Film adhesive, dicing and die-bonding two-in-one film, semiconductor device, and manufacturing method for same

MYPI2025006587A0Undetermined Publication Date: 2025-04-20RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025006587
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-10-20
Publication Date
2025-04-20

AI Technical Summary

Technical Problem

Chip cracks occur during the pick-up process of semiconductor chips due to their brittleness when the semiconductor layer becomes thin, leading to vibrations, especially in stacked semiconductor devices with thick circuit layers and thin semiconductor layers.

Method used

A film-like adhesive comprising an epoxy resin, phenolic resin, and an elastomer, optionally with an inorganic filler, is formulated to have a specific storage modulus at 25°C, reducing the edge peel strength and enhancing peelability from the dicing film's adhesive layer.

Benefits of technology

The adhesive effectively reduces chip cracks by improving peelability, ensuring secure bonding and handling of semiconductor chips without damage during the pick-up process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025006587_DRAWING_001
    Figure PI2025006587_DRAWING_001
  • Figure PI2025006587_DRAWING_002
    Figure PI2025006587_DRAWING_002
  • Figure PI2025006587_DRAWING_003
    Figure PI2025006587_DRAWING_003
Patent Text Reader

Abstract

A film-shaped adhesive is disclosed that contains an epoxy resin, a phenolic resin, and an elastomer, and may further contain an inorganic filler. A content of the inorganic filler is from 0 to 5% by mass based on a total amount of the film-shaped adhesive. A storage modulus of the film-shaped adhesive at 25°C is 1200 MPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Film-like adhesive, dicing / die bonding integrated film, semiconductor device, and manufacturing method thereof

[0001] The present disclosure relates to a film adhesive, a dicing and die bonding integrated film, a semiconductor device, and a method for manufacturing the same.

[0002] In recent years, stacked MCPs (Multi Chip Packages), in which semiconductor chips are stacked in multiple stages, have become widespread and are installed as memory semiconductor packages for mobile phones, mobile audio devices, etc. Furthermore, as mobile phones and other devices become more multifunctional, semiconductor packages are being made faster, denser, and more highly integrated.

[0003] A known method for manufacturing a semiconductor device (semiconductor package) involves attaching a dicing / die-bonding integrated film having an adhesive layer and an adhesive layer, in which an adhesive layer is disposed on the adhesive layer of a dicing film, to the back surface of a semiconductor wafer, and then cutting and dividing the semiconductor wafer, adhesive layer, and part of the adhesive layer to produce multiple individual semiconductor chips with adhesive pieces. For example, Patent Documents 1 and 2 disclose film-like adhesives used as adhesive layers in such methods.

[0004] International Publication No. WO 2013 / 133275 International Publication No. WO 2020 / 013250

[0005] By using a semiconductor chip with an adhesive piece, the semiconductor chip and a support member are bonded via the adhesive piece. Meanwhile, in recent semiconductor devices (semiconductor packages), semiconductor chips composed of a circuit layer and a semiconductor layer tend to have thicker circuit layers and thinner semiconductor layers. In such semiconductor chips, chip cracks may occur, for example, when the semiconductor chip with the adhesive piece is picked up from the adhesive layer of the dicing film. It is believed that such chip cracks occur due to vibrations during pick-up caused by the thinning of the semiconductor layer, making the semiconductor chip brittle. Therefore, film-like adhesives used in dicing and die-bonding integrated films are required to be able to suppress the occurrence of chip cracks.

[0006] Therefore, a main object of the present disclosure is to provide a film-like adhesive that, when applied to the adhesive layer of a dicing / die bonding integrated film, has excellent peelability from the pressure-sensitive adhesive layer of the dicing film.

[0007] The present inventors conducted extensive research to solve the above-mentioned problems and discovered that, by adjusting the storage modulus at 25°C within a predetermined range in a film-like adhesive that contains an epoxy resin, a phenolic resin, and an elastomer, and may further contain an inorganic filler, it is possible to reduce the edge peel strength between the pressure-sensitive adhesive layer and the adhesive layer of a dicing film (the peak of peel strength that occurs at the edge of the adhesive layer when the pressure-sensitive adhesive layer of the dicing film is peeled from the adhesive layer), which led to the completion of the invention of the present disclosure.

[0008] The present disclosure provides the film-like adhesives described in [1] to [8], the dicing-die bonding integrated film described in [9], the semiconductor device described in

[10] and

[11] , and the methods for manufacturing a semiconductor device described in

[12] to

[17] . [1] A film-like adhesive containing an epoxy resin, a phenolic resin, and an elastomer, and optionally further containing an inorganic filler, wherein the content of the inorganic filler is 0 to 5 mass% based on the total amount of the film-like adhesive, and the film-like adhesive has a storage modulus of 1200 MPa or more at 25°C. [2] The film-like adhesive described in [1], wherein the content of the elastomer is 20 to 50 mass% based on the total amount of the film-like adhesive, and the combined content of the epoxy resin and the phenolic resin is 45 to 80 mass% based on the total amount of the film-like adhesive. [3] The film-like adhesive according to [1] or [2], wherein the epoxy resin comprises a first epoxy resin having a softening point of 40°C or lower, and the content of the first epoxy resin is 2 to 20 mass% based on the total amount of the film-like adhesive. [4] The film-like adhesive according to [3], wherein the epoxy resin further comprises a second epoxy resin having a softening point of higher than 40°C, and the softening point of the second epoxy resin is 120°C or lower. [5] The film-like adhesive according to any of [1] to [4], wherein the film-like adhesive is cured at 150°C for 30 minutes, and the cured product has a storage modulus at 150°C of 40 MPa or higher. [6] The film-like adhesive according to any of [1] to [5], wherein the thickness of the film-like adhesive is 1 to 15 μm. [7] The film-like adhesive according to any of [1] to [6], which is used in a manufacturing process for a semiconductor device comprising a plurality of stacked semiconductor chips. [8] The film-like adhesive according to [7], wherein the semiconductor device is a three-dimensional NAND memory. [9] A dicing and die bonding integrated film comprising, in this order, a base layer, a pressure-sensitive adhesive layer, and an adhesive layer made of the film-like adhesive according to any one of [1] to [6].

[10] A semiconductor device comprising: a semiconductor chip; a support member on which the semiconductor chip is mounted; and a cured product of the film-like adhesive according to any one of [1] to [6], which is provided between the semiconductor chip and the support member and bonds the semiconductor chip to the support member.

[11] The semiconductor device according to

[10] , further comprising a semiconductor chip different from the semiconductor chip stacked on a surface of the semiconductor chip.

[12] A method for manufacturing a semiconductor device, comprising the steps of: attaching the adhesive layer of the integrated dicing and die bonding film according to [9] to a semiconductor wafer; cutting the semiconductor wafer with the adhesive layer attached to produce a plurality of individual adhesive piece-attached semiconductor chips; and bonding, as the adhesive piece-attached semiconductor chips, first adhesive piece-attached semiconductor chips having a first semiconductor chip and a first adhesive piece to a support member via the first adhesive piece.

[13] The method for manufacturing a semiconductor device according to

[12] , further comprising the step of bonding, as the adhesive piece-attached semiconductor chip, a second adhesive piece-attached semiconductor chip having a second semiconductor chip and a second adhesive piece to a surface of the first semiconductor chip in the first adhesive piece-attached semiconductor chip adhered to the support member via the second adhesive piece.

[14] The method for manufacturing a semiconductor device according to

[12] , further comprising the steps of: preparing a laminate including the dicing and die bonding integrated film according to [9], and a plurality of semiconductor chips formed by dividing a semiconductor wafer and provided on the adhesive layer of the dicing and die bonding integrated film; irradiating the adhesive layer with a laser through gaps between the plurality of semiconductor chips to divide the adhesive layer, thereby producing adhesive piece-attached semiconductor chips; and bonding, as the adhesive piece-attached semiconductor chip, a first adhesive piece-attached semiconductor chip having a first semiconductor chip and a first adhesive piece to a support member via the first adhesive piece.

[15] The method for manufacturing a semiconductor device according to

[14] , wherein the laminate is a laminate manufactured by a method including the steps of: forming grooves along dicing lines on a circuit formation surface of the semiconductor wafer; grinding a back surface of the semiconductor wafer opposite to the circuit formation surface on which the grooves are formed to a depth at least reaching the grooves to manufacture the plurality of semiconductor chips; and attaching the adhesive layer of the dicing and die bonding integrated film to the back surfaces of the plurality of semiconductor chips.

[16] The method for manufacturing a semiconductor device according to

[14] or

[15] , further comprising the step of: bonding, as the adhesive piece-attached semiconductor chip, a second adhesive piece-attached semiconductor chip having a second semiconductor chip and a second adhesive piece, to the front surface of the first semiconductor chip in the first adhesive piece-attached semiconductor chip adhered to the support member, via the second adhesive piece.

[17] A method for manufacturing a semiconductor device, comprising a step of interposing a film adhesive described in any one of [1] to [6] between a first semiconductor chip and a support member, or between a first semiconductor chip and a second semiconductor chip different from the first semiconductor chip, and bonding the first semiconductor chip and the support member, or the first semiconductor chip and the second semiconductor chip.

