Film-like adhesive agent, adhesive film, dicing / die-bonding integrated film, and method for producing semiconductor device

MYPI2025006687A0Undetermined Publication Date: 2025-02-09RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025006687
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-09
Filing Date
2024-08-08
Publication Date
2025-02-09

Smart Images

  • Figure PI2025006687_DRAWING_001
    Figure PI2025006687_DRAWING_001
  • Figure PI2025006687_DRAWING_002
    Figure PI2025006687_DRAWING_002
  • Figure PI2025006687_DRAWING_003
    Figure PI2025006687_DRAWING_003
Patent Text Reader

Abstract

A film-like adhesive agent is composed of a resin composition having a thermosetting property and containing a rubber component, the film-like adhesive agent having a first surface and a second surface, wherein the film-like adhesive agent has a region in a vicinity of the first surface, in which a content of the rubber component increases from a side of the second surface toward a side of the first surface, and a graph obtained by indentation measurement using an atomic force microscope has: a portion G1 in which an elastic modulus gradually increases starting from a measurement result at the first surface; and a portion G2 in which the elastic modulus is substantially constant from an end point of the portion G1.
Need to check novelty before this filing date? Find Prior Art

Description

Film-like adhesive, adhesive film, dicing / die bonding integrated film, and method for manufacturing semiconductor device

[0001] The present disclosure relates to a film-like adhesive, an adhesive film, a dicing and die bonding integrated film, and a method for manufacturing a semiconductor device.

[0002] In recent years, as smartphones, tablet PCs, etc. have become more functional and faster, the semiconductor packages used therein are being required to be even smaller, have higher capacity, are faster, are thinner, etc. In wafers used in such semiconductor packages, the wiring is becoming finer and finer, and the chips tend to become thinner during assembly of the semiconductor package.

[0003] In the midst of this trend, particularly in the fields of DRAMs and NAND flash memories, problems of operational malfunctions caused by trace amounts of heavy metal ions such as copper ions have begun to become apparent. It has been known that when heavy metal ions come into contact with silicon crystals, they can diffuse within the crystal and reach the circuit surface, causing operational malfunctions. To prevent operational malfunctions, in the assembly of semiconductor packages, it is common to perform a gettering process on the silicon wafer to capture heavy metal ions so that the heavy metal ions attached to the silicon wafer do not diffuse to the circuit surface.

[0004] Gettering processes mainly include a method of providing a gettering layer inside the wafer (intrinsic gettering, hereinafter referred to as "IG") and a method of providing a gettering layer on the backside of the wafer (extrinsic gettering, hereinafter referred to as "EG"). However, with IG, the thickness of the gettering layer that can be formed inside the wafer is reduced due to the thinning of the chip, and its effectiveness is no longer sufficient. Furthermore, with EG, microcracks are formed on the backside of the wafer, reducing the die strength of the chip. Therefore, excessive gettering is difficult to perform, especially on ultra-thin wafers that are difficult to handle. In light of this situation, it has been investigated to impart a gettering function for capturing heavy metal ions to resin films (adhesive films used in the manufacturing process of semiconductor devices), more specifically, film-like adhesives (die-bonding films) used to bond between chips and substrates or between chips themselves (see, for example, Patent Documents 1 and 2).

[0005] JP 2011-213878 A JP 2012-241157 A

[0006] However, conventional film-like adhesives are insufficient in terms of suppressing defects associated with the migration of copper ions within the adhesive, and there is still room for improvement. Furthermore, further improvement in the adhesion strength of film-like adhesives is desired. The present disclosure provides a film-like adhesive that has a barrier function that prevents the migration of heavy metal ions, such as copper ions, and excellent adhesion, and an adhesive film that includes the same. The present disclosure also provides an integrated dicing and die bonding film that includes the film-like adhesive as a first adhesive layer, and a method for manufacturing a semiconductor device using the same.

[0007] A film-like adhesive according to a first embodiment of the present disclosure is composed of a thermosetting resin composition containing a rubber component, and has a first surface and a second surface. The film-like adhesive has a region near the first surface where the rubber component content increases from the second surface side toward the first surface side. The film-like adhesive is subjected to indentation measurement using an atomic force microscope according to the following procedure, and the resulting graph has a portion G1 where the elastic modulus gradually increases starting from the measurement result on the first surface, and a portion G2 where the elastic modulus becomes substantially constant from the end point of portion G1. (Procedure for indentation measurement using an atomic force microscope) (1) The film-like adhesive is cured, and the cured film-like adhesive is fixed to the sample stage of the atomic force microscope, and a cantilever is placed on a cantilever holder. (2) The cantilever is pressed into the film-like adhesive to obtain a curve showing the relationship between the applied load and the pressing depth. (3) The Hertz contact theory is used to obtain the graph showing the relationship between the elastic modulus of the film-like adhesive and the distance from the first surface from the curve.

[0008] The state in which the film-like adhesive has been cured by heating means a state in which the reaction rate is 90% or higher, as generally measured by comparing the amount of heat generated before and after the reaction using a DSC (differential scanning calorimeter, for example, Thermo Plus 2 manufactured by Rigaku Corporation) to evaluate the degree of curing. To cure the film-like adhesive, for example, it is sufficient to heat it at 170°C for 3 hours.

[0009] A film-like adhesive having the above-described region has a barrier function that prevents the migration of heavy metal ions and excellent adhesion. While the reason for this is not entirely clear, the inventors speculate as follows. That is, the region located near the first surface has a relatively high rubber component content. In other words, near the first surface, a region with a relatively high rubber component content is formed locally in the thickness direction, while being continuously spread in the plane direction. This makes the above-described region denser than other regions, and it is speculated that the presence of such a region with a certain thickness allows it to exhibit a barrier function that prevents the migration of heavy metal ions. Furthermore, the increased elastic modulus of the bulk itself, not just the vicinity of the first surface, tends to enhance the barrier function that prevents the migration of heavy metal ions.

[0010] Furthermore, it has been found that when indentation measurements are performed on a film adhesive using an atomic force microscope, if a graph showing a specific behavior is obtained, the film adhesive tends to have excellent adhesion. While the reason for this is not entirely clear, it is presumed that the elastic modulus near the first surface is relatively smaller than that of other portions (i.e., somewhat softer), which allows the film adhesive to deform moderately and tends to result in excellent adhesion between the film adhesive and the adherend. Another commonly known method for improving adhesion is to add low-molecular-weight additives to increase adhesion, but this method often deteriorates the reliability of semiconductors. Therefore, the film adhesive according to this embodiment is preferable because it can improve adhesion without impairing reliability.

