Polymer-coated separator with secondary agglomerates, preparation method therefor, and battery

MYPI2025006814A0Undetermined Publication Date: 2024-11-04SINOMA LITHIUM BATTERY SEPARATOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025006814
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-04
Filing Date
2023-08-10
Publication Date
2024-11-04

AI Technical Summary

Technical Problem

The existing lithium-ion battery separators are prone to disengage during charging and discharging, resulting in a decrease in battery cycle life. While improving the adhesion of the separator and the electrode sheet, the internal resistance of the battery increases, reducing the charge and discharge rate, making it difficult to equalize the polymer coating. adhesion and permeability.

Method used

The polymer-coated separator is used to coat the separator with secondary agglomerates. By controlling the agglomeration state and spray point distribution of polymer secondary agglomerates, it can achieve high bonding, high ion permeability, high liquid absorption and liquid retention properties, and rotate Spraying technology and adhesive dispersion treatment have prepared coated diaphragms with excellent properties.

Benefits of technology

It achieves a balance between high bonding strength and high ion permeability, improves the cycle life and charge and discharge rate of the battery, and reduces the powder depilation rate, ensuring the performance stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025006814_DRAWING_001
    Figure PI2025006814_DRAWING_001
  • Figure PI2025006814_DRAWING_002
    Figure PI2025006814_DRAWING_002
  • Figure PI2025006814_DRAWING_003
    Figure PI2025006814_DRAWING_003
Patent Text Reader

Abstract

The present invention discloses a polymer-coated separator with secondary agglomerates, a preparation method therefor, and a battery. The polymer-coated separator includes: a separator substrate, and a polymer coating applied on a surface of at least one side of the separator substrate, wherein the polymer coating includes a plurality of randomly distributed spray coating points, the spray coating points including a plurality of polymer secondary agglomerates formed by agglomeration of polymer primary particles; any one spray coating point in the polymer coating satisfies the following conditions: 25≤A / B≤40000, and 100≤C / A≤106, wherein A represents a projected area of the polymer secondary agglomerates on the separator substrate; B represents a projected area of the polymer primary particles on the separator substrate; and C represents a projected area of the spray coating point on the separator substrate. In the present invention, a coated separator with high adhesion, high ion permeability, high electrolyte uptake and retention, and low powder shedding rate is obtained by controlling the size of the polymer secondary agglomerates and the size distribution of the secondary agglomerates within the spray coating points. [FIG. 1]
Need to check novelty before this filing date? Find Prior Art

Description

Polymer coated separator with secondary aggregates, preparation method thereof, and battery Technical Field

[0001] The present invention relates to the technical field of battery separators, and in particular to a polymer-coated separator with secondary aggregates, a preparation method thereof, and a battery. Background Art

[0002] In recent years, with the rapid growth in electric vehicle sales, the demand for power lithium-ion batteries has increased significantly. Data shows that as the demand for lithium-ion batteries develops, the demand for lithium-ion batteries will continue to grow at a high rate in the future. As the demand for lithium-ion batteries increases, the market has increasingly higher performance requirements for lithium-ion batteries, which in turn places higher demands on lithium-ion battery separators.

[0003] Conventional lithium-ion battery separators have little adhesion to the electrode, resulting in easy detachment during charge and discharge, thus reducing the battery's cycle life. To address this issue, existing approaches involve applying a polymer coating with adhesive properties to one or both sides of the separator. These polymers can be PVDF or PMMA. However, while existing polymer coatings improve the adhesion between the separator and the electrode, they often alter the separator's pore structure, increasing the battery's internal resistance and reducing the battery's charge and discharge rates. Therefore, achieving a separator that balances both adhesion and permeability is extremely difficult.

[0004] Summary of the Invention

[0005] In view of this, the present invention provides a polymer-coated separator with high adhesion, high permeability, high liquid absorption and retention, and secondary aggregates, a preparation method thereof, and a battery.

