethylene fibers, polyamide fibers (e.g., polyamide 6, polyamide 6,6, and polyamide 6,10), aramid fibers (e.g., para-aramid fibers), polyparaphenylene benzobisoxazole fibers (e.g., polyparaphenylene benzoxazole (PBO) fibers), nylon fibers, acrylic fibers, rayon fibers (e.g., polynosic fibers and solvent-spun cellulose fibers), acetate fibers, polyphenylene sulfide fibers (PPS fibers), and polyether ether ketone fibers (PEEK fibers). These alkali-resistant fibers may be used alone or in combination of two or more. In this specification, different types of alkali-resistant fibers include not only different types of systems constituting the fibers, such as polyvinyl alcohol-based fibers and polyolefin-based fibers, but also different physical properties of the materials constituting the fibers, such as polyvinyl alcohol-based fibers with different degrees of polymerization and / or saponification.

[0015] Among these fibers, polyvinyl alcohol fibers, polypropylene fibers, and polyethylene fibers are preferably used because they can impart superior reinforcing properties to the cured product and can be produced at low cost. Therefore, in one embodiment of the present invention, the alkali-resistant fiber is preferably one or more fibers selected from the group consisting of polyvinyl alcohol fibers, polypropylene fibers, and polyethylene fibers.

[0016] In a preferred embodiment of the present invention, the alkali-resistant fiber is preferably a polyvinyl alcohol-based fiber. When the alkali-resistant fiber is a polyvinyl alcohol-based fiber, a cured product having higher impact resistance or higher bending strength, particularly high bending strength, can be obtained. The reason for this is not clear, and it is not intended to be limited to the following reasons. However, it is thought that polyvinyl alcohol-based fibers produced by solution spinning are easily fibrillated due to less entanglement of the resin molecular structure in the fiber, and when the cured product is broken, the polyvinyl alcohol-based fiber fibrillates in the process, absorbing the breaking energy and imparting impact resistance or bending strength, particularly bending strength, to the cured product.

[0017] The average fiber diameter of the alkali-resistant fiber is preferably 3 to 900 μm, more preferably 4 to 300 μm, even more preferably 5 to 50 μm, still more preferably 5 to 30 μm, and most preferably 8 to 25 μm. Furthermore, the preferred average fiber diameter for each construction method is 5 to 15 μm for systems that do not use aggregate, and 15 to 40 μm for systems that use aggregate. When the average fiber diameter of the alkali-resistant fiber is within the above range, such alkali-resistant fiber has sufficient fiber strength, can be produced industrially stably, and can be more uniformly dispersed in the hydraulic composition or hardened body. The average fiber diameter of the alkali-resistant fiber can be determined by randomly selecting 100 fibers, measuring the fiber diameter at the center of each fiber in the longitudinal direction using an optical microscope, and calculating the average value.

[0018] The average fiber length of the alkali-resistant fiber is preferably 1 to 40 mm, more preferably 1.5 to 18 mm, and even more preferably 2 to 10 mm, from the viewpoint of achieving both good dispersibility of the fiber in the hydraulic composition and good reinforcing properties of the hydraulic composition after hardening. The average fiber length of the alkali-resistant fiber and the tensile strength described later can be determined in accordance with JIS L 1015:2010.

[0019] From the viewpoint of achieving both good dispersibility of the fibers in the hydraulic composition and good reinforcing properties of the hydraulic composition after hardening, the aspect ratio of the alkali-resistant fiber is preferably 30 to 2500, more preferably 50 to 1000, and even more preferably 200 to 600. The aspect ratio means the ratio of fiber length to fiber diameter (fiber length / fiber diameter). The aspect ratio of the alkali-resistant fiber can be calculated from the average fiber length and average fiber diameter described above.

[0020] The tensile strength of the alkali-resistant fiber is preferably 5 cN / dtex or more, more preferably 8 cN / dtex or more, even more preferably 10 cN / dtex or more, and even more preferably 13 cN / dtex or more. When the tensile strength of the alkali-resistant fiber is equal to or greater than the lower limit, the reinforcing performance of the cured body can be improved. The upper limit of the tensile strength of the alkali-resistant fiber is set appropriately depending on the type of fiber, but may be, for example, 30 cN / dtex or less, 25 cN / dtex or less, or 20 cN / dtex or less. The tensile strength is preferably 5 to 30 cN / dtex, more preferably 8 to 25 cN / dtex, even more preferably 10 to 20 cN / dtex, and even more preferably 13 to 20 cN / dtex.

[0021] When a PVA-based fiber, such as a vinylon fiber, is used as the alkali-resistant fiber, the PVA-based fiber may have the following properties. The degree of polymerization of the PVA-based polymer constituting the PVA-based fiber can be appropriately selected depending on the purpose and is not particularly limited. In consideration of the mechanical properties of the resulting fiber, the viscosity-average degree of polymerization of the PVA-based polymer determined from the viscosity of an aqueous solution at 30°C is preferably about 500 to 20,000, more preferably about 800 to 15,000, and even more preferably about 1,000 to 10,000. Among these, from the viewpoint of the strength of the resulting fiber, the viscosity-average degree of polymerization of the PVA-based polymer is preferably 1,000 or more, more preferably 1,200 or more, more preferably 1,500 or more, and particularly preferably 1,750 or more. The PVA-based polymer may be a medium-degree of polymerization product with a viscosity-average degree of polymerization of 1,000 to less than 3,000, or a high-degree of polymerization product with an average degree of polymerization of 3,000 or more.

[0022] The degree of saponification of the PVA-based polymer can also be appropriately selected depending on the purpose and is not particularly limited. From the viewpoint of the mechanical properties of the resulting fiber, the degree of saponification of the PVA-based polymer may be, for example, 95 mol% or more, preferably 98 mol% or more. The degree of saponification of the PVA-based polymer may be 99 mol% or more, or may be 99.8 mol% or more. The degree of saponification of the PVA-based polymer may be, for example, 95 to 100 mol%, preferably 98 to 100 mol% (e.g., 99 to 100 mol% or 99.8 mol% to less than 100 mol%). When the degree of saponification of the PVA-based polymer is equal to or greater than the above-mentioned lower limit or within the above-mentioned range, the resulting fiber can have better mechanical properties, processability, production costs, etc.

[0023] PVA-based fibers can be produced by dissolving such a PVA-based polymer in a solvent, spinning it by any of wet, dry-wet, and dry methods, and then hot-drawing it. Wet spinning is a method in which the spinning dope is directly discharged from a spinning nozzle into a solidification bath. Dry-wet spinning is a method in which the spinning dope is once discharged from a spinning nozzle into air or an inert gas at a given distance and then introduced into a solidification bath. Dry spinning is a method in which the spinning dope is discharged into air or an inert gas. After spinning, the PVA-based fibers may be stretched as necessary. Furthermore, they may be subjected to acetalization or other treatments commonly performed on PVA-based fibers.