[0011] The adhesive film according to the present disclosure comprises the above-mentioned film-like adhesive and a base film in contact with the second surface of the film-like adhesive. The integrated dicing and die bonding film according to the present disclosure comprises, in this order, a first adhesive layer made of the above-mentioned film-like adhesive, a second adhesive layer in contact with the second surface of the film-like adhesive, and a base film in contact with the second adhesive layer.

[0012] The method for manufacturing a semiconductor device according to the present disclosure includes the steps of attaching a wafer to the first surface of the film-like adhesive (first adhesive layer) in the dicing / die bonding integrated film, singulating the wafer and film-like adhesive into a plurality of chips with adhesive pieces, picking up the chips with adhesive pieces from the second adhesive layer, and pressing the chip onto a substrate or another chip via the adhesive pieces.

[0013] The present disclosure provides a film-like adhesive having a barrier function that prevents the migration of heavy metal ions, such as copper ions, and excellent adhesion, and an adhesive film including the film-like adhesive. The present disclosure also provides an integrated dicing and die bonding film including the film-like adhesive as a first adhesive layer, and a method for manufacturing a semiconductor device using the film-like adhesive.

[0014] FIG. 1 is a cross-sectional view schematically showing one embodiment of a film-like adhesive according to the present disclosure. FIG. 2 is an example of a graph obtained when indentation measurement is performed on a film-like adhesive according to the present disclosure. FIGS. 3(a) and 3(b) are examples of graphs obtained when indentation measurement is not performed correctly. FIGS. 4(a) and 4(b) are examples of graphs obtained when indentation measurement is not performed correctly. FIGS. 5(a) and 5(b) are examples of graphs obtained when indentation measurement is not performed correctly. FIG. 6 is an example of a graph obtained when indentation measurement is not performed correctly. FIG. 7 is a cross-sectional view schematically showing an example of an adhesive film comprising the film-like adhesive shown in FIG. 1. FIG. 8 is a cross-sectional view schematically showing one embodiment of a dicing-die bonding integrated film according to the present disclosure. FIG. 9 is a cross-sectional view schematically showing an example of a semiconductor device. FIG. 10 is a cross-sectional view schematically showing another example of a semiconductor device. FIG. 11 is a cross-sectional view schematically showing another embodiment of a film-like adhesive according to the present disclosure.

[0015] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings as appropriate. However, the present disclosure is not limited to the following embodiments. In the following embodiments, components (including steps, etc.) are not essential unless specifically stated. The sizes of the components in each figure are conceptual, and the relative size relationships between the components are not limited to those shown in each figure.

[0016] The same applies to numerical values ​​and ranges in this specification, and do not limit the present invention. In this specification, numerical ranges indicated using "to" indicate ranges that include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this specification, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in numerical ranges described in this specification, the upper or lower limit value of that numerical range may be replaced with a value shown in the examples. In this specification, (meth)acrylate means acrylate or the corresponding methacrylate. The same applies to other similar expressions such as (meth)acryloyl group, (meth)acrylic copolymer, etc.

[0017] <Film-like adhesive> FIG. 1 is a cross-sectional view schematically illustrating a film-like adhesive according to this embodiment. The film-like adhesive 1 shown in this figure has a single-layer structure composed of a thermosetting resin composition containing a rubber component. The film-like adhesive may also have a multilayer structure. The thickness of the film-like adhesive 1 may be 50 μm or less, for example, 40 μm or less, 30 μm or less, 20 μm or less, or 10 μm or less. If the thickness of the film-like adhesive 1 is 50 μm or less, the distance between the semiconductor element and the support member on which the semiconductor element is mounted becomes short, which tends to increase the likelihood of defects caused by heavy metal ions, thereby making it easier to achieve the effects of the present invention. The lower limit of the thickness of the film-like adhesive 1 is not particularly limited, but is, for example, 2 μm or more. If the thickness of the film-like adhesive 1 is 2 μm or more, a film with a better appearance tends to be obtained.

[0018] The film adhesive 1 has a region A (the region whose thickness is indicated by the arrow in the enlarged view shown in FIG. 1 ) near the first surface F1, in which the rubber component content increases from the second surface F2 side toward the first surface F1 side. Region A is composed of multiple rubber components 1f and a resin component other than the rubber components. In region A, the rubber component 1f content may increase continuously or stepwise. Region A serves to prevent the migration of heavy metal ions. In other words, region A located near the first surface F1 is formed locally in the thickness direction, while it is formed with a continuous spread in the planar direction. Such region A is denser than other regions, and is therefore presumed to have a barrier function that prevents the migration of heavy metal ions.

[0019] Region A is located at a depth of less than 2 μm from the first surface F1, although this varies depending on the thickness of the film-like adhesive 1. In other words, "the vicinity of the first surface F1" in this embodiment refers to a region that is less than 2 μm deep from the first surface F1. It is sufficient that region A exists in the vicinity of the first surface F1, and for example, a region with a low content of rubber component 1f may be locally present on the first surface F1.

[0020] The film adhesive 1 has a region B in which the content of the rubber component 1f does not substantially change in the direction from the region A toward the second surface F2. The region B is composed of a plurality of rubber components 1f and a resin component other than the rubber components.

[0021] The film adhesive 1 is subjected to indentation measurement using an atomic force microscope, which is carried out according to the following procedure. The graph (as shown in FIG. 2 ) obtained has a portion G1 where the elastic modulus gradually increases starting from the measurement result on the first surface F1, and a portion G2 where the elastic modulus becomes approximately constant from the end of portion G1. (Procedure for indentation measurement using an atomic force microscope) (1) The film adhesive 1 is cured, and the cured film adhesive 1 is fixed to the sample stage of the atomic force microscope, and a cantilever is placed in a cantilever holder. (2) The cantilever is pressed in, and a curve showing the relationship between the applied load and the pressing depth is obtained. (3) From the curve, Hertz contact theory is used to obtain a graph showing the relationship between the elastic modulus of the film adhesive and the distance from the first surface F1.

[0022] In step (1), the atomic force microscope may be, for example, an SPM400 manufactured by Hitachi High-Tech Corporation. The cantilever may be, for example, an SI-DF-40 manufactured by Hitachi High-Tech Corporation. The cantilever used has a radius of curvature of 10 nm or less.

