Polybutadiene latex and preparation method therefor, and ABS resin and preparation methods therefor

MYPI2025006577A0Undetermined Publication Date: 2024-10-28KINGFA SCI & TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025006577
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-08-29
Publication Date
2024-10-28

AI Technical Summary

Technical Problem

During the electroplating process, ABS resin materials cause pitting defects due to the agglomeration of butadiene rubber, which reduces the yield rate of electroplated parts, especially in automotive interior and exterior parts.

Method used

Use polybutadiene latex with an average particle size of 290-315nm and a number-average particle size distribution curve with a half-peak width of 20-150nm, and control the residual butadiene monomer content at 0.005%-1.6%, and conduct quantitative analysis by gas chromatography. , combined with specific polymerization reaction conditions and component ratios, a polybutadiene latex with excellent dispersion properties is prepared for blending with ABS resin to avoid rubber agglomeration.

Benefits of technology

It significantly improves the electroplated surface appearance and coating bonding strength of ABS resin, reduces the occurrence of pitting defects, improves the yield rate of electroplated parts, and ensures high-quality production of automotive interior and exterior parts.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a polybutadiene latex and an ABS resin, and preparation methods therefor. An average particle size of the polybutadiene latex is 290 - 315 nm, a half-peak width of a number-average particle size distribution curve is 20 - 150 nm, and meanwhile, a content of a residual butadiene monomer in the latex accounts for 0.005%-1.6% of a dry basis of the entire polybutadiene latex. The ABS resin includes: 15-40 parts of ABS high-rubber powder and 60-78 parts of a styrene-acrylonitrile copolymer. The ABS resin has a good electroplated surface appearance and plating adhesion. No Figure
Need to check novelty before this filing date? Find Prior Art

Description

Polybutadiene latex and ABS resin and preparation method thereof Technical Field

[0001] The invention belongs to the field of polymer technology, and particularly relates to polybutadiene latex and ABS resin and a preparation method thereof. Background Art

[0002] Compared with metal parts, plastic electroplated parts can not only achieve a good metallic texture, but also significantly reduce the weight of the parts. While effectively improving the appearance and decorativeness of the plastic material, it also improves its electrical, thermal and corrosion resistance properties, while also increasing the surface mechanical strength. However, the selection of plastic materials for electroplating requires comprehensive consideration of factors such as the material's processing performance, mechanical properties, material cost, electroplating cost, the difficulty of electroplating, and dimensional accuracy. Among many polymer materials, ABS resin material has excellent overall performance and is easy to process and shape due to its structural advantages. In addition, the ABS surface is easily corroded by the electroplating solution, resulting in a high coating adhesion. Therefore, it is currently widely used in electroplating. ABS resin specifically refers to a blend of a graft copolymer of polybutadiene rubber and monomers styrene and acrylonitrile with a matrix SAN resin, where A represents acrylonitrile, B represents butadiene, and S represents styrene. For electroplating-grade ABS plastic, the content of each material component is critical, among which the butadiene content has a greater impact on electroplating. This is because ABS is a non-conductor. To electroplate it, a conductive layer must be covered on the surface of the material. The formation of the conductive layer requires processes such as roughening, neutralization, sensitization, activation, and chemical plating. Roughening is the process of etching away butadiene through an oxidation reaction, forming an activated hydrophilic surface and anchor-like structure on the part to improve the adhesion of the coating. Therefore, the higher the butadiene content, the better the adhesion of the coating. In actual application, in order to blindly improve the adhesion of the coating, material designers significantly increase the butadiene rubber content and increase the particle size of the butadiene rubber. This makes the butadiene rubber very easy to agglomerate in the ABS resin, resulting in a large number of defects such as pitting on the surface of the injection-molded parts, significantly reducing the yield rate of electroplated parts. Especially for automotive electroplated door handles, grilles, decorative strips and other interior and exterior parts that have very stringent usage requirements, defects such as pitting make the yield rate of electroplated products less than 50%, causing great trouble to automobile OEMs and parts suppliers.