[0009] According to the present disclosure, a film-like adhesive is provided that, when applied to the adhesive layer of a dicing / die bonding integrated film, exhibits excellent peelability from the pressure-sensitive adhesive layer of the dicing film. Also, according to the present disclosure, a dicing / die bonding integrated film using such a film-like adhesive, a semiconductor device, and a method for manufacturing the same are provided. Furthermore, according to the present disclosure, a method for manufacturing a semiconductor device using such a dicing / die bonding integrated film is provided.

[0010] Fig. 1 is a schematic cross-sectional view showing one embodiment of a film-like adhesive. Fig. 2 is a schematic cross-sectional view showing one embodiment of a dicing / die bonding integrated film. Fig. 3 is a schematic cross-sectional view showing one embodiment of a semiconductor device. Fig. 4 is a schematic cross-sectional view showing another embodiment of a semiconductor device. Fig. 5 is a schematic cross-sectional view showing another embodiment of a semiconductor device.

[0011] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings as appropriate. However, the present disclosure is not limited to the following embodiments. In the following embodiments, components (including steps, etc.) are not essential unless specifically stated. The sizes of the components in each figure are conceptual, and the relative size relationships between the components are not limited to those shown in each figure.

[0012] The same applies to numerical values ​​and ranges in the present disclosure and do not limit the present disclosure. In this specification, numerical ranges indicated using "to" indicate ranges that include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this specification, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in numerical ranges described in this specification, the upper or lower limit value of that numerical range may be replaced with a value shown in the examples. In addition, the upper and lower limits described individually can be arbitrarily combined. In addition, "A or B" may include either A or B, or may include both. In addition, unless otherwise specified, the materials exemplified below may be used alone or in combination of two or more. When multiple substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified.

[0013] In this specification, (meth)acrylate means acrylate or its corresponding methacrylate, and the same applies to other similar expressions such as (meth)acryloyl group, (meth)acrylic copolymer, etc.

[0014] [Film-like adhesive] Fig. 1 is a schematic cross-sectional view showing one embodiment of a film-like adhesive. The film-like adhesive 1 (adhesive film) shown in Fig. 1 may be thermosetting, and may be capable of passing through a semi-cured (B-stage) state and then becoming fully cured (C-stage) after a curing treatment.

[0015] B-stage refers to an intermediate stage in the reaction of certain thermosetting resins where the material swells when in contact with certain liquids and softens when heated, but does not completely dissolve or melt; C-stage refers to the final stage in the reaction of certain thermosetting resins where the material becomes virtually insoluble and infusible.

[0016] According to the studies of the inventors of the present disclosure, it has been found that when the storage modulus of the film-like adhesive 1 in a semi-cured (B-stage) state at 25°C is 1200 MPa or more, the edge peel strength between the pressure-sensitive adhesive layer of the dicing film and the adhesive layer can be reduced, and the peelability of the dicing film from the pressure-sensitive adhesive layer can be improved. The storage modulus at 25°C may be 1250 MPa or more, 1300 MPa or more, 1350 MPa or more, 1400 MPa or more, 1450 MPa or more, or 1500 MPa or more. The upper limit of the storage modulus at 25°C may be, for example, 5000 MPa or less or 3000 MPa or less.

[0017] In this specification, the storage modulus of a film-like adhesive at 25°C can be measured, for example, by the following method. A sample for measurement is prepared by laminating multiple 10 μm thick film-like adhesives to a thickness of approximately 160 μm, and cutting this into a size of 4 mm wide x 33 mm long. The prepared sample is placed in a dynamic viscoelasticity measuring device, and viscoelasticity is measured in a temperature dependency measurement mode under conditions of a tensile load, a frequency of 10 Hz, a heating rate of 3°C / min, and a temperature range of -30 to 300°C. Here, the value of the storage modulus at 25°C is taken as the storage modulus at 25°C.

[0018] Next, we will explain one embodiment of each component that makes up the film-like adhesive 1. By using these components, it tends to be easier to adjust the storage modulus at 25°C of the film-like adhesive to fall within a predetermined range.

[0019] The film-like adhesive 1 contains an epoxy resin (hereinafter sometimes referred to as "component (A)"), a phenolic resin (hereinafter sometimes referred to as "component (B)"), and an elastomer (hereinafter sometimes referred to as "component (C)"), and may further contain an inorganic filler (hereinafter sometimes referred to as "component (D)"). In addition to components (A), (B), (C), and (D), the film-like adhesive 1 may further contain a coupling agent (hereinafter sometimes referred to as "component (E)"), a curing accelerator (hereinafter sometimes referred to as "component (F)"), other components, and the like.

[0020] Component (A): Epoxy Resin Component (A) can be any epoxy resin having an epoxy group in the molecule. Examples of component (A) include bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, bisphenol A novolac epoxy resins, bisphenol F novolac epoxy resins, stilbene epoxy resins, triazine skeleton-containing epoxy resins, fluorene skeleton-containing epoxy resins, triphenolmethane epoxy resins, biphenyl epoxy resins, xylylene epoxy resins, biphenyl aralkyl epoxy resins, naphthalene epoxy resins, and diglycidyl ether compounds of polyfunctional phenols and polycyclic aromatics such as anthracene. Among these, component (A) may contain cresol novolac epoxy resins, bisphenol F epoxy resins, or bisphenol A epoxy resins from the viewpoint of film tackiness, flexibility, and the like.

[0021] The epoxy equivalent of component (A) is not particularly limited, but may be 90 to 300 g / eq, 100 to 290 g / eq, or 110 to 280 g / eq. When the epoxy equivalent of component (A) is within this range, it tends to be easier to ensure the fluidity of the adhesive composition when forming the film adhesive while maintaining the bulk strength of the film adhesive.

[0022] The component (A) may contain a first epoxy resin having a softening point of 40°C or lower (or an epoxy resin that is liquid at 30°C, hereinafter sometimes referred to as "component (Aa)"). The component (A) may be a combination of component (Aa) and a second epoxy resin having a softening point of more than 40°C (or an epoxy resin that is solid at 30°C, hereinafter sometimes referred to as "component (Ab)"). The softening point of component (Ab) may be, for example, 120°C or lower, 110°C or lower, or 100°C or lower. When component (A) contains component (Aa), the break resistance of the film-like adhesive tends to be more easily improved, and the storage modulus after curing tends to be more easily improved. Furthermore, when component (A) is a combination of component (Aa) and component (Ab), thinning tends to be even easier to achieve.

[0023] In this specification, the softening point refers to a value measured by the ring and ball method in accordance with JIS K7234:1986.

[0024] Examples of commercially available products of component (Aa) include EXA-830CRP (trade name, manufactured by DIC Corporation, liquid at 30°C), YDF-8170C (trade name, manufactured by Nippon Steel Chemical & Material Co., Ltd., liquid at 30°C), and EP-4088S (trade name, manufactured by ADEKA Corporation, liquid at 30°C).

[0025] When the component (A) is a combination of the component (Aa) and the component (Ab), the content of the component (Aa) may be 1 mass % or more, 3 mass % or more, 5 mass % or more, 7 mass % or more, or 10 mass % or more, and may be 50 mass % or less, 45 mass % or less, 40 mass % or less, 35 mass % or less, or 30 mass % or less, based on the total amount of the component (A), from the viewpoint of peelability from the pressure-sensitive adhesive layer. Note that the content of the component (Aa) in the component (A) in the adhesive composition when forming the film-like adhesive may be the same as the above range.

[0026] From the viewpoint of peelability from the pressure-sensitive adhesive layer, the content of component (Aa) may be 2 to 20 mass% based on the total amount of the film-like adhesive. The content of component (Aa) may be 3 mass% or more, 4 mass% or more, or 5 mass% or more based on the total amount of the film-like adhesive, and may be 17 mass% or less, 15 mass% or less, or 12 mass% or less. The content of component (Aa) in the adhesive composition when forming the film-like adhesive may be the same as the above range.

[0027] In one embodiment, the component (Ab) may include a cresol novolac epoxy resin. In one embodiment, the component (Ab) may include a naphthalene epoxy resin. In one embodiment, the component (Ab) may include a cresol novolac epoxy resin and a naphthalene epoxy resin. Examples of naphthalene epoxy resins include epoxy resins represented by the following formula (X):

[0028]

[0029] Commercially available naphthalene-type epoxy resins for component (Ab) include, for example, HP-4700 (trade name, manufactured by DIC Corporation, softening point: 85 to 95°C), HP-4770 (trade name, manufactured by DIC Corporation, softening point: 67 to 77°C), and HP-4710 (trade name, manufactured by DIC Corporation, softening point: 85 to 105°C).

[0030] When component (A) is a combination of component (Aa) and component (Ab), the content of component (Ab) may be 50 mass% or more, 55 mass% or more, 60 mass% or more, 65 mass% or more, or 70 mass% or more, and may be 99 mass% or less, 97 mass% or less, 95 mass% or less, 93 mass% or less, or 90 mass% or less, based on the total amount of component (A). Note that the content of component (Ab) in component (A) in the adhesive composition when forming a film-like adhesive may be the same as the above range.