[0024] The solvent used in the spinning solution for PVA-based fibers is not particularly limited as long as it is capable of dissolving PVA. For example, water, dimethyl sulfoxide (DMSO), dimethylformamide, dimethylacetamide, and polyhydric alcohols (e.g., glycerin, ethylene glycol, triethylene glycol, etc.) may be used alone or in combination. In the present invention, when wet spinning is performed, water or an organic solvent is preferably used as the solvent. Among these, water and DMSO are particularly preferred from the viewpoints of ease of supply and environmental impact. The polymer concentration in the spinning solution varies depending on the composition and degree of polymerization of the PVA-based polymer and the type of solvent, but is generally 6 to 60% by mass.

[0025] The above solvents may also be used in dry spinning, and in that case, either water or an organic solvent may be used.

[0026] The spinning dope may contain additives other than the PVA polymer depending on the purpose, as long as the effects of the present invention are not impaired. Examples of additives include boric acid, surfactants, antioxidants, decomposition inhibitors, antifreeze agents, pH adjusters, opacifying agents, colorants, and oils. These may be contained alone or in combination of two or more.

[0027] The solvent used in the solidification bath may be appropriately selected depending on the type of solvent used in the spinning dope. When the spinning dope is an aqueous solution, the solidification bath may be, for example, an aqueous solution of an inorganic salt (e.g., sodium sulfate, ammonium sulfate, sodium carbonate, sodium hydroxide, etc.) capable of solidifying a PVA-based polymer, or an alkaline aqueous solution. When the spinning dope is an organic solvent, the solidification bath may be, for example, an organic solvent capable of solidifying a PVA-based polymer, such as an alcohol (e.g., methanol, ethanol, propanol, butanol, etc.), or a ketone (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.).

[0028] In the present invention, PVA-based fibers obtained by dry spinning or PVA-based fibers obtained by wet spinning from a spinning dope containing water or an organic solvent as a solvent are preferred from the viewpoint of the tensile strength of the fibers.

[0029] In order to extract and remove the solvent of the spinning dope from the solidified raw yarn, the raw yarn may be passed through an extraction bath, or the raw yarn may be wet-stretched simultaneously during extraction. After wet stretching, the fiber may be dried and, if necessary, further subjected to hot stretching. When stretching is performed, the total stretch ratio (the product of the wet stretching ratio and the stretch ratio after drying) may be, for example, 5 to 25 times, preferably about 8 to 20 times.

[0030] As the alkali-resistant fiber, commercially available fibers may be used, and examples thereof include organic fibers such as polyvinyl alcohol fibers manufactured by Kuraray Co., Ltd. and polypropylene fibers manufactured by Valchip Corporation, and inorganic fibers such as glass fibers manufactured by Nippon Electric Glass Co., Ltd. and Pacific Materials Corporation.

[0031] In a preferred embodiment of the present invention, the content of the alkali-resistant fiber is preferably 0.3 mass% or more, more preferably 0.5 mass% or more, even more preferably 1.0 mass% or more, and preferably 5.0 mass% or less, more preferably 4.5 mass% or less, and even more preferably 4.0 mass% or less, relative to the mass of the cured body. Furthermore, the content of the alkali-resistant fiber is preferably 0.3 to 5.0 mass%, more preferably 0.5 to 4.5 mass%, and even more preferably 1.0 to 4.0 mass%, relative to the mass of the cured body. When the content of the alkali-resistant fiber is at least the lower limit and is at most the upper limit, or is within the above range, the produced cured body can have higher impact resistance, higher bending strength, and higher dimensional stability.

[0032] The content of alkali-resistant fiber in the hardened body can be calculated from the blending ratio of each component when preparing the hydraulic composition before hardening the hardened body. Naturally, the content of alkali-resistant fiber in the hardened body can be determined by this calculation whether or not the hardened body contains organic substances other than alkali-resistant fiber.

[0033] In the pore size distribution of the cured body determined by mercury intrusion porosimetry, the ratio (B) of the pore volume (B) in the range of 11 to 300,000 nm to the pore volume (A) in the range of 6 to 10 nm is 14 or less, preferably 13 or less, more preferably 12 or less, and even more preferably 11 or less (e.g., 10 or less). The ratio (B) / (A) is usually 3 or more, preferably 4 or more, more preferably 5 or more, and even more preferably 6 or more. The ratio (B) / (A) is usually 3 to 14, preferably 4 to 13, more preferably 5 to 12, and even more preferably 6 to 11 (e.g., 6 to 10).

[0034] In a preferred embodiment of the present invention, the pore volume (A) in the 6 to 10 nm range (commonly referred to as gel voids) in the pore size distribution of the cured product determined by mercury intrusion porosimetry is preferably 0.05 mL / g or more, more preferably 0.08 mL / g or more, even more preferably 0.10 mL / g or more, even more preferably 0.11 mL / g or more, and most preferably 0.12 mL / g or more, and may be 0.90 mL / g or less, 0.70 mL / g or less, 0.50 mL / g or less, or 0.30 mL / g or less. The pore volume (A) is preferably 0.05 to 0.90 mL / g, more preferably 0.08 to 0.70 mL / g, even more preferably 0.10 to 0.50 mL / g, even more preferably 0.11 to 0.30 mL / g, and most preferably 0.12 to 0.30 mL / g. The pore volume (A) indicates the dense structure that water cannot penetrate, which is obtained by the reaction of the hardened body matrix. When the pore volume (A) is equal to or greater than the lower limit and equal to or less than the upper limit, or within the above range, the hardened body can have suitable denseness, and therefore the hardened body can have higher impact resistance, higher dimensional stability, lower water absorption, and / or higher bending strength. The pore volume (A) can be adjusted to a value equal to or greater than the lower limit and equal to or less than the upper limit, or within the above range, by, for example, adjusting the proportions of cement, slag, slaked lime, etc., and / or adjusting the conditions for molding the hardened body (e.g., curing conditions).

[0035] In a preferred embodiment of the present invention, the pore volume (B) in the pore size distribution of the cured body measured by mercury intrusion porosimetry in the range of 11 to 300,000 nm (commonly referred to as capillary voids) is preferably 3.0 mL / g or less, more preferably 2.0 mL / g or less, more preferably 1.9 mL / g or less, even more preferably 1.5 mL / g or less, and particularly preferably 1.3 mL / g or less. The pore volume (B) indicates the coarse structure obtained by the reaction of the cured body matrix, into which water can enter. When the pore volume (B) is equal to or less than the upper limit, the cured body can have suitable density, thereby resulting in higher impact resistance, higher dimensional stability, lower water absorption, and / or higher bending strength. The lower limit of the pore volume (B) is not particularly limited. The pore volume (B) may be 0.3 mL / g or more, 0.5 mL / g or more, 0.7 mL / g or more, or 1.0 mL / g or more. The pore volume (B) is preferably 0.3 to 3.0 mL / g, more preferably 0.5 to 2.0 mL / g, even more preferably 0.7 to 1.9 mL / g, still more preferably 1.0 to 1.5 mL / g, and particularly preferably 1.0 to 1.3 mL / g. The pore volume (B) can be adjusted to be equal to or greater than the lower limit and equal to or less than the upper limit, or to a value within the above range, for example, by adjusting the proportions of cement, slag, slaked lime, etc., and / or by adjusting the conditions for molding the hardened body (e.g., pressing conditions), and / or by adjusting the particle size of the materials used.

