High-resistance laminated steel and manufacturing method therefor

MYPI2025006553A0Undetermined Publication Date: 2024-10-26BAOSHAN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025006553
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-25
Publication Date
2024-10-26

AI Technical Summary

Technical Problem

Existing coated iron has deficiencies in corrosion resistance, especially in salty or sulfur-containing environments, and the existing technology does not fully pay attention to the impact of the substrate surface and the interface between the film and the substrate on product resistance.

Method used

Using a low-roughness substrate and a three-layer structure of polyester film, including a thermal lamination layer, an intermediate layer and a barrier layer, a coated iron with high interface adhesion performance is formed through lamination thermal lamination technology. The amount of oil applied on the surface of the substrate is controlled within 1.5~3.5mg/m2, the combined design of modified copolyester and homopolyester ensures resistance under high temperature sterilization conditions.

Benefits of technology

It significantly improves the salt resistance and sulfur resistance of coated iron, avoids the decrease in interface adhesion during high-temperature sterilization, and meets the demand for food metal packaging with high resistance requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Disclosed in the present invention is high-resistance laminated steel, which comprises a substrate and a polyester film covering the surface of the substrate, wherein the surface roughness of the substrate is 0.15-0.35 μm, and the surface of the substrate is subjected to an oiling treatment; and the polyester film sequentially comprises a thermal coating layer, a middle layer and a barrier layer from top to bottom in the thickness direction, the thermal coating layer being composed of a modified copolyester, the middle layer being a mixture of a modified copolyester and a homopolyester, and the barrier layer being composed of a non-modified homopolyester. Correspondingly, further disclosed in the present invention is a manufacturing method for the high-resistance laminated steel.
Need to check novelty before this filing date? Find Prior Art

Description

High-resistance coated iron and manufacturing method thereof Technical Field

[0001] The present invention relates to a composite material and a manufacturing method thereof, in particular to a coated iron and a manufacturing method thereof. Background Art

[0002] Coated iron generally refers to a composite material obtained by directly laminating a high-molecular-weight polyester film onto a steel substrate through a heat-melting method. It can be used for both can bodies and lids, and is suitable for food cans, beverage cans, standard lids, easy-open lids, and more. Food canning applications are a key development area for coated iron. When the contents of the can are primarily meat-based, or when differentiating foods such as pickled garlic or crab are involved, higher resistance requirements are placed on the can body. The resistance of coated iron is closely related to the type and structure of the surface film, as well as the interface properties between the film and the substrate.

[0003] A Chinese patent document entitled "Polyester Resin for Metal Sheet Coating and Preparation Method Thereof," with publication number CN101646712A and publication date February 10, 2010, provides a polyester resin for metal sheet coating. The polyester resin is composed of an acid component primarily composed of terephthalic acid, containing 1 to 15 mol% of isophthalic acid and 2 to 10 mol% of dimer acid, and an alcohol component primarily composed of ethylene glycol. The polyester resin is characterized by excellent impact resistance and processing adhesion. However, its corrosion resistance is evaluated using a distilled water simulant at 125°C for 30 minutes, and does not demonstrate resistance to saline or sulfur-containing simulants.

[0004] Furthermore, the current focus on the performance of coated iron is on its adhesion, while its corrosion resistance is typically enhanced through the design of modified polymer films. However, as a composite material, existing technologies have not yet addressed the impact of the substrate surface and the interface between the film and the substrate on the product's resistance.

[0005] Based on this, it is hoped to provide a coated iron and a manufacturing method thereof that can meet the demand for high resistance.

[0006] Summary of the Invention

[0007] One of the purposes of the present invention is to provide a highly resistant coated iron, which adopts a low-roughness substrate and then laminarly coats a polyester film with a multi-layer structure on the substrate to form a coated iron product that has high resistance to high-temperature sterilization after deformation during canning, especially resistance to salt and sulfur.