[0023] In step (2), a curve (force curve) is obtained that shows the relationship between the applied load (load on the cantilever) and the indentation depth (displacement of the piezoelectric element) in the region where the cantilever is pressed into the sample (cured film-like adhesive 1). The indentation depth at this time may be, for example, 500 nm or more, or 1000 nm or more. The indentation depth is set to a depth that allows at least region A to be identified.

[0024] In step (3), the force curve of the indentation region obtained in step (2) is converted into a graph showing the relationship between the elastic modulus and the distance from the first surface (the indentation depth of the cantilever) using the Hertz contact theory. In a series of measurements, a corrected cantilever spring constant is used, and the condition of the cantilever is monitored. If obvious wear, deterioration, or the like is observed, the cantilever is replaced.

[0025] The reason why a graph such as that shown in Figure 2 can be obtained by performing indentation measurement on the film-like adhesive 1 is as follows. Specifically, in region A, the content of rubber component 1f decreases from the first surface F1 side toward the second surface F2 side, and therefore the curve in Figure 2 shows a tendency for the elastic modulus to gradually increase (part G1 in Figure 2). On the other hand, in region B, which is deeper in the thickness direction than region A (the region in the direction from region A toward the second surface F2 side), the content of rubber component 1f does not substantially change, and therefore the curve in Figure 2 shows a substantially constant value for the elastic modulus (part G2 in Figure 2). It is believed that the film-like adhesive has excellent adhesion because the elastic modulus of region A is smaller than that of region B (i.e., it is somewhat softer).

[0026] It is extremely difficult to manufacture a film adhesive that produces a graph similar to that shown in Figure 2 when subjected to indentation measurement. Specifically, even when film adhesives are manufactured using the same materials and under the same conditions, due to the influence of temperature and humidity conditions during manufacturing, temperature variations when drying the film adhesive, and the like, film adhesives that produce a graph similar to that shown in Figure 2 when subjected to indentation measurement may be manufactured, while film adhesives that do not produce a graph similar to that shown in Figure 2 when subjected to indentation measurement may also be manufactured. However, by manufacturing a film adhesive based on the manufacturing method for a film adhesive described below, the yield of the film adhesive according to this embodiment can be improved.

[0027] When the following (1) and (2) are satisfied, it can be determined that the film adhesive has a graph like that shown in Figure 2. (1) As the distance from the first surface increases from the start of the elastic modulus measurement (the left end of the graph, the starting point of the measurement result on the first surface), the elastic modulus increases almost monotonically (the graph showing the relationship between the elastic modulus and the distance from the first surface has the G1 portion shown in Figure 2). (2) After the elastic modulus increases almost monotonically (from the end point of portion G1), the elastic modulus becomes almost constant (the graph showing the relationship between the elastic modulus and the thickness of the film adhesive has the G2 portion shown in Figure 2).

[0028] Indentation measurements using an atomic force microscope measure the local elastic modulus of the resin component on the first surface F1, and therefore may not provide results such as those shown in Figure 2 for the film adhesive 1. For example, if the cantilever comes into contact with the rubber component 1f during indentation measurement, the elastic modulus of the resin component cannot be measured correctly, and a graph showing the relationship between the elastic modulus and the thickness of the film adhesive such as that shown in Figure 2 cannot be obtained. If the measurement is not performed correctly, the indentation measurement can be performed again to check whether a graph such as that shown in Figure 2 can be obtained. Note that if a graph such as that shown in Figure 2 is not obtained even once when indentation measurements are performed 10 times on the film adhesive, it is determined that the film adhesive does not qualify as this. Examples of graphs that can be obtained when indentation measurements are not performed correctly are shown in Figures 3 to 6.

[0029] Because the elastic modulus of the film adhesive differs between Region A and Region B, the behavior of the curve changes at the boundary between Region A and Region B. Therefore, the intersection of the G1 and G2 portions of the curve can be regarded as the thickness a (μm) of Region A.

[0030] The thickness a of region A is, for example, 0.05 to 2 μm, and may be 0.1 to 1.5 μm, 0.2 to 1.5 μm, or 0.3 to 1 μm. When the thickness a of region A is 0.05 μm or more, region A tends to be able to function as an impediment to the migration of heavy metal ions. Furthermore, when the thickness a of region A is 0.1 μm or more, region A tends to be able to fully function as an impediment to the migration of heavy metal ions. On the other hand, when the thickness a of region A is 2 μm or less, the handleability of the film-like adhesive 1 tends to be easily maintained. The ratio of the thickness a of region A to the overall thickness of the film-like adhesive 1 is, for example, 0.3 to 25%, and may be 1 to 20%, or 3 to 15%. When this ratio is 0.3% or more, region A tends to be able to function as an impediment to the migration of heavy metal ions. Furthermore, when this ratio is 1% or more, region A tends to be able to fully function as an impediment to the migration of heavy metal ions. On the other hand, if this proportion is 25% or less, the mechanical strength of the film adhesive 1 can be maintained.

[0031] In region B, the composition is uniform, so the content of the rubber component 1f does not change substantially. Therefore, the G2 portion of the curve remains flat, and the elastic modulus b at the intersection of the G1 portion and the G2 portion of the curve can be regarded as the elastic modulus of region B.

[0032] The film-like adhesive 1 is composed of an adhesive composition containing (A) a thermosetting resin component and (B) a rubber component. The film-like adhesive 1 may be capable of passing through a semi-cured (B-stage) state and then becoming a cured (C-stage) state after a curing treatment.

[0033] Component (A): Thermosetting Resin From the viewpoint of adhesiveness, component (A) may be an epoxy resin. Any epoxy resin having an epoxy group in the molecule may be used without particular limitation. Examples of epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, bisphenol A novolac epoxy resins, bisphenol F novolac epoxy resins, stilbene epoxy resins, triazine skeleton-containing epoxy resins, fluorene skeleton-containing epoxy resins, triphenolmethane epoxy resins, biphenyl epoxy resins, xylylene epoxy resins, biphenyl aralkyl epoxy resins, naphthalene epoxy resins, polyfunctional phenols, and diglycidyl ether compounds of polycyclic aromatics such as anthracene. These may be used alone or in combination of two or more. Among these, component (A) may be a cresol novolac epoxy resin, a phenol novolac epoxy resin, a bisphenol F epoxy resin, or a bisphenol A epoxy resin from the viewpoint of film tackiness, flexibility, etc.