[0036] Furthermore, the ratio (B) / (A) was defined as a parameter expressing the dense structure (the gel voids). The ratio (B) / (A) represents the ratio of coarse structure to dense structure, and a smaller value indicates a denser structure. When the ratio (B) / (A) is equal to or less than the upper limit and equal to or greater than the lower limit, the hardened body can have suitable density, resulting in higher impact resistance, higher dimensional stability, lower water absorption, and / or higher bending strength. The ratio (B) / (A) can be adjusted to a value equal to or greater than the lower limit by, for example, adjusting the proportions of cement, slag, and hydrated lime, and / or by adjusting the conditions for molding the hardened body (e.g., pressing conditions), and / or by adjusting the particle size of the materials used. The pore volume (A), pore volume (B), and pore volume ratio (B) / (A) can be determined by the methods described in the Examples.

[0037] In a preferred embodiment of the present invention, the total content of calcium oxide, calcium hydroxide, and calcium carbonate crystals, as measured by powder X-ray diffraction, is preferably 15% by mass or less, more preferably 12% by mass or less, even more preferably 10% by mass or less, and particularly preferably 8% by mass or less, based on the mass of the hardened body excluding fibrous components. Calcium oxide and calcium hydroxide are present in the hardened body primarily as unreacted reactants (e.g., a mixture containing cement, slag, and hydrated lime), while calcium carbonate is present in the hardened body primarily as a reaction product of calcium hydroxide and carbon dioxide. Therefore, a total content of calcium oxide and calcium hydroxide below the upper limit indicates that the hardened body contains few unreacted reactants, i.e., the reactants have reacted in just the right amount. A total content below the upper limit ensures that the hardened body has a dense structure and a desirable pore volume ratio (B) / (A). Furthermore, deterioration of the hardened body's physical properties (e.g., impact resistance, dimensional stability, and / or low water absorption), particularly over time, due primarily to unreacted reactants, can be suppressed. The total content can be adjusted to be equal to or less than the upper limit, for example, by adjusting the proportions of cement, slag, slaked lime, etc., by adjusting the slaked lime so that it has a specific average particle size in the hydraulic composition, and / or by adjusting the curing conditions (temperature, humidity, etc.). The total content, as well as the calcium oxide crystalline content, calcium hydroxide crystalline content, and calcium carbonate crystalline content measured by powder X-ray diffraction described below, can be measured by the method described in the Examples described below. Since the lower the total content, the better, the lower limit is not particularly limited and is equal to the detection limit of the measuring device.

[0038] In a preferred embodiment of the present invention, the total content of unreacted calcium components, i.e., calcium oxide and calcium hydroxide crystals, as measured by powder X-ray diffraction, is preferably 12% by mass or less, more preferably 8% by mass or less, and even more preferably 4% by mass or less, based on the mass of the cured body excluding the fiber component. The lower limits of these contents are similarly not particularly limited and are equal to the detection limit of the measuring device.

[0039] In one embodiment of the present invention, the cured product further contains pulp in an amount of preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, based on the mass of the cured product. Pulp has the effect of improving the yield rate in the papermaking process when producing the cured product by a papermaking method, and of increasing the impact resistance and bending strength of the cured product. Therefore, when the pulp content is equal to or greater than the lower limit, the yield rate in the papermaking process when producing the cured product by a papermaking method can be increased, and a cured product with higher impact resistance and bending strength can be obtained. On the other hand, if the pulp content is too high, the water absorbency of the cured product may be reduced. Therefore, from the viewpoint of water absorbency, the pulp content is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 6.5% by mass or less, based on the mass of the cured product. When the pulp content is equal to or less than the upper limit, problems such as a decrease in the effect of inhibiting the penetration of corrosive substances (chlorine, carbon dioxide, various organic acids such as sulfate ions) can be avoided. The pulp content is preferably 0.1 to 10 mass %, more preferably 1 to 8 mass %, and even more preferably 2 to 6.5 mass %, based on the mass of the hardened body. The pulp content can be calculated from the blending ratio of each component when preparing the hydraulic composition before hardening the hardened body.

[0040] Examples of pulp include natural pulp such as wood pulp, cotton linter pulp, and hemp.

[0041] The pulp that can be blended in the hydraulic composition may be beaten or unbeaten. From the viewpoint of impact resistance and bending strength, it is preferable to use beaten pulp, and it is more preferable to use pulp whose beating degree, measured in accordance with the Canadian standard type of freeness test method JIS P8121-1976, is preferably 50 to 400 mL, more preferably 100 to 150 mL, in terms of CSF value.

[0042] Examples of pulp include conifers, hardwoods, Manila hemp, Mitsumata, paper mulberry, gampi, salago, mulberry, straw, bamboo, reeds, sabai, larang grass, esparto, bagasse, sisal, kenaf, linter, banana, and waste paper. Examples of conifers include those of the Cedaraceae, Pinaceae, Cupressaceae, and Araucaria families. Examples of hardwoods include those of the Ulmaceae, Fagaceae, Myrtaceae, Cerifera, Oleaceae, Rutaceae, Birchaceae, Mapleaceae, Juglandaceae, Tiliaceae, Araliaceae, Sapotaceae, Celastraceae, Apocynaceae, Verbenaceae, Magnoliaceae, and Sterculiaceae families. These pulps may be bleached or unbleached. These pulps may be used alone or in combination.

[0043] [Method for Producing a Hardened Product] The hardened product of the present invention is based on a hydraulic composition. That is, the hardened product of the present invention can be produced by hardening the hydraulic composition, for example, by a method (papermaking method) comprising suspending solids such as cement, slag, slaked lime, and alkali-resistant fibers in an aqueous medium to prepare a slurry (hydraulic composition), filtering the filtered slurry through a wire mesh, and molding and curing the sheet-like product, or by a method comprising suspending solids such as cement, slag, slaked lime, and alkali-resistant fibers in an aqueous medium to prepare a hydraulic composition, and molding the hydraulic composition using a mold.

[0044] <Papermaking method> Papermaking methods include the cylinder-net papermaking method (Hatchek method) or Fourdrinier papermaking method, in which the filtered thin sheet-like material is successively laminated on a making roll until it reaches the desired thickness to obtain a hardened body, and the flow-on papermaking method, in which a thickened slurry is supplied onto a felt and successively laminated on a making roll in one or several times until it reaches the desired thickness to obtain a hardened body, etc. From the viewpoints of uniformity of the hardened body and ease of thickness adjustment, the cylinder-net papermaking method or Fourdrinier papermaking method is preferred, and from the viewpoint of mass production, the cylinder-net papermaking method is more preferred.

[0045] The method for producing a hardened body by the cylinder molding method usually includes the steps of: preparing a hydraulic composition by mixing cement, slag, slaked lime, alkali-resistant fiber, water, and, if necessary, optional components described below (hydraulic composition preparation step); molding the obtained hydraulic composition into sheets using a cylinder mold, and stacking the sheets to a desired thickness (sheet stacking step); squeezing the liquid out of the stacked sheets by applying pressure to the sheets and shaping them (squeezing and molding step); and curing the sheets after squeezing (curing step).