[0008] In order to achieve the above-mentioned object, the present invention proposes a high-resistance coated iron, which includes a substrate and a polyester film coated on the surface of the substrate, wherein:

[0009] The surface roughness of the substrate is 0.15 to 0.35 μm, and the surface of the substrate is oiled;

[0010] The polyester film comprises a heat-sealing layer, an intermediate layer and a barrier layer in order from top to bottom in the thickness direction, wherein the heat-sealing layer is composed of modified copolyester, the intermediate layer is a mixture of modified copolyester and homopolyester, and the barrier layer is composed of unmodified homopolyester.

[0011] In the high-resistance coated iron of the present invention, the heat-coated layer of the polyester film is in contact with the substrate.

[0012] The present invention adopts a substrate with low surface roughness and a three-layer polyester film, and laminates the polyester film on the substrate by heat lamination. While achieving high interface adhesion performance, after canning and forming, high-temperature sterilization can greatly improve its resistance. It is suitable for the field of food metal packaging that has high resistance requirements for the filled contents.

[0013] Among them, the low surface roughness of 0.15 to 0.35 μm is an important surface quality indicator of the substrate, which is closely related to the surface properties of the coated iron and is related to the adhesion and corrosion resistance of the coated iron described in the present invention.

[0014] In some embodiments, the surface roughness of the substrate in the high-resistance coated iron of the present invention is 0.25 to 0.30 μm.

[0015] The three-layer polyester film has an upper layer (thermal lamination layer) that can well meet the thermal lamination between the substrate and the film, has excellent adhesion performance, and can meet the processing and forming requirements. At the same time, the lower layer (barrier layer) can provide good barrier properties and meet the requirements of high resistance. The middle layer is a transition layer, which avoids structural damage to the non-laminating layer due to heat and can prevent delamination during the deformation process of the film.

[0016] Furthermore, in the high-resistance coated iron of the present invention, the substrate is a chrome-plated plate.

[0017] Of course, in other embodiments, the substrate may also be other plates, such as a tin-plated plate.

[0018] Furthermore, in the high-resistance coated iron of the present invention, the surface of the substrate is oiled, and the amount of oil applied to the surface of the substrate is 1.5 to 3.5 mg / m 2 .

[0019] Generally speaking, the main purpose of oiling the substrate is to prevent rust and lubricate it to prevent friction. However, the inventors of this case found that excessive oiling can easily have a negative impact on the interface adhesion performance after coating. During normal use, the coated iron will be deformed after canning, which will lead to a decrease in interface adhesion and thus affect its corrosion resistance. Based on this, the present invention reduces the amount of oil applied to the substrate surface to 1.5-3.5 mg / m 2 , to ensure better interface adhesion performance.

[0020] Furthermore, in the high-resistance coated iron of the present invention, the type of oil is selected from at least one of the following: dioctyl sebacate (DOS), cottonseed oil (CSO), and acetyl tri-n-butyl citrate (ATBC).

[0021] Furthermore, in the high-resistance coated iron of the present invention, the melting point of the modified copolyester is 220-232°C.

[0022] Furthermore, in the high-resistance coated iron of the present invention, the modified copolyester is obtained by copolymerizing polyester with isophthalic acid or aliphatic diols. In some embodiments, the modified copolyester is obtained by copolymerizing polyethylene terephthalate with isophthalic acid or aliphatic diols.

[0023] Furthermore, in the high-resistance coated iron of the present invention, the aliphatic diol is selected from at least one of the following: propylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, and 1,4-cyclohexanedimethanol.

[0024] Furthermore, in the high-resistance coated iron of the present invention, the aliphatic diol is selected from: neopentyl glycol and / or 1,4-cyclohexanedimethanol.

[0025] Furthermore, in the high-resistance coated iron of the present invention, the unmodified homopolymer is polyethylene terephthalate.

[0026] Furthermore, in the high-resistance coated iron of the present invention, the melting point of the unmodified homopolyester is 250-260°C.

[0027] Furthermore, in the high-resistance coated iron of the present invention, the mass percentage of the modified copolyester in the intermediate layer is 20% to 80%.

[0028] Furthermore, in the high-resistance coated iron of the present invention, the homopolymer polyester in the intermediate layer is a non-modified homopolymer polyester, such as polyethylene terephthalate.