[0034] The epoxy equivalent of the epoxy resin is not particularly limited, but may be 90 to 300 g / eq or 110 to 290 g / eq. When the epoxy equivalent of the epoxy resin is within this range, the film adhesive tends to maintain its bulk strength while ensuring its fluidity.

[0035] The content of component (A) is 15 to 80 mass%, based on the total mass of the film adhesive (adhesive composition), and may be 20 to 75 mass%, 30 to 70 mass%, 30 to 60 mass%, or 35 to 50 mass%. When the content of component (A) is within this range, the film adhesive according to this embodiment is easier to produce, and the migration (permeation) of heavy metal ions within the film adhesive tends to be more sufficiently suppressed, resulting in excellent adhesion. A content of 15 mass% or more facilitates the formation of region A, while a content of 80 mass% or less facilitates the maintenance of workability in the production of the film adhesive.

[0036] Component (B): Rubber Component Examples of component (B) include acrylic rubber, isoprene rubber, butyl rubber, styrene-butadiene rubber, butadiene rubber, styrene-butylene-styrene rubber, styrene-ethylene-propylene-styrene rubber, styrene-ethylene-butylene-styrene rubber, acrylonitrile-butadiene rubber, silicone rubber, urethane rubber, chloroprene rubber, ethylene-propylene rubber, fluororubber, vulcanized rubber, epichlorohydrin rubber, and chlorinated butyl rubber. Component (B) may be incompatible with component (A), and some or all of component (B) may not be completely dissolved in component (A). From the viewpoint of making it easier to produce the film-like adhesive according to this embodiment, component (B) may be an acrylic rubber having a structural unit derived from a (meth)acrylic acid ester as the main component. The content of the structural units derived from a (meth)acrylic acid ester in component (B) may be, for example, 70% by mass or more, 80% by mass or more, or 90% by mass or more, based on the total amount of structural units, from the viewpoint of making it easier to produce the film-like adhesive according to this embodiment. The acrylic rubber may contain structural units derived from a (meth)acrylic acid ester having a crosslinkable functional group such as an epoxy group, an alcoholic or phenolic hydroxyl group, or a carboxyl group. Furthermore, the acrylic rubber may contain structural units derived from acrylonitrile. However, since this makes it possible to more effectively suppress the permeation of heavy metal ions into the film-like adhesive and provides better embeddability, component (B) may not contain structural units derived from acrylonitrile.

[0037] The glass transition temperature (Tg) of component (B) may be -50 to 50°C or -30 to 30°C. When the Tg of component (B) is -50°C or higher, the flexibility of the film-like adhesive tends to be prevented from becoming too high. This makes it easier to cut the film-like adhesive during wafer dicing, and makes it possible to prevent the occurrence of burrs. When the Tg of component (B) is 50°C or lower, the flexibility of the film-like adhesive tends to be suppressed from decreasing. This tends to make it easier to sufficiently fill voids when the film-like adhesive is attached to a wafer. It also makes it possible to prevent chipping during dicing due to a decrease in wafer adhesion. Here, the glass transition temperature (Tg) refers to a value measured using a DSC (differential scanning calorimeter) (e.g., Thermo Plus 2, manufactured by Rigaku Corporation).

[0038] The weight average molecular weight (Mw) of component (B) may be 100,000 to 3,000,000 or 200,000 to 2,000,000. When the Mw of component (B) is within this range, it is possible to appropriately control the film-forming properties, strength, flexibility, tackiness, etc. of the film-like adhesive, and it is also possible to achieve excellent reflow properties and improved embeddability. Here, Mw refers to a value measured by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene.

[0039] Commercially available products of component (B) include, for example, improved SG-P3 and SG-80H (both manufactured by Nagase ChemteX Corporation).

[0040] The content of component (B) is 20 to 85% by mass, based on the total mass of the film-like adhesive (adhesive composition), and may be 25 to 80% by mass, 20 to 65% by mass, 20 to 50% by mass, 20 to 40% by mass, or 30 to 70% by mass. When the content of component (B) is within this range, the film-like adhesive according to this embodiment is easier to produce, and the migration (permeation) of heavy metal ions within the film-like adhesive tends to be more sufficiently suppressed, resulting in excellent adhesion. A content of 20% by mass or more facilitates the formation of region A, while a content of 85% by mass or less facilitates the maintenance of workability in the production of the film-like adhesive.

[0041] The content of component (B) may be 5 to 80 parts by mass, 20 to 60 parts by mass, or 30 to 45 parts by mass, relative to 100 parts by mass of the total mass of components (A) and (B). When the content of component (B) is 5 parts by mass or more, the film adhesive according to this embodiment is easier to produce, and the migration (permeation) of heavy metal ions within the film adhesive tends to be more sufficiently suppressed, resulting in excellent adhesion. When the content of component (B) is 80 parts by mass or less, the effect of easily forming region A is achieved, while when the content is 85 mass% or less, the effect of easily maintaining workability in the production of the film adhesive is achieved.

[0042] The film-like adhesive (adhesive composition) may contain components other than the (A) thermosetting resin component and the (B) rubber component. For example, the film-like adhesive (adhesive composition) may further contain a (C) curing agent, a (D) filler, a (E) coupling agent, a (F) curing accelerator, etc.

[0043] Component (C): Curing Agent Component (C) may be a phenolic resin that can serve as a curing agent for epoxy resins. Any phenolic resin can be used without particular limitation as long as it has a phenolic hydroxyl group in the molecule. Examples of phenolic resins include novolak-type phenolic resins obtained by condensing or co-condensing phenols such as phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol and / or naphthols such as α-naphthol, β-naphthol, and dihydroxynaphthalene with a compound having an aldehyde group such as formaldehyde under an acidic catalyst; phenol aralkyl resins synthesized from allylated bisphenol A, allylated bisphenol F, allylated naphthalenediol, phenol novolak, and phenol and / or naphthols with dimethoxyparaxylene or bis(methoxymethyl)biphenyl; and naphthol aralkyl resins. These may be used alone or in combination of two or more. Among these, the phenolic resin may be a novolac type phenolic resin or a naphthol aralkyl resin.

[0044] The hydroxyl equivalent of the phenolic resin may be 70 g / eq or more, or 70 to 300 g / eq. When the hydroxyl equivalent of the phenolic resin is 70 g / eq or more, the storage modulus of the film tends to be further improved, and when it is 300 g / eq or less, problems due to the generation of foaming, outgassing, etc. can be prevented.

