Low-hardenability narrow-bandwidth mn-cr series round gear steel and manufacturing method therefor
Patent Information
- Application Number
- MYPI2025006476
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-23
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-23
AI Technical Summary
The hardenability and hardenability bandwidth of the existing Mn-Cr series gear steel are difficult to effectively control, resulting in large heat treatment deformation and insufficient strength, which cannot meet the performance requirements of application scenarios such as new energy vehicles.
By optimizing the chemical composition and process technology, Mn-Cr series gear round steel with low hardenability and narrow bandwidth is prepared. The chemical composition includes C: 0.15~0.18%, Si: 0.040~0.10%, Mn: 1.10~1.40%, Cr: 1.00~1.20%, Mo: 0.006~0.02%, Ni: 0.020~0. 10%, Al: 0.020~0.050%, N: 0.007~0.015%, and adopts secondary quenching + tempering process to control the hardenability coefficient between 1.18~1.65 to ensure that the yield strength is ≥800MPa and the tensile strength is ≥1100MPa , elongation ≥ 12%, area shrinkage ≥ 50%, impact energy KU2 ≥ 90J.
It achieves a narrow bandwidth of hardenability at J5=33~36HRC, J9=25~28HRC, J15=20~24HRC, reduces heat treatment deformation, meets the performance requirements of gear steel for new energy vehicles, and improves the stability and safety of the steel. sex.
Smart Images

Figure PI2025006476_DRAWING_001
Abstract
Description
A Mn-Cr series gear round steel with low hardenability and narrow bandwidth and its manufacturing method Technical Field
[0001] The present invention relates to the field of gear steel manufacturing, and in particular to a Mn-Cr series gear round steel with low hardenability and narrow bandwidth and a manufacturing method thereof. Background Art
[0002] Gear steel is one of the most demanding special alloy steels used in the automotive, railway, marine, and engineering machinery industries. It is the material used to manufacture core components that ensure safety. With the advancement of industrial technology, gear steel is developing towards high performance, longevity, smooth gear operation, low noise, safety, low cost, ease of processing, and a wide variety of products.
[0003] Mn-Cr gear steels are a family of high-standard steels used in automotive gears. These grades offer excellent hardenability. For example, the most widely used 20MnCr5 steel has a hardenability of 36-45 HRC (J5mm), 34-40 HRC (J9mm), and 28-34 HRC (J15mm). The hardenability value reflects the core hardness of gears of varying sizes, and the hardenability bandwidth significantly influences gear heat treatment deformation. High-quality gear steels abroad typically have a hardenability bandwidth of less than 4 HRC, while advanced domestic steels achieve 4-6 HRC, a significant gap between these standards. Low-hardenability, narrow-bandwidth gear steels offer ease of forging, excellent machinability, and minimal heat treatment deformation, making them suitable for the fabrication of certain parts. Consequently, demand for these steels is increasing, while the high hardenability of 20MnCr5 no longer meets the specific requirements of customers.
[0004] The control of the hardenability and hardenability bandwidth of gear steel mainly depends on the chemical composition and its uniformity. The internal control composition range of the steel is determined based on the influence of carbon and alloy elements in the steel on the hardness value at each hardenability point.
[0005] For example, Chinese patent application CN108193029A discloses a method for controlling the narrow hardenability bandwidth of gear steel, which uses production data to optimize the hardenability calculation formula to obtain calculation parameters suitable for gear steel grades. Then, the upper and lower limits of the composition of elements C, Si, Mn, Cr, Ni, Mo, Ti, and B that affect hardenability are calculated based on the optimized calculation formula, requiring that the hardenability bandwidth at J5, J9, J11, and J13 is less than 3.5HRC, and the obtained composition range is consistent with ΔC≤±0.01%, ΔSi≤±0.02%, ΔMn≤±0.02%, ΔCr≤±0.01%, ΔNi≤±0.01%, ΔMo≤±0.01%, ΔTi≤±0.01%, ΔAl≤±0.01%, ΔB≤±0.005%, ΔS≤±0.002% were compared, and the narrowest control range was finally determined as the composition control range for gear steel with narrow hardenability bandwidth requirements. Low superheat casting of 10-20°C was adopted to ensure that the heating temperature fluctuation of the continuous casting billet was ≤±7°C and the holding time fluctuation was ≤±5min, thus obtaining a gear steel bar with a hardenability bandwidth of less than 4HRC. However, the composition control requirements of the design of this patent application are extremely high, which is not easy to be produced on a large scale in industry, and the hardness values at J5 and J9 are still relatively high.
