Thermally conductive filler, resin composition, resin sheet, and method for producing hexagonal boron nitride powder
Patent Information
- Application Number
- MYPI2025006401
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-02-27
- Publication Date
- 2024-10-26
AI Technical Summary
Current hexagonal boron nitride powders lack high crystallinity, which hinders their ability to effectively improve the thermal conductivity of resins used in electronic components, necessitating the development of materials with enhanced thermal dissipation capabilities.
A method involving a raw material mixture of an oxygen-containing boron compound, a carbon source, and an oxygen-containing calcium compound, heated in a nitrogen atmosphere at controlled temperatures and rates to produce hexagonal boron nitride powder with high crystallinity, characterized by a specific cathodoluminescence spectral intensity ratio and optimized particle size, enhancing thermal conductivity.
The produced hexagonal boron nitride powder achieves high crystallinity and improved thermal conductivity, making it suitable as a filler for efficient heat dissipation in electronic components, with thermal conductivity exceeding 15 W/m·K in resin compositions.
Smart Images

Figure PI2025006401_DRAWING_001
Abstract
Description
Hexagonal boron nitride powder and its manufacturing method
[0001] The present invention relates to a hexagonal boron nitride powder and a method for producing the same.
[0002] In recent years, as electronic components have become smaller and more powerful, the amount of heat generated by them has become an issue. Therefore, materials with excellent thermal conductivity are being developed to efficiently dissipate heat from electronic components.
[0003] Hexagonal boron nitride powder is blended with resins used in electronic components to improve the thermal conductivity of the resin. Therefore, research and development of hexagonal boron nitride powder as a thermally conductive filler has been actively conducted. For example, Patent Document 1 discloses a high-purity hexagonal boron nitride single crystal that has a unique ultraviolet emission band at wavelengths of 235 nm or less.
[0004] Japanese Patent Application Publication No. 2005-145788
[0005] While the high-purity hexagonal boron nitride single crystals described above are single crystals that are not affected by impurities, no highly crystalline hexagonal boron nitride powder has yet been reported. Research and development of highly crystalline hexagonal boron nitride powder that improves the thermal conductivity of resins is desired.
[0006] An object of one aspect of the present invention is to provide a hexagonal boron nitride powder that has high crystallinity and improves the thermal conductivity of resins.
[0007] In order to solve the above problems, a hexagonal boron nitride powder according to one embodiment of the present invention is a hexagonal boron nitride powder in which the ratio of the spectral intensity at a wavelength of 227 nm to the spectral intensity at a wavelength of 330 nm, as measured by a cathodoluminescence (CL) method, is 1.0 or more.
[0008] Furthermore, a method for producing hexagonal boron nitride powder according to one embodiment of the present invention is a method for producing hexagonal boron nitride powder, comprising the following steps: (1) a reduction-nitridation step of heating a raw material mixture containing an oxygen-containing boron compound, a carbon source, an oxygen-containing calcium compound, and a carbon-containing boron compound in a furnace under a nitrogen atmosphere to a temperature of 1500°C or higher and 1850°C or lower at a temperature increase rate of 10°C / min or lower to obtain hexagonal boron nitride; (2) an acid washing step of acid washing the hexagonal boron nitride powder containing unreacted raw materials obtained by the reduction-nitridation step; (3) a heating step of heating the hexagonal boron nitride powder after the acid washing step to a temperature of more than 1850°C and lower than 2050°C at a temperature increase rate of 5°C / min or lower; (4) a cooling step of cooling the hexagonal boron nitride powder after the heating step to a temperature of at least 1550°C at a temperature decrease rate of 5°C / min or lower; (5) A recovery step of removing the hexagonal boron nitride powder, whose temperature has been lowered to 50° C. or less, from the furnace after the temperature lowering step.
[0009] According to one aspect of the present invention, it is possible to realize a hexagonal boron nitride powder that is highly crystalline and improves the thermal conductivity of a resin composition filled with the powder.
[0010] FIG. 1 is a diagram showing the results of measuring a CL spectrum in one embodiment of a hexagonal boron nitride powder of the present invention.
[0011] In this specification, "A to B" means A or more and B or less unless otherwise specified.
[0012] [Hexagonal Boron Nitride Powder] The hexagonal boron nitride powder according to one embodiment of the present invention has a ratio of the spectral intensity at a wavelength of 227 nm to the spectral intensity at a wavelength of 330 nm (CL spectral intensity at 227 nm / CL spectral intensity at 330 nm) of 1.0 or more, as measured by a cathodoluminescence method.