[0006] To achieve the above-mentioned object, the present invention provides, in a first aspect, a polymer-coated diaphragm having secondary agglomerates, comprising a diaphragm substrate and a polymer coating applied on at least one surface of the diaphragm substrate; the polymer coating comprises a plurality of randomly distributed spray points, each of which comprises a plurality of polymer secondary agglomerates formed by agglomeration of polymer primary particles;

[0007] Any spraying point in the polymer coating satisfies the following conditions: 25≤A / B≤40000, 100≤C / A≤10 6 ,in,

[0008] A represents the projected area of ​​the polymer secondary aggregates on the diaphragm substrate within the spraying point;

[0009] B represents the projected area of ​​the polymer primary particles on the diaphragm substrate within the spraying point;

[0010] C represents the projected area of ​​the spray point on the diaphragm substrate;

[0011] The effective bonding area ratio of the polymer coating n×∑A / S satisfies: 4%≤n×∑A / S≤50%, where:

[0012] S represents the surface area of ​​the diaphragm substrate;

[0013] ∑A represents the sum of the projected areas of all polymer secondary aggregates within the spraying point on the diaphragm substrate;

[0014] n represents the number of spray points within the area S.

[0015] According to any embodiment of the first aspect of the present invention, 25≤A / B≤10000, 2500≤C / A≤5×10 5 ;

[0016] 6%≤n×∑A / S≤30%.

[0017] According to any embodiment of the first aspect of the present invention, the thickness of the polymer coating is 0.5 μm-10 μm.

[0018] According to any embodiment of the first aspect of the present invention, the bonding strength of the polymer-coated separator to the ternary positive electrode is ≥1 N / m, and the bonding strength to the graphite negative electrode is ≥0.5 N / m; and / or

[0019] The ionic conductivity of the polymer-coated separator is 80% to 110% of the ionic conductivity of the separator substrate; and / or

[0020] The polymer-coated membrane has a liquid absorption rate of ≥70% and a liquid retention rate of ≥70%; and / or

[0021] The powder removal rate of the polymer coated diaphragm is ≤5%.

[0022] According to any embodiment of the first aspect of the present invention, the polymer coating comprises:

[0023] 80-100 parts by mass of a polymer having secondary aggregates;

[0024] Binder, 2 to 20 parts by mass;

[0025] Dispersant, 0.01 to 3 parts by mass.

[0026] According to any embodiment of the first aspect of the present invention, the polymer having secondary agglomerates includes at least one of polyvinylidene fluoride homopolymer (PVDF), polyvinylidene fluoride-trifluoroethylene copolymer (PVDF-TrFE), polyvinylidene fluoride-methyl methacrylate copolymer (PVDF-PMMA), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyvinylidene fluoride-acrylic acid copolymer, polymethyl methacrylate (PMMA), polyethylene (PE), and acrylate polymer.

[0027] According to any embodiment of the first aspect of the present invention, the binder includes at least one of carboxymethyl cellulose, hydroxyethyl cellulose, polyacrylic acid, polymethacrylic acid, polymethyl methacrylate, and acrylonitrile multipolymer.

[0028] According to any embodiment of the first aspect of the present invention, the dispersant includes at least one of ethylene-acrylic acid copolymer, ethylene-vinyl acetate copolymer, acrylic acid-polyurethane and polyethylene glycol.

[0029] According to any embodiment of the first aspect of the present invention, the diaphragm substrate is selected from at least one of polyethylene film, polypropylene film, polyimide film, polyvinylidene fluoride film, polyvinylidene fluoride-hexafluoropropylene film, polyamide film, and polyethylene terephthalate film.

[0030] According to any embodiment of the first aspect of the present invention, the thickness of the separator substrate is 3 μm to 25 μm, and the porosity is 20% to 80%.

[0031] A second aspect of the present invention provides a method for preparing a polymer-coated diaphragm having secondary aggregates, comprising:

[0032] S01. Mix the dispersant and water evenly, then add the polymer in a batches, with the mass of each polymer added being 1 / a of the total amount. After each addition of the polymer, stir slowly, then stir quickly, and then stir slowly again until all the polymer is added, wherein a ≥ 2; optionally, grind the mixture, and finally add the binder, mix evenly, and filter to obtain a polymer slurry;

[0033] S02. Coating the polymer slurry onto the surface of at least one side of the diaphragm substrate by rotary spraying to obtain a polymer coating, wherein the rotary spraying parameters are: coating speed 100 m / min-300 m / min, spraying slurry flow rate 1500 mL / min-15000 mL / min, spraying speed 5000 rpm-15000 rpm, number of teeth of the spraying turntable 200 teeth-600 teeth, and distance from the turntable to the membrane surface 20 cm-50 cm;

[0034] S03, drying the membrane substrate and the polymer coating to obtain a polymer-coated membrane having secondary aggregates.