[0031] From the viewpoint of peelability from the pressure-sensitive adhesive layer, the content of component (A) may be 15 to 55 mass% based on the total amount of the film-like adhesive. The content of component (A) may be 20 mass% or more, 25 mass% or more, or 30 mass% or more, based on the total amount of the film-like adhesive, and may be 50 mass% or less, 45 mass% or less, or 40 mass% or less. The content of component (A) in the adhesive composition when forming the film-like adhesive may be the same as the above range.

[0032] Component (B): Phenolic Resin Component (B) acts as a curing agent for component (A), i.e., it can be a curing agent for epoxy resin. By including component (B) in the film-like adhesive, the film-like adhesive becomes highly crosslinked, and the storage modulus after curing can be improved.

[0033] Component (B) can be any compound having a phenolic hydroxyl group in the molecule. Component (B) can be a polycondensation product of a phenol (e.g., phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, aminophenol, etc.) and / or a naphthol (e.g., α-naphthol, β-naphthol, dihydroxynaphthalene, etc.) with an aldehyde (e.g., formaldehyde). Polycondensation is typically carried out in the presence of a catalyst such as an acid or a base. Phenolic resins obtained using an acid catalyst are particularly called novolak-type phenolic resins. Examples of novolak-type phenolic resins include phenol / formaldehyde novolak resins, cresol / formaldehyde novolak resins, xylenol / formaldehyde novolak resins, resorcinol / formaldehyde novolak resins, and phenol-naphthol / formaldehyde novolak resins. Further, examples of the phenol resin include phenol aralkyl resins, naphthol aralkyl resins, biphenyl aralkyl type phenol resins, and phenyl aralkyl type phenol resins, which are synthesized from phenols and / or naphthols such as allylated bisphenol A, allylated bisphenol F, allylated naphthalenediol, phenol novolak, and phenol, and dimethoxyparaxylene or bis(methoxymethyl)biphenyl.

[0034] The hydroxyl equivalent of component (B) is not particularly limited, but may be, for example, 80 to 250 g / eq, 90 to 200 g / eq, or 100 to 180 g / eq. When the hydroxyl equivalent of component (B) is 80 g / eq or more, the storage modulus tends to be further improved, and when it is 250 g / eq or less, problems due to foaming, outgassing, etc. can be prevented.

[0035] The softening point of component (B) is not particularly limited, but may be, for example, 50 to 140°C, 55 to 115°C, or 60 to 100°C.

[0036] From the viewpoint of curability, the ratio of the epoxy equivalent of component (A) to the hydroxyl equivalent of component (B) (epoxy equivalent of component (A) / hydroxyl equivalent of component (B)) may be 0.30 / 0.70 to 0.70 / 0.30, 0.35 / 0.65 to 0.65 / 0.35, 0.40 / 0.60 to 0.60 / 0.40, or 0.45 / 0.55 to 0.55 / 0.45. When the equivalent ratio is 0.30 / 0.70 or more, more sufficient curability tends to be obtained. When the equivalent ratio is 0.70 / 0.30 or less, excessive viscosity increase can be prevented, and more sufficient fluidity can be obtained.

[0037] The total content of components (A) and (B) may be 45 to 80% by mass, based on the total amount of the film-like adhesive. When the total content of components (A) and (B), based on the total amount of the film-like adhesive, is 40% by mass or more, the storage modulus after curing tends to be more easily improved, and when it is 80% by mass or less, the handleability tends to be better. The total content of components (A) and (B), based on the total amount of the film-like adhesive, may be 50% by mass or more, 55% by mass or more, or 60% by mass or more, and may be 75% by mass or less, 72% by mass or less, or 70% by mass or less. The total content of components (A) and (B) in the adhesive composition when forming the film-like adhesive may be the same as the above range.

[0038] Component (C): Elastomer Examples of component (C) include acrylic resins, polyester resins, polyamide resins, polyimide resins, silicone resins, butadiene resins, and modified versions of these resins. Among these, component (C) may be an acrylic resin (acrylic rubber) primarily composed of structural units derived from (meth)acrylic esters, because it contains fewer ionic impurities, has better heat resistance, facilitates ensuring the connection reliability of semiconductor devices, and has better fluidity. The content of structural units derived from (meth)acrylic esters in component (C) may be, for example, 70% by mass or more, 80% by mass or more, or 90% by mass or more, based on the total amount of structural units. The acrylic resin (acrylic rubber) may contain structural units derived from (meth)acrylic esters having crosslinkable functional groups such as epoxy groups, alcoholic or phenolic hydroxyl groups, and carboxyl groups.

[0039] The glass transition temperature (Tg) of component (C) may be -30 to 30°C. When the Tg of component (C) is -30°C or higher, it is possible to further improve the adhesive strength of the film-like adhesive, and it also tends to be possible to prevent the flexibility of the film-like adhesive from becoming too high. When the Tg of component (C) is 30°C or lower, it is possible to suppress a decrease in the flexibility of the film-like adhesive, and it tends to have excellent breaking strength when formed into a thin film and excellent processability. The glass transition temperature (Tg) of component (C) may be -20°C or higher or -10°C or higher, and may be 25°C or lower or 20°C or lower. Here, Tg refers to a value measured using a DSC (differential scanning calorimeter) (for example, Thermo Plus 2, manufactured by Rigaku Corporation). The Tg of the component (C) can be adjusted to fall within a desired range by adjusting the type and content of the structural units that make up the component (C) (in the case where the component (C) is an acrylic resin (acrylic rubber), the structural units derived from a (meth)acrylic acid ester).

[0040] The weight average molecular weight (Mw) of component (C) may be 100,000 or more, 300,000 or more, or 500,000 or more, and may be 3,000,000 or less, 2,000,000 or less, or 1,000,000 or less. When the Mw of component (C) is within this range, film formability, film strength, flexibility, tackiness, etc. can be appropriately controlled, and excellent reflowability and embeddability can be achieved. Here, Mw refers to a value measured by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene. When multiple peaks are observed in GPC, the weight average molecular weight corresponding to the peak with the highest peak intensity is defined as the weight average molecular weight in this specification.

[0041] Examples of commercially available products of component (C) include SG-70L, SG-708-6, WS-023 EK30, SG-P3, SG-280 EK23, SG-80H, HTR-860P, HTR-860P-3, HTR-860P-3CSP, HTR-860P-3CSP-3DB, and HTR-860P-30B (all manufactured by Nagase ChemteX Corporation), and KH-CT-865 (manufactured by Resonac Corporation).

[0042] The content of component (C) is 20 to 50 mass% based on the total amount of the film-like adhesive. When the content of component (C) is 20 mass% or more based on the total amount of the film-like adhesive, the film-like adhesive tends to have excellent thin-film formability and excellent breakage resistance when formed. When the content of component (C) is 50 mass% or less based on the total amount of the film-like adhesive, the fluidity is improved, thereby improving embeddability and the storage modulus after curing tends to be more easily improved. The content of component (C) may be 22 mass% or more, 25 mass% or more, or 28 mass% or more based on the total amount of the film-like adhesive, and may be 45 mass% or less, 40 mass% or less, or 38 mass% or less. The content of component (C) in the adhesive composition when forming the film-like adhesive may be the same as the above range.

[0043] Component (D): Inorganic Filler The film adhesive 1 may further contain component (D). That is, the film adhesive 1 may include an embodiment that contains component (D) and an embodiment that contains substantially no component (D).

[0044] Examples of component (D) include aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whisker, boron nitride, and silica. Among these, component (D) may be silica from the viewpoint of adjusting the melt viscosity. The shape of component (D) is not particularly limited, but may be spherical.

[0045] From the viewpoint of fluidity and storage modulus, the average particle size of component (D) may be 700 nm or less, 600 nm or less, 500 nm or less, 400 nm or less, 300 nm or less, 200 nm or less, 150 nm or less, or 100 nm or less. The average particle size of component (D) may be, for example, 1 nm or more. Here, the average particle size refers to the particle size at a cumulative frequency of 50% in the particle size distribution determined by laser diffraction / scattering. The average particle size of component (D) can also be determined by using a film-like adhesive containing component (D). In this case, the film-like adhesive is heated to decompose the resin component, and the resulting residue is dispersed in a solvent to prepare a dispersion. The average particle size of component (D) can be determined from the particle size distribution obtained by applying laser diffraction / scattering to this dispersion.

[0046] The content of the (D) component may be 0 to 5% by mass, based on the total amount of the film-like adhesive. When the content of the (D) component is in this range, thinner films tend to be more readily formed. In one embodiment, the content of the (D) component may be 3% by mass or less, 2% by mass or less, or 1% by mass or less, based on the total amount of the film-like adhesive. In one embodiment, the content of the (D) component may be 0% by mass or more, more than 0% by mass, 1% by mass or more, 2% by mass or more, or 3% by mass or more, based on the total amount of the film-like adhesive. In one embodiment, the content of the (D) component may be 0% by mass, based on the total amount of the film-like adhesive. The content of the (D) component in the adhesive composition when forming the film-like adhesive may be the same as the above range.