[0046] The method for preparing the hydraulic composition is not particularly limited. The hydraulic composition can be prepared by mixing the components using a known or commonly used mixing means such as a mixer. Examples of the mixing means include mixers with high mixing performance, such as vertical mixers, blade mixers, screw mixers, cone mixers, and agitator mixers used in papermaking methods.

[0047] The order of mixing the components is not particularly limited. From the viewpoint of uniform dispersion of the solid components in the hydraulic composition, when pulp is added, it is preferable to first add the pulp to water and stir, then add cement, slag, slaked lime, and any optional components other than pulp, if any, in any order and stir, and finally add the alkali-resistant fiber.

[0048] Examples of cement include Portland cement such as ordinary Portland cement, high-early-strength Portland cement, extra-early-strength Portland cement, and moderate-heat Portland cement; alumina cement; blast-furnace cement; silica cement; and fly ash cement; white Portland cement. These cements may be used alone or in combination of two or more. From the viewpoint of versatility and / or cost, it is preferable to use ordinary Portland cement. From the viewpoint of early strength development, it is preferable to use high-early-strength Portland cement or extra-early-strength Portland cement. From the viewpoint of improving long-term strength, it is preferable to use blast-furnace cement.

[0049] The above-mentioned cement is commercially available, and an example of a commercially available product is ordinary Portland cement manufactured by Taiheiyo Cement Corporation.

[0050] In this specification, slag refers to iron and steel slag. Iron and steel slag is broadly divided into blast furnace slag and steelmaking slag, and either can be used in the present invention. Blast furnace slag is preferred from the viewpoints of higher impact resistance, higher dimensional stability, and lower water absorption of the hardened body. Blast furnace slag includes crystalline slowly cooled slag and amorphous granulated slag, and either can be used in the present invention. Granulated slag is preferred from the viewpoints of further improving the strength of the hardened body or accelerating curing.

[0051] The Blaine specific surface area of ​​the blast furnace slag is preferably 1000 to 9000 cm 2 / g, more preferably 2000 to 8000 cm 2 / g, more preferably 3000 to 7000 cm 2 / g. When the Blaine specific surface area of ​​blast furnace slag is within the above range, the blast furnace slag can have sufficient reaction sites and a suitable average particle size, and as a result, the produced hardened body can exhibit higher impact resistance, higher dimensional stability, and lower water absorption. The Blaine specific surface area of ​​blast furnace slag can be adjusted to fall within the above range, for example, by crushing and classifying the blast furnace slag and using a specific fraction. The Blaine specific surface area of ​​blast furnace slag can be measured, for example, by laser diffraction / scattering.

[0052] The slaked lime may be, for example, solid slaked lime, slaked lime dissolved in water, or a combination thereof, but is not limited thereto. In one embodiment of the present invention, it is preferable to use solid slaked lime as the slaked lime. By using solid slaked lime, the slaked lime can react locally with the slag near the surface of the slag, and a hardened body having suitable density can be obtained.

[0053] In a preferred embodiment, the average particle size of the slaked lime in the hydraulic composition is preferably 3 to 600 μm, more preferably 5 to 400 μm, even more preferably 7 to 200 μm, and particularly preferably 10 to 100 μm. When the average particle size is within the above range, a hardened body with more suitable density can be obtained. The average particle size can be adjusted to within the above range by pulverization and classification. The average particle size can be determined by a common method, for example, by measuring the equivalent circle diameter of 100 randomly selected slaked lime particles using an optical microscope and calculating the average value.

[0054] In another embodiment of the present invention, it is preferable to use slaked lime dissolved in water. Examples of slaked lime dissolved in water include an aqueous solution of slaked lime, such as the circulating water (white water) used in the papermaking process when producing a hardened body by a papermaking method. The circulating water used in the papermaking process may contain solid slaked lime, and such circulating water can be used as slaked lime. Alternatively, a combination of an aqueous solution of slaked lime other than the circulating water used in the papermaking process and solid slaked lime can be used as slaked lime. In these cases, the slaked lime corresponds to a combination of solid slaked lime and slaked lime dissolved in water, and in one embodiment of the present invention, such a combination is preferably used as slaked lime. By using slaked lime dissolved in water or a combination of solid slaked lime and slaked lime dissolved in water, the slaked lime is present in a thin distribution in the hydraulic composition, allowing it to react locally with the slag near the surface of the slag, resulting in a hardened body with suitable density.

[0055] The concentration of slaked lime in the aqueous solution of slaked lime or in the circulation water in the papermaking process is preferably 3 to 12 mass %, more preferably 4 to 11 mass %, and particularly preferably 5 to 10 mass %, from the viewpoint of suitable reactivity.

[0056] As the alkali-resistant fiber, the alkali-resistant fiber described in the previous section [Cured product] can be used. The preferred embodiments described in the previous section [Cured product] also apply to the alkali-resistant fiber.

[0057] In addition to the pulp mentioned above, examples of optional components include mica, aggregates (e.g., fine aggregates such as silica sand, river sand, sea sand, mountain sand, and crushed sand, and coarse aggregates such as gravel and crushed stone), non-reactive fillers such as attapulgite, bentonite, wollastonite, sepiolite, precipitated calcium carbonate, and ground calcium carbonate; fly ash, silica fume, red mud; anionic polymer flocculants; and combinations of two or more of these. When the hydraulic composition contains these optional components, the set body of the hydraulic composition also contains the corresponding optional components. When the hydraulic composition contains silica fume, the pozzolanic reactivity and fine average particle size of silica fume contribute to the densification of the set body. The average particle size of silica fume is typically 0.01 to 1.0 μm, preferably 0.05 to 0.5 μm, and more preferably 0.1 to 0.2 μm.

[0058] The solid content of the hydraulic composition is usually 55 to 6 mass %, preferably 40 to 8 mass %, more preferably 25 to 10 mass %.

[0059] Based on the total solid content of the hydraulic composition, i.e., based on the total mass of the components other than water in the hydraulic composition, the amount of cement is preferably 8 to 72 mass% (more preferably 16 to 60 mass%, even more preferably 24 to 50 mass%), the amount of slag is preferably 72 to 18 mass% (more preferably 66 to 24 mass%, even more preferably 60 to 36 mass%), the amount of slaked lime is preferably 0.5 to 12 mass% (more preferably 2 to 11 mass%, even more preferably 3 to 10%), the amount of alkali-resistant fiber is preferably 0.1 to 5 mass% (more preferably 0.3 to 4.5 mass%, The amount of fly ash is preferably 0 to 10% by mass (more preferably 0.1 to 10% by mass, even more preferably 1 to 8% by mass, and still more preferably 2 to 6.5% by mass), the amount of aggregate is preferably 0 to 50% by mass (more preferably 0 to 40% by mass, even more preferably 0 to 35% by mass), and the amount of silica fume is preferably 0 to 15% by mass (more preferably 0 to 11% by mass, and even more preferably 0 to 8% by mass). When the hydraulic composition contains optional components other than pulp, fly ash, aggregate, and silica fume, the amount thereof may be appropriately selected depending on the type of the optional component.