[0035] According to any implementation of the second aspect of the present invention, step S01 includes:

[0036] S011, mixing water and a dispersant uniformly to obtain a first mixed solution;

[0037] S012. Adding a polymer to the first mixed solution in a times, each time adding 1 / a of the total amount of the polymer, performing a first stage dispersion after each addition: stirring at a speed of 100 rpm-600 rpm, stirring for 10 min-50 min, then performing a second stage dispersion: stirring at a speed of 1000 rpm-2000 rpm, stirring for 30 min-180 min, and finally performing a third stage dispersion: stirring at a speed of 100 rpm-600 rpm, stirring for 10 min-50 min until all the polymer is added, to obtain a second mixed solution;

[0038] S013. Add a binder to the second mixed solution and stir evenly, and filter through a 40-300 mesh filter to obtain a polymer slurry.

[0039] According to any embodiment of the second aspect of the present invention, the particle size D10 of the polymer slurry is 1 μm-4 μm, and D90 is 6 μm-20 μm.

[0040] According to any embodiment of the second aspect of the present invention, the polymer coating amount is 0.05g / m 2 -1.5g / m 2 .

[0041] According to any embodiment of the second aspect of the present invention, the temperature of the drying process in step S03 is 50°C to 90°C.

[0042] The third aspect of the present invention provides a battery, comprising the polymer-coated separator having secondary aggregates provided by the first aspect of the present invention or the polymer-coated separator having secondary aggregates prepared by the preparation method provided by the second aspect of the present invention. Beneficial effects:

[0043] The polymer coated diaphragm with secondary aggregates provided by the present invention controls the aggregation state of the polymer secondary aggregates and the distribution of the secondary aggregates in the spraying point, thereby obtaining a coated diaphragm with high adhesion, high ion permeability, high liquid absorption and retention performance, and low powder shedding rate.

[0044] Additional aspects and advantages of the present invention will be set forth in part in the description which follows and, in part, will be obvious from the description which follows, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following detailed description, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0046] FIG1 is a scanning electron micrograph of a PVDF coating of a polymer-coated diaphragm according to the present invention at 200 times magnification;

[0047] FIG2 is a scanning electron micrograph of the PVDF coating of the polymer-coated diaphragm of the present invention at 1000 times magnification;

[0048] FIG3 is a scanning electron micrograph of the PVDF coating of the polymer-coated diaphragm of the present invention at 10,000 times magnification;

[0049] FIG4 is a schematic diagram of a turntable of a high-speed rotary spraying machine;

[0050] FIG5 is a process flow diagram of a method for preparing a polymer-coated separator having secondary aggregates. DETAILED DESCRIPTION

[0051] The following describes the specific embodiments of the present invention in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention.

[0052] In a first aspect, the present invention provides a polymer-coated diaphragm having secondary aggregates, comprising a diaphragm substrate and a polymer coating applied to at least one surface of the diaphragm substrate; the polymer coating comprises a plurality of randomly distributed spray points, each of which comprises a plurality of polymer secondary aggregates formed by agglomeration of polymer primary particles;

[0053] Any spraying point in the polymer coating satisfies the following conditions: 25≤A / B≤40000, 100≤C / A≤10 6 ,in,

[0054] A represents the projected area of ​​the polymer secondary aggregates on the diaphragm substrate within the spraying point;

[0055] B represents the projected area of ​​the polymer primary particles on the diaphragm substrate within the spraying point;

[0056] C represents the projected area of ​​the spray point on the diaphragm substrate;

[0057] The effective bonding area ratio of the polymer coating n×∑A / S satisfies: 4%≤n×∑A / S≤50%, where:

[0058] S represents the surface area of ​​the diaphragm substrate;

[0059] ∑A represents the sum of the projected areas of all polymer secondary aggregates within the spraying point on the diaphragm substrate;

[0060] n represents the number of spray points within the area S.

[0061] The following details are provided:

[0062] The separator substrate may be a substrate without a coating layer or a substrate coated with an inorganic particle layer, without any particular limitation.