[0003] Chinese patent CN114479300A discloses an electroplating-grade ABS resin composition comprising, by weight, 15-30 parts of a polybutadiene rubber grafted with acrylonitrile and styrene copolymer, 60-80 parts of a base SAN resin, and 5-10 parts of a compatibilized SAN resin. The base SAN resin has an acrylonitrile content of 30-34% by weight, while the compatibilized SAN resin has an acrylonitrile content of 24-27% by weight. The addition of the compatibilized SAN resin improves the compatibility of the polybutadiene rubber with the base SAN resin, resulting in a sharp-edged inverted shoe structure during the electroplating roughening stage. This provides greater coating tensile strength, significantly reduces pitting defects, and improves the yield rate of electroplated products. Chinese patent CN104045963B discloses a glass fiber reinforced high-gloss ABS resin composition suitable for electroplating. This patent uses a low-molecular-weight SAN additive, which not only enhances the rigidity of the ABS resin composition but also effectively improves its fluidity, reduces glass fiber exposure, and makes the surface of the injection-molded part appear glossy. It can effectively reduce the linear thermal expansion coefficient of plastic electroplated products and effectively reduce plating defects and pitting caused by glass fiber leakage. Chinese patent CN112489635A discloses a transparent PC / ABS alloy and its preparation method. This invention first blends and extrudes ABS resin and styrene-grafted butadiene rubber, then uses a compatibilizer to encapsulate the rubber phase in the ABS within the styrene phase to prevent rubber agglomeration. The two-step method first prepares a transparent ABS masterbatch with a refractive index close to that of PC, and then co-extrudes the masterbatch and PC resin into pellets to produce the transparent PC / ABS alloy. The above technical solutions can reduce the possibility of pitting to a certain extent, but they all involve back-end modification, forcing the rubber to disperse by introducing a third component or compatibilizer, and cannot fundamentally address the thermodynamic tendency of rubber to self-agglomerate.

[0004] Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide a polybutadiene latex and ABS resin and a preparation method thereof, so as to overcome the defect that a large number of pits are easily generated during the electroplating process of ABS resin in the prior art.

[0006] The invention provides a polybutadiene latex. The average particle size of the polybutadiene latex is 290-315 nm, the half-peak width of the number-average particle size distribution curve is 20-150 nm, and the residual butadiene monomer content in the polybutadiene latex accounts for 0.005%-1.6% of the dry basis of the entire polybutadiene latex.

[0007] The above-mentioned residual butadiene monomer content ratio is quantitatively obtained by gas chromatography according to the external standard method, specifically: 0.1-0.5 g of the sample is weighed and constant to 0.1 mg, and the headspace bottle containing the sample is placed in a headspace automatic sampler. The gas chromatography of the non-polar chromatographic column (PC-1) of the gas chromatography is used, and the FID detector measures the gas chromatography spectrum integral area of ​​the residual butadiene in the latex. The amount of residual butadiene is converted by the standard curve, and the value is divided by the total dry basis amount of the entire polybutadiene latex to obtain the amount.

[0008] The average particle size of the polybutadiene latex in the present invention is 290-315 nm, which can be understood to include but not limited to 290 nm, 295 nm, 298 nm, 300 nm, 302 nm, 303 nm, 305 nm, 308 nm, 310 nm, 312 nm, and 315 nm.

[0009] The half-peak width of the number average particle size distribution curve in the present invention is 20-150nm, which can be understood to include but not limited to 20nm, 22nm, 25nm, 28nm, 30nm, 33nm, 35nm, 40nm, 42nm, 45nm, 50nm, 53nm, 55nm, 58nm, 60nm, 63nm, 65nm, 70nm, 72nm, 75nm, 78nm, 80nm, 83nm, 84nm, 86nm, 87nm, 88nm, 89nm, 90nm, 91nm, 92nm, 93nm, 94nm, 95nm, 96nm, 97nm, 98nm, 99nm, 100nm, 101nm, 102nm, 103nm, 104 5nm, 88nm, 90nm, 92nm, 95nm, 98nm, 100nm, 103nm, 105nm, 107nm, 110nm, 113nm, 115nm, 117nm, 120nm, 123nm, 125nm, 128nm, 130nm, 133nm, 135nm, 138nm, 140nm, 142nm, 145nm, 148nm, 150nm.