[0060] In a preferred embodiment, the amount of the strongly alkaline compound relative to the total solids content of the hydraulic composition is preferably 1.0% by mass or less, more preferably 0.5% by mass or less, even more preferably 0.1% by mass or less, and particularly preferably 0% by mass. When the amount of the strongly alkaline compound is below the upper limit or 0% by mass, the geopolymer-like hardening reaction between the strongly alkaline compound and slag, which can result in a porous hardened body, is less likely to occur, resulting in a denser hardened body. Such hardened body can have high impact resistance, high dimensional stability, low water absorption, and high flexural strength. Strongly alkaline compounds include alkali metal hydroxides such as sodium hydroxide, potassium hydroxide, and lithium hydroxide, alkali metal carbonates such as sodium carbonate and potassium carbonate, and combinations of two or more of these, but do not include alkaline earth metal hydroxides such as calcium hydroxide or alkaline earth metal carbonates.

[0061] The hydraulic composition is then placed in the feed tank of a wet papermaking machine, and the solids concentration of the hydraulic composition is usually adjusted to about 10 to 1 mass % (preferably 8 to 3 mass %) using circulating water in the papermaking process. The hydraulic composition supplied from the feed tank to the vat is formed into a sheet on the surface of a cylinder with internal negative pressure by the rotation of the cylinder in the vat, and is then transported to the making roll. The making roll stacks the sheets to the desired thickness, and the stacked sheets are cut to a predetermined length.

[0062] In a preferred embodiment, the yield rate in the papermaking process is preferably 85% or more, more preferably 90% or more. A yield rate equal to or greater than the lower limit mentioned above can provide higher bending strength, higher interlayer adhesion strength, and / or a lower dimensional change rate. The yield rate can be adjusted to equal to or greater than the lower limit mentioned above by adjusting the Blaine specific surface area of ​​the slag, selecting the mesh size of the cylindrical mesh, and / or adjusting the degree of beating of the beaten pulp, if added. From the viewpoint of achieving both yield rate and productivity, the mesh size of the cylindrical mesh is preferably 45 to 55 meshes per inch. The yield rate in the papermaking process can be determined, for example, by the following method. The slurry poured into the cylindrical mesh is scooped up and its mass (A1) is measured. The solid content is filtered using a common filtering device (e.g., a Nutsche filter and a suction bottle), and dried in a dryer at 105°C for 12 hours or more until the dry mass becomes constant, and the mass (B1) of the solid content is measured. The concentration C of the slurry poured into the cylindrical mesh is calculated using the following formula: 1 Calculate the concentration C 1 = (B1 / A1) × 100 Similarly, the slurry that has passed through the cylindrical net is scooped up and its concentration C 2 is calculated using the following formula: 2 = (B2 / A2) x 100 where A2 is the mass of the slurry that has passed through the cylindrical screen and B2 is the mass of the solid content. The yield rate in the papermaking process can be calculated using the following formula: Yield rate in the papermaking process (%) = {(C 1 -C 2 ) / C 1} x 100

[0063] The number of sheets to be laminated depends on the solids concentration of the hydraulic composition and the thickness of the hardened body to be produced, but is usually 12 to 18 sheets when the thickness of the hardened body is about 6 mm.

[0064] The cut sheets are then squeezed and molded using a press. The pressure applied by the press is preferably 2 to 30 MPa, more preferably 3 to 27 MPa, and particularly preferably 4 to 25 MPa. The time for which the pressure is applied is usually 10 to 60 minutes, preferably 15 to 50 minutes, and more preferably 20 to 40 minutes. By setting the pressure within the above range or the time for which the pressure is applied within the above range, the desired pore volume ratio (B) / (A) can be obtained in the cured product, resulting in a cured product with higher impact resistance, higher dimensional stability, lower water absorption, and / or higher bending strength.

[0065] The squeezed sheet is then cured. Curing promotes hardening. Hardening occurs due to the hydration (setting) reaction between cement and slag. However, evaporation of moisture from the sheet inhibits the hydration reaction, potentially preventing hardening. Therefore, the primary curing step is preferably performed in a high-humidity atmosphere where moisture in the sheet does not evaporate, i.e., a relative humidity of preferably 30 to 100%, more preferably 50 to 100%, even more preferably 65 to 100%, even more preferably 80 to 100%, and particularly preferably 90 to 100% (e.g., 100%). The secondary curing step is preferably performed in a high-humidity atmosphere (preferably 30 to 100%, more preferably 40 to 90%, even more preferably 50 to 80%) by placing the sheet in a moisture-impermeable container or bag, or sandwiching the sheet between plastic plates, plastic films (e.g., polyethylene sheets), or metal plates, thereby making it more difficult for moisture in the sheet to evaporate.

[0066] The curing temperature is not particularly limited. The primary curing temperature is, for example, 10 to 90°C, preferably 30 to 80°C, and more preferably 40 to 80°C. The curing temperature may be changed midway within the above-mentioned range. The secondary curing temperature is, for example, 10 to 70°C, preferably 20 to 50°C. The primary curing time depends on the composition of the hydraulic composition and the curing temperature, but is usually 6 to 48 hours, preferably 8 to 36 hours, and more preferably 12 to 24 hours. The secondary curing time is usually 1 to 14 days.

[0067] Secondary curing may also be performed by underwater curing. In this case, the water temperature is typically 10 to 30°C, and the curing time is typically 8 hours to 13 days. After underwater curing at a water temperature of 10 to 30°C for 4 to 24 hours, the secondary curing described in the previous paragraph may be performed for 2 to 13 days.

[0068] A hardened body is obtained by drying after the secondary curing. There are no particular limitations on the drying method, as long as a uniformly dried hardened body is obtained. Usually, the equilibrium moisture content of the hardened body (for example, the moisture content reached when the hardened body is stored in a well-ventilated room for 7 days or more) is about 6% to about 10% by mass, so drying is carried out to a moisture content similar to the equilibrium moisture content. The moisture content and equilibrium moisture content of the hardened body can be simply measured using a Kett moisture meter. Alternatively, the hardened body after drying can be weighed (W 12 ), and then dried in an air dryer equipped with a stirrer at 105°C until a constant weight was reached. The cured product was then weighed (W 13 ) and the following formula: {(W 12 -W 13 ) / W 13}×100.

[0069] <Methods Including Molding Using a Mold> Methods including molding using a mold typically include a step of preparing a hydraulic composition by mixing cement, slag, slaked lime, alkali-resistant fiber, and water, as well as the optional components described above, as needed, and any of the following steps (i) to (iv): (i) a step of pouring the obtained hydraulic composition into an open formwork (casting method), (ii) a step of dehydrating the hydraulic composition by pressing or suction (dehydration molding method), (iii) a step of injecting the hydraulic composition into a closed formwork (injection molding method), and (iv) a step of passing the hydraulic composition through a die to form a product of a specific shape (extrusion molding method). A vacuum extruder may be used in the extrusion molding method. Furthermore, pressure and / or vibration may be applied during molding, as needed, and the hydraulic composition may be pressed by a press using an upper mold, a roll, or the like.