[0047] Component (E): Coupling Agent Component (E) may be a silane coupling agent. Examples of the silane coupling agent include γ-ureidopropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane.

[0048] Component (F): Curing Accelerator Examples of the component (F) include imidazoles and derivatives thereof, organic phosphorus compounds, secondary amines, tertiary amines, quaternary ammonium salts, etc. Among these, from the viewpoint of reactivity, the component (F) may be imidazoles and derivatives thereof.

[0049] Examples of imidazoles include 2-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-methylimidazole.

[0050] Other Components The film adhesive may further contain other components, such as pigments, ion scavengers, and antioxidants.

[0051] The total content of component (E), component (F), and other components may be 0.1 mass% or more, 0.3 mass% or more, or 0.5 mass% or more, and may be 30 mass% or less, 20 mass% or less, 10 mass% or less, or 5 mass% or less, based on the total mass of the film-like adhesive. The total content of component (E), component (F), and other components in the adhesive composition when forming the film-like adhesive may be in the same range as above.

[0052] The thickness of the film adhesive 1 may be 1 to 15 μm. The thickness of the film adhesive 1 may also be 12 μm or less, 10 μm or less, 8 μm or less, or 7 μm or less. The thickness of the film adhesive 1 can be determined, for example, by measuring the thickness at five points on a scanning microscope photograph of the cross section of the film adhesive 1 and calculating the average of the measured values.

[0053] When the film-like adhesive 1 is cured at 150°C for 30 minutes, the storage modulus of the cured product at 150°C may be 10 MPa or more, 20 MPa or more, 30 MPa or more, 40 MPa or more, 50 MPa or more, 60 MPa or more, 70 MPa or more, 80 MPa or more, 90 MPa or more, or 100 MPa or more. If the storage modulus is 10 MPa or more, the brittleness of the semiconductor chip due to thinning can be compensated for, and as a result, the occurrence of chip cracks can be suppressed. The upper limit of the storage modulus is not particularly limited, but may be, for example, 500 MPa or less, 300 MPa or less, or 250 MPa or less.

[0054] In this specification, the storage modulus at 150°C of the cured product obtained by curing a film-like adhesive at 150°C for 30 minutes can be measured, for example, by the following method. A measurement sample is prepared by laminating multiple 10 μm-thick film-like adhesives to a thickness of approximately 160 μm, and then cutting this into a sheet measuring 4 mm wide x 33 mm long. The prepared sample is cured at 150°C for 30 minutes, and then the cured sample is placed in a dynamic viscoelasticity measuring device. Viscoelasticity is measured under a tensile load in a temperature dependence measurement mode under conditions of a frequency of 10 Hz, a heating rate of 3°C / min, and a temperature range of -30 to 300°C. Here, the storage modulus at 150°C is defined as the storage modulus at 150°C.

[0055] The minimum melt viscosity of the film-like adhesive 1 in the range of 60 to 160°C may be, for example, 3000 Pa·s or less. If the minimum melt viscosity is 3000 Pa·s or less, the fluidity of the film-like adhesive tends to improve, and embeddability tends to improve. The minimum melt viscosity may be, for example, 2500 Pa·s or less or 2000 Pa·s or less. The lower limit of the minimum melt viscosity may be, for example, 500 Pa·s or more or 700 Pa·s or more.

[0056] From the viewpoint of achieving superior embeddability, the shear viscosity (melt viscosity) of the film-like adhesive 1 at 100°C may be, for example, 3500 Pa·s or less. The shear viscosity (melt viscosity) at 100°C may be, for example, 3000 Pa·s or less or 2500 Pa·s or less. The lower limit of the shear viscosity (melt viscosity) at 100°C may be, for example, 500 Pa·s or more or 1000 Pa·s or more.

[0057] In this specification, the minimum melt viscosity in the range of 60 to 160°C or the shear viscosity (melt viscosity) at 100°C can be measured as follows. First, a film-like adhesive is laminated using a laminator to a thickness of 1000 μm (1 mm) or more to obtain a laminate. A measurement sample having a circular surface with a diameter of 9 mm is punched out from the obtained laminate. Measurements are then performed on the obtained measurement sample using a viscoelasticity measuring device under the following conditions: a measurement temperature of 60 to 160°C, a heating rate of 5°C / min, a strain of 5%, a measurement frequency of 4 Hz, and an initial load of 10 g, and the minimum melt viscosity, which is the lowest value within the measurement temperature range, and the melt viscosity at 100°C are calculated.

[0058] The film-like adhesive 1 (adhesive film) shown in FIG. 1 is obtained by forming an adhesive composition containing components (A), (B), (C), (D), (E), (F), and other components into a film. Such a film-like adhesive 1 can be formed by applying the adhesive composition to a support film. A varnish (adhesive varnish) containing the adhesive composition and a solvent may be used to form the film-like adhesive 1. When using an adhesive varnish, the components are mixed or kneaded in a solvent to prepare the adhesive varnish, and the resulting adhesive varnish is applied to a support film, and the solvent is removed by heating and drying, thereby obtaining the film-like adhesive 1.

[0059] The support film is not particularly limited as long as it can withstand the above-mentioned heat drying, and may be, for example, a polyester film, a polypropylene film, a polyethylene terephthalate film, a polyimide film, a polyetherimide film, a polyethylene naphthalate film, a polymethylpentene film, etc. The support film may be a multilayer film made by combining two or more types of film, and may have a surface treated with a silicone-based, silica-based, or other mold release agent. The thickness of the support film may be, for example, 10 to 200 μm or 20 to 170 μm.

[0060] The mixing or kneading can be carried out using a dispersing machine such as a conventional stirrer, a mortar and pestle, a three-roll mill, or a ball mill, and by appropriately combining these.

[0061] The solvent used in preparing the adhesive varnish is not limited as long as it can uniformly dissolve, knead, or disperse each component, and conventionally known solvents can be used. Examples of such solvents include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, as well as dimethylformamide, dimethylacetamide, N-methylpyrrolidone, toluene, and xylene. From the viewpoints of drying speed and cost, the solvent may be methyl ethyl ketone or cyclohexanone.

[0062] The adhesive varnish can be applied to the support film by any known method, such as knife coating, roll coating, spray coating, gravure coating, bar coating, curtain coating, etc. The heat drying conditions are not particularly limited as long as the solvent used is sufficiently evaporated, but may be 50 to 150°C for 1 to 30 minutes.

[0063] Since the film adhesive 1 can be thinned, it can be suitably used in the manufacturing process of a semiconductor device in which multiple semiconductor chips are stacked. In this case, the semiconductor device may be a stacked MCP or a three-dimensional NAND memory.

[0064] [Dicing and die bonding integrated film] Figure 2 is a schematic cross-sectional view showing one embodiment of a dicing and die bonding integrated film. The dicing and die bonding integrated film 10 shown in Figure 2 comprises, in this order, a base layer 2, a pressure-sensitive adhesive layer 3, and an adhesive layer 1A made of the above-mentioned film-like adhesive 1. A laminate composed of the base layer 2 and the pressure-sensitive adhesive layer 3 can be a dicing film 4. Use of such a dicing and die bonding integrated film 10 reduces the lamination process to a single step on a semiconductor wafer, thereby improving work efficiency. The dicing and die bonding integrated film may be in the form of a film, sheet, tape, or the like.

[0065] The dicing film 4 includes a base layer 2 and a pressure-sensitive adhesive layer 3 provided on the base layer 2 .

[0066] Examples of the substrate layer 2 include plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, polyimide film, and polyethylene vinyl acetate. These substrate layers 2 may also be multilayer films combining two or more types. These substrate layers 2 may be subjected to surface treatment such as primer coating, UV treatment, corona discharge treatment, polishing treatment, and etching treatment, as necessary.

[0067] The adhesive layer 3 is a layer made of an adhesive. There are no particular limitations on the adhesive, so long as it has sufficient adhesive strength to prevent the semiconductor chips from scattering during the dicing process and low adhesive strength to prevent damage to the semiconductor chips during the subsequent semiconductor chip pick-up process, and any adhesive conventionally known in the field of dicing films can be used. The adhesive may be either a radiation-curable or non-radiation-curable adhesive. A non-radiation-curable adhesive is an adhesive that exhibits a certain level of adhesiveness when pressure is applied for a short period of time. On the other hand, a radiation-curable adhesive is an adhesive that has the property of decreasing its adhesiveness upon irradiation with radiation (e.g., ultraviolet light).

[0068] The thickness of the dicing film 4 (base layer 2 and adhesive layer 3) may be 60 to 150 μm or 70 to 130 μm from the viewpoints of economy and film handling.

[0069] The dicing and die bonding integrated film 10 can be obtained, for example, by preparing a film adhesive 1 and a dicing film 4, and bonding the film adhesive 1 to the pressure-sensitive adhesive layer 3 of the dicing film 4. The dicing and die bonding integrated film 10 can also be obtained, for example, by preparing a dicing film 4, and applying an adhesive composition (adhesive varnish) onto the pressure-sensitive adhesive layer 3 of the dicing film 4, in the same manner as in the method of forming the film adhesive 1 described above.