[0010] The content of residual butadiene monomer in the polybutadiene latex of the present invention is 0.005%-1.6% of the dry basis of the entire polybutadiene latex, which can be understood to include but not limited to 0.005%, 0.008%, 0.01%, 0.012%, 0.015%, 0.018%, 0.021%, 0.025%, 0.028%, 0.030%, 0.032%, 0.035%, 0.038%, 0.040%, 0.045%, 0.050%, 0.055%, 0.060%. %, 0.065%, 0.070%, 0.075%, 0.08%, 0.085%, 0.090%, 0.095%, 0.1%, 0.15%, 0.2%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50%, 0.55%, 0.60%, 0.65%, 0.70%, 0.75%, 0.80%, 0.85%, 0.90%, 0.95%, 1.0%, 1.2%, 1.3%, 1.5%, 1.6%.

[0011] Preferably, the average particle size of the polybutadiene latex is 300-310 nm, and the half-peak width of the number average particle size distribution curve is 30-100 nm.

[0012] Preferably, the content of residual butadiene monomer in the polybutadiene latex accounts for 0.01% to 0.8% of the dry basis of the entire polybutadiene latex.

[0013] Preferably, the polybutadiene latex has a gel weight fraction of 50-95%. Controlling the gel content within a reasonable range ensures excellent dispersion during subsequent polymerization and mixing processes, effectively preventing poor electroplating due to rubber agglomeration. The gel content is tested in accordance with the "Determination of Gel Content of Synthetic Raw Rubber," standard number SH / T 1050-1991.

[0014] The present invention also provides a method for preparing polybutadiene latex, comprising:

[0015] The raw materials are mixed and polymerized to obtain polybutadiene latex, wherein the raw materials are as follows by weight: 95-115 parts of butadiene, 0.02-6 parts of initiator, 0.02-10 parts of electrolyte, 0.1-12 parts of emulsifier, 0.01-6 parts of chain transfer agent, 0.02-8 parts of rubber particle size controller, 0-6 parts of gel content regulator, 40-400 parts of water, and the rubber particle size controller is polyoxyethylene carboxylate.

[0016] Preferably, the initiator includes one or more of sodium persulfate, potassium persulfate, ammonium persulfate, and azobisisobutylnitrile.

[0017] Preferably, the electrolyte includes one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, and potassium hydroxide.

[0018] Preferably, the emulsifier includes one or more of naphthalenesulfonic acid formaldehyde condensate sodium salt, naphthalenesulfonic acid formaldehyde condensate potassium salt, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzenesulfonate, and sodium dodecylsulfonate.

[0019] Preferably, the chain transfer agent includes one or more of tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan, and decanyl mercaptan.

[0020] Preferably, the raw materials are calculated by weight as follows: 98-110 parts by weight of butadiene, 0.12-5 parts by weight of initiator, 0.05-6 parts by weight of electrolyte, 1-8 parts by weight of emulsifier, 0.1-4 parts by weight of chain transfer agent, 0.05-5 parts by weight of rubber particle size controller, 0.2-5 parts by weight of gel content regulator and 50-300 parts by weight of water.

[0021] Preferably, the rubber particle size control agent has the structural formula RCOO (CH2CH2O) m H, wherein R is a long-chain alkyl group, the number of carbon atoms in the long-chain alkyl group is 4-19, and m is 4-11. More preferably, the number of carbon atoms in the long-chain alkyl group is 5-12, and m is 4-8.