[0070] The step of preparing a hydraulic composition in a method including molding using a mold may be carried out in the same manner as the step of preparing a hydraulic composition in a papermaking method. A predetermined amount of the obtained hydraulic composition may be placed in a press lower mold and dehydrated and molded by a press while applying pressure. The applied pressure may be, for example, 1 to 30 MPa, and the pressing time may be 0.01 to 30 minutes.

[0071] The curing after the molding may be carried out in the same manner as the curing step in the papermaking method. After the secondary curing, a hardened body is obtained by drying. This drying method may also be carried out in the same manner as the drying method in the papermaking method.

[0072] The impact strength of the cured product when dry is preferably 3.0 kJ / m 2 More preferably, 3.5 kJ / m 2 More preferably, 4.0 kJ / m 2 The upper limit of the impact strength of the cured product in a dry state is not limited, but is usually 20.0 kJ / m 2 The impact strength of the cured product in a dry state is preferably 3.0 to 20.0 kJ / m 2 , more preferably 3.5 to 20.0 kJ / m 2 , more preferably 4.0 to 20.0 kJ / m 2The impact strength of the cured body when it absorbs water is preferably 5.0 kJ / m 2 More preferably, 5.3 kJ / m 2 More preferably, 5.5 kJ / m 2 The upper limit of the impact strength of the cured body when it absorbs water is not limited, but is usually 20 kJ / m 2 The impact strength of the cured product when it absorbs water is preferably 5.0 to 20.0 kJ / m 2 , more preferably 5.3 to 20.0 kJ / m 2 , more preferably 5.5 to 20.0 kJ / m 2 is.

[0073] The dimensional change rate of the cured product is preferably 0.20% or less, more preferably 0.16% or less, and even more preferably 0.12% or less. The lower limit of the dimensional change rate of the cured product is not limited, but is usually 0.01% or more. The dimensional change rate is preferably 0.01 to 0.20%, more preferably 0.01 to 0.16%, and even more preferably 0.01 to 0.12%.

[0074] When the cured product does not contain pulp, the water absorption of the cured product measured in accordance with JIS A 5430: 2018 is preferably 1 to 25%, more preferably 3 to 20%, and even more preferably 5 to 15%. When the cured product contains pulp, the water absorption of the cured product measured in accordance with JIS A 5430: 2018 is preferably 5 to 40%, more preferably 7 to 30%, and even more preferably 10 to 20%.

[0075] The bending strength of the cured product when dry is preferably 7 N / mm 2 More preferably, 10 N / mm 2 More preferably, 15 N / mm 2 The upper limit of the bending strength of the cured body in a dry state is not limited, but is usually 100 N / mm 2 The bending strength of the cured product in a dry state is preferably 7 to 100 N / mm 2 , more preferably 10 to 100 N / mm 2 , more preferably 15 to 100 N / mm 2 The bending strength of the cured body when it absorbs water is preferably 6 N / mm2 More preferably, 10 N / mm 2 More preferably, 14 N / mm 2 The upper limit of the bending strength of the cured body when it absorbs water is not limited, but is usually 100 N / mm 2 The bending strength of the cured body when it absorbs water is preferably 6 to 100 N / mm 2 , more preferably 10 to 100 N / mm 2 , more preferably 14 to 100 N / mm 2 is.

[0076] The physical properties of the cured product described above (impact strength in a dry state, impact strength after absorbing water, dimensional change rate, water absorption rate, flexural strength in a dry state, and flexural strength after absorbing water) can be measured by the methods described in the Examples.

[0077] The cured product of the present invention has high impact resistance, high dimensional stability, low water absorption, and high bending strength, and is therefore suitable for use as building boards for interior and exterior wall materials, roofing materials, flooring materials, etc. Accordingly, the present invention also encompasses building boards comprising the cured product of the present invention and building boards made from the cured product of the present invention.

[0078] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Physical properties in the examples and comparative examples were measured or evaluated according to the following procedures.

[0079] <Calcium Silicate, Calcium Aluminate, Calcium Oxide, Calcium Hydroxide, and Calcium Carbonate Crystal Contents> The hardened body was crushed in a mortar and pulverized, and fibers were removed from the crushed material with tweezers. The crushed material from which fibers were removed was analyzed by powder X-ray diffraction to determine the calcium silicate, calcium aluminate, calcium oxide, calcium hydroxide, and calcium carbonate crystal contents in the hardened body. The powder X-ray diffraction measurement conditions were tube voltage: 40 kV, tube current: 15 mA, scan range: 2θ = 5-70°, step width: 0.01°, scan speed: 2° / min. Rietveld analysis was performed using PDXL2 (Rigaku Corporation). In quantitative analysis, alite, belite, ubic C3A, orthorhombic C3A, C4AF, and corundum (internal standard), as well as calcite, portlandite, and lime were appropriately selected depending on the phase contained in the sample, and the crystal content of each mineral phase was quantified. As for the quantitative conditions for C3A, two types of polymorphism were set for calculation purposes, but the evaluation was carried out by summing both polymorphisms and determining the amount of C3A.

[0080] <Pore Volume and Pore Volume Ratio> Two test pieces, approximately 1 cm square, were cut from the cured product to be measured and dried at 105°C ± 5°C for at least 12 hours. They were then placed in a desiccator conditioned with silica gel and allowed to cool to 20°C ± 1.5°C. The pore size distribution of these test pieces was measured by mercury intrusion porosimetry using a mercury intrusion porosimetry pore volume analyzer (MicroActive AutoPore V 9600, manufactured by Micromeritics). The log differential pore volume obtained from the resulting pore size distribution was used to calculate the pore volume (A) in the 6-10 nm range and the pore volume (B) in the 11-300,000 nm range for each test piece. The ratio of the pore volume (B) in the 6-10 nm range to the pore volume (A) in the 11-300,000 nm range for each test piece was calculated using the following formula, and the average value was used as the pore volume ratio (B) / (A) of the cured product. Pore ​​volume ratio (B) / (A)={pore volume (B) in the range of 11 to 300,000 nm} / {pore volume (A) in the range of 6 to 10 nm}

[0081] <Average fiber diameter, aspect ratio, and tensile strength of alkali-resistant fiber> The average fiber diameter of the alkali-resistant fiber was determined by randomly selecting 100 fibers, measuring the fiber diameter at the center of each fiber's length using an optical microscope, and calculating the average value. The aspect ratio (fiber length / fiber diameter) of the alkali-resistant fiber was calculated from the average fiber length and the average fiber diameter. The average fiber length of the alkali-resistant fiber was determined in accordance with JIS L 1015:2010. The tensile strength of the alkali-resistant fiber was determined in accordance with JIS L 1015:2010.

[0082] <Impact Strength> Six Type 1 test specimens conforming to JIS K 7111-1:2012 were cut from the cured product to be measured. To measure the dry impact strength, three test specimens were first dried for 72 hours in an air dryer equipped with a stirrer set at 40°C. The removed test specimens were then placed in a desiccator conditioned with silica gel and allowed to stand until the temperature reached 20°C ± 1.5°C. The impact strength (unnotched) of each test specimen was measured according to JIS K 7111-1:2012, and the average value was used as the dry impact strength of the cured product. To measure the water-absorbed impact strength, three test specimens were first immersed in water at 20°C for 72 hours. The test specimens were then removed, and the water adhering to the surface was wiped off. Immediately thereafter, the impact strength (unnotched) of each test specimen was measured according to JIS K 7111-1:2012, and the average value was used as the water-absorbed impact strength of the cured product. The impact strength in the dry state and when water is absorbed was measured using a Charpy (digital) impact tester, model DG-CB, manufactured by Toyo Seiki Seisakusho Co., Ltd.