[0006] Chinese patent application CN115029618A discloses a narrow hardenability cold-forged gear steel and a manufacturing method thereof. The steel comprises, by mass percentage, 0.15-0.17% C, 0.10-0.20% Si, 1.0-1.10% Mn, 0.80-0.90% Cr, and 0.02-0.04% Al. The cold-forged gear steel has a hardenability of J5mm=30-34HRC and J9mm=21-25HRC. Although the hardenability value is low, its strength is also reduced, and thus it cannot meet the strength requirements of low hardenability steel.
[0007] Chinese patent application CN111945070A discloses a narrow hardenability gear steel and a manufacturing method thereof. The narrow hardenability gear steel comprises, by mass percentage, the following: C: 0.19-0.21%, Si: 0.22-0.28%, Mn: 0.82-0.87%, Cr: 0.52-0.58%, Ni: 0.50-0.55%, Mo: 0.19-0.21%, Al: 0.025-0.035%, N: 0.0080-0.0120%, and the balance Fe and unavoidable impurities. The ratio of Al to N is 3-3.6. The resulting narrow hardenability gear steel not only meets the steel's hardenability requirements but also reduces the tendency of the steel's composition to affect surface quality, effectively improving the surface quality of the narrow hardenability gear steel. This patent application reduces the surface crack sensitivity of steel by regulating the Ni content and optimizing the Al / N ratio, so that the end hardenability of the gear steel meets J4.7mm=36-41HRC, J7.9mm=28-32HRC. However, the gear steel hardenability value of this invention still cannot meet the current user processing requirements.
[0008] Summary of the Invention
[0009] The present invention aims to provide a Mn-Cr-based gear round steel with low hardenability and narrow bandwidth, and a method for manufacturing the same. The Mn-Cr-based gear round steel satisfies J5 = 33-36 HRC, J9 = 25-28 HRC, and J15 = 20-24 HRC, with a hardenability bandwidth of ≤3 HRC before J9, thereby reducing heat treatment deformation. Furthermore, the steel exhibits yield strength ≥800 MPa, tensile strength ≥1100 MPa, elongation ≥12%, reduction of area ≥50%, impact energy KU2 ≥80 J, and a grain size of no less than grade 6. The gear round steel described in the present invention can meet the performance requirements of gear steel materials for applications such as new energy vehicles, improving the stability and safety of steel used in new energy vehicles.
[0010] To achieve the above object, the technical solution of the present invention is:
[0011] A Mn-Cr gear round steel with low hardenability and narrow bandwidth, the chemical composition by mass percentage of which is: C: 0.15-0.18%, Si: 0.040-0.10%, Mn: 1.10-1.40%, P≤0.02%, S: 0.0 15~0.030%, Cr: 1.00~1.20%, Mo: 0.006~0.02%, Ni: 0.020~0.10%, Al: 0.020~0.050%, N: 0.007~0.015%, Al / N ≥ 2.0, Nb: 0.004~0.03%, [O] ≤ 0.0015%, the balance includes Fe and other unavoidable impurities; and the length b of the full martensite zone obtained at the end of the end quenching specimen made of gear round steel is in the range of: 0.70≤b≤1.16, b=0.22h-0.45,
[0012] h=(6.9[Mn] 2 +3.2[Si]+22.6[Cr] 2 +23.1[Mo]+(13.0[Cr]+2.5[Mo]+9.7)[Ni]+2.5)[C];
[0013] At the same time, the hardenability coefficient k satisfies: 1.18≤k≤1.65,
[0014] k=0.54*[C]*(-1.12+5.1*[Mn])*(1+0.7*[Si])*(1+2.16*[Cr]).
[0015] Furthermore, in the chemical composition of the gear round steel of the present invention, the balance is Fe and other inevitable impurities.
[0016] Preferably, among the unavoidable impurities, Ti≤0.003%, B≤0.0004%, and Ca≤0.003%.
[0017] Preferably, the harmful elements in the composition are As≤0.02%, Sn≤0.02%, Pb≤0.012%, Sb≤0.012%, Bi≤0.012, and the total amount of harmful elements is ≤0.05%.
[0018] The measured hardenability values of the gear round steel of the present invention satisfy J5=33-36HRC, J9=25-28HRC, J15=20-24HRC, and the hardenability bandwidth before J9 is ≤3HRC. In some embodiments, 1HRC≤the hardenability bandwidth before J9≤3HRC.