[0013] The present inventors have conducted extensive detailed studies on hexagonal boron nitride powder and have succeeded in making new discoveries. Specifically, they independently discovered that by employing specific conditions when producing hexagonal boron nitride powder, it is possible to obtain hexagonal boron nitride powder having a CL spectral intensity at 227 nm / CL spectral intensity at 330 nm of 1.0 or more. They also independently discovered that this hexagonal boron nitride powder is highly crystalline and close to being a single crystal. They also independently discovered that this hexagonal boron nitride powder improves the thermal conductivity of resins and is suitable as a thermally conductive filler.
[0014] Cathodoluminescence is a method for detecting light emitted when a sample is irradiated with an electron beam. Cathodoluminescence reflects crystalline properties (crystal defects, impurities, carrier concentration, stress, etc.). The CL spectrum at 227 nm is a spectrum indicating high crystallinity. The CL spectrum at 330 nm is a spectrum caused by carbon impurities. The CL spectrum intensity may be the peak intensity of the CL spectrum.
[0015] As the measuring device for the cathodoluminescence method, a known measuring device can be used.
[0016] In order to achieve higher crystallinity and further improve the thermal conductivity of the resin, the CL spectrum intensity at 227 nm / CL spectrum intensity at 330 nm is preferably 1.1 or more, more preferably 1.2 or more, and even more preferably 1.3 or more.
[0017] The hexagonal boron nitride powder has an amount of eluted boron of B after immersion in a sulfuric acid aqueous solution having a concentration of 2 mol / L at 25°C for 120 minutes. 2 O 3The amount of dissolved boron is preferably 250 ppm or less, calculated as a percentage of oxygen in the hexagonal boron nitride powder. The amount of dissolved boron correlates with the surface oxygen concentration of the hexagonal boron nitride powder, and when the amount of dissolved boron is 250 ppm or less, the oxygen concentration on the powder surface is low and the crystallinity of the hexagonal boron nitride powder is high. The amount of dissolved boron can be measured, for example, by inductively coupled plasma (ICP) atomic emission spectrometry. The amount of dissolved boron may be 200 ppm or less, or may be 180 ppm or less.
[0018] The average particle size of the hexagonal boron nitride powder is preferably 2 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more, from the viewpoints of further improving the thermal conductivity of the resin and ease of handling. Furthermore, from the viewpoint of facilitating uniform dispersion in the resin composition, the average particle size is preferably 90 μm or less, more preferably 70 μm or less, and even more preferably 50 μm or less. The average particle size is the volume-based average particle size (D50).
[0019] In order to achieve higher crystallinity and further improve the thermal conductivity of the resin, the whiteness of the hexagonal boron nitride powder is preferably at least 90. The whiteness is measured by a color difference meter.
[0020] [Method for producing hexagonal boron nitride powder] A method for producing hexagonal boron nitride powder according to one embodiment of the present invention (hereinafter sometimes referred to as "this production method") includes a reduction-nitridation step, an acid washing step, a heating step, a temperature-lowering step, and a recovery step. Each step will be described below.
[0021] In the reduction-nitridation step, a raw material mixture containing an oxygen-containing boron compound, a carbon source, an oxygen-containing calcium compound, and a boron carbon-containing compound is heated in a furnace under a nitrogen atmosphere to a temperature of 1500° C. to 1850° C. at a heating rate of 10° C. / min or less. This step allows for the production of hexagonal boron nitride containing unreacted raw materials.
[0022] (Raw Material) As the oxygen-containing boron compound, a compound containing boron and oxygen atoms may be used. Examples of oxygen-containing boron compounds include boric acid, boric anhydride, metaboric acid, perboric acid, hypoboric acid, sodium tetraborate, and sodium perborate. Among these, boric acid or boron oxide, which are easily available, may be preferably used.
[0023] Examples of carbon sources include amorphous carbon such as carbon black, activated carbon, and carbon fiber, as well as crystalline carbon such as diamond, graphite, and nanocarbon, and pyrolytic carbon obtained by pyrolyzing a monomer or polymer. Among these, highly reactive amorphous carbon is preferred, and carbon black is particularly preferred because of its industrial quality control. Examples of carbon black include acetylene black, furnace black, and thermal black.
[0024] Examples of oxygen-containing calcium compounds include calcium carbonate, calcium bicarbonate, calcium hydroxide, calcium oxide, calcium nitrate, calcium sulfate, calcium phosphate, and calcium oxalate. These compounds can be used alone or in combination of two or more. Among these, calcium oxide or calcium carbonate is preferably used. By including an oxygen-containing calcium compound in the raw material mixture, a highly crystalline hexagonal boron nitride powder can be obtained when the raw material mixture is heated at a temperature increase rate of 10°C / min or less in the reduction-nitridation step.