[0083] <Dimensional Change Rate> The dimensional change rate (length change rate) of the cured body was measured in accordance with JIS A 5430:2018. Specifically, three rectangular test pieces measuring approximately 160 mm in length and approximately 50 mm in width were cut out from the cured body to be measured, and then these test pieces were placed in a dryer, and the temperature inside the dryer was maintained at 60°C ± 3°C for 24 hours. The test pieces were then removed, placed in a desiccator whose humidity had been adjusted with silica gel, and left to cool to 20°C ± 1.5°C. Next, milky glass was attached to each test piece, and marks were engraved so that the distance between the marks was approximately 140 mm. The length between the marks was measured using a comparator with an accuracy of 1 / 500 mm, and this length was taken as L. 1 The test piece was then placed on a stand so that the longitudinal direction was horizontal, and the top end of the test piece was immersed in water at 20°C ± 1.5°C so that it was approximately 30 mm below the water surface. After 24 hours, the test piece was removed from the water, the water adhering to the surface was wiped off, and the length between the gauge lines was measured again, and this length was recorded as L 2 The dimensional change rate (%) due to water absorption was calculated for each test piece using the following formula, and the average value was used as the dimensional change rate of the cured body. Dimensional change rate = {(L 2 -L 1 ) / L 1} x 100

[0084] <Water absorption rate> The water absorption rate of the cured body was measured in accordance with JIS A 5430:2018. Specifically, four rectangular test pieces, each about 180 mm long and about 50 mm wide, were cut out from the cured body to be measured, and then the test pieces were immersed in water at 20°C ± 1.5°C. After 24 hours, the test pieces were removed, and the water adhering to the surface was wiped off. Immediately, the mass of each test piece (mass W of the test piece at the time of water absorption) was measured. 14 Next, these test pieces were placed in a dryer equipped with a stirrer adjusted to 105°C ± 5°C, dried for 24 hours, then removed, placed in a desiccator whose humidity had been adjusted with silica gel, and left to stand until the temperature reached room temperature of 20°C ± 1.5°C. Thereafter, the mass of each test piece (mass W of the test piece when dried) was measured. 0 The water absorption (%) of each test piece was calculated using the following formula, and the average value was used as the water absorption of the cured body. Water absorption = {(W 14 -W 0 ) / W 0} x 100

[0085] <Flexural Strength> Eight rectangular test pieces, each approximately 180 mm long and 50 mm wide, were cut from the cured product to be measured. To measure the flexural strength in the dry state, four test pieces were first dried for 72 hours in an air dryer equipped with a stirrer set at 40°C. The removed test pieces were then placed in a desiccator conditioned with silica gel and allowed to stand until the temperature reached 20±1.5°C. The flexural strength of each test piece was measured in accordance with JIS A 1408:2017, and the average value was used as the flexural strength of the cured product in the dry state. To measure the flexural strength after water absorption, four test pieces were first immersed in water at 20°C for 72 hours. The test pieces were then removed, and the water adhering to the surface was wiped off. The flexural strength of each test piece was then immediately measured in accordance with JIS A 1408:2017, and the average value was used as the flexural strength of the cured product in the water-absorbed state. The flexural strength in the dry state and when water is absorbed was measured using an autograph "AG50kNX" manufactured by Shimadzu Corporation under the conditions of a central loading method, a bending span of 14.6 cm, and a test speed (loading head speed) of 20 mm / min.

[0086] [Example 1] Pulp (NBKP, Cellofiber manufactured by Partex Co., Ltd., CSF value: 115 mL) was dispersed in water. The resulting dispersion was mixed with ground granulated blast furnace slag (manufactured by DC Corporation: Blaine specific surface area: 4000 cm). 2 / g), ordinary Portland cement (ordinary Portland cement manufactured by Taiheiyo Cement Corporation), fly ash (equivalent to Type II manufactured by Shiden Business Co., Ltd.), and slaked lime (industrial slaked lime No. 1 manufactured by Kochi Lime Industry Co., Ltd., average particle size: 20 μm) were added and mixed. Polyvinyl alcohol fiber 1 (average fiber diameter: 14 μm, aspect ratio: 429, tensile strength: 14.3 cN / dtex, designated PVA1 in Table 1) was added as an alkali-resistant fiber to the resulting mixture and further mixed. The mass ratio of each component is shown in Table 1, and a hydraulic composition with a solids concentration of 16% by mass was obtained. The resulting hydraulic composition was transferred to a feed tank of a metering device and fed from the feed tank to a cylinder. Papermaking Process: The solids concentration of the hydraulic composition was adjusted to 4% by mass using circulating water, and papermaking was performed using a Mini-Hatchek machine. Next, 15 sheets of the molded sheets obtained in the cylinder molding process were stacked on a making roll, and the stacked sheets were pressed for 20 minutes while applying a pressure of 5.0 MPa to squeeze out the liquid. The squeezed sheets were cured in a constant temperature and humidity curing device at a temperature of 50°C and saturated humidity (RH 98%) for 24 hours, then wrapped in plastic wrap and cured at a temperature of 20°C and humidity of 60% for 13 days (total curing age of 14 days). After removing the plastic wrap, the sheets were dried in a roll dryer set at 120°C for 2 hours to obtain a hardened product. The physical properties of the hydraulic composition and the hardened product were measured and evaluated using the methods described above. The results are shown in Table 1.

[0087] [Example 2 and Comparative Examples 1 and 2] Hydraulic compositions and their hardened products were obtained in the same manner as in Example 1, except that the materials and / or amounts to be blended were changed as shown in Table 1. The physical properties of the hydraulic compositions and the hardened products were measured and evaluated. The results are shown in Table 1.

[0088] [Example 3] A hydraulic composition and its hardened product were obtained in the same manner as in Example 2, except that the pressure applied to the laminated paper sheets was changed from 5.0 MPa to 10.0 MPa, and the physical properties of the hydraulic composition and the hardened product were measured and evaluated. The results are shown in Table 1.

[0089] [Example 4] A hydraulic composition and its set product were obtained in the same manner as in Example 1, except that polyvinyl alcohol fiber 2 (average fiber diameter: 7 μm, aspect ratio: 571, tensile strength: 14.5 cN / dtex, shown as PVA2 in Table 1) was used as the alkali-resistant fiber instead of polyvinyl alcohol fiber 1, and the amounts of alkali-resistant fiber and fly ash were changed as shown in Table 1. The physical properties of the hydraulic composition and the set product were measured and evaluated. The results are shown in Table 1.