[0019] The gear round steel of the present invention has a yield strength of 800 MPa or more, a tensile strength of 1100 MPa or more, an elongation of 12% or more, a cross-sectional shrinkage of 50% or more, an impact energy KU2 of 90 J, and a grain size of not less than grade 6.
[0020] In some embodiments, the yield strength of the gear round steel of the present invention is 800-820 MPa.
[0021] In some embodiments, the tensile strength of the gear round steel of the present invention is 1100-1150 MPa.
[0022] In some embodiments, the gear round steel of the present invention has an elongation of 12% to 19%.
[0023] In some embodiments, the cross-sectional reduction rate of the gear round steel of the present invention is 50% to 65%.
[0024] In some embodiments, the impact energy KU2 of the gear round steel of the present invention is 90-100J.
[0025] In some embodiments, the grain size of the gear round steel of the present invention is 7.0 to 9.0.
[0026] In the composition design of the gear round steel of the present invention:
[0027] Carbon (C) is the most important element affecting the hardenability of gear steel, significantly impacting the terminal hardenability value. It is also the most fundamental and effective strengthening element in steel. Because carburized gear steel must maintain toughness and a certain strength at the gear core, the C content in this invention is controlled to 0.15-0.18%.
[0028] Si: Si has a strong solid solution strengthening effect in steel, replacing Fe atoms by substitution, thereby hindering dislocation motion and significantly increasing the yield strength of the steel. Si can also reduce the critical cooling rate of steel to a certain extent, increasing the hardenability value. It has a significant impact on the terminal hardenability value after J5mm, but mainly improves the stability of supercooled austenite in the medium temperature range. It has little effect on the high temperature range of 650°C to 700°C, and may even reduce its stability. The present invention requires a Si content range of 0.040% to 0.10%.
[0029] Mn: Mn strengthens the steel through solid solution strengthening and grain refinement, thereby increasing its strength. It also significantly improves the steel's hardenability, with a greater impact on the terminal hardenability above J7mm. However, Mn can lower the steel's Al temperature, promote austenite grain growth, and increase the steel's sensitivity to overheating. Therefore, in the present invention, the Mn content is controlled within a range of 1.10 to 1.40%.
[0030] Cr: Cr increases the nucleation work and transformation activation energy of pearlite, reduces the nucleation rate and growth rate of pearlite, increases the stability of supercooled austenite, improves the hardenability of steel, achieves a strengthening effect, and has a positive impact on impact toughness. Cr has a significant impact on the values at J5, J9, and J15. In the present invention, Cr is controlled within the range of 1.00-1.20%.
[0031] Ni: Ni can effectively increase the core toughness of gear steel, lower the ductile-brittle transition temperature, and improve low-temperature impact resistance. It can also refine the microstructure and achieve a strengthening effect. However, excessive Ni content can reduce the machinability of gear steel after hot working. Ni has a certain impact on J5, but a greater impact on J9 and J15. The present invention requires a Ni content range of 0.020-0.10%.
[0032] Mo: A reasonable combination of Mo and Cr significantly improves the steel's hardenability and tempering resistance, and Mo also refines grain size. However, excessive Mo content can lead to the formation of ferrite films at grain boundaries, which negatively impacts the steel's thermoplastic properties, increases its tendency to reheat cracking, and increases its cost. Mo has little effect on values above J5, but has a greater impact on values above J7. Therefore, the Mo content in this invention ranges from 0.006% to 0.020%.
[0033] The present invention requires that the P content is ≤ 0.02%. In some embodiments, the P content ranges from 0.005 to 0.02%, such as 0.007% or 0.010%.
[0034] The present invention requires that the [O] content is ≤ 0.0015%. In some embodiments, the [O] content ranges from 0.0010 to 0.0015%, for example, 0.0012%.
[0035] Hardenability refers to the ability of steel to obtain martensite during quenching after austenitization. Its magnitude is related to the cooling rate at each point on the round steel cross section. If the cooling rate exceeds the critical quenching rate of the steel, full martensite will be obtained. C is the main component affecting hardenability. Si, Mn, Cr, and Ni will reduce the critical quenching rate of steel and improve the hardenability of steel. In order to ensure the hardenability of the gear steel of the present invention, the length b of the full martensite zone at the end of the end-quenched specimen made of the round steel of the present invention must meet the following requirements: 0.70≤b≤1.16, b=0.22h-0.45,
[0036] h=(6.9[Mn] 2 +3.2[Si]+22.6[Cr] 2 +23.1[Mo]+(13.0[Cr]+2.5[Mo]+9.7)[Ni]+2.5)[C].