[0022] Preferably, the gel content regulator is a dialkyl dithioxanthate, wherein the number of carbon atoms of the alkyl group is 1 to 13, and more preferably, the number of carbon atoms of the alkyl group is 1 to 10.

[0023] Preferably, the polymerization reaction is carried out by heating the mixture to 55-85° C. and reacting the mixture for 23-38 hours.

[0024] The present invention also provides an ABS high-rubber powder, which is a copolymer of the above-mentioned polybutadiene latex, styrene and acrylonitrile.

[0025] Preferably, the weight fraction of the polybutadiene latex is 50-70%, and the weight fraction of acrylonitrile is 4-20%. More preferably, the weight fraction of the polybutadiene latex is 52-66%, and the weight fraction of acrylonitrile is 6-15%.

[0026] The present invention also provides an ABS resin, wherein the ABS resin components comprise, by weight, 15-40 parts of the above-mentioned ABS high-rubber powder and 60-78 parts of styrene-acrylonitrile copolymer.

[0027] The present invention also provides a method for preparing ABS resin, comprising:

[0028] The components are mixed, extruded through a twin-screw extruder, cooled, and pelletized to obtain ABS resin.

[0029] The present invention also provides an application of ABS resin in automobile interior and exterior electroplating parts, such as front and rear door handles, front grilles, interior trim strips, navigation panel frames, etc.

[0030] The polybutadiene latex of the present invention has an average particle size of 290-315 nm, and the half-maximum width of the number-average particle size distribution curve is 20-150 nm. This extremely narrow particle size distribution makes the butadiene rubber in the latex exhibit near-monodisperse properties. This property differs significantly from the particle size distribution of butadiene rubber obtained by conventional polymerization methods: the closer the particle size is to the average, the more rubber particles there are; the further away from the average, the number of rubber particles tends to zero. The butadiene latex with this characteristic exhibits excellent stability during subsequent grafting and coagulation processes, particularly in terms of grafting efficiency. The uniform grafting efficiency ensures that each piece of butadiene rubber is well grafted and coated, thereby preventing agglomeration between rubbers and reducing the likelihood of pitting in the ABS resin during electroplating. Furthermore, the uniform dispersion of the rubber helps improve the bonding strength of the plating layer and prevents defects such as plating skipping. On the other hand, the residual butadiene monomer content in the polybutadiene latex accounts for 0.005%-1.6% of the dry basis of the entire polybutadiene latex. Since the residual butadiene monomer is very easy to react with the grafted monomers styrene and acrylonitrile, the appropriate residual butadiene monomer content can affect the proportion of butadiene units in the grafted chain segment in the grafted rubber, thereby improving the compatibility of the grafted rubber with the blended SAN resin, improving the dispersion of the rubber, and further reducing the possibility of appearance pitting on electroplated parts. Beneficial effects

[0031] The polybutadiene latex used in the present invention enables the ABS resin to have better electroplating surface appearance and plating adhesion.

[0032] The surface pitting grade of the ABS resin of the present invention is 3A-5A, and the coating adhesion is 0.62-1.28 kgf / cm. DETAILED DESCRIPTION

[0033] Below in conjunction with specific embodiment, further set forth the present invention.Should be understood that these embodiments are only used to illustrate the present invention and are not used in limiting the scope of the present invention.In addition, should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall equally within the scope limited by the appended claims of the application.

[0034] Reagent Source:

[0035] Butadiene: Industrial grade butadiene, purity greater than 96%, Huarui Chemical;

[0036] Initiator: potassium persulfate, commercially available;

[0037] Electrolyte: sodium bicarbonate, commercially available;

[0038] Emulsifier: sodium dodecylbenzenesulfonate, commercially available;

[0039] Chain transfer agent: n-dodecyl mercaptan, commercially available;

[0040] Rubber particle size control agent 1: polyoxyethylene hexanoate, C5H 11 COO(CH2CH2O)6H;USA CIHEEM, LMEO-6;