[0063] In an embodiment of the present invention, there is no particular restriction on the type of the diaphragm substrate, and it can be selected according to actual needs; preferably, the diaphragm substrate can be selected from one or more of polyethylene film, polypropylene film, polyimide film, polyvinylidene fluoride film, polyvinylidene fluoride-hexafluoropropylene film, polyamide film, and polyethylene terephthalate film.

[0064] In the embodiment of the present invention, there is no particular restriction on the type of inorganic particles, and they can be selected according to actual needs; preferably, the inorganic particles can be selected from one or more of silicon dioxide (SiO2), aluminum oxide (Al2O3), magnesium oxide (MgO), zirconium oxide (ZrO2), titanium oxide (TiO2), calcium oxide (CaO), boehmite (AlOOH), aluminum nitride (AlN), boron nitride (BN), barium sulfate (BaSO4), calcium fluoride (CaF2), and barium fluoride (BaF2).

[0065] The thickness of the separator substrate may be 3 μm to 25 μm, and preferably 5 μm to 16 μm.

[0066] The porosity of the diaphragm substrate may be 20% to 80%, preferably 30% to 50%.

[0067] Any spraying point in the polymer coating of the present invention meets the following conditions: 25≤A / B≤40000, 100≤C / A≤10 6 , where A represents the projected area of ​​the polymer secondary aggregates on the diaphragm substrate within the spraying point; B represents the projected area of ​​the polymer primary particles on the diaphragm substrate within the spraying point; and C represents the projected area of ​​the spraying point on the diaphragm substrate.

[0068] The effective bonding area ratio n×∑A / S of the polymer coating satisfies: 4%≤n×∑A / S≤50%, wherein ∑A represents the sum of the projected areas of all polymer secondary aggregates within any spraying point within S on the diaphragm substrate; n represents the number of spraying points within S; and S represents the surface area of ​​the diaphragm substrate.

[0069] There is no particular limitation on the shapes of the secondary agglomerates and the spraying spots.

[0070] 1. A / B represents the aggregation state of primary particles in polymer secondary aggregates. When A / B>40000, the polymer secondary aggregates are too large, the polymer coating has uneven thickness, the coating is easy to fall off and powder, affecting the local ion permeability of the membrane; when A / B<25, the polymer secondary aggregates are too small, the bonding strength of the polymer coating is weak, and the liquid absorption and retention performance of the membrane is poor.

[0071] Wherein, A represents the projected area of ​​the polymer secondary aggregates on the polymer coating. The test method is as follows: arbitrarily select a spraying point, take a photo of the spraying point at 200x magnification using a scanning electron microscope, and use software (such as image processing software such as Image J) to mark the edge range of the polymer secondary aggregates. The area of ​​this range is the projected area of ​​the polymer secondary aggregates on the polymer coating. The method for marking the edge range of the secondary aggregates is as follows: Starting from a point on the edge of the secondary aggregate, draw a line around the edge of the secondary aggregate, requiring that the angle of each line segment is less than 180° (the internal angle between each line segment and the previous line segment is less than 180°). When the line segment angle is greater than 180°, disconnect the line segment directly connected to the starting point. The line segment encloses a closed area, i.e., the range, and its area is the projected area of ​​the secondary aggregate.

[0072] In some embodiments, A ranges from 0.785 μm 2 -314μm 2 .

[0073] B represents the projected area of ​​the polymer primary particles on the polymer coating. The test method is as follows: arbitrarily select a spraying point and take a photo of the spraying point at 10,000x magnification using a scanning electron microscope. The range of the polymer primary particles (circle) can be marked using software (such as Image J or other image processing software). The area of ​​this range is the projected area of ​​the polymer primary particles on the polymer coating.

[0074] In some embodiments, B ranges from 7.85×10 -3 μm 2 -0.785μm 2 .

[0075] A / B range 25≤A / B≤40000, for example, 100~2500, 100~3600, 100~6000, 100~10000, 100~40000 or 200~1600, 200~3600, 200~6000, 200~40000 or 250~6000, 250~8000, 250~10000, 250~40000, etc.