[0037] In some embodiments, b satisfies: 0.80≤b≤1.15.
[0038] The end quenching specimen is a standard end quenching specimen made by making the gear round steel of the present invention according to GB / T 225-2006 "End quenching test method for hardenability of steel".
[0039] In order to ensure the hardenability of the gear steel of the present invention and limit the distance from the rear end surface of the round steel after quenching to the semi-martensite zone, the hardenability coefficient k of the round steel of the present invention is required to meet 1.18≤k≤1.65 according to calculations and data analysis;
[0040] k=0.54*[C]*(-1.12+5.1*[Mn])*(1+0.7*[Si])*(1+2.16*[Cr]).
[0041] In some embodiments, k satisfies: 1.25≤k≤1.55.
[0042] Among them, C is the main element affecting hardenability. The volume and size of carbides formed by C and carbide elements will affect the hardness at different distances from the end of the end-quenched specimen. At the same time, the pinning effect of carbides on austenite grains will affect the austenite grain size, thereby affecting hardenability. The delaying effect of Mn, Cr, and Si on bainite transformation is much greater than that on pearlite transformation. The delaying effect of Mo on pearlite transformation is much greater than that on bainite. Ni can also delay pearlite transformation. Therefore, Mn, Cr, Si, Mo, and Ni improve the hardenability of round steel by increasing the stability of supercooled austenite.
[0043] To ensure that the gear steel of the present invention meets the requirements of high-temperature carburizing, the following elements are used: Al: 0.020-0.050%, N: 0.007-0.015%, Al / N ≥ 2.0, and Nb: 0.004-0.03%. This is because AlN, formed by Al and N, effectively inhibits austenite grain growth and refines austenite grains during rolling heating and high-temperature carburizing. However, AlN aggregates and dissolves at around 940°C. As the temperature rises, Al has a detrimental effect on the austenite grain size. Niobium is a very effective alloying element for grain refinement. Nb (C, N) can pin grain boundaries, hinder austenite grain growth, and effectively reduce carburizing and quenching deformation. However, when the niobium content exceeds a certain value, the carbonitride precipitates of Nb in the ingot cannot dissolve back into the gear steel matrix. As subsequent hot working or heat treatment processes are performed, some precipitates coarsen. The coarse precipitates cannot prevent the growth of austenite grains during high-temperature carburizing. Therefore, the gear steel designed by the present invention has an Al content of 0.020-0.050% and a Nb content of 0.004-0.03%. The present invention requires Al / N ≥ 2.0. In some embodiments, 2.0 ≤ Al / N ≤ 4.0.
[0044] The method for manufacturing the Mn-Cr series gear round steel with low hardenability and narrow bandwidth of the present invention comprises the following steps:
[0045] 1) Smelting and casting
[0046] Smelting and casting into ingots according to the above composition;
[0047] 2) Heating
[0048] The temperature of the preheating section is 840-880°C, the temperature of the heating section is controlled at 1120-1175°C, the temperature of the soaking section is 1150-1230°C, and the total heating time in the heating furnace is not less than 4 hours;
[0049] 3) Rolling
[0050] Control the starting rolling temperature to 1100-1170℃ and the finishing rolling temperature to 950-1000℃;
[0051] 4) Quenching + tempering
[0052] The primary quenching temperature is 850-910°C, the holding time is 30-60 minutes, and the steel is oil-cooled or water-cooled to room temperature. The secondary quenching temperature is 800-830°C, the holding time is 30-60 minutes, and the steel is oil-cooled or water-cooled to room temperature. The tempering temperature is 150-200°C, the holding time is 60-150 minutes, and the steel is air-cooled to room temperature after tempering.
[0053] In some embodiments, the total heating time in the heating furnace is 4 to 6 hours, such as 4 to 5.5 hours.