[0045] From the viewpoint of curability, the ratio of the epoxy equivalent of the epoxy resin to the hydroxyl equivalent of the phenolic resin (epoxy equivalent of the epoxy resin / hydroxyl equivalent of the phenolic resin) may be 0.30 / 0.70 to 0.70 / 0.30, 0.35 / 0.65 to 0.65 / 0.35, 0.40 / 0.60 to 0.60 / 0.40, or 0.45 / 0.55 to 0.55 / 0.45. When the equivalent ratio is 0.30 / 0.70 or more, more sufficient curability tends to be obtained. When the equivalent ratio is 0.70 / 0.30 or less, excessive viscosity increase can be prevented, and more sufficient fluidity can be obtained.

[0046] The total content of the (A) component and the (C) component may be 5 to 80 parts by mass, 20 to 80 parts by mass, 40 to 80 parts by mass, 60 to 80 parts by mass, 10 to 75 parts by mass, or 15 to 70 parts by mass, based on 100 parts by mass of the total mass of the (A), (B), and (C) components. When the total content of the (A) component and the (C) component is 5 parts by mass or more, the elastic modulus tends to be improved by crosslinking, and the effect of improving the bulk elastic modulus in particular is exhibited. When the total content of the (A) component and the (C) component is 80 parts by mass or less, the handleability of the film tends to be maintained. When the film has strong tack, the (A) component and the (C) component that are solid at room temperature may be used. When the film has weak tack, the (A) component and the (C) component that are liquid at room temperature may be used.

[0047] In another embodiment, the thermosetting resin component (A) may contain an elastomer having a crosslinkable functional group such as an epoxy group, an alcoholic or phenolic hydroxyl group, or a carboxyl group, and a curing agent capable of reacting with the crosslinkable functional group. Examples of a combination of an elastomer having a crosslinkable functional group and a curing agent capable of reacting with the crosslinkable functional group include a combination of an acrylic rubber having an epoxy group and a phenolic resin.

[0048] Component (D): Filler The film-like adhesive (adhesive composition) may or may not contain a filler (D). Component (D) may be either an inorganic filler or an organic filler. Examples of inorganic fillers include aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whiskers, boron nitride, and silica. These may be used alone or in combination of two or more. Among these, component (D) may be silica from the viewpoint of adjusting the melt viscosity. Examples of organic fillers include carbon, rubber-based fillers, silicone-based microparticles, polyamide microparticles, and polyimide microparticles. The shape of component (D) is not particularly limited, but may be spherical.

[0049] From the viewpoint of flowability, the average particle size of component (D) may be 0.01 to 1 μm, 0.01 to 0.8 μm, or 0.03 to 0.5 μm. Here, the average particle size refers to the value determined by conversion from the BET specific surface area.

[0050] The content of component (D) may be 0.1 to 50 parts by mass, 0.1 to 30 parts by mass, or 0.1 to 20 parts by mass, relative to 100 parts by mass of the total mass of component (A), component (B), and component (C). Based on the total mass of the film-like adhesive (adhesive composition), the content of component (D) is, for example, 3 to 55% by mass, or may be 5 to 50% by mass, or 7 to 40% by mass. A content of 3% by mass or more provides the effect of maintaining the mechanical strength of the film-like adhesive, while a content of 55% by mass or less provides the effect of maintaining a good appearance of the film-like adhesive.

[0051] Component (E): Coupling Agent Component (E) may be a silane coupling agent. Examples of silane coupling agents include γ-ureidopropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane. These may be used alone or in combination of two or more.

[0052] Component (F): Curing Accelerator Component (F) is not particularly limited, and a commonly used one can be used. Examples of component (F) include imidazoles and their derivatives, organic phosphorus compounds, secondary amines, tertiary amines, and quaternary ammonium salts. These may be used alone or in combination of two or more. Among these, from the perspective of reactivity, component (F) may be imidazoles and their derivatives. Examples of imidazoles include 2-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-methylimidazole. These may be used alone or in combination of two or more.

[0053] The film adhesive 1 may further contain other components. Examples of other components include leveling agents, pigments, ion scavengers, antioxidants, etc. The content of component (E), component (F), and other components may be 0 to 30 parts by mass per 100 parts by mass of the total mass of component (A), component (B), and component (C).

[0054] <Method for producing film-like adhesive> The film-like adhesive 1 can be formed by applying the adhesive composition to a support film. When a varnish of the adhesive composition (adhesive varnish) is used, the components (A) and (B) and other components added as needed are mixed in a solvent, the mixed liquid is mixed or kneaded to prepare the adhesive varnish, the adhesive varnish is applied to a support film 5, and the solvent is removed by drying, thereby obtaining the film-like adhesive 1. The adhesive sheet 100 shown in Figure 7 is composed of a support film 5 and a film-like adhesive 1 provided on the surface of the support film 5.

[0055] When forming the film adhesive 1 from the coating of adhesive varnish, the solvent is removed by drying while blowing air onto the surface of the coating, which makes it easier to produce the film adhesive according to this embodiment. The speed of the air flowing parallel to the upper surface of the coating is, for example, 3 to 20 m / s. When this speed is 3 m / s or more, the drying of component (A) on the surface of the coating that is exposed to the air is promoted, making it easier to produce the film adhesive according to this embodiment and making it easier to form a region A with sufficient thickness near the first surface F1 of the film adhesive 1. On the other hand, when the speed is 20 m / s or less, the appearance of the coating surface is more easily maintained.

[0056] The drying temperature of the adhesive varnish is, for example, 25 to 150° C., and may be 60 to 145° C. or 70 to 140° C. A drying temperature of 70° C. or higher has the effect of facilitating production of the film-like adhesive according to this embodiment, while a drying temperature of 150° C. or lower has the effect of making it easier to suppress poor appearance.

[0057] The support film 5 is not particularly limited as long as it can withstand the above-mentioned heat drying, and may be, for example, a polyester film, a polypropylene film, a polyethylene terephthalate film, a polyimide film, a polyetherimide film, a polyether naphthalate film, a polymethylpentene film, etc. The support film 5 may be a multilayer film made by combining two or more types of film, and may have a surface treated with a silicone-based, silica-based, or other mold release agent. The thickness of the support film 5 may be, for example, 10 to 200 μm or 20 to 170 μm.