[0041] Rubber particle size control agent 2: polyoxyethylene laurate, C 11 H 23 COO(CH2CH2O)6H;USA CIHEEM, LMEO-12;

[0042] Rubber particle size control agent 3: polyoxyethylene stearate, C 17 H 35 COO(CH2CH2O)9H;USA CIHEEM, LMEO-18;

[0043] Gel content regulator 1: di-n-butyl xanthate disulfide, CP8, Zhengzhou Aikemu Chemical Co., Ltd.;

[0044] Gel content regulator 2: diisopropyl dithioxanthate, DIP, Shanghai Yuanye Biotechnology Co., Ltd.;

[0045] Gel content regulator 3: didodecyl dithioxanthate, DP, Chemical Research Institute of Hubei Xinkang Pharmaceutical Co., Ltd.;

[0046] Styrene: purchased from Aladdin Reagent Company, purity greater than or equal to 99%;

[0047] Acrylonitrile: purchased from Aladdin Reagent Company, purity greater than or equal to 99%;

[0048] [Corrected 11.09.2023 according to Rule 26] Styrene-acrylonitrile copolymer: PN-118, Chi Mei, Taiwan, China;

[0049] Unless otherwise specified, a component (such as an initiator, an electrolyte) in the parallel examples and comparative examples of the present invention is the same commercially available product.

[0050] A method for preparing polybutadiene latex, comprising:

[0051] The components were mixed according to the proportions in Table 1 and Table 2, and the temperature was raised to 55° C. to start the polymerization reaction. The temperature was continuously raised to 85° C. within 30 hours. The reaction was completed after 32 hours to obtain polybutadiene latex.

[0052] Polybutadiene latex performance test:

[0053] (1) Particle size and particle size distribution test: Malvern laser diffraction particle size analyzer, model Mastersizer 3000E, was used to analyze the average particle size and particle size distribution of polybutadiene latex, and the number average particle size distribution curve was drawn and the half-peak width was tested;

[0054] (2) Gel content (weight fraction) test: carried out in accordance with the test standard "Determination of gel content of synthetic raw rubber", standard number SH / T 1050-1991.

[0055] (3) Residual butadiene content: After drying, the latex was dissolved in a headspace vial with N,N-dimethylformamide. The components to be tested were heated to reach gas-liquid equilibrium, and then the headspace was quantitatively aspirated for gas chromatography. Qualitative analysis was performed based on retention time, and n-pentane was used as the internal standard for quantitative analysis. The peak at 2.25-2.50 min was the residual butadiene. A Shimadzu GC-MS-QP2010 gas chromatograph was used, with an RTX-WAX quartz capillary column, 30 m × 0.25 mm × 0.5 μm. Column temperature: 80°C for 12 min, then 10°C / min to 120°C for 10 min. Inlet temperature: 220°C; detector temperature: 250°C.

[0056] ABS high-rubber powder: a copolymer of polybutadiene latex, styrene and acrylonitrile, the preparation method of which is as follows: polybutadiene latex, styrene and acrylonitrile are mixed according to the ratio in Table 3, the polybutadiene latex is added to the reactor, and 0.015 parts of ferrous sulfate is added to the reactor and stirred evenly, the reactor is heated to 67°C, and 2.51 parts of cumene hydroperoxide, acrylonitrile, styrene, 1.5 parts of tert-dodecyl mercaptan, 5 parts of sodium dodecylsulfonate and 175 parts of deionized water are added, and the addition is continued dropwise for 2 hours. After heating is completed, the reaction is continued for 5 hours to obtain the grafted latex. 1000 parts of the grafted latex were added to a coagulant reactor, stirred and heated to 75°C, 450 parts of 5% sulfuric acid were gradually added thereto over a period of 2 hours, and the temperature was raised to 91°C and maintained at that temperature for 3 hours. The obtained coagulant latex was filtered through a 325-mesh filter and dried in a fluidized bed dryer at 60°C for 6 hours to obtain an ABS high-rubber powder with a moisture content of <1%. The ABS high-rubber powders prepared in Examples 11-20, Comparative Examples 4-6, and Examples 21-22 were respectively recorded as ABS high-rubber powder 1, ABS high-rubber powder 2, ABS high-rubber powder 3, ABS high-rubber powder 4, ABS high-rubber powder 5, ABS high-rubber powder 6, ABS high-rubber powder 7, ABS high-rubber powder 8, ABS high-rubber powder 9, ABS high-rubber powder 10, ABS high-rubber powder 11, ABS high-rubber powder 12, ABS high-rubber powder 13, ABS high-rubber powder 14, and ABS high-rubber powder 15.