[0054] Preferably, the smelting is performed in an electric furnace or a converter, followed by LF (Ladle Furnace) refining and VD (Vacuum Degassing) vacuum degassing. During the LF refining process, the refining time is ≥50 minutes, the FeO content in the slag is less than 1.0wt%, and the white slag time is ≥20 minutes. During the VD vacuum degassing process, the vacuum degree is controlled to be ≤66.7Pa, the high vacuum time is ≥20 minutes, the calming time is ≥10 minutes, and the VD final temperature is 1550°C to 1580°C. In some embodiments, the refining time is 50 to 65 minutes. In some embodiments, the white slag time is 20 to 30 minutes. In some embodiments, the high vacuum time is 20 to 35 minutes. In some embodiments, the calming time is 10 to 20 minutes.
[0055] Preferably, the casting adopts continuous casting. In order to ensure the uniformity of the composition of the continuous casting billet from the surface to the inside, the superheat of the molten steel is controlled. At the same time, according to the narrow composition requirements of Cr, Ni, and Mo of the steel of the present invention, the narrow hardenability bandwidth requirements, and the cross-sectional dimensions of the billet, the frequency of the electromagnetic stirring of the crystallizer is controlled to 2.0~3.0HZ, and the current is 150~300A; the frequency of the end electromagnetic stirring is 8.0~8.5HZ, and the current is 300~350A; the superheat of the molten steel is controlled at 22~38°C, and the continuous casting billet drawing speed is controlled between 0.62~0.68m / min.
[0056] In the manufacturing method of the present invention,
[0057] The whole process of VD vacuum degassing can be specifically nitrogen-enriched by bottom blowing to prevent secondary oxidation of molten steel and improve the purity of molten steel.
[0058] During the continuous casting process, the frequency of the electromagnetic stirring in the mold is controlled at 2.0 to 3.0 Hz and the current is 150 to 300 A. The frequency of the electromagnetic stirring at the end is 8.0 to 8.5 Hz and the current is 300 to 350 A. During the continuous casting process, electromagnetic stirring can promote the rapid floating of larger inclusions, improve the purity of the molten steel, prevent inclusion aggregation, reduce inclusion size, and reduce the damage caused by inclusions to steel properties.
[0059] The temperature of the preheating section in the continuous casting billet heating is increased by 40°C compared with the existing technology, so it needs to be hot-charged into the furnace, which increases the heating speed from the preheating section to the heating section, makes the composition more uniform, promotes the dissolution of the precipitated phase, and facilitates the dispersion and precipitation during the rolling and cooling processes, making the hardenability of the round steel stable.
[0060] During the rolling process, the starting rolling temperature is controlled at 1100-1170℃, and the finishing rolling temperature is 950-1000℃; air cooling (such as the above cooling bed) is used to obtain ferrite + pearlite structure, and cold air blowing and water spraying are avoided to prevent the formation of bainite structure, which causes uneven structure and affects the performance of round steel obtained by subsequent heat treatment;
[0061] The heat treatment process is quenching + tempering, wherein the primary quenching temperature is 850-910°C, the holding time is 30-60 minutes, and the steel is oil-cooled or water-cooled to room temperature to promote the formation of more nucleation points and refine the austenite grains; the secondary quenching temperature is 800-830°C, the holding time is 30-60 minutes, and the steel is oil-cooled or water-cooled to room temperature; the tempering temperature is 150-200°C, the holding time is 60-150 minutes, so that the carbides are fully dispersed and precipitated, and then air-cooled to room temperature after tempering.
[0062] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0063] The invention studies the influence of elements C, Si, Mn, Cr, Mo and Ni on hardenability based on a physical metallurgical single factor method, designs and manufactures a Mn-Cr series gear round steel with low hardenability and narrow bandwidth, wherein the Mn-Cr series gear round steel meets the requirements of J5=33-36HRC, J9=25-28HRC, J15=20-24HRC, and the hardenability bandwidth before J9 is ≤3HRC, thereby meeting the user's requirement of small heat treatment deformation; and the mechanical properties meet the requirements of yield strength ≥800MPa, tensile strength ≥1100MPa, elongation ≥12%, cross-sectional shrinkage ≥50% and impact energy KU2 ≥90J.
[0064] Compared with Chinese patent applications CN115029618A and CN111945070A, the gear round steel described in the present invention has lower J5, J9 and J15 values, meeting the processing and use requirements of low hardenability gear steel, and is more suitable for application scenarios with strict requirements on heat treatment deformation, such as new energy vehicle transmission ring gears.
[0065] Compared with Chinese patent application CN115029618A, the gear round steel described in the present invention has clearer requirements on the relationship between the content of C, Si, Mn, Cr, Mo, and Ni elements. By utilizing the interaction between the elements, its mechanical properties are not reduced while meeting the low hardenability requirements, and the application scenarios are different.