[0058] Mixing or kneading can be carried out using a dispersing machine such as a conventional stirrer, a mortar and pestle, a three-roll mill, or a ball mill, or by appropriately combining these. The solvent used in preparing the adhesive varnish is not limited as long as it can uniformly dissolve, knead, or disperse the components, and conventionally known solvents can be used. Examples of such solvents include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, as well as dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, toluene, and xylene. Methyl ethyl ketone, cyclohexanone, and the like may be used as the solvent because of their fast drying rate and low cost. Known methods can be used to apply the adhesive varnish to the support film, including, for example, knife coating, roll coating, spray coating, gravure coating, bar coating, and curtain coating.

[0059] <Dicing and die bonding integrated film> Figure 8 is a schematic cross-sectional view of a dicing and die bonding integrated film comprising a film-like adhesive 1. The dicing and die bonding integrated film 120 shown in this figure comprises, in this order, a first adhesive layer L1 made of the film-like adhesive 1, a second adhesive layer L2 in contact with the second surface F2 of the film-like adhesive 1, and a base film L3 in contact with the second adhesive layer L2. The second adhesive layer L2 and the base film L3 form a dicing tape.

[0060] <Semiconductor Device> Using the dicing and die bonding integrated film 120, for example, a semiconductor device as shown in FIG. 9 can be manufactured. The semiconductor device 200 shown in FIG. 9 includes a semiconductor chip 9, a support member 10 on which the semiconductor chip 9 is mounted, and a cured adhesive piece 1c provided between the semiconductor chip 9 and the support member 10. The adhesive piece is an individualized film-like adhesive 1. The cured adhesive 1c bonds the semiconductor chip 9 and the support member 10. The connection terminals (not shown) of the semiconductor chip 9 are electrically connected to external connection terminals (not shown) via wires 11 and are sealed with a sealing material 12.

[0061] The semiconductor device shown in Fig. 10 can also be manufactured using the dicing / die bonding integrated film 120. In the semiconductor device 210 shown in Fig. 10, a first-tier semiconductor chip 9a is bonded to a support member 10 with a cured material 1c, and a second-tier semiconductor chip 9b is further bonded onto the first-tier semiconductor chip 9a with a cured material 1c. The connection terminals (not shown) of the first-tier semiconductor chip 9a and the second-tier semiconductor chip 9b are electrically connected to external connection terminals via wires 11 and are sealed with a sealing material 12. Terminals 13 are formed on the underside of the support member 10.

[0062] <Method for Manufacturing Semiconductor Device> The semiconductor devices 200 and 210 are manufactured, for example, through the following steps: A step of attaching a wafer to the first surface F1 of the first adhesive layer L1 (film-like adhesive) in the dicing and die bonding integrated film 120; A step of singulating the wafer and the first adhesive layer L1 (film-like adhesive) into a plurality of chips with adhesive pieces; A step of picking up the chips with adhesive pieces from the second adhesive layer L2; A step of pressing the semiconductor chip onto a substrate or another semiconductor chip via the adhesive pieces.

[0063] The semiconductor devices 200, 210 are obtained, for example, by interposing an adhesive piece between a semiconductor chip and a support member or between two semiconductor chips, bonding them together by heat and pressure, and then, as necessary, undergoing a wire bonding process, a sealing process using a sealing material, a heat melting process including solder reflow, etc. In the heat and pressure bonding process, the heating temperature is typically 20 to 250°C, the load is typically 0.1 to 200 N, and the heating time is typically 0.1 to 300 seconds.

[0064] The support member may include a copper-based material. The semiconductor devices 200 and 210 are manufactured using the film-like adhesive 1, which has a barrier function that prevents the migration of heavy metal ions (e.g., copper ions). Therefore, even when copper-based materials are used as components of the semiconductor device, the effects of copper ions generated from the materials can be reduced, and electrical defects caused by copper ions can be sufficiently suppressed. Examples of copper-based materials include lead frames, wiring, wires, and heat dissipation materials. Regardless of the type of material, copper can be used to reduce the effects of copper ions.

[0065] Although the embodiments of the present disclosure have been described in detail above, the present disclosure is not limited to the above embodiments. For example, in the above embodiments, an embodiment in which region A is formed near the first surface F1 has been illustrated. However, as shown in FIG. 11 , a region C similar to region A may also be formed near the second surface F2. The film-like adhesive 2 shown in the same figure has the same configuration as the film-like adhesive 1, except that it further includes region C, which is a region near the second surface F2 and in which the rubber content increases from the first surface F1 side toward the second surface F2 side. Region C is located at a depth of less than 2 μm from the second surface F2. In other words, "near the second surface F2" refers to a region shallower than a depth of 2 μm from the second surface F2. Note that it is sufficient that region C exists near the second surface F2; for example, a region with a low rubber content may be locally present on the second surface F2.

[0066] The thickness of the film-like adhesive 2 may be 50 μm or less, and may be, for example, 40 μm or less, 30 μm, 20 μm or less, or 10 μm or less. If the thickness of the film-like adhesive 2 is 50 μm or less, the distance between the semiconductor element and the support member on which the semiconductor element is mounted becomes short, which tends to make problems due to heavy metal ions more likely to occur, and therefore the effects of the present invention are more easily achieved. The lower limit of the thickness of the film-like adhesive 2 is not particularly limited, but can be, for example, 2 μm or more. If the thickness of the film-like adhesive 2 is 2 μm or more, a film with a better appearance tends to be obtained. The thickness of region C is, for example, 0.05 to 2 μm, and may be 0.1 to 1.5 μm, 0.2 to 1.5 μm, or 0.3 to 1 μm. When the thickness of region C is 0.05 μm or more, region C tends to be able to function as an impediment to the migration of heavy metal ions. Furthermore, when the thickness of region C is 0.1 μm or more, region C tends to be able to fully function as an impediment to the migration of heavy metal ions. On the other hand, when the thickness of region C is 2 μm or less, the effect of easily maintaining the handleability of the film-like adhesive 2 is achieved. The ratio of the thickness of region C to the overall thickness of the film-like adhesive 2 is, for example, 0.3 to 25%, and may be 1 to 20%, or 3 to 15%. When this ratio is 0.3% or more, region C tends to be able to function as an impediment to the migration of copper ions. Furthermore, when this ratio is 1% or more, region C tends to be able to fully function as an impediment to the migration of heavy metal ions. On the other hand, when this ratio is 25% or less, the effect of maintaining the mechanical strength of the film-like adhesive 2 is achieved.