[0025] The oxygen-containing calcium compound forms a complex oxide with the oxygen-containing boron compound, which forms a complex oxide with a high melting point and plays a role in preventing the oxygen-containing boron compound from volatilizing.It has also been confirmed that the oxygen-containing calcium compound plays a role in the direct nitriding reaction of boron carbide.
[0026] The boron-carbon compound may be a compound containing carbon and boron (e.g., boron carbide). The particle size of the boron-carbon compound is preferably 1 to 500 μm, more preferably 10 to 400 μm, and even more preferably 20 to 300 μm.
[0027] The mixture may be obtained by mixing the oxygen-containing boron compound, the carbon source, the oxygen-containing calcium compound, and the carbon-containing boron compound in the ratio shown below. The ratio B / C (element ratio) of the mass of the oxygen-containing boron compound in B equivalent to the mass of the carbon source in C equivalent is set to 0.75 to 1.05. 2 O 3 The oxygen-containing calcium compound is 5 to 20 parts by mass in terms of CaO relative to 100 parts by mass of the total of the converted mass of the oxygen-containing boron compound and the converted mass of the carbon source. 2 O 3 The carbon-containing boron compound is contained in an amount of 5 to 45 parts by mass relative to 100 parts by mass of the total mass calculated as C and CaO.
[0028] The raw material mixture containing the raw materials may be supplied to the reduction-nitridation reaction in the form of, for example, powder or granules. The raw materials can be mixed using a mixer such as a vibration mill, a bead mill, a ball mill, a Henschel mixer, a drum mixer, a vibration agitator, or a V-shaped mixer.
[0029] The raw material mixture in the reduction-nitridation step is heated in a furnace under a nitrogen atmosphere. Examples of gases introduced into the furnace include nitrogen gas and ammonia gas. A gas obtained by mixing nitrogen gas or ammonia gas with a non-oxidizing gas such as hydrogen, argon, or helium may also be used. Nitrogen gas is preferred as the gas introduced into the heating furnace. Furthermore, the nitrogen gas is preferably nitrogen gas whose dew point temperature is controlled, and the dew point temperature is preferably −85° C. or lower.
[0030] The raw material mixture in the reduction-nitridation step is heated at a temperature rise rate of 10°C / min or less from 1500°C to a temperature of 1850°C or less (maximum reduction-nitridation temperature). Heating at this temperature rise rate can slow the grain growth rate of the hexagonal boron nitride powder, making it possible to obtain hexagonal boron nitride powder with high crystallinity. Since slowing the grain growth rate of hexagonal boron nitride powder allows for the production of hexagonal boron nitride powder with higher crystallinity, the temperature rise rate from 1500°C to the maximum reduction-nitridation temperature is preferably 7°C / min or less, more preferably 5°C / min or less, and even more preferably 3°C / min or less.
[0031] In the reduction-nitridation reaction, a holding time may be set as necessary within a temperature range up to 1500° C. After the maximum reduction-nitridation temperature is reached, the holding time at the maximum reduction-nitridation temperature is preferably 1 hour or more, more preferably 2 hours or more, in terms of accelerating the reduction-nitridation reaction. Moreover, the holding time at the maximum reduction-nitridation temperature is preferably 10 hours or less, more preferably 5 hours or less.
[0032] The reduction-nitriding step can be carried out using a known reaction apparatus capable of controlling the reaction atmosphere, such as an atmosphere-controlled high-temperature furnace that performs heat treatment by high-frequency induction heating or heater heating, and a batch furnace as well as a continuous heating furnace such as a pusher-type tunnel furnace or a vertical reactor can also be used.
[0033] The hexagonal boron nitride powder obtained after the reduction-nitriding step may be crushed to adjust the particle size distribution to a predetermined value. Crushing is preferably carried out gently using a jet mill, ball mill, hammer mill, or stone mill. The crushed powder may also be classified by air classification or sieving to adjust the particle size appropriately.
[0034] (Acid washing step) In the acid washing step, the hexagonal boron nitride powder containing unreacted raw materials obtained in the reduction-nitridation step is subjected to acid washing. The hexagonal boron nitride powder obtained by the reduction-nitridation reaction contains unreacted raw materials such as oxides and metal impurities. The acid washing step allows the production of hexagonal boron nitride powder from which the unreacted raw materials have been removed.
[0035] The method for acid washing the hexagonal boron nitride powder containing unreacted raw materials is not particularly limited, and any known method may be used without limitation. For example, there is a method in which the hexagonal boron nitride powder containing unreacted raw materials obtained after the reduction-nitridation reaction is placed in a container, and dilute hydrochloric acid (10 to 20 mass % HCl) is added in an amount 5 to 10 times the amount of the hexagonal boron nitride powder containing unreacted raw materials, and the mixture is allowed to come into contact for 4 to 8 hours.