[0057] Preparation method of ABS resin: According to Table 4-6, the components are mixed, extruded through a twin-screw extruder, cooled, and pelletized to obtain the ABS resin, wherein the extrusion temperature is 185-220°C, the screw speed is 300 r / min, and the screw aspect ratio is 25:1.

[0058] ABS resin performance test:

[0059] (1) ABS surface pitting test: ABS resin was injection molded into a standard square plate (100 mm * 100 mm * 2 mm). A Leica optical microscope, model DM6M LIBS, was used to count the pitting on the square plate. Three samples were tested for each sample and the average number of pitting was calculated. The pitting was graded into 5A (0), 4A (1 to 2), 3A (3 to 5), 2A (6 to 10), and 1A (more than 10).

[0060] (2) Coating adhesion: The coating adhesion was tested according to ASTM B533(85)-2013 Peel strength of alloy-plated plastics. Five specimens were tested for each sample, and the average adhesion was calculated.

[0061] (3) Standard deviation of grafting rate: After drying, weigh about 1.000g of ABS high-glue powder, record it as m0; weigh the weight of the reagent bottle, record it as m1; put the high-glue powder into the reagent bottle and add about 25ml of acetone; shake it for 2 hours to fully dissolve the high-glue powder; put it into a high-speed centrifuge and centrifuge it for 30 minutes, and the centrifuge speed is set to 15,000 rpm; immediately remove the acetone solution after centrifugation, and be careful not to bring out the powder at the bottom; add acetone to about 25ml and then shake it to fully mix the solution, and centrifuge it again; remove the acetone solution after centrifugation; then put the bottle containing the insoluble matter into an oven and dry it at 80℃ for 8 hours, and put it into a vacuum oven and continue drying it at 80℃ for 4 hours, cool it to room temperature, and weigh it m2. Grafting rate = (m2 - m1 - m0 * n) / (m0 * n), where: m0: mass of ABS high-strength rubber powder, g; m1: weight of the reagent bottle, g; m2: sum of the mass of the reagent bottle and the separated material after drying, g; n: rubber content in the ABS high-strength rubber powder, which is the feed ratio of butadiene latex on a dry basis (weight of polybutadiene latex / (weight of polybutadiene latex + weight of styrene + weight of acrylonitrile)) in Table 3. Grafting rate standard deviation calculation method: 10 samples of the same ABS high-strength rubber powder were tested for grafting rate. First, the average of the 10 tests was subtracted from each test value to obtain a set of 10 data points. Second, the squares of the 10 data points obtained in the previous step were summed. Third, the sum was divided by 10, and the square root was taken to obtain the standard deviation of the grafting rate. A smaller standard deviation of the grafting rate indicates a more stable grafting rate.

[0062] Table 1 Examples 1-10 Proportions (parts by weight)

[0063] Table 2 Comparative Examples 1-3 Proportions (parts by weight)

[0064] Table 3 Proportions of Examples 11-22 and Comparative Examples 4-6 (parts by weight)

[0065] Table 4 Proportions of Examples 23-34 (parts by weight)

[0066] Table 5 Example 35-36 ratio (parts by weight)

[0067] Table 6 Comparative Examples 7-9 Proportions (parts by weight)

[0068] As shown in Tables 4-6, the average particle size and half-peak width of the number-average particle size distribution curve of the polybutadiene latex used are within the scope of the present invention, so that the ABS resin has a better electroplating surface appearance and coating adhesion, thereby improving the electroplating yield.