[0029] Furthermore, in the high-resistance coated iron of the present invention, the modified copolyester in the intermediate layer is the same as the modified copolyester in the thermal lamination layer, and the homopolyester in the intermediate layer is the same as the unmodified homopolyester in the barrier layer.

[0030] Furthermore, the mass percentage of the modified copolyester in the middle layer is 30% to 70%, for example, 30% to 50%.

[0031] Furthermore, in the high-resistance coated iron of the present invention, the thickness of the polyester film is 20 to 35 μm.

[0032] Furthermore, the polyester film has a thickness of 25 to 30 μm.

[0033] Furthermore, in the polyester film, the thickness of the heat-bonding layer is 5-10 μm, the thickness of the intermediate layer is 10-15 μm, and the thickness of the barrier layer is 5-10 μm.

[0034] Another object of the present invention is to provide a method for manufacturing high-resistance coated iron, by which a highly resistant coated iron product can be produced.

[0035] Based on the above objectives, the present invention also provides a method for manufacturing the high-resistance coated iron as described above, which comprises the steps of:

[0036] (1) performing heating pretreatment on the substrate;

[0037] (2) Film thermal lamination;

[0038] (3) Cool and squeeze dry.

[0039] Furthermore, in the heating pretreatment step of the manufacturing method of the present invention, the substrate with the surface coated with oil is heated to 150-180°C.

[0040] Heating the substrate to a temperature of 150-180°C facilitates the volatilization of the oil on the substrate surface, further reducing the amount of oil on the substrate surface. After the oil evaporates, the substrate temperature can be stabilized by the induction heating roller to the target lamination temperature.

[0041] Furthermore, in the manufacturing method of the present invention, in the film thermal lamination step, the lamination speed is controlled to be 60-120 m / min.

[0042] Furthermore, in the cooling and squeezing step of the manufacturing method of the present invention, the coated iron is first cooled to below 80° C. by spraying water, then water quenched in a water quenching tank, and then squeezed by a squeezing roller.

[0043] The high-resistance coated iron of the present invention has the following advantages and beneficial effects:

[0044] The present invention adopts a low-roughness, low-oil substrate, pre-treats the surface by heating to remove oil, and then laminates a three-layer polyester film on the substrate through hot lamination to form a coated iron product that can meet high resistance requirements, especially salt resistance and sulfur resistance.

[0045] The three-layer polyester film used in the present invention has an upper layer that can well meet the thermal bonding between the substrate and the film, a lower layer that can provide good barrier properties and meet the requirements of high resistance, and a middle layer that is a transition layer that can prevent delamination during film deformation.

[0046] In some preferred embodiments of the present invention, the roughness Ra value range is 0.15 to 0.35 μm, and the surface oil coating amount is 1.5 to 3.5 mg / m 2 The substrate can effectively improve the interface adhesion performance of the coated iron and meet the high resistance requirements after canning deformation.

[0047] After the coated iron of the present invention is formed into a can, it is sterilized at a high temperature of 121°C for 60 minutes using a 3wt% NaCl solution and a cysteine ​​simulation solution. The inner wall has no abnormal phenomena such as whitening, white bubbles, and sulfide spots, and can meet the high resistance requirements of foods such as fish and meat as the contents. DETAILED DESCRIPTION

[0048] The high-resistance coated iron and the manufacturing method thereof described in the present invention will be further explained and illustrated below in conjunction with specific embodiments. However, such explanation and illustration do not constitute an undue limitation to the technical solution of the present invention.

[0049] Examples 1-6 and Comparative Examples 1-2

[0050] In the present invention, the coated iron of Examples 1-6 are all prepared by the following steps:

[0051] (1) Use an induction heater to pre-heat the chrome-plated or tin-plated substrate: the surface roughness Ra of the substrate is 0.15-0.35 μm, and the amount of oil applied on the substrate surface is 1.5-3.5 mg / m 2 , heat the substrate to a temperature of 150-180°C.