[0036] The acid used in the acid washing may be hydrochloric acid, or may be nitric acid, sulfuric acid, acetic acid, or the like.
[0037] After the acid washing, water washing using pure water may be performed to wash away any remaining acid. As a method of water washing, the acid used in the acid washing may be filtered, and then the pickled hexagonal boron nitride powder may be dispersed in pure water in the same amount as the acid used, followed by filtering again.
[0038] After pickling or water washing, the hydrous aggregate may be dried. Drying conditions are preferably, for example, in the atmosphere at 50 to 250°C or under reduced pressure. There is no particular restriction on the drying time, but it is preferable to dry until the moisture content approaches 0%.
[0039] (Heating Step) In the heating step, the hexagonal boron nitride powder obtained in the acid washing step is heated to a temperature of more than 1850° C. and less than 2050° C. at a temperature increase rate of 5° C. / min or less.
[0040] The heating step may be performed under a nitrogen atmosphere. The nitrogen source may be supplied to the reaction system in the heating step in the same manner as in the reduction-nitridation step. The reaction apparatus may also be the same as that used in the reduction-nitridation step.
[0041] In the heating step, the hexagonal boron nitride powder is heated to a temperature of more than 1850°C and less than 2050°C (maximum re-firing temperature) at a temperature increase rate of 5°C / min or less. This heating makes it possible to obtain a hexagonal boron nitride powder with high crystallinity. However, if the hexagonal boron nitride powder is heated to 2050°C or higher, the hexagonal boron nitride powder may turn yellow due to nitrogen defects or the like, resulting in a hexagonal boron nitride powder with low crystallinity.
[0042] The temperature at which the temperature rise rate adjustment in the heating step starts is not particularly limited, and may be, for example, room temperature (20° C. to 25° C.).
[0043] From the viewpoint of improving the efficiency of the heating step, the temperature at which adjustment of the temperature rise rate starts is preferably at least 1450° C. The phrase "the temperature at which adjustment of the temperature rise rate starts is at least 1450° C." includes starting adjustment of the temperature rise rate after the temperature of the hexagonal boron nitride powder reaches 1450° C.
[0044] In order to obtain hexagonal boron nitride powder with higher crystallinity, the temperature rise rate in the heating step is preferably 4° C. / min or less, and more preferably 3° C. / min or less.
[0045] After the re-firing temperature is reached, the holding time at the re-firing maximum temperature is preferably 1 hour or more, more preferably 3 hours or more, so that the hexagonal boron nitride powder can be sufficiently heated (re-firing) and is preferably 15 hours or less, more preferably 10 hours or less.
[0046] In the temperature-reducing step, the hexagonal boron nitride powder obtained after the heating step is cooled at a rate of 5° C. / min or less to a temperature of at least 1550° C. This temperature-reducing step can provide a hexagonal boron nitride powder having a CL spectrum intensity at 227 nm / CL spectrum intensity at 330 nm ratio of 1.0 or more.
[0047] Lowering the temperature to at least 1550°C includes lowering the temperature of the hexagonal boron nitride powder to 1550°C.
[0048] The temperature increase rate in the temperature decreasing step is preferably 4°C / min or less, and more preferably 3°C / min or less, in that a hexagonal boron nitride powder having a higher CL spectrum intensity at 227 nm / CL spectrum intensity at 330 nm can be obtained.
[0049] (Recovery Step) In the recovery step, the hexagonal boron nitride powder, whose temperature has been reduced to 50°C or less after the temperature reduction step, is removed from the furnace. By reducing the temperature of the hexagonal boron nitride powder recovered from the furnace to 50°C or less, it is possible to suppress the reaction with moisture in the air. By suppressing this reaction, the surface oxygen concentration (B 2 O 3 In addition, by lowering the temperature of the hexagonal boron nitride powder recovered from the furnace to 50°C or less, it is possible to obtain hexagonal boron nitride powder having a CL spectrum intensity at 227 nm / CL spectrum intensity at 330 nm ratio of 1.0 or more.
[0050] The temperature of the hexagonal boron nitride powder recovered from the furnace is preferably 40°C or lower, and more preferably 30°C or lower, in order to sufficiently suppress reaction with moisture in the air and improve the crystallinity of the hexagonal boron nitride powder.
[0051] [Uses of hexagonal boron nitride powder] (Resin composition) A resin composition according to one embodiment of the present invention contains the hexagonal boron nitride powder. By including the hexagonal boron nitride powder, the resin composition has high thermal conductivity and is suitable for heat dissipation applications.