[0066] The gear round steel of the present invention adopts a secondary quenching + tempering process to achieve a match of high strength and high toughness, meeting the use requirements of high-strength steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] FIG1 is a hardenability curve of Examples 1 to 6 of the present invention and Comparative Examples 1 to 2;
[0068] FIG2 is a metallographic photograph of the microstructure of Example 2 of the present invention after quenching and tempering treatment (magnification 500x). DETAILED DESCRIPTION
[0069] The present invention will be further explained and illustrated below in conjunction with the accompanying drawings and specific embodiments. However, such explanation and illustration do not constitute an improper limitation on the technical solution of the present invention.
[0070] The compositions of the embodiments of the low hardenability and narrow bandwidth Mn-Cr gear steel according to the present invention are shown in Tables 1 and 2, with the remainder being Fe and unavoidable impurities.
[0071] The composition coefficients of the round steel for gears in the embodiments are shown in Table 3. It can be seen that the length b of the martensite region of the round steel in each embodiment ranges from 0.70 to 1.16, and the hardenability coefficient k ranges from 1.18 to 1.65.
[0072] The process parameters of the manufacturing method of the embodiment of the present invention are shown in Table 4-1, Table 4-2, and Table 5. The method adopts electric furnace smelting-LF refining-VD vacuum degassing-continuous casting-heating-rolling-slow cooling, and includes the following steps:
[0073] 1) Smelting and casting
[0074] According to the components in Tables 1 and 2, the steel was smelted and cast into ingots; an electric furnace was used for smelting, followed by LF refining and VD vacuum degassing; during the LF refining process, the refining time was ≥50 min, the FeO content in the slag was less than 1.0 wt%, and the white slag time was ≥20 min; during the VD vacuum degassing process, the vacuum degree was controlled to be ≤66.7 Pa, the high vacuum time was ≥20 min, the calming time was ≥10 min, the VD final temperature was 1550° C. to 1580° C., and bottom blowing nitrogen was used throughout the VD vacuum degassing process to increase nitrogen; continuous casting was used for casting, and the frequency of the electromagnetic stirring of the crystallizer was controlled to be 2.0 to 3.0 Hz and the current was 150 to 300 A; the frequency of the end electromagnetic stirring was 8.0 to 8.5 Hz and the current was 300 to 350 A; the superheat of the molten steel was controlled to be 22 to 38° C., and the continuous casting casting speed was controlled to be between 0.62 and 0.68 m / min;
[0075] 2) Heating
[0076] The temperature of the preheating section is 840-880°C, the temperature of the heating section is controlled at 1120-1175°C, the temperature of the soaking section is 1150-1230°C, and the total heating time in the heating furnace is not less than 4 hours;
[0077] 3) Rolling
[0078] Control the starting rolling temperature to 1100-1170℃ and the finishing rolling temperature to 950-1000℃;
[0079] 4) Quenching + tempering
[0080] The primary quenching temperature is 850-910°C, the holding time is 30-60 minutes, and the steel is oil-cooled or water-cooled to room temperature. The secondary quenching temperature is 800-830°C, the holding time is 30-60 minutes, and the steel is oil-cooled or water-cooled to room temperature. The tempering temperature is 150-200°C, the holding time is 60-150 minutes, and the steel is air-cooled to room temperature after tempering.
[0081] The microstructure of the hot-rolled gear round steel obtained in step 3) was observed by metallographic method. The results showed that the microstructure of the hot-rolled gear round steel of Examples 1 to 6 was ferrite+pearlite.
[0082] The obtained round steel was subjected to end quenching experiments according to GB / T 225-2006, and the hardness at different positions away from the end of the specimen was measured (hardness test standards are: GB / T 230.1, GB / T 230.2, GB / T 230.3), as shown in Table 6 and Figure 1.
[0083] Room temperature tensile and room temperature impact tests were carried out according to GB / T 228.1-2010 and GB / T 229-2007. The measured mechanical properties are shown in Table 7.
[0084] Since different heats of steel were obtained after smelting in each embodiment and comparative example, multiple batches of bars can be produced from each heat of steel corresponding to each embodiment and comparative example. The hardenability of multiple batches of bars obtained from the same embodiment or comparative example at points J5, J9, and J15 are not exactly the same. Therefore, in Table 6, the hardenability values at points J5, J9, and J15 for Examples 1 to 6 and Comparative Examples 1 and 2 are within a range.