[0076] 2. C / A indicates the distribution of polymer secondary agglomerates in the spraying point. When C / A is less than 100, the polymer secondary agglomerates in the spraying point are too large and the number is small, the polymer coating has uneven thickness, and the coating is easy to fall off and powder; when C / A is greater than 10 6 When the effective polymer agglomerates are too few in the spraying point, the coating adhesion is poor, the liquid absorption and retention performance is poor, the exposed area of ​​the diaphragm substrate in the spraying point is small, and the ion penetration performance is poor.

[0077] Where C represents the projected area of ​​the spray point on the polymer coating. The test method is as follows: arbitrarily select a spray point and take a photograph of the spray point at 200x magnification using a scanning electron microscope. Use software (such as Image J) to mark the spray point range. The area of ​​this range is the projected area of ​​the spray point on the polymer coating.

[0078] It should be noted that A, B, and C were tested at the same spraying point.

[0079] In some embodiments, C ranges from 7.85×10 -3 mm 2 -0.785mm 2 between.

[0080] A is defined as above.

[0081] C / A range 100≤C / A≤10 6 , for example, 100~160000, 600~200000, 600~300000, 800~300000, etc.

[0082] 3. n×∑A / S represents the effective bonding area ratio of the polymer coating. When n×∑A / S<4%, the effective bonding area is small and the bonding strength is low. When n×∑A / S>50%, the effective bonding area is large, the exposed substrate area is small, the membrane permeability is poor, and the ion penetration performance is poor.

[0083] Wherein, S represents the area of ​​the substrate, and n represents the number of spray points within the area S. The test method is to place the finished diaphragm under a static CCD lens, take a photo under a 3x magnification field of view, and use image processing software to calculate the area S of the photo and the number n of spray points in the photo.

[0084] ∑A is to select any spraying point within the area S (preferably a spraying point with a D50 of 300-600 μm), test the projected area of ​​each secondary agglomerate according to the test method A above, and then sum it.

[0085] The range of n×ΣA / S is, for example, 10 to 40%, 10 to 30%, 10 to 20%, or 10 to 15%.

[0086] In an embodiment of the present invention, the thickness of the polymer coating is 0.5 μm-10 μm, for example, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, ... 8 μm, 9 μm, and 10 μm. The polymer coating thickness is controlled within the range of 0.5 μm-10 μm. If the thickness is too thin, the adhesion performance will be poor; if the thickness is too thick, the polymer coating thickness will be uneven, the coating will easily fall off, and the ion penetration performance will be poor.

[0087] In an embodiment of the present invention, the bonding strength between the polymer coated diaphragm and the ternary positive electrode is ≥1.0N / m. For example, the bonding strength between the polymer coating and the ternary positive electrode plate is 1N / m...4N / m, 4.2N / m, 4.5N / m, 4.6N / m, 4.8N / m, 5N / m,...

[0088] In an embodiment of the present invention, the bonding strength between the polymer coated separator and the graphite negative electrode sheet is ≥0.5 N / m. For example, the bonding strength between the polymer coated separator and the graphite negative electrode sheet is 0.5 N / m...4 N / m, 4.2 N / m, 4.5 N / m, 4.6 N / m, 4.8 N / m, 5 N / m,...

[0089] The bond strength between the polymer-coated separator and the battery electrode can be tested using methods known in the art. Specifically, the test method for bond strength may include stacking the polymer coating of the battery separator and the ternary cathode or graphite anode together in a hot press. The bond strength is then measured using a tensile testing machine at a speed of 50 mm / min, with the 180-degree peel strength being the bond strength. The hot press conditions are preferably a temperature of 90°C, a pressure of 6.5 MPa, and a time of 60 seconds.

[0090] In an embodiment of the present invention, the ionic conductivity of the polymer-coated membrane is 80%-110% of the ionic conductivity of the membrane substrate, for example, 81%, 82%, 85%, 90%, ..., 110%.