[0052] The resin composition can be used for various purposes. By mixing it with a resin described below to form a thermally conductive resin composition or a thermally conductive molded body, it can be preferably used for applications such as thermal interface materials such as polymer-based heat dissipation sheets and phase change sheets, organic heat dissipation sheets such as heat dissipation tapes, heat dissipation greases, heat dissipation adhesives, and gap fillers, heat dissipation paints such as heat dissipation paints and heat dissipation coats, heat dissipation resin substrates such as PWB-based resin substrates and CCL-based resin substrates, insulating layers for metal-based substrates such as aluminum-based substrates and copper-based substrates, and sealing materials for power devices.
[0053] Examples of resins contained in the resin composition include thermoplastic resins such as polyolefins, vinyl chloride resins, methyl methacrylate resins, nylons, and fluororesins; thermosetting resins such as epoxy resins, phenolic resins, urea resins, melamine resins, unsaturated polyester resins, silicone resins, and bismaleimide triazine resins; and synthetic rubbers.
[0054] The resin composition may contain a thermally conductive filler such as aluminum nitride and aluminum oxide, which are known highly thermally conductive insulating fillers.
[0055] Furthermore, the resin composition may contain, as necessary, as compounding agents for the resin composition, known polymerization initiators, curing agents, polymerization inhibitors, polymerization retarders, coupling agents, plasticizers, ultraviolet absorbers, pigments, dyes, antibacterial agents, organic fillers, organic-inorganic composite fillers, etc. Furthermore, the resin composition may contain other inorganic fillers within a range that does not impair the effects of the present invention.
[0056] The content of the hexagonal boron nitride powder in the resin composition is preferably 20 to 80% by volume, and more preferably 30 to 70% by volume, in order to obtain higher thermal conductivity.
[0057] The content of the resin in the resin composition corresponds to the amount obtained by subtracting the content of the hexagonal boron nitride powder when the total volume of the resin composition is taken as 100% by volume, and includes the volume of a curing agent, if any, and is preferably 80 to 20% by volume, and more preferably 70 to 30% by volume.
[0058] (Resin Sheet) The resin sheet according to one embodiment of the present invention is made of the resin composition described above. The use of the resin sheet is not particularly limited, but it can be used, for example, for circuit boards and heat dissipation of electronic components such as multilayer printed wiring boards.
[0059] The method for producing the resin sheet is not particularly limited, and for example, when the resin is a curable epoxy resin, a method for producing a resin sheet can be adopted, which includes a mixing step of mixing the curable epoxy resin, the hexagonal boron nitride powder, and, if necessary, other components to obtain a curable composition, a molding step of molding the curable composition into a desired shape, and a curing step of curing the curable composition.
[0060] (Other Applications) Due to its high crystallinity, the hexagonal boron nitride powder of the present invention can also be used for applications such as a raw material for cubic boron nitride or boron nitride processed products such as boron nitride molded products, a nucleating agent for engineering plastics, a phase change material, a solid or liquid thermal interface material, a release agent for molten metal or molten glass molds, cosmetics, and a composite ceramic raw material.
[0061] [Summary] The hexagonal boron nitride powder according to aspect 1 of the present invention has a ratio of the spectral intensity at a wavelength of 227 nm to the spectral intensity at a wavelength of 330 nm of 1.0 or more, as measured by cathodoluminescence.
[0062] The hexagonal boron nitride powder according to aspect 2 of the present invention is the same as that according to aspect 1 of the present invention, except that the amount of eluted boron after immersion in a sulfuric acid aqueous solution having a concentration of 2 mol / L at 25° C. for 120 minutes is B 2 O 3 In terms of carbon dioxide, the carbon dioxide concentration may be 250 ppm or less.
[0063] The hexagonal boron nitride powder according to Aspect 3 of the present invention may be the powder of Aspect 1 or 2 of the present invention, and may have an average particle size of 2 μm or more and 150 μm or less.
[0064] A resin composition according to a fourth aspect of the present invention contains the hexagonal boron nitride powder according to any one of the first to third aspects of the present invention.
[0065] A resin sheet according to a fifth aspect of the present invention is a resin sheet comprising the resin composition according to the fourth aspect of the present invention.
[0066] A method for producing hexagonal boron nitride powder according to a sixth aspect of the present invention comprises the following steps: (1) a reduction-nitridation step in which a raw material mixture containing an oxygen-containing boron compound, a carbon source, an oxygen-containing calcium compound, and a boron carbon-containing compound is heated in a furnace under a nitrogen atmosphere to a temperature of 1500°C or higher and 1850°C or lower at a heating rate of 10°C / min or lower to obtain hexagonal boron nitride; (2) an acid washing step in which the hexagonal boron nitride powder containing unreacted raw materials obtained by the reduction-nitridation step is acid washed; (3) a heating step in which the hexagonal boron nitride powder after the acid washing step is heated to a temperature of more than 1850°C and lower than 2050°C at a heating rate of 5°C / min or lower; (4) a cooling step in which the hexagonal boron nitride powder after the heating step is cooled to a temperature of at least 1550°C at a cooling rate of 5°C / min or lower; and (5) a recovery step in which the hexagonal boron nitride powder cooled to 50°C or lower is removed from the furnace after the cooling step.