[0070] When bonding the film-like adhesive 1 and the pressure-sensitive adhesive layer 3 of the dicing film 4 together, the dicing / die bonding integrated film 10 can be formed by laminating the film-like adhesive 1 onto the dicing film 4 under predetermined conditions (for example, room temperature (20°C) or in a heated state) using a roll laminator, vacuum laminator, or the like. The dicing / die bonding integrated film 10 can be produced continuously and efficiently, so it may be formed in a heated state using a roll laminator.

[0071] The film-like adhesive and dicing / die bonding integrated film may be used in a manufacturing process for a semiconductor device, or may be used in a manufacturing process for a semiconductor device comprising stacked semiconductor chips. The film-like adhesive and dicing / die bonding integrated film may be used in a manufacturing process for a semiconductor device including a step of laminating an adhesive layer of the film-like adhesive or dicing / die bonding integrated film to a semiconductor wafer or an already-diced semiconductor chip, and cutting it with a rotary blade, a laser, or stretching to obtain a semiconductor chip with an adhesive piece attached, and a step of bonding the semiconductor chip with the adhesive piece attached to a support member or another semiconductor chip via the adhesive piece.

[0072] The film adhesive is also suitable for use as an adhesive for bonding semiconductor chips together in a stacked MCP (for example, a three-dimensional NAND memory), which is a semiconductor device formed by stacking multiple semiconductor chips.

[0073] The film adhesive can also be used, for example, as a protective sheet for protecting the back surface of a semiconductor chip in a flip-chip type semiconductor device, or as a sealing sheet for sealing the gap between the surface of the semiconductor chip in a flip-chip type semiconductor device and an adherend.

[0074] A semiconductor device manufactured using the film adhesive and the dicing / die bonding integrated film will be specifically described below with reference to the drawings. Note that, in recent years, semiconductor devices with various structures have been proposed, and the use of the film adhesive and dicing / die bonding integrated film of this embodiment is not limited to semiconductor devices with the structures described below.

[0075] [Semiconductor Device] Fig. 3 is a schematic cross-sectional view showing one embodiment of a semiconductor device. The semiconductor device 100 shown in Fig. 3 includes a semiconductor chip 11 (first semiconductor chip), a support member 12 on which the semiconductor chip 11 is mounted, and an adhesive member 15. The adhesive member 15 is provided between the semiconductor chip 11 and the support member 12 and bonds the semiconductor chip 11 to the support member 12. The adhesive member 15 is a cured product of an adhesive composition (a cured product of a film-like adhesive). Connection terminals (not shown) of the semiconductor chip 11 are electrically connected to external connection terminals (not shown) via bonding wires 13 and are sealed with a sealing material 14.

[0076] FIG. 4 is a schematic cross-sectional view showing another embodiment of a semiconductor device. In the semiconductor device 110 shown in FIG. 4, a first-tier semiconductor chip 11a (first semiconductor chip) is adhered to a support member 12 on which terminals 16 are formed by an adhesive member 15a (a cured product of an adhesive composition (a cured product of a film-like adhesive)). A second-tier semiconductor chip 11b (second semiconductor chip) is further adhered to the first-tier semiconductor chip 11a by an adhesive member 15b (a cured product of an adhesive composition (a cured product of a film-like adhesive)). Connection terminals (not shown) of the first-tier semiconductor chip 11a and the second-tier semiconductor chip 11b are electrically connected to external connection terminals via bonding wires 13 and are sealed with a sealing material 14. The semiconductor device 110 shown in FIG. 4 can also be said to be the semiconductor device 100 shown in FIG. 3, further including another semiconductor chip (11b) stacked on the surface of the semiconductor chip (11a).

[0077] FIG. 5 is a schematic cross-sectional view showing another embodiment of a semiconductor device. The semiconductor device 120 shown in FIG. 5 includes a support member 12 and semiconductor chips 11a (first semiconductor chip), 11b (second semiconductor chip), 11c (third semiconductor chip), and 11d (fourth semiconductor chip) stacked on the support member 12. The four semiconductor chips 11a, 11b, 11c, and 11d are stacked at positions shifted from one another in the horizontal direction (a direction perpendicular to the stacking direction) for connection to connection terminals (not shown) formed on the surface of the support member 12 (see FIG. 5). The semiconductor chip 11a is adhered to the support member 12 by an adhesive member 15a (a cured product of an adhesive composition (a cured product of a film-like adhesive)), and adhesive members 15b, 15c, and 15d (cured products of an adhesive composition (a cured product of a film-like adhesive)) are also interposed between the three semiconductor chips 11b, 11c, and 11d, respectively. The semiconductor device 120 shown in Figure 5 can also be said to be the semiconductor device 100 shown in Figure 3, further comprising other semiconductor chips (11b, 11c, 11d) stacked on the surface of the semiconductor chip (11a).

[0078] Although the semiconductor device (semiconductor package) according to the embodiment of the present disclosure has been described in detail above, the present disclosure is not limited to the above embodiment. For example, while Fig. 5 illustrates a semiconductor device in which four semiconductor chips are stacked, the number of stacked semiconductor chips is not limited to this. Furthermore, Fig. 5 illustrates a semiconductor device in which the semiconductor chips are stacked in positions offset from each other in the horizontal direction (a direction perpendicular to the stacking direction), the semiconductor device may also be one in which the semiconductor chips are stacked in positions not offset from each other in the horizontal direction (a direction perpendicular to the stacking direction).

[0079] 3, 4, and 5 can be obtained by a method including a step of interposing the above-mentioned film-like adhesive between a semiconductor chip (first semiconductor chip) and a support member, or between the semiconductor chip (first semiconductor chip) and the semiconductor chip (second semiconductor chip), and bonding the semiconductor chip (first semiconductor chip) and the support member, or between the semiconductor chip (first semiconductor chip) and the semiconductor chip (second semiconductor chip). More specifically, the semiconductor device can be obtained by interposing the above-mentioned film-like adhesive between the semiconductor chip and the support member, or between the semiconductor chip (first semiconductor chip) and the semiconductor chip (second semiconductor chip), bonding them together by heat and pressure, and then, as necessary, undergoing a thermosetting step, a wire bonding step, a sealing step using a sealing material, a heat-melting step including solder reflow, and the like.

[0080] A method for interposing a film-like adhesive between a semiconductor chip (first semiconductor chip) and a support member, or between a semiconductor chip (first semiconductor chip) and a semiconductor chip (second semiconductor chip), may be a method in which a semiconductor chip with an adhesive piece is prepared in advance and then attached to a support member or another semiconductor chip, as described below.

[0081] Next, an embodiment of a method for manufacturing a semiconductor device using the dicing and die bonding integrated film shown in Fig. 2 will be described. Note that the method for manufacturing a semiconductor device using the dicing and die bonding integrated film is not limited to the method for manufacturing a semiconductor device described below.

[0082] One embodiment of a method for manufacturing a semiconductor device includes, for example, a step of attaching a semiconductor wafer to the adhesive layer of the above-mentioned dicing / die bonding integrated film (laminating step), a step of cutting the semiconductor wafer with the adhesive layer attached to produce a plurality of individual adhesive piece-attached semiconductor chips (dicing step), and a step of adhering a first adhesive piece-attached semiconductor chip having a first semiconductor chip and a first adhesive piece to a support member via the first adhesive piece (step of adhering adhesive piece-attached semiconductor chip to a support member via an adhesive piece) (first adhering step). Another embodiment of the method for manufacturing a semiconductor device includes, for example, a step of preparing a laminate comprising the above-mentioned dicing / die bonding integrated film and a plurality of semiconductor chips formed by singulating a semiconductor wafer and disposed on the adhesive layer of the dicing / die bonding integrated film (laminate preparation step); a step of irradiating a laser onto the adhesive layer through the gaps between the plurality of semiconductor chips to singulate the adhesive layer, thereby producing semiconductor chips with adhesive pieces (adhesive layer singulation step); and a step of adhering a first semiconductor chip with adhesive pieces, which has a first semiconductor chip and a first adhesive piece, to a support member via the first adhesive piece (step of adhering the semiconductor chip with adhesive piece to a support member via the adhesive piece) (first adhering step).

[0083] The method for manufacturing a semiconductor device may further include a step of adhering a second semiconductor chip with adhesive piece, which has a second semiconductor chip and a second adhesive piece, to the surface of the first semiconductor chip in the first semiconductor chip with adhesive piece adhered to a support member via the second adhesive piece (a step of adhering another semiconductor chip with adhesive piece to the surface of the semiconductor chip adhered to a support member via an adhesive piece possessed by the other semiconductor chip with adhesive piece) (second adhering step).

[0084] The laminating step is a step of pressing a semiconductor wafer onto the adhesive layer 1A of the dicing and die bonding integrated film 10, adhesively holding and attaching the semiconductor wafer. This step may be performed while pressing with a pressing means such as a pressing roll.

[0085] Examples of semiconductor wafers include single crystal silicon, polycrystalline silicon, various ceramics, and compound semiconductors such as gallium arsenide.