[0085] As can be seen from Table 6, compared with Comparative Examples 1 and 2, the round steel hardenability bandwidth of Examples 1 to 6 is narrower, and can reach ≤3HRC before J9; and the values of J5, J9, and J15 are significantly lower than those of the comparative examples, which have excellent technical effects and meet the requirements of the present invention for low hardenability narrow bandwidth.
[0086] As shown in Table 7, the examples exhibited yield strength ≥800 MPa, tensile strength ≥1100 MPa, elongation ≥12%, reduction of area ≥50%, and impact energy KU2 ≥90 J, meeting the design requirements of the present invention and demonstrating excellent comprehensive mechanical properties. KU2 represents the impact energy absorbed by the U-notch specimen in a Charpy pendulum impact test.
[0087] As shown in FIG2 , the gear round steel according to the embodiment of the present invention obtains a fine tempered martensite structure after quenching and tempering.
[0088] After the hot-rolled round steels of Examples 1 to 6 were kept at 980° C. for 4 hours, the grain size was tested according to the standard GB / T 6394-2017 “Method for Determination of Average Grain Size of Metals”. The test results are shown in Table 8.
[0089] The low-hardenability, narrow-bandwidth gear round steel produced by the method of the present invention satisfies J5=33-36HRC, J9=25-28HRC, and J15=20-24HRC, with a hardenability bandwidth of ≤3HRC before J9. Furthermore, the Al and N contents are controlled, and Nb is added, so that the grain size of the hot-rolled round steel after being held at 980°C for 4 hours is no less than grade 6. Therefore, the low-hardenability, narrow-bandwidth gear round steel produced by the method of the present invention can meet the processing requirements of high-temperature carburized gear rings for new energy vehicles.
[0090] The above embodiments are intended to enable those skilled in the art to understand the contents of the present invention and implement them accordingly. The scope of protection of the present invention is not limited to the above embodiments. Therefore, any equivalent changes or modifications made based on the principles and design ideas disclosed in the present invention are within the scope of protection of the present invention.
[0091] Table 1: Main chemical components (wt.%) of Examples and Comparative Examples
[0092] Note: Comparative Example 1-CN113444979A, Comparative Example 2-CN115029618A.
[0093] Table 2: Chemical composition of harmful elements in the examples (wt.%)
[0094] Table 3: Composition coefficients of round steel bars of Examples and Comparative Examples
[0095] Note: Comparative Example 1-CN113444979A, Comparative Example 2-CN115029618A.
[0096] Table 4-1
[0097] Note: Comparative Example 1-CN113444979A, Comparative Example 2-CN115029618A.
[0098] Table 4-2
[0099] Table 5
[0100] Table 6: Hardenability values of round steel in Examples and Comparative Examples
[0101] Note: J5 indicates the hardness at 5 mm from the end of the end-quenched specimen, J9 indicates the hardness at 9 mm from the end of the end-quenched specimen, and J15 indicates the hardness at 15 mm from the end of the end-quenched specimen.
[0102] Table 7: Mechanical properties of round steel in the examples
[0103] Table 8: Grain size of round steel in the examples
Claims
1. A Mn-Cr gear round steel with low hardenability and narrow bandwidth, the chemical composition by mass percentage is: C: 0.15-0.18%, Si: 0.040-0.10%, Mn: 1.10-1.40%, P≤0.02%, S: 0.015-0.030%, Cr: 1.00-1.20%, Mo: 0.006-0.02%, Ni: 0.020-0.1 0%, Al: 0.020~0.050%, N: 0.007~0.015%, Al / N≥2.0, Nb: 0.004~0.03%, [O]≤0.0015%, the balance includes Fe and other unavoidable impurities; and the length b range of the end of the end quenching sample made of gear round steel to obtain the full martensite zone is: 0.70≤b≤1.16, b=0.22h-0.45, h=(6.9[Mn] 2 +3.2[Si]+22.6[Cr] 2 +23.1[Mo]+(13.0[Cr]+2.5[Mo]+9.7)[Ni]+2.5)[C]; At the same time, the hardenability coefficient k satisfies: 1.18≤k≤1.65, k=0.54*[C]*(-1.12+5.1*[Mn])*(1+0.7*[Si])*(1+2.16*[Cr]).
2. The low hardenability and narrow bandwidth Mn-Cr gear round steel according to claim 1, characterized in that: In its chemical composition, the balance is Fe and other inevitable impurities.