[0067] A seventh aspect of the present invention relates to the method for producing a hexagonal boron nitride powder in the sixth aspect of the present invention, wherein the temperature increase rate in the heating step may be adjusted from a temperature of at least 1450°C.
[0068] The following examples are provided to further explain the embodiments of the present invention. It goes without saying that the present invention is not limited to the following examples, and various modifications are possible in detail. Furthermore, the present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed herein are also included in the technical scope of the present invention. Furthermore, all of the documents described in this specification are incorporated by reference.
[0069] Preparation Example 1: Preparation of hexagonal boron nitride powder. 259 g of a mixture containing 141 g of boron oxide, 56 g of carbon black, 32 g of calcium oxide, and 30 g of boron carbide was mixed using a ball mill. The mixture was heated to 1500°C in a graphite Tammann furnace under a nitrogen gas atmosphere, held at 1500°C for 4 hours, and then heated at a rate of 2°C / min to a maximum reduction-nitridation temperature of 1850°C. The mixture was then held at 1850°C for 2 hours to carry out a reduction-nitridation treatment (reduction-nitridation step).
[0070] The hexagonal boron nitride powder after the reduction-nitridation treatment was placed in a container, and a five-fold amount of hydrochloric acid (7 mass% HCl) was added. The mixture was stirred at 700 rpm for 24 hours to perform pickling (pickling step). After the pickling treatment, the acid was filtered, and the hexagonal boron nitride powder obtained by filtration was dispersed in pure water in the same amount as the acid used, and then filtered again. This procedure was repeated five times, and the powder was then vacuum dried at 200°C for 6 hours.
[0071] The hexagonal boron nitride powder obtained after drying was heated to 1500°C in a graphite Tammann furnace under a nitrogen gas atmosphere, and then heated at a rate of 2°C / min to a maximum re-firing temperature of 1950°C, and then held at 1950°C for 6 hours to carry out a re-firing treatment (heating step).
[0072] Next, nitrogen gas was flowed into the furnace to lower the temperature to 1500°C at a rate of 1°C / min (temperature lowering step), and nitrogen gas was further flowed to cool the inside of the furnace to 25°C, after which the hexagonal boron nitride powder was recovered from the furnace (recovery step).
[0073] Example 2 Preparation of Hexagonal Boron Nitride Powder Hexagonal boron nitride powder was prepared in the same manner as in Example 1, except that the temperature-lowering rate in the temperature-lowering step was changed to 2°C / min.
[0074] Example 3 Preparation of Hexagonal Boron Nitride Powder Hexagonal boron nitride powder was prepared in the same manner as in Example 1, except that the maximum re-firing temperature in the heating step was set to 2010°C.
[0075] Example 4 Preparation of Hexagonal Boron Nitride Powder Hexagonal boron nitride powder was prepared in the same manner as in Example 1, except that the temperature-lowering rate in the temperature-lowering step was changed to 3°C / min.
[0076] Example 5 Preparation of Hexagonal Boron Nitride Powder Hexagonal boron nitride powder was prepared in the same manner as in Example 1, except that the maximum re-firing temperature in the heating step was set to 1900°C.
[0077] Comparative Example 1 Preparation of Hexagonal Boron Nitride Powder Hexagonal boron nitride powder was prepared in the same manner as in Example 1, except that the maximum re-firing temperature in the heating step was set to 2050°C.
[0078] Comparative Example 2 Preparation of Hexagonal Boron Nitride Powder Hexagonal boron nitride powder was prepared by only undergoing the reduction-nitridation step and acid washing step of Example 1. The temperature increase from 1500°C to 1850°C in the reduction-nitridation step was carried out at a rate of 1°C / min. Other than that, the reduction-nitridation step and acid washing step were carried out under the same conditions as those of Example 1.
[0079] Comparative Example 3 Preparation of Hexagonal Boron Nitride Powder Hexagonal boron nitride powder was prepared in the same manner as in Example 1, except that the temperature-lowering rate in the temperature-lowering step was changed to 10° C. / min.
[0080] Comparative Example 4 Hexagonal boron nitride powder was prepared in the same manner as in Example 1, except that the maximum firing temperature in the heating step was set to 1800°C.