[0052] (2) Film thermal lamination: A polyester film having a three-layer structure is thermally laminated onto a substrate by a laminating roller at a laminating speed of 60 to 120 m / min. The polyester film comprises a thermal laminating layer, an intermediate layer, and a barrier layer in the thickness direction from top to bottom. The thermal laminating layer is composed of a modified copolyester, the intermediate layer is a mixture of a modified copolyester and a homopolyester, and the barrier layer is composed of an unmodified homopolyester. The unmodified homopolyester is polyethylene terephthalate (PET). The modified copolyester is obtained by copolymerizing and modifying PET with isophthalic acid or aliphatic diols. The modified copolyester in the intermediate layer is the same as the modified copolyester in the thermal laminating layer, and the homopolyester in the intermediate layer is the same as the unmodified homopolyester in the barrier layer. The thermal laminating layer of the polyester film is in contact with the substrate.

[0053] In some embodiments, the modified copolyester is obtained by copolymerizing polyester with isophthalic acid or aliphatic diol, wherein the aliphatic diol can be selected from: neopentyl glycol and / or 1,4-cyclohexanedimethanol.

[0054] It should be noted that, although not listed in the following examples, the aliphatic diol can also be selected from at least one of the following: propylene glycol, butanediol, pentanediol, and hexanediol.

[0055] In some embodiments, the melting point of the modified copolyester may be 220-232° C. The melting point of the unmodified homopolyester is 250-260° C. The mass percentage of the modified copolyester in the middle layer is 20%-80%.

[0056] In some embodiments, the polyester film has a thickness of 20-35 μm, wherein the heat-sealing layer has a thickness of 5-10 μm, the intermediate layer has a thickness of 10-15 μm, and the barrier layer has a thickness of 5-10 μm.

[0057] (3) Cooling and squeezing: First, use water spray to cool the coated iron to ≤80℃, then water quench it in a water quenching tank, and then squeeze it dry with a squeezing roller.

[0058] Table 1, Table 2-1 and Table 2-2 list the specific process parameters of Examples 1-6 of the present invention and Comparative Examples 1-2.

[0059] In the present invention, the test standard for the surface roughness Ra of the substrate is: GB / T 1031-2016 Product Geometry Specification (GPS) Surface Structure Profile Method Surface Roughness Parameters and Their Values.

[0060] Table 1.

[0061] Table 2-1.

[0062] Table 2-2.

[0063] The coated iron of Examples 1-6 and the comparative coated iron of Comparative Examples 1-2, which were ultimately produced using the above-mentioned process of the present invention, were sampled, and the interface adhesion performance, salt resistance performance, and sulfur resistance of each example and comparative example sample were tested. The test results are listed in Table 3 below. The test methods for interface adhesion performance, salt resistance performance, and sulfur resistance are as follows:

[0064] Interface Adhesion: Adhesion after deformation is measured using the cross-hatch cupping tape peeling method. A 10cm x 10cm sheet of coated iron is scratched on a flat surface in a "well" pattern with 5mm intervals. After scratching through the film (taking care not to pierce the substrate), the tape is deformed using a cupping technique, keeping the highest point of the cupping tape in the center of the "well" pattern. The specimen is then placed in a pressure steam sterilizer and sterilized at 121°C for 60 minutes. After removing the specimen, observe the cross-hatch areas, particularly at the intersections of the "well" pattern, to evaluate film adhesion.

[0065] Salt resistance: After the coated iron is canned (can type 538), it is filled with a 3wt% NaCl solution. After sealing, the can is steamed at 121°C for 30 minutes. After cooling, the sample is removed and observed for abnormalities such as whitening, blistering, and film shedding. This is used to evaluate the salt resistance of the coated metal sheet.

[0066] Sulfur resistance: After the coated iron is canned (can type 538), it is filled with a cysteine ​​simulation solution (sulfur resistance test reagent: 0.56g L-cysteine, 3.6g potassium dihydrogen phosphate, and 7.2g disodium hydrogen phosphate are dissolved and the volume is fixed to 1000mL). After sealing, the can is steamed at 121°C for 60 minutes. After cooling, the sample is removed and observed for abnormalities such as whitening, sulfide spots, and film shedding on the surface. This is used to evaluate the sulfur resistance of the coated metal sheet.