3. The low hardenability and narrow bandwidth Mn-Cr gear round steel according to claim 1 or 2, characterized in that: Among the unavoidable impurities, Ti≤0.003%, B≤0.0004%, and Ca≤0.003%.
4. The Mn-Cr gear round steel with low hardenability and narrow bandwidth according to claim 1, 2 or 3, characterized in that: Harmful elements in the composition are As≤0.02%, Sn≤0.02%, Pb≤0.012%, Sb≤0.012%, Bi≤0.012, and the total amount of harmful elements is ≤0.05%.
5. The low hardenability narrow bandwidth Mn-Cr gear round steel according to any one of claims 1 to 4, characterized in that: The microstructure of the hot-rolled gear round steel is ferrite+pearlite.
6. Low hardenability narrow bandwidth Mn-Cr gear round steel according to any one of claims 1 to 5, characterized in that: The measured hardenability values of the gear round steel satisfy J5=33-36HRC, J9=25-28HRC, J15=20-24HRC, and the hardenability bandwidth before J9 is ≤3HRC.
7. The low hardenability narrow bandwidth Mn-Cr gear round steel according to any one of claims 1 to 6, characterized in that: The mechanical properties of the gear round steel meet the following requirements: yield strength ≥800MPa, tensile strength ≥1100MPa, elongation ≥12%, cross-sectional shrinkage ≥50%, impact energy KU2 ≥90J, and grain size not less than grade 6.
8. The low hardenability and narrow bandwidth Mn-Cr gear round steel according to claim 6, characterized in that: The hardenability bandwidth before J9 satisfies: 1HRC≤hardenability bandwidth before J9≤3HRC.
9. The low hardenability and narrow bandwidth Mn-Cr gear round steel according to claim 7 is characterized in that the yield strength of the gear round steel is 800-820 MPa, the tensile strength is 1100-1150 MPa, the elongation is 12%-19%, the cross-sectional reduction rate is 50%-65%, the impact energy KU2 is 90-100 J, and the grain size is 7.0-9.
0.
10. The low hardenability and narrow bandwidth Mn-Cr gear round steel according to claim 1, characterized in that: b satisfies: 0.80≤b≤1.15, and / or, k satisfies: 1.25≤k≤1.
55.
11. The method for producing a Mn-Cr gear round steel with low hardenability and narrow bandwidth according to any one of claims 1 to 10, characterized in that: The steps include: (1) Smelting and casting Smelting and casting into ingots according to the composition of claim 1, 2, 3 or 4; (2) Heating The temperature of the preheating section is 840-880°C, the temperature of the heating section is controlled at 1120-1175°C, the temperature of the soaking section is 1150-1230°C, and the total heating time in the heating furnace is not less than 4 hours; (3) Rolling Control the starting rolling temperature to 1100-1170°C and the final rolling temperature to 950-1000°C; (4) Quenching + tempering The primary quenching temperature is 850-910°C, the holding time is 30-60 minutes, and it is oil-cooled or water-cooled to room temperature; the secondary quenching temperature is 800-830°C, the holding time is 30-60 minutes, and it is oil-cooled or water-cooled to room temperature; the tempering temperature is 150-200°C, the holding time is 60-150 minutes, and it is air-cooled to room temperature after tempering.
12. The method for manufacturing Mn-Cr gear round steel with low hardenability and narrow bandwidth according to claim 11, characterized in that: The smelting adopts an electric furnace or a converter, and then undergoes LF refining and VD vacuum degassing; in the LF refining process, the refining time is ≥50min, the FeO content in the slag is less than 1.0wt%, and the white slag time is ≥20min; in the VD vacuum degassing process, the vacuum degree is controlled to be ≤66.7Pa, the high vacuum time is ≥20min, the calming time is ≥10min, the VD final temperature is 1550°C to 1580°C, and bottom blowing nitrogen is used to increase nitrogen in the entire VD vacuum degassing process.
13. The method for manufacturing Mn-Cr gear round steel with low hardenability and narrow bandwidth according to claim 11, characterized in that: The casting adopts continuous casting, and the frequency of electromagnetic stirring of the crystallizer is controlled to be 2.0-3.0HZ, and the current is 150-300A; the frequency of electromagnetic stirring at the end is 8.0-8.5HZ, and the current is 300-350A; the superheat of molten steel is controlled at 22-38°C, and the continuous casting billet drawing speed is controlled between 0.62-0.68m / min.