[0081] Comparative Example 5 Hexagonal boron nitride powder was prepared in the same manner as in Example 1, except that in the reduction-nitriding step, the temperature was increased from 1500° C. to 1850° C. at a rate of 15° C. / min.
[0082] Comparative Example 6 Hexagonal boron nitride powder was prepared in the same manner as in Example 1, except that in the recovery step, the furnace was cooled to 100°C and then the hexagonal boron nitride powder was recovered from the furnace.
[0083] Comparative Example 7 Hexagonal boron nitride powder was prepared in the same manner as in Example 1, except that the reduction-nitriding step was carried out by the melamine method, which involved thermal decomposition of melamine borate at 1950°C.
[0084] [Evaluation Example 1] Evaluation of hexagonal boron nitride powder The hexagonal boron nitride powders obtained in Examples 1 to 5 and Comparative Examples 1 to 7 were evaluated by the following evaluation methods.
[0085] (Measurement by Cathodoluminescence (CL) Method) Measurement by the CL method was carried out using a Hitachi Schottky Emission SEM S-4300SE and a spectrometer HR-320 (manufactured by Horiba, Ltd.) under the following conditions: Electron beam acceleration voltage: 5 kV; Sample temperature: 296 K; Measurement area: 50 × 50 μm 2 (Measure at three different locations)
[0086] (Measurement of Total Oxygen Content) The total oxygen content in the hexagonal boron nitride powder was measured using a ceramic oxygen and nitrogen analyzer EMGA-620W manufactured by Horiba Ltd.
[0087] (Measurement of Total Carbon Content) The total carbon content in the hexagonal boron nitride powder was measured using a ceramic carbon analyzer EMIA-110 manufactured by Horiba Ltd. The powder was burned in an oxygen stream, and the generated CO gas and CO 2 The total carbon content was determined from the gas volume.
[0088] (B 2 O 3 Measurement of concentration) 50 g of a 2% aqueous sulfuric acid solution and 2 g of hexagonal boron nitride powder were placed in a 50 mL i-boy, and the solution was shaken and stirred for 1 minute while the temperature of the solution was adjusted to 25°C. After leaving the solution to stand for 120 minutes, the amount of boron in the solution was analyzed using an ICP optical emission spectrometer (iCAP6500 manufactured by Thermo Fisher Scientific). The measurement result was divided by the mass of the hexagonal boron nitride powder used in the test to determine the amount of eluted boron per unit mass of the hexagonal boron nitride powder (B 2 O 3 The concentration (ppm) was determined.
[0089] (Measurement of Whiteness) The whiteness of the hexagonal boron nitride powder was measured using a color difference meter ZE7700 (manufactured by Nippon Denshoku Industries Co., Ltd.).
[0090] (Average Particle Diameter) The average particle diameter (volume-based average particle diameter (D50)) of the hexagonal boron nitride powder was measured by a laser diffraction method using a laser diffraction / scattering particle size measuring device MT3000 (manufactured by Microtrac Bell).
[0091] [Evaluation Example 1] Evaluation of Thermal Conductivity of Resin Compositions The hexagonal boron nitride powder obtained in each Example and Comparative Example was filled into an epoxy resin to prepare a resin composition, and its thermal conductivity was evaluated. A mixture of 100 parts by weight of epoxy resin (JER828 manufactured by Mitsubishi Chemical Corporation), 5 parts by weight of a curing agent (imidazole-based curing agent, Curesol 2E4MZ manufactured by Shikoku Kasei Co., Ltd.), and 210 parts by weight of methyl ethyl ketone as a solvent was prepared. Next, the varnish-like mixture and the hexagonal boron nitride powder were mixed in a rotation / revolution mixer (MAZERUSTAR manufactured by Kurabo Industries Co., Ltd.) to obtain a resin composition consisting of 35% by volume of base resin and 65% by volume of the specific boron nitride powder, 40% by volume of base resin and 63% by volume of the specific boron nitride powder, or 45% by volume of base resin and 55% by volume of the specific boron nitride powder.
[0092] The resin composition was coated onto a PET film to a thickness of approximately 180 to 220 μm using a Tester Sangyo automatic coater PI-1210, dried, and cured under reduced pressure at a temperature of 200°C, a pressure of 5 MPa, and a holding time of 30 minutes to produce a 150 μm thick sheet. The sheet was analyzed using a temperature wave thermal analyzer to calculate the thermal conductivity.
[0093] Table 1 shows the production conditions for the hexagonal boron nitride powders of the examples and comparative examples, as well as the evaluation results of Evaluation Example 1.