[0086] The dicing process is a process of dicing a semiconductor wafer. This allows the semiconductor wafer to be cut to a predetermined size, producing multiple individual semiconductor chips with adhesive. Dicing can be performed, for example, from the circuit side of the semiconductor wafer according to a conventional method. This process can also employ a method known as a full cut, in which a cut is made all the way to the dicing film; a method in which a half cut is made in the semiconductor wafer and the wafer is separated by cooling and pulling; or a method in which the wafer is separated by a laser. The dicing device used in this process is not particularly limited, and conventionally known devices can be used.

[0087] A semiconductor chip is composed of, for example, a circuit layer and a semiconductor layer (for example, single crystal silicon, polycrystalline silicon, various ceramics, compound semiconductors such as gallium arsenide, etc.). Examples of semiconductor chips include integrated circuits (ICs). Examples of support members include lead frames such as 42 alloy lead frames and copper lead frames; plastic films such as polyimide resin and epoxy resin; modified plastic films obtained by impregnating and curing a substrate such as glass nonwoven fabric with a plastic such as polyimide resin or epoxy resin; and ceramics such as alumina.

[0088] The laminate preparation step is a step of preparing a laminate including a dicing / die bonding integrated film and a plurality of semiconductor chips formed by dividing a semiconductor wafer and disposed on the adhesive layer of the dicing / die bonding integrated film. In this step, the manufacturing method is not particularly limited as long as a laminate having a predetermined configuration is obtained. For example, the laminate may be a laminate manufactured by a method including the steps of: forming grooves along dicing lines on the circuit-forming surface of the semiconductor wafer (step (a)); grinding the back surface of the semiconductor wafer opposite the circuit-forming surface on which the grooves are formed to a depth that reaches at least the grooves to manufacture a plurality of semiconductor chips (step (b)); and attaching an adhesive layer of the dicing / die bonding integrated film to the back surfaces of the plurality of semiconductor chips (step (c)).

[0089] In step (a), grooves are formed along dicing lines on the circuit-forming surface of a semiconductor wafer. Examples of the semiconductor wafer include those described above. A semiconductor wafer typically has a circuit-forming surface and a back surface opposite the circuit-forming surface.

[0090] The thickness of the semiconductor wafer is greater than the thickness of the semiconductor chip, and may be, for example, 50 to 3000 μm, 100 to 2000 μm, or 200 to 1500 μm.

[0091] The grooves are formed by half-cut dicing using a dicing blade along the dicing lines of the semiconductor wafer. Half-cut dicing means cutting the semiconductor wafer to a predetermined depth without completely cutting it. Half-cut dicing using a dicing blade can be performed using a commercially available dicing saw. The grooves are formed on the circuit formation surface of the semiconductor wafer, for example, so as to form a grid pattern in a plan view.

[0092] In step (b), the back surface of the semiconductor wafer on which the grooves are formed, opposite to the circuit-forming surface, is ground to a depth that reaches at least the grooves, thereby producing a plurality of semiconductor chips.

[0093] In step (b), a backgrinding tape is first applied to the circuit-forming surface of the semiconductor wafer on which the grooves have been formed. The backgrinding tape may be any backgrinding tape commonly used in the field, and may be, for example, a backgrinding tape having an adhesive layer containing an ultraviolet-curable adhesive.

[0094] Next, the back surface of the semiconductor wafer with the grooves formed therein is ground. Grinding the back surface of the semiconductor wafer with the grooves formed therein can be performed using a general grinder. By grinding the back surface in this manner, it is possible to produce multiple semiconductor chips with a thickness thinner than that of the semiconductor wafer. A semiconductor chip typically has a circuit-forming surface and a back surface opposite the circuit-forming surface. The thickness of the semiconductor chip is smaller than that of the semiconductor wafer. The thickness of the semiconductor chip may be, for example, 10 to 200 μm, or may be 20 to 100 μm. The thicknesses of the semiconductor chips may all be the same or may be different from each other.

[0095] In step (c), the adhesive layer of the integrated dicing and die bonding film is attached to the backside of the semiconductor chips obtained above, thereby obtaining a laminate A having, in this order, a base layer, a pressure-sensitive adhesive layer, an adhesive layer, the semiconductor chips, and a backgrind tape.

[0096] The laminate can then be obtained by peeling the backgrind tape from the laminate A. When the backgrind tape has an adhesive layer containing an ultraviolet-curable adhesive, the adhesive layer of the backgrind tape can be irradiated with ultraviolet light to harden the adhesive layer and reduce its adhesive strength, thereby enabling the backgrind tape to be efficiently peeled from the laminate A.

[0097] The adhesive layer singulation process involves irradiating the adhesive layer with a laser through the gaps between multiple semiconductor chips to singulate the adhesive layer, thereby producing a semiconductor chip with adhesive pieces that has a semiconductor chip and an adhesive piece.

[0098] The semiconductor chips obtained by dividing a semiconductor wafer usually have gaps between them, and by irradiating the adhesive layer with a laser through the gaps, adhesive layer pieces having the same shape as the semiconductor chips in a plan view can be obtained.

[0099] The laser irradiation is carried out, for example, from the semiconductor chip side through the gaps between the multiple semiconductor chips. The laser irradiation can be carried out using a commercially available laser saw. The laser frequency may be, for example, 30 to 250 kHz, 50 to 200 kHz, or 80 to 120 kHz. The laser output may be, for example, 0.05 to 2.0 W, 0.1 to 1.0 W, or 0.2 to 0.5 W. The feed speed during laser irradiation may be, for example, 20 to 500 mm / s, 50 to 400 mm / s, or 100 to 300 mm / s.

[0100] The method for manufacturing a semiconductor device may include a pick-up step, if necessary. The pick-up step is a step of picking up semiconductor chips with adhesive pieces attached thereto in order to peel off the semiconductor chips with adhesive pieces attached thereto that have been adhesively fixed to a dicing / die bonding integrated film or a dicing film. The pick-up method is not particularly limited, and various conventionally known methods can be used. Examples of such methods include a method in which individual semiconductor chips with adhesive pieces are pushed up from the dicing / die bonding integrated film or dicing film side by a needle, and the pushed-up semiconductor chips with adhesive pieces attached thereto are picked up by a pick-up device.

[0101] Here, if the adhesive layer is a radiation-curable (e.g., ultraviolet) adhesive layer, the pickup can be performed after irradiating the adhesive layer with radiation. This reduces the adhesive strength of the adhesive layer to the adhesive piece, making it easier to peel off the semiconductor chip with the adhesive piece. As a result, the semiconductor chip with the adhesive piece can be picked up without damaging it.

[0102] The first bonding step is a step of bonding a semiconductor chip with a first adhesive piece formed by dicing to a support member for mounting the semiconductor chip via the first adhesive piece. The semiconductor device manufacturing method may optionally include a step (second bonding step) of bonding a semiconductor chip with a second adhesive piece to the surface of the semiconductor chip bonded to the support member via the second adhesive piece. Both bonding steps can be performed by pressure bonding. The pressure bonding conditions are not particularly limited and can be set appropriately as needed. The pressure bonding conditions may be, for example, a temperature of 80 to 160°C, a load of 5 to 15 N, and a time of 1 to 10 seconds. The support member may be the same as the support member described above.

[0103] The method for manufacturing a semiconductor device may, if necessary, include a step of further thermally curing the adhesive pieces (the first adhesive pieces in the semiconductor chip with the first adhesive pieces, and the second adhesive pieces in the semiconductor chip with the second adhesive pieces) or the film-like adhesive (thermal curing step). Further thermally curing the adhesive pieces (the first adhesive pieces in the semiconductor chip with the first adhesive pieces, and the second adhesive pieces in the semiconductor chip with the second adhesive pieces) bonding the semiconductor chip (first semiconductor chip) and the support member, and the semiconductor chip (first semiconductor chip) and the semiconductor chip (second semiconductor chip), enables more firmly bonded and fixed. When thermal curing is performed, pressure may be applied simultaneously to harden the adhesive pieces. The heating temperature in this step can be appropriately changed depending on the constituent components of the adhesive pieces. The heating temperature may be, for example, 60 to 200°C or 100 to 180°C. The temperature or pressure may be changed stepwise. The heating time may be, for example, 1 to 120 minutes or 15 to 60 minutes.

[0104] The method for manufacturing a semiconductor device may optionally include a step of electrically connecting the first semiconductor chip and the second semiconductor chip to a support member with bonding wires, more specifically, a step of electrically connecting electrode pads on the semiconductor chip to the tips of terminal portions (inner leads) of the support member with bonding wires (wire bonding step). Examples of bonding wires that can be used include gold wires, aluminum wires, copper wires, etc. The temperature during wire bonding may be within a range of 80 to 250°C or 80 to 220°C. The heating time may be several seconds to several minutes. Wire bonding may be performed by combining ultrasonic vibration energy and compression energy due to applied pressure while the substrate is heated within the above temperature range.

[0105] The method for manufacturing a semiconductor device may optionally include a step of encapsulating the semiconductor chip with an encapsulant (encapsulation step). This step is performed to protect the semiconductor chip or bonding wires mounted on the support member. This step can be performed by molding the encapsulating resin (encapsulation resin) in a mold. The encapsulation resin may be, for example, an epoxy-based resin. The heat and pressure during encapsulation bury the support member and residue, preventing peeling due to air bubbles at the adhesive interface.