[0067] The present disclosure relates to the following: [1] A film-like adhesive comprising a thermosetting resin composition containing a rubber component, the film-like adhesive having a first surface and a second surface, the film-like adhesive having a region near the first surface where the content of the rubber component increases from the second surface side toward the first surface side, the film-like adhesive being characterized by an indentation measurement using an atomic force microscope performed according to the following procedure, the graph obtained having a portion G1 where the elastic modulus gradually increases starting from the measurement result on the first surface, and a portion G2 where the elastic modulus becomes substantially constant from the end point of portion G1. (Procedure for indentation measurement using an atomic force microscope) (1) The film-like adhesive is cured, the cured film-like adhesive is fixed to the sample stage of the atomic force microscope, and the tip of a cantilever with a radius of curvature of 10 nm or less is positioned so that it is perpendicular to the first surface of the cured film-like adhesive. (2) Measurement is performed in contact mode, the cantilever is pressed in, and a curve showing the relationship between the applied load and the indentation depth is obtained. (3) The graph showing the relationship between the elastic modulus of the film adhesive and the distance from the first surface is obtained from the curve using Hertz contact theory. [2] The film adhesive according to [1], wherein the thickness of the region is 2 μm or less. [3] The film adhesive according to [1] or [2], wherein the ratio of the thickness of the region to the total thickness of the film adhesive is 0.3 to 25%. [4] The film adhesive according to any one of [1] to [3], wherein the region is located at a depth of less than 2 μm from the first surface. [5] The film adhesive according to any one of [1] to [4], wherein the rubber component content is 20 to 85 mass% based on the total mass of the resin composition. [6] The film adhesive according to any one of [1] to [5], wherein the rubber component is an acrylic rubber. [7] The film adhesive according to any one of [1] to [6], wherein the film adhesive has a single-layer structure. [8] An adhesive film comprising: the film adhesive according to any one of [1] to [7]; and a base film in contact with the second surface of the film adhesive.[9] A dicing and die bonding integrated film comprising, in this order: a first adhesive layer made of the film adhesive according to any one of [1] to [7], a second adhesive layer in contact with the second surface of the film adhesive, and a base film in contact with the second adhesive layer.

[10] A method for manufacturing a semiconductor device, comprising: a step of attaching a wafer to the first surface of the film adhesive in the dicing and die bonding integrated film according to [9], a step of singulating the wafer and the film adhesive into a plurality of chips with adhesive pieces attached, a step of picking up the chips with adhesive pieces attached from the second adhesive layer, and a step of pressure-bonding the chips onto a substrate or another chip via the adhesive pieces.

[0068] The present disclosure will be specifically described below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0069] [Preparation of Film-Like Adhesive] <Preparation of Adhesive Varnish> The acrylic rubber solutions shown in Table 1 were used as adhesive varnishes. The numerical values ​​relating to the compositions shown in Table 1 refer to parts by mass of the solid content of the acrylic rubber solution.

[0070] Epoxy resins: HP-4710 (trade name, manufactured by DIC Corporation, naphthalene type epoxy resin, epoxy equivalent: 170 g / eq) N-500P-10 (trade name, manufactured by DIC Corporation, o-cresol novolac type epoxy resin, epoxy equivalent: 203 g / eq) EXA-830CRP (trade name, manufactured by DIC Corporation, bisphenol F type epoxy resin, epoxy equivalent: 155-163 g / eq) Curing agent (phenolic resin): PSM-4326 (trade name, manufactured by Gun-ei Chemical Industry Co., Ltd., softening point: 120°C) Acrylic rubber: Improved SG-P3 (trade name, manufactured by Nagase ChemteX Corporation) Coupling agent: Z-6119 (trade name, manufactured by Dow-Toray Industries, Inc., 3-ureidopropyltriethoxysilane) A-189 (trade name, manufactured by Nippon Unicar Co., Ltd., γ-mercaptopropyltrimethoxysilane) Curing accelerator: 2PZ (trade name, manufactured by Shikoku Chemicals Corporation, 2-phenylimidazole)

[0071] <Preparation of Film-Like Adhesive> An adhesive varnish having the composition shown in Table 1 was filtered through a 100-mesh filter and vacuum degassed. A 38 μm-thick polyethylene terephthalate (PET) film that had been subjected to a release treatment was prepared as a substrate film, and the vacuum degassed adhesive varnish was applied to the PET film. The amount of adhesive varnish applied was adjusted so that the thickness after drying would be 20 μm. The applied adhesive varnish was dried at a drying temperature of 110° C. by blowing air at a speed of 3 m / s or more parallel to the top surface of the coating film, thereby obtaining three film-like adhesives in a B-stage state.

[0072] [Indentation Measurement Using an Atomic Force Microscope] The three film adhesives were heated at 175 ° C for 5 hours and cured. Next, the cured film adhesive was fixed to the sample stage of an atomic force microscope (SPM400, manufactured by Hitachi High-Tech Corporation), and a cantilever (manufactured by Hitachi High-Tech Corporation, product name SI-DF-40, material Si, spring constant 40 N / m, tip curvature radius 8 nm) was placed on a cantilever holder, and the cantilever was pressed into the sample (cured film adhesive) to obtain a force curve of the region where the cantilever was pressed. From the obtained force curve, a graph showing the relationship between the elastic modulus and the thickness of the film adhesive (cantilever indentation depth) was obtained using Hertz contact theory. At this time, a corrected cantilever spring constant was used, and the state of the cantilever was monitored to confirm that no obvious wear or deterioration was observed. For one film-like adhesive (Example 1), a graph (as shown in Figure 2) was obtained, which had a portion G1 where the elastic modulus gradually increased starting from the measurement results on the first surface, and a portion G2 where the elastic modulus remained approximately constant from the end of portion G1. On the other hand, such a graph could not be obtained for the remaining two film-like adhesives (Comparative Examples 1 and 2). In the graph obtained from the film-like adhesive of Example 1, the length from the surface of the film to the intersection of portions G1 and G2 (the thickness of the region where the rubber component content increases) was 230 nm, and the ratio of the thickness of this region to the total thickness of the film-like adhesive was 1.15%.

[0073] [Evaluation of copper ion permeation suppression effect] <Preparation of solution A> 2.0 g of anhydrous copper (II) sulfate was dissolved in 1,020 g of distilled water and stirred until the copper sulfate was completely dissolved, to prepare an aqueous copper sulfate solution having a copper ion concentration of 500 mg / kg in terms of Cu element. The obtained aqueous copper sulfate solution was designated as solution A.