Claims

1. A polybutadiene latex, characterized in that: The average particle size of the polybutadiene latex is 290-315 nm, and the half-peak width of the number average particle size distribution curve is 20-150 nm. The residual butadiene monomer content in the polybutadiene latex accounts for 0.005%-1.6% of the dry basis of the entire polybutadiene latex.

2. The polybutadiene latex according to claim 1, characterized in that The average particle size of the polybutadiene latex is 300-310nm, and the half-peak width of the number average particle size distribution curve is 30-100nm; the residual butadiene monomer content in the polybutadiene latex accounts for 0.01%-0.8% of the dry basis of the entire polybutadiene latex.

3. The polybutadiene latex according to claim 1, characterized in that The weight fraction of the polybutadiene latex gel is 50-95%.

4. A method for preparing a polybutadiene latex as claimed in any one of claims 1 to 3, comprising: The raw materials are mixed and polymerized to obtain polybutadiene latex, wherein the raw materials are calculated by weight as follows: 95-115 parts of butadiene, 0.02-6 parts of initiator, 0.02-10 parts of electrolyte, 0.1-12 parts of emulsifier, 0.01-6 parts of chain transfer agent, 0.02-8 parts of rubber particle size controller, 0-6 parts of gel content regulator, 40-400 parts of water, and the rubber particle size controller is polyoxyethylene carboxylate.

5. The preparation method according to claim 4, characterized in that: The initiator includes one or more of sodium persulfate, potassium persulfate, ammonium persulfate, and azobisisobutylnitrile; the electrolyte includes one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, and potassium hydroxide; and the emulsifier includes one or more of naphthalenesulfonic acid formaldehyde condensate sodium salt, naphthalenesulfonic acid formaldehyde condensate potassium salt, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzene sulfonate, and sodium dodecyl sulfonate.

6. The preparation method according to claim 4, characterized in that: The chain transfer agent includes one or more of tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan, and decanyl mercaptan; the rubber particle size control agent has a structural formula of RCOO (CH2CH2O) m H, wherein R is a long-chain alkyl group, the number of carbon atoms in the long-chain alkyl group is 4-19, and m is 4-11; the gel content regulator is a dialkyl dithioxanthate, wherein the number of carbon atoms in the alkyl group is 1-13.

7. The preparation method according to claim 4, characterized in that: The raw materials are calculated by weight as follows: 98-110 parts by weight of butadiene, 0.12-5 parts by weight of initiator, 0.05-6 parts by weight of electrolyte, 1-8 parts by weight of emulsifier, 0.1-4 parts by weight of chain transfer agent, 0.05-5 parts by weight of rubber particle size controller, 0.2-5 parts by weight of gel content regulator and 50-300 parts by weight of water.

8. The preparation method according to claim 4, characterized in that: The polymerization reaction is as follows: heating to 55-85° C. and reacting for 23-38 hours.

9. An ABS high-rubber powder, characterized in that: The ABS high-rubber powder is: a copolymer of polybutadiene latex, styrene and acrylonitrile as described in any one of claims 1 to 3.

10. The ABS high-rubber powder according to claim 9, characterized in that: The weight fraction of the polybutadiene latex is 50-70%, and the weight fraction of acrylonitrile is 4-20%.

11. An ABS resin, characterized in that: The ABS resin component comprises, by weight: 15-40 parts of the ABS high-rubber powder according to claim 9 and 60-78 parts of styrene-acrylonitrile copolymer.

12. A method for preparing the ABS resin according to claim 11, comprising: The components are mixed, extruded through a twin-screw extruder, cooled, and pelletized to obtain ABS resin.

13. Use of the ABS resin as claimed in claim 11 in electroplating parts for interior and exterior decoration of automobiles.