[0094] The measured CL spectra are shown in Figure 1. In Figure 1, "1" is the measurement result of the hexagonal boron nitride powder of Comparative Example 2. "2" is the measurement result of the hexagonal boron nitride powder of Example 4. "3" is the measurement result of the hexagonal boron nitride powder of Example 2. "4" is the measurement result of the hexagonal boron nitride powder of Example 1. "5" is the measurement result of the hexagonal boron nitride powder of Comparative Example 1.
[0095]
[0096] In Table 1, "reduction nitridation heating rate" indicates the rate of temperature increase from 1500°C to the maximum re-firing temperature in the reduction nitridation step. "temperature decrease rate" indicates the rate of temperature decrease from the maximum re-firing temperature to 1500°C in the temperature decrease step. "removal temperature" indicates the temperature inside the furnace when the re-firing hexagonal boron nitride powder is recovered from the furnace. "227 nm / 330 nm" indicates the ratio of (CL peak intensity at a wavelength of 227 nm) / (CL peak intensity at a wavelength of 330 nm).
[0097] As shown in Table 1, the thermal conductivity of the resin composition containing the hexagonal boron nitride powder of the example, which had a CL peak intensity ratio of 227 nm / 330 nm of 1.0 or more, exceeded 15 W / m K, demonstrating that the hexagonal boron nitride powder of the example is suitable as a heat dissipation filler.
[0098] In Comparative Example 1, in which the maximum re-firing temperature was 2050°C, the CL peak intensity ratio at 227 nm / 330 nm was as low as 0.2, and the powder turned yellow. The yellowed powder developed nitrogen defects and other defects, resulting in poor crystallinity. Furthermore, the resin composition containing hexagonal boron nitride powder in Comparative Example 4, in which the maximum re-firing temperature was 1850°C, had a thermal conductivity of 15 W / m K or less, suggesting that the purification effect of re-firing was not achieved.
[0099] In Comparative Examples 3 and 5, in which the heating rate in the heating step (re-baking) or the cooling rate in the cooling step was high, the 227 nm / 330 nm CL peak intensity ratio was 0.9, and the thermal conductivity of the resin composition was 15 W / m K or less. These results show that the heating rate and cooling rate during re-baking affect the 227 nm / 330 nm CL peak intensity ratio and the thermal conductivity of the resin composition.
[0100] It is believed that the hexagonal boron nitride powder of Comparative Example 6, in which the hexagonal boron nitride powder was removed at a high temperature, reacted with moisture in the air, increasing the surface oxygen concentration, which reduced the crystallinity of the hexagonal boron nitride powder surface and resulted in a low CL peak intensity ratio at 227 nm / 330 nm.
[0101] The hexagonal boron nitride powder of the present invention has high crystallinity and improves the thermal conductivity of resins, and can be used as a raw material for materials used in electronic parts.
Claims
1. Hexagonal boron nitride powder having a ratio of the spectral intensity at a wavelength of 227 nm to the spectral intensity at a wavelength of 330 nm of 1.0 or more, as measured by a cathode luminescence method.
2. The amount of eluted boron after immersion in a sulfuric acid solution with a concentration of 2 mol / L at 25°C for 120 minutes is 2 O 3 The hexagonal boron nitride powder according to claim 1, wherein the ZnO content is 250 ppm or less in terms of ZnO content.
3. The hexagonal boron nitride powder according to claim 1, having an average particle size of 2 μm or more and 150 μm or less.
4. A resin composition comprising the hexagonal boron nitride powder according to any one of claims 1 to 3.
5. A resin sheet comprising the resin composition according to claim 4.
6. A method for producing hexagonal boron nitride powder, comprising the following steps: (1) a reduction-nitridation step of heating a raw material mixture containing an oxygen-containing boron compound, a carbon source, an oxygen-containing calcium compound, and a carbon-containing boron compound in a furnace under a nitrogen atmosphere to a temperature of 1500°C or more and 1850°C or less at a heating rate of 10°C / min or less to obtain hexagonal boron nitride; (2) an acid washing step of acid washing the hexagonal boron nitride powder containing unreacted raw materials obtained by the reduction-nitridation step; (3) a heating step of heating the hexagonal boron nitride powder after the acid washing step to a temperature of more than 1850°C and less than 2050°C at a heating rate of 5°C / min or less; (4) a cooling step of cooling the hexagonal boron nitride powder after the heating step to a temperature of at least 1550°C at a cooling rate of 5°C / min or less; (5) A recovery step of removing the hexagonal boron nitride powder, whose temperature has been lowered to 50° C. or less, from the furnace after the temperature lowering step.
7. A method for producing hexagonal boron nitride powder according to claim 6, wherein in the heating step, the temperature rise rate is adjusted from a temperature of at least 1450°C.