[0074] <Preparation of Solution B> 1.0 g of anhydrous sodium sulfate was dissolved in 1000 g of distilled water and stirred until the sodium sulfate was completely dissolved. 1000 g of N-methyl-2-pyrrolidone (NMP) was then added and stirred. The mixture was then air-cooled to room temperature to obtain an aqueous sodium sulfate solution. The resulting solution was designated Solution B.

[0075] <Measurement of copper ion permeation time> After curing the film-like adhesive (thickness: 10 μm) prepared above, each was cut into a circle with a diameter of approximately 3 cm. Next, two silicone packing sheets with a thickness of 1.5 mm, an outer diameter of approximately 3 cm, and an inner diameter of 1.8 cm were prepared. The circular cut-out film-like adhesive was sandwiched between the two silicone packing sheets, and this was sandwiched between the flanges of two glass cells with a volume of 50 mL and secured with rubber bands.

[0076] Next, 50 g of Solution A was poured into one glass cell, and then 50 g of Solution B was poured into the other glass cell. A Mars Carbon (manufactured by Staedtler GmbH, φ2 mm / 130 mm) was inserted into each cell as a carbon electrode. The Solution A side was the anode, and the Solution B side was the cathode, and the anode was connected to a DC power supply (manufactured by A&D Co., Ltd., DC power supply AD-9723D). The cathode and DC power supply were also connected in series via an ammeter (manufactured by Sanwa Electric Instruments Co., Ltd., Digital multimeter PC-720M). A voltage of 24.0 V was applied at room temperature, and measurement of the current value began after application. The measurement time was up to 500 minutes, and the time for the current value to rise was defined as the copper ion permeation time. The rise time was defined as the time when the current value reached 1.0 μA. In this evaluation, the slower the time for the current value to rise, the more suppressed the copper ion permeation. The evaluation was carried out according to the following criteria. The results are shown in Table 1. A: Copper ion permeation time is 100 minutes or more. B: Copper ion permeation time is less than 100 minutes.

[0077] [Evaluation of Adhesion] The adhesive varnish side of the film-like adhesive prepared above was attached to a glass plate (manufactured by Matsunami Glass Industrial Co., Ltd., product name: S1225) with a cleaned surface to obtain a sample. The sample was left to stand on a hot plate at 60 ° C. for 1 minute, then returned to room temperature (25 ° C.), and the PET film was peeled off. A support tape (manufactured by Oji Tack Co., Ltd., product name: EC tape) was attached to the release surface of the PET film to prepare an evaluation sample with a width of 15 mm and a length of 75 mm. The peel force was measured using an adhesive / film peeling analyzer (manufactured by Kyowa Interface Science Co., Ltd., product name: VPA-3). The peel force was measured by moving the rotary stage and setting the scale on the angle adjustment unit to 30 ° (i.e., the peel force is the peel strength at a peel angle of 30 °). The evaluation sample was peeled off at the interface between the film adhesive and the support tape by about several centimeters, and a 10 mm wide piece of peel-inducing tape (EC tape, manufactured by Oji Tack Co., Ltd.) was attached to the tip of the film adhesive side and fixed to the tip of a load cell. The position of the load cell was finely adjusted so that the peel progress was parallel to the tape width. The peel force was measured by pulling 70 mm at a rate of 150 mm / min, and the average value for the region with a peel distance of 40 to 70 mm was calculated from the obtained measurement chart, and this average value was used as the peel force. The results are shown in Table 1.

[0078]

[0079] 1, 2...film-like adhesive, 1c...cured product, 5...support film, 9, 9a, 9b...semiconductor chip, 10...support member, 11...wire, 12...sealing material, 13...terminal, 100...adhesive sheet, 120...dicing and die bonding integrated film, F1...first surface, F2...second surface, L1...first adhesive layer (film-like adhesive), L2...second adhesive layer, L3...base film, A, B, C...regions.

Claims

1. A film-like adhesive comprising a resin composition having thermosetting properties and containing a rubber component, the film-like adhesive having a first surface and a second surface, the film-like adhesive having a region in the vicinity of the first surface, the region having an increasing content of the rubber component from the second surface side toward the first surface side, the film-like adhesive being subjected to an indentation measurement using an atomic force microscope performed according to the following procedure, the graph obtained has a portion G1 in which the elastic modulus gradually increases from the measurement result on the first surface as a starting point, and a portion G2 in which the elastic modulus becomes substantially constant from the end point of the portion G1. (Procedure for indentation measurement using an atomic force microscope) (1) The film-like adhesive is cured, the cured film-like adhesive is fixed to the sample stage of the atomic force microscope, and a cantilever is placed on a cantilever holder. (2) The cantilever is pressed in, and a curve showing the relationship between the applied load and the pressing depth is obtained. (3) The graph showing the relationship between the elastic modulus of the film-like adhesive and the distance from the first surface is obtained from the curve using the Hertz contact theory.

2. The film adhesive according to claim 1, wherein the thickness of said region is 2 μm or less.

3. The film adhesive according to claim 1, wherein the ratio of the thickness of said region to the total thickness of the film adhesive is 0.3 to 25%.

4. The film adhesive according to claim 1, wherein the region is located at a depth less than 2 μm from the first surface.

5. The film-like adhesive according to claim 1, wherein the content of the rubber component is 20 to 85 mass % based on the total mass of the resin composition.

6. The film adhesive according to claim 1, wherein the rubber component is an acrylic rubber.

7. The film adhesive according to claim 1, wherein the film adhesive has a single layer structure.

8. An adhesive film comprising: a film-like adhesive according to any one of claims 1 to 7; and a base film in contact with the second surface of the film-like adhesive.

9. A dicing and die bonding integrated film comprising, in this order: a first adhesive layer made of a film-like adhesive according to any one of claims 1 to 7; a second adhesive layer in contact with the second surface of the film-like adhesive; and a base film in contact with the second adhesive layer.

10. A method for manufacturing a semiconductor device, comprising the steps of: attaching a wafer onto the first surface of the film-like adhesive in the dicing and die bonding integrated film described in claim 9; singulating the wafer and the film-like adhesive into a plurality of chips with adhesive pieces; picking up the chips with adhesive pieces from the second adhesive layer; and pressing the chip onto a substrate or another chip via the adhesive pieces.