[0090] [Examples 5 and 6] Hydraulic compositions and their cured products were obtained in the same manner as in Example 1, except that polyvinyl alcohol fiber 3 (average fiber diameter: 14 μm, aspect ratio: 429, tensile strength: 12.6 cN / dtex, shown as PVA3 in Table 1) or polypropylene fiber (average fiber diameter: 17 μm, aspect ratio: 353, tensile strength: 5.3 cN / dtex, shown as PP in Table 1) was used as the alkali-resistant fiber instead of polyvinyl alcohol fiber 1. The physical properties of the hydraulic compositions and the cured products were measured and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0091]

[0092] Example 7 3.5 parts by mass of pulp (NBKP, Cellofiber manufactured by Partex Co., Ltd., CSF value: 115 mL) was dispersed in water. 28 parts by mass of ground granulated blast furnace slag (manufactured by DC Corporation: Blaine specific surface area: 4000 cm) was added to the resulting dispersion. 243 parts by mass of ordinary Portland cement (ordinary Portland cement manufactured by Taiheiyo Cement Corporation), 3 parts by mass of fly ash (equivalent to Type II manufactured by Shiden Business Co., Ltd.), 6 parts by mass of silica fume (EFACO manufactured by Tomoe Engineering Co., Ltd., average particle size: 2 μm), and 14.5 parts by mass of non-reactive filler were added and mixed. 2 parts by mass of polyvinyl alcohol fiber 2 (average fiber diameter: 7 μm, aspect ratio: 571, tensile strength: 14.5 cN / dtex) was added as an alkali-resistant fiber to the resulting mixture and further mixed. A hydraulic composition with a solids concentration of 16% by mass was obtained. A hardened product was obtained in the same manner as in Example 1, except that the obtained hydraulic composition was used. The physical properties of the hydraulic composition and the hardened product were measured and evaluated. The physical properties after 14 days of curing are shown below. Total content of calcium silicate and calcium aluminate: 8.81% by mass, calcium oxide content: 1.55% by mass, calcium hydroxide content: 0.32% by mass, calcium carbonate content: 2.67% by mass, total content of calcium oxide, calcium hydroxide, and calcium carbonate: 4.54% by mass, pore volume ratio (B) / (A): 5.64, pore volume (A): 0.3407 mL / g, pore volume (B): 1.9203 mL / g, impact strength in dry state: 3.55 kJ / m 2 , Impact strength when absorbing water: 4.67 kJ / m 2 Dimensional change rate: 0.15%, Water absorption rate: 20.6%, Bending strength in dry state: 32.3 N / mm 2 , flexural strength when absorbing water: 22.3 N / mm 2 .

[0093] [Example 8] 31.75 parts by mass of granulated blast furnace slag powder (manufactured by DC Corporation: Blaine specific surface area: 4000 cm) was added to water. 21 / g), 28 parts by mass of ordinary Portland cement (ordinary Portland cement manufactured by Taiheiyo Cement Corporation), 3.18 parts by mass of fly ash (equivalent to Type II manufactured by Shiden Business Co., Ltd.), 5 parts by mass of slaked lime (industrial slaked lime No. 1 manufactured by Kochi Lime Industry Co., Ltd., average particle size: 20 μm), and 31.16 parts by mass of silica sand (No. 5 silica sand manufactured by Tohoku Silica Co., Ltd., average particle size: 425 μm) were added and mixed. 0.91 parts by mass of polyvinyl alcohol fiber 4 (average fiber diameter: 26 μm, aspect ratio: 231, tensile strength: 13.8 cN / dtex) was added as an alkali-resistant fiber to the resulting mixture and further mixed. A hydraulic composition with a solids concentration of 16% by mass was obtained. A predetermined amount of the resulting hydraulic composition was placed in a press lower die and dehydrated and molded in a press for 0.5 minutes while applying a pressure of 5 MPa. The composition was then cured and dried under the same conditions as in Example 1 to obtain a hardened product. The physical properties of the obtained hydraulic composition and the hardened body were measured and evaluated in the same manner as in Example 1. The physical properties after 14 days of curing are shown below: Total content of calcium silicate and calcium aluminate: 5.01 mass%, calcium oxide content: 1.93 mass%, calcium hydroxide content: 3.2 mass%, calcium carbonate content: 0.89 mass%, total content of calcium oxide, calcium hydroxide and calcium carbonate: 6.02 mass%, pore volume ratio (B) / (A): 11.06, pore volume (A): 0.0693 mL / g, pore volume (B): 0.7661 mL / g, impact strength in dry state: 3.8 kJ / m 2 , Impact strength when absorbing water: 5.1 kJ / m 2 Dimensional change rate: 0.14%, Water absorption rate: 19.6%, Bending strength in dry state: 12.1 N / mm 2 , flexural strength when absorbing water: 8.9 N / mm 2 .

[0094] The cured product of the present invention has high impact resistance, high dimensional stability, low water absorption, and high bending strength, and is therefore suitable for use as building boards such as interior and exterior wall materials, roofing materials, and flooring materials, as well as civil engineering components.

Claims

1. A hardened body of a hydraulic composition, the hardened body comprising an alkali-resistant fiber, calcium silicate and calcium aluminate, and a ratio of the volume of pores in the range of 11 to 300,000 nm to the volume of pores in the range of 6 to 10 nm in the pore size distribution of the hardened body as determined by mercury intrusion porosimetry is 14 or less.

2. The hardened body according to claim 1, wherein the total content of calcium oxide, calcium hydroxide and calcium carbonate crystals as measured by powder X-ray diffraction is 15 mass% or less based on the mass of the hardened body excluding the fiber components.

3. The cured product according to claim 1, wherein the average fiber diameter of the alkali-resistant fiber is 3 to 900 μm.

4. The hardened body according to claim 1, wherein the aspect ratio of the alkali-resistant fiber is 30 to 2,500.

5. The cured product according to claim 1, wherein the alkali-resistant fiber has a tensile strength of 5 cN / dtex or more.

6. The cured body according to claim 1, wherein the alkali-resistant fiber is one or more types of fiber selected from the group consisting of polyvinyl alcohol-based fibers, polypropylene fibers, and polyethylene fibers.

7. The hardened body according to claim 1, wherein the hydraulic composition comprises 8 to 72 mass % of cement, 72 to 18 mass % of slag, 0.5 to 12 mass % of hydrated lime, and 0.1 to 5 mass % of alkali-resistant fiber, based on the total solid content of the hydraulic composition.

8. The hardened body according to claim 7, wherein the average particle size of the slaked lime is 3 to 600 μm.

9. The hardened body according to claim 1, further comprising 0.1 to 10% by mass of pulp based on the mass of the hardened body.

10. The hardened body according to claim 1, wherein the hardened body does not contain pulp and has a water absorption rate of 1 to 25% as determined in accordance with JIS A 5430:2018.

11. The hardened body according to claim 9, wherein the water absorption of the hardened body determined in accordance with JIS A 5430:2018 is 5 to 40%.

12. The hardened body according to claim 1, wherein the pore volume in the range of 6 to 10 nm in the pore size distribution of the hardened body measured by mercury intrusion porosimetry is 0.05 mL / g or more.

13. The hardened body according to claim 1, wherein the pore volume in the range of 11 to 300,000 nm in the pore size distribution of the hardened body measured by mercury intrusion porosimetry is 0.3 to 3.0 mL / g.

14. A building board comprising the hardened product according to claim 1.