[0106] The method for manufacturing a semiconductor device may, if necessary, include a step (post-curing step) of completely curing the encapsulating resin that is insufficiently cured in the encapsulating step. Even if the adhesive piece is not thermally cured in the encapsulating step, in this step, the adhesive piece can be thermally cured along with the curing of the encapsulating resin, thereby enabling adhesive fixation. The heating temperature in this step can be appropriately set depending on the type of encapsulating resin, and may be, for example, in the range of 165 to 185°C, and the heating time may be approximately 0.5 to 8 hours.

[0107] The method for manufacturing a semiconductor device may optionally include a step of heating the semiconductor chip with adhesive attached to the support member using a reflow furnace (heat melting step). In this step, the resin-encapsulated semiconductor device may be surface-mounted on the support member. Examples of surface mounting methods include reflow soldering, in which solder is first supplied onto a printed wiring board, then heated and melted using hot air or the like to perform soldering. Examples of heating methods include hot air reflow and infrared reflow. The heating method may involve heating the entire device or localized heating. The heating temperature may be, for example, within the range of 240 to 280°C.

[0108] The present disclosure will be specifically described below based on examples, but the present disclosure is not limited to these examples.

[0109] [Preparation of Film-Like Adhesive] (Examples 1 to 7 and Comparative Example 1) <Preparation of Adhesive Varnish> Cyclohexanone was added to a mixture of components (A), (B), (D), and (E) in the amounts (parts by mass) shown in Table 1. The mixture was stirred and mixed. Component (C) was added to the mixture in the amounts (parts by mass) shown in Table 1, and the mixture was stirred. Component (F) was then added and stirred until the components were uniform, thereby preparing the adhesive varnishes of Examples 1 to 6 and Comparative Examples 1 and 2. The components shown in Table 1 have the following meanings, and the numerical values ​​shown in Table 1 indicate the parts by mass of the components excluding solvents, etc.

[0110] Component (A): Epoxy resin Component (A): Epoxy resin Component (Aa): First epoxy resin (Aa-1) EXA-830CRP (trade name, manufactured by DIC Corporation, bisphenol F type epoxy resin, epoxy equivalent: 160 g / eq, liquid at 30°C) Component (Ab): Second epoxy resin (Ab-1) HP-4710 (trade name, manufactured by DIC Corporation, epoxy resin represented by the above formula (X), epoxy equivalent: 170 g / eq, softening point: 85 to 105°C) (Ab-2) N-500P-10 (trade name, manufactured by DIC Corporation, o-cresol novolac type epoxy resin, epoxy equivalent: 204 g / eq, softening point: 75 to 85°C)

[0111] Component (B): Phenolic resin (B-1) MEH-7800M (trade name, manufactured by Meiwa Chemical Industry Co., Ltd., phenol novolac type phenolic resin, hydroxyl group equivalent: 175 g / eq, softening point: 61 to 90°C)

[0112] Component (C): Elastomer (C-1) HTR-860P-3CSP (trade name, manufactured by Nagase ChemteX Corporation, acrylic rubber, glass transition temperature: -7°C, weight average molecular weight: 800,000)

[0113] Component (D): Inorganic filler (D-1) R972 (trade name, manufactured by Nippon Aerosil Co., Ltd., silica, average particle size 0.016 μm (16 nm))

[0114] Component (E): Coupling agent (E-1) A-189 (trade name, manufactured by Nippon Unicar Co., Ltd., γ-mercaptopropyltrimethoxysilane)

[0115] Component (F): Curing accelerator (F-1) 2PZ-CN (trade name, manufactured by Shikoku Chemicals Corporation, 1-cyanoethyl-2-phenylimidazole)

[0116] <Preparation of Film-Like Adhesive> The adhesive varnishes of Examples 1 to 7 and Comparative Example 1 were filtered through a 500-mesh filter and vacuum degassed. A 38 μm-thick polyethylene terephthalate (PET) film that had been subjected to a release treatment was prepared as a support film, and the vacuum degassed adhesive varnish was applied to the PET film. The applied adhesive varnish was dried by heating at 90°C for 5 minutes and then at 130°C for 5 minutes, yielding film-like adhesives of Examples 1 to 7 and Comparative Example 1 that were in a B-stage state and had a thickness of 10 μm. The thickness of the film-like adhesive was adjusted by the amount of adhesive varnish applied.

[0117] [Evaluation of Film-Like Adhesives] <Measurement of Storage Modulus at 25°C> The storage modulus at 25°C was measured using the film-like adhesives of Examples 1 to 7 and Comparative Example 1. The storage modulus at 25°C was measured using the following method. Specifically, a measurement sample was prepared by laminating multiple 10 μm-thick film-like adhesives to a thickness of approximately 160 μm, and cutting this into a size of 4 mm wide x 33 mm long. The prepared sample was placed in a dynamic viscoelasticity measuring device (Rheogel E-4000, manufactured by UBM Corporation), and viscoelasticity was measured under a tensile load in a temperature dependency measurement mode under conditions of a frequency of 10 Hz, a heating rate of 3°C / min, and a temperature range of -30 to 300°C, and the storage modulus at 25°C was determined. The results are shown in Table 1.

[0118] <Measurement of Shear Viscosity (Melt Viscosity)> Multiple sheets of each of the film adhesives of Examples 1 to 7 and Comparative Example 1 were laminated at 70°C to form laminates with a thickness of 1000 μm (1 mm) or more. Measurement samples with circular surfaces measuring 9 mm in diameter were punched out from the laminates, and the measurement samples were attached to circular aluminum plate jigs with a diameter of 8 mm. The shear viscosity of the measurement samples was measured using an ARES (manufactured by TA Instruments Japan Co., Ltd.) under the following conditions. From the measurement results, the minimum shear viscosity (minimum melt viscosity) within the range of 60 to 160°C and the shear viscosity at 100°C were calculated. The smaller the minimum melt viscosity and shear viscosity at 100°C (e.g., 3000 Pa·s or less (minimum melt viscosity) and 3500 Pa·s or less (shear viscosity at 100°C)), the higher the fluidity and the better the embeddability. The results are shown in Table 1. (Measurement conditions) Measurement temperature: 60 to 160°C Heating rate: 5°C / min Distortion: 5% Frequency: 4Hz Initial load: 10g

[0119] <Measurement of High-Temperature Storage Modulus After Curing> The film-like adhesives of Examples 1 to 7 and Comparative Example 1 were used to measure the high-temperature storage modulus after curing. The high-temperature storage modulus after curing was measured using the following method. Specifically, a measurement sample was prepared by laminating multiple 10 μm-thick film-like adhesives to a thickness of approximately 160 μm, and then cutting this into a size of 4 mm wide x 33 mm long. The prepared sample was cured at 150°C for 30 minutes, and then the cured sample was placed in a dynamic viscoelasticity measuring device (Rheogel E-4000, manufactured by UBM Co., Ltd.). Viscoelasticity was measured under a tensile load in a temperature-dependent measurement mode under conditions of a frequency of 10 Hz, a heating rate of 3°C / min, and a temperature range of -30 to 300°C. The storage modulus value at 150°C was taken as the high-temperature storage modulus. A higher high-temperature storage modulus value (e.g., 10 MPa or higher) indicates greater suppression of chip cracking. The results are shown in Table 1.

[0120] <Measurement of Edge Peel Strength> Edge peel strength was measured using the film-like adhesives of Examples 1 to 7 and Comparative Example 1. The edge peel strength was measured by the following method. First, a dicing film was prepared, which included a base layer (polypropylene / ethylene vinyl acetate / polypropylene (PP / EVA / PP) film, thickness: 100 μm) and a pressure-sensitive adhesive layer (thickness: 10 μm) made of an ultraviolet-curable pressure-sensitive adhesive provided on the base layer. Next, the film-like adhesive and the pressure-sensitive adhesive layer of the dicing film were bonded together to produce the integrated dicing and die-bonding films of Examples 1 to 7 and Comparative Example 1, which included the base layer, pressure-sensitive adhesive layer, and adhesive layer in this order.

[0121] A semiconductor wafer with a thickness of 775 μm was prepared, and a fully automatic dicer (DFD6361, manufactured by Disco Corporation) was used to half-cut the circuit-forming surface (front surface) of the semiconductor wafer to form a groove with a depth of 60 μm. A dicing blade manufactured by Disco Corporation, ZH05-SD4000-N1-70-DD, was used, and the rotation speed and cutting speed were set to 40,000 rpm and 30 mm / s, respectively. The size of the semiconductor chip was 4 mm × 12 mm.

[0122] Next, a backgrinding tape laminator (RAD-3520F / 12, manufactured by Lintec Corporation) was used to attach a backgrinding tape to the circuit formation surface (front surface) of the semiconductor wafer, and then a grinder (DGP8761, manufactured by Disco Corporation) was used to grind the semiconductor wafer from the back surface side so that the thickness of the semiconductor chips finally obtained would be 25 μm, and the semiconductor wafer was diced into a plurality of semiconductor chips.