[0067] Table 3 lists the relevant performance test results of the coated iron of Examples 1-6 and Comparative Examples 1-2.

[0068] Table 3. Note: In Table 3 above, "×" indicates that the corresponding performance is unqualified; "△" indicates that the corresponding performance is qualified; "○" indicates that the corresponding performance is good; and "◎" indicates that the corresponding performance is excellent. The evaluation criteria are shown in Table 4 below.

[0069] Table 4.

[0070] It can be seen from Table 3 that the coated iron of Examples 1-6 of the present invention has excellent surface adhesion performance, and also has excellent salt resistance and sulfur resistance.

[0071] After the coated iron of the present invention is formed into a can, it is sterilized at a high temperature of 121°C for 60 minutes using a 3wt% NaCl solution and a cysteine ​​simulation solution. The inner wall has no abnormal phenomena such as whitening, white bubbles, and sulfide spots, and can meet the high resistance requirements of foods such as fish and meat as the contents.

[0072] It should be noted that the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.

[0073] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therefrom that can be directly derived from or easily conceived by those skilled in the art based on the disclosure of the present invention are intended to fall within the scope of protection of the present invention.

Claims

1. A high-resistance coated iron, comprising a substrate and a polyester film coated on the surface of the substrate, characterized in that: The surface roughness of the substrate is 0.15 to 0.35 μm; The polyester film comprises a heat-bonding layer, an intermediate layer and a barrier layer in order from top to bottom in the thickness direction, wherein the heat-bonding layer is composed of modified copolyester, the intermediate layer is a mixture of modified copolyester and homopolyester, and the barrier layer is composed of unmodified homopolyester.

2. The high-resistance coated iron according to claim 1, characterized in that: The substrate is a chrome-plated plate.

3. The high-resistance coated iron according to claim 1, characterized in that: The surface of the substrate is coated with oil, and the amount of oil applied to the surface of the substrate is 1.5 to 3.5 mg / m 2 .

4. The high-resistance coated iron according to claim 3, characterized in that: The coating oil is selected from at least one of the following: dioctyl sebacate, cottonseed oil, and acetyl tri-n-butyl citrate.

5. The high-resistance coated iron according to claim 1, characterized in that: The melting point of the modified copolyester is 220-232°C.

6. The high-resistance coated iron according to claim 1, characterized in that: The modified copolymer polyester is obtained by copolymerizing and modifying polyester with isophthalic acid or aliphatic diol.

7. The high-resistance coated iron according to claim 6, characterized in that: The aliphatic diol is selected from at least one of the following: propylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, and 1,4-cyclohexanedimethanol.

8. The high-resistance coated iron according to claim 7, characterized in that: The aliphatic diol is selected from neopentyl glycol and / or 1,4-cyclohexanedimethanol.

9. The high-resistance coated iron according to claim 1, characterized in that: The non-modified homopolymer polyester is polyethylene terephthalate.

10. The high-resistance coated iron according to claim 1, characterized in that: The melting point of the non-modified homopolyester is 250-260°C.

11. The high-resistance coated iron according to claim 1, characterized in that: The mass percentage of the modified copolyester in the middle layer is 20% to 80%.

12. The high-resistance coated iron according to claim 1, characterized in that: The polyester film has a thickness of 20 to 35 μm.

13. The method for producing high-resistance coated iron according to any one of claims 1 to 12, characterized in that: Includes steps: (1) performing heating pretreatment on the substrate; (2) Film thermal lamination; (3) Cool and squeeze dry.

14. The manufacturing method according to claim 13, characterized in that: In the heating pretreatment step, the substrate with the surface oiled is heated to 150-180° C.; and / or, in the thin film thermal lamination step, the lamination speed is controlled to be 60-120 m / min.

15. The manufacturing method according to claim 13, characterized in that: In the cooling and squeezing step, the coated iron is first cooled to ≤80°C by spraying water, then water quenched in a water quenching tank, and then squeezed by a squeezing roller.