[0123] Next, in order to reduce the adhesive strength between the backgrinding tape and the semiconductor chip, ultraviolet light was irradiated onto the backgrinding tape using a wafer mounter (DFM2800, manufactured by Disco Corporation). Then, using the same wafer mounter (DFM2800, manufactured by Disco Corporation), each dicing / die bonding integrated film was attached to the back surface of the individualized semiconductor wafer (the back surface of the semiconductor chip) under conditions of a temperature of 70 ° C, a tension level of 5, and an attachment speed of 10 mm / sec. At this time, a ring frame was attached to the outer peripheral region of the dicing tape. Then, by peeling off the backgrinding tape, a laminate (1) was obtained, which included a dicing / die bonding integrated film and a plurality of semiconductor chips formed by individualizing the semiconductor wafer and provided on the adhesive layer of the dicing / die bonding integrated film.

[0124] Next, in the laminate (1), a laser was irradiated through the gaps between the semiconductor chips using a laser saw (DFL7160, manufactured by Disco Corporation) to cut the adhesive layer. The laser irradiation conditions were a frequency of 100 kHz, an output of 0.3 W, and a feed rate of 200 mm / s. In this way, the adhesive layer was singulated to produce a plurality of semiconductor chips with adhesive pieces, each having a semiconductor chip and an adhesive piece.

[0125] Next, a die separator (DDS2300, manufactured by Disco Corporation) was used to apply an illuminance of 80 mW / cm to the adhesive layer from the base layer side to the adhesive layer in order to reduce the adhesive strength between the adhesive layer and the adhesive piece. 2 and an irradiation dose of 130 mJ / cm 2By irradiating the substrate with ultraviolet light of 1000 W at ...

[0126] From the resulting laminate (2) having a plurality of semiconductor chips with adhesive pieces attached, excess semiconductor chips were removed using adhesive tape or the like so that the semiconductor chips with adhesive pieces were arranged in alternate rows. Double-sided tape was attached to the surfaces of the remaining semiconductor chips, and a support substrate was attached thereto. The dicing film was then cut from the back side along the size of the support substrate, and the laminate with the support substrate was separated from the dicing ring. The dicing film in areas where alternate rows of semiconductor chips were not present was cut into strips and removed to prepare a sample for measuring edge peel strength, which had the support substrate, double-sided tape, semiconductor chips, adhesive pieces, a cured adhesive layer, and a base layer in this order.

[0127] The edge peel strength of the prepared samples was measured using a benchtop peel tester (EZ-Test, manufactured by Shimadzu Corporation). The strip-shaped dicing film was clamped between a jig so that the peel angle between the cured adhesive layer and the adhesive piece was 90°, and then set into the tester. The feed rate was 60 mm / min, and the support substrate was manually fed during peeling so that the peel angle between the cured adhesive layer and the adhesive piece was always 90°. The peel force corresponding to the edge of the resulting semiconductor chip was converted to a 20 mm width to calculate the edge peel strength. For a 4 mm x 12 mm semiconductor chip with adhesive piece, the peel strength in the direction perpendicular to the 4 mm side was designated Ch1, and the peel strength in the direction parallel to the 4 mm side (perpendicular to the 12 mm side) was designated Ch2. The average of these values ​​was calculated from the peaks of N = 5 for each. Three samples each for Ch1 and Ch2 were measured, the average values ​​for Ch1 and Ch2 were calculated, and the sum of the average values ​​for Ch1 and Ch2 was calculated and divided by 2 to obtain the value of the edge peel strength for each sample. The results are shown in Table 1.

[0128]

[0129] As shown in Table 1, the film adhesives of Examples 1 to 7, whose storage modulus at 25° C. satisfied the specified requirement, had sufficiently reduced edge peel strength compared to the film adhesive of Comparative Example 1, whose storage modulus at 25° C. did not satisfy the specified requirement. These results confirmed that the film adhesive of the present disclosure, when applied to the adhesive layer of a dicing and die bonding integrated film, exhibits excellent peelability from the pressure-sensitive adhesive layer of the dicing film.

[0130] 1...film-like adhesive, 1A...adhesive layer, 2...base material layer, 3...pressure-sensitive adhesive layer, 4...dicing film, 10...dicing / die bonding integrated film, 11, 11a, 11b, 11c, 11d...semiconductor chip, 12...support member, 13...bonding wire, 14...sealing material, 15, 15a, 15b, 15c, 15d...adhesive member, 16...terminal, 100, 110, 120...semiconductor device.

Claims

1. A film-like adhesive comprising an epoxy resin, a phenolic resin, and an elastomer, and optionally further comprising an inorganic filler, wherein the content of the inorganic filler is 0 to 5 mass % based on the total amount of the film-like adhesive, and the film-like adhesive has a storage modulus of 1,200 MPa or more at 25°C.

2. The film-like adhesive according to claim 1, wherein the content of the elastomer is 20 to 50 mass% based on the total amount of the film-like adhesive, and the combined content of the epoxy resin and the phenolic resin is 45 to 80 mass% based on the total amount of the film-like adhesive.

3. A film-like adhesive as described in claim 1 or 2, wherein the epoxy resin comprises a first epoxy resin having a softening point of 40°C or lower, and the content of the first epoxy resin is 2 to 20 mass% based on the total amount of the film-like adhesive.

4. The film-like adhesive according to claim 3, wherein the epoxy resin further comprises a second epoxy resin having a softening point of more than 40°C, and the softening point of the second epoxy resin is 120°C or lower.

5. The film-like adhesive according to claim 1 or 2, wherein when the film-like adhesive is cured at 150°C for 30 minutes, the cured product has a storage modulus at 150°C of 10 MPa or more.

6. The film-like adhesive according to claim 1 or 2, wherein the film-like adhesive has a thickness of 1 to 15 μm.

7. The film-like adhesive according to claim 1 or 2, which is used in the manufacturing process of a semiconductor device comprising a plurality of stacked semiconductor chips.

8. The film adhesive according to claim 7, wherein the semiconductor device is a three-dimensional NAND type memory.

9. A dicing and die bonding integrated film comprising, in this order, a base layer, a pressure-sensitive adhesive layer, and an adhesive layer made of the film-like adhesive according to claim 1 or 2.

10. A semiconductor device comprising: a semiconductor chip; a support member on which the semiconductor chip is mounted; and a cured film-like adhesive according to claim 1 or 2, which is provided between the semiconductor chip and the support member and bonds the semiconductor chip to the support member.

11. The semiconductor device according to claim 10, further comprising a semiconductor chip different from the semiconductor chip, stacked on a surface of the semiconductor chip.

12. A method for manufacturing a semiconductor device, comprising the steps of: attaching the adhesive layer of the dicing and die bonding integrated film described in claim 9 to a semiconductor wafer; producing a plurality of individual adhesive piece-attached semiconductor chips by cutting the semiconductor wafer to which the adhesive layer has been attached; and adhering a first adhesive piece-attached semiconductor chip having a first semiconductor chip and a first adhesive piece, as the adhesive piece-attached semiconductor chip, to a support member via the first adhesive piece.

13. The method for manufacturing a semiconductor device according to claim 12, further comprising a step of adhering, as the semiconductor chip with adhesive piece, a second semiconductor chip with a second adhesive piece having a second semiconductor chip and a second adhesive piece, to a surface of the first semiconductor chip in the first semiconductor chip with adhesive piece adhered to the support member via the second adhesive piece.

14. A method for manufacturing a semiconductor device, comprising: a step of preparing a laminate comprising the dicing / die bonding integrated film according to claim 9 and a plurality of semiconductor chips formed by singulating a semiconductor wafer and disposed on the adhesive layer of the dicing / die bonding integrated film; a step of irradiating the adhesive layer with a laser through gaps between the plurality of semiconductor chips to singulate the adhesive layer, thereby producing a semiconductor chip with an adhesive piece; and a step of adhering a first semiconductor chip with an adhesive piece, the first semiconductor chip having a first adhesive piece and a first adhesive piece, to a support member via the first adhesive piece, as the semiconductor chip with an adhesive piece.

15. The method for manufacturing a semiconductor device according to claim 14, wherein the laminate is a laminate produced by a method including the steps of: forming grooves along dicing lines on the circuit formation surface of the semiconductor wafer; grinding the back surface of the semiconductor wafer opposite the circuit formation surface on which the grooves are formed to a depth that reaches at least the grooves to produce the multiple semiconductor chips; and attaching the adhesive layer of the dicing and die bonding integrated film to the back surfaces of the multiple semiconductor chips.

16. The method for manufacturing a semiconductor device according to claim 14, further comprising a step of adhering, as the semiconductor chip with adhesive piece, a second semiconductor chip with a second adhesive piece having a second semiconductor chip and a second adhesive piece, to a surface of the first semiconductor chip in the first semiconductor chip with adhesive piece adhered to the support member via the second adhesive piece.

17. A method for manufacturing a semiconductor device, comprising the step of interposing a film-like adhesive according to claim 1 or 2 between a first semiconductor chip and a support member, or between a first semiconductor chip and a second semiconductor chip different from the first semiconductor chip, and bonding the first semiconductor chip and the support member, or the first semiconductor chip and the second semiconductor chip.