[0091] The ionic conductivity of the membrane can be tested by methods known in the art. As a specific example, the ionic conductivity test method can be: the ionic conductivity of the membrane can be measured by the formula Calculation is performed, σs is the conductivity of the diaphragm, Rs is the resistance of the diaphragm, d is the thickness of the diaphragm, and S is the effective area of ​​the diaphragm;

[0092] In an embodiment of the present invention, the liquid absorption rate of the polymer-coated membrane is ≥70%, such as 70%, 80%, 90%, or 95%, and the liquid retention rate is ≥70%, such as 70%, 80%, 90%, or 95%;

[0093] The liquid absorption rate and liquid retention rate of the diaphragm can be tested by methods known in the art. As a specific example, the test method for the liquid absorption rate and liquid retention rate can be: refer to QB / T 2303.11-2008 "Battery pulp layer paper Part 11: Determination of liquid absorption rate" for measurement, cut a 50mm×50mm diaphragm sample and weigh it as m0, then immerse it in a beaker filled with electrolyte after weighing, soak it for 1 hour, take it out, hang it in the air for 3 minutes to drip off the electrolyte, and weigh it as m, then let it stand at room temperature for 1 hour and weigh it as m1. The liquid absorption rate X and liquid retention rate Y of lithium-ion battery diaphragms can be calculated by the following formula:

[0094] Where m0 is the mass of the diaphragm before soaking, m is the mass of the diaphragm after soaking, and m1 is the mass after standing at room temperature for 1 hour.

[0095] In an embodiment of the present invention, the powder removal rate of the polymer-coated separator is ≤5%, for example, 4%, 3%, 2%, or 1%.

[0096] The powder loss rate mainly characterizes the powder loss of the polymer spray coating. Powder loss of the diaphragm will cause the adhesion of the diaphragm to decrease and there is a risk of false hot pressing. The specific test method is: take a roll of finished polymer spray diaphragm and weigh it, the weight is recorded as m0, then place the film on the slitting machine for empty running, and weigh it again after winding, the weight is recorded as m1, then the powder loss rate P = (m0-m1) / m0×100%.

[0097] In an embodiment of the present invention, the components of the polymer coating include: 80 to 100 parts by mass of a polymer; 2 to 20 parts by mass of a binder; and 0.01 to 3 parts by mass of a dispersant.

[0098] In an embodiment of the present invention, the polymer having secondary agglomerates includes at least one of polyvinylidene fluoride homopolymer (PVDF), polyvinylidene fluoride-trifluoroethylene copolymer (PVDF-TrFE), polyvinylidene fluoride-methyl methacrylate copolymer (PVDF-PMMA), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyvinylidene fluoride-acrylic acid copolymer, polymethyl methacrylate (PMMA), polyethylene (PE), and acrylate polymer.

[0099] The polymer having secondary agglomerates in the present invention mainly refers to its solid form.

[0100] In some embodiments, the primary particle size of the polymer is in the range of 0.1 μm to 1 μm, and the B value is controlled by selecting different types of polymers (eg, PVDF resin).

[0101] In the embodiment of the present invention, the type of binder is not particularly limited and can be selected according to actual needs; preferably, the binder can be selected from one or more of carboxymethyl cellulose, hydroxyethyl cellulose, polyacrylic acid, polymethacrylic acid, polymethyl methacrylate, and acrylonitrile copolymer.

[0102] In the embodiment of the present invention, the type of dispersant is not particularly limited and can be selected according to actual needs; preferably, the dispersant can be selected from one or more of ethylene-acrylic acid copolymer, ethylene-vinyl acetate copolymer, acrylic acid-polyurethane and polyethylene glycol.

[0103] The battery separator provided by the embodiments of the present invention can be used in various types of batteries. Therefore, there is no particular limitation on the type of battery and the separator can be selected according to actual needs. Preferably, the separator can be used in secondary batteries, particularly those containing liquid electrolytes, such as lithium-ion batteries and sodium-ion batteries.

[0104] In a second aspect of the present invention, a method for preparing a polymer-coated diaphragm having secondary aggregates is provided, as shown in FIG5 , comprising:

[0105] S01. Mix the dispersant and water evenly, then add the polymer in a batches, with the mass of each polymer added being 1 / a of the total amount. After each addition of the polymer, stir slowly, then stir quickly, and then stir slowly again until all the polymer is added, wherein a ≥ 2; optionally, grind the mixture, and finally add the binder, mix evenly, and filter to obtain a polymer slurry;

[0106] S02, applying the polymer slurry to the surface of at least one side of the diaphragm substrate by rotary spraying to obtain a polymer coating having spray points, wherein the rotary spraying parameters are: coating speed 100m / min-300m / min, spraying slurry flow rate 1500mL / min-15000mL / min, spraying speed 5000rpm-15000rpm, the number of teeth of the spraying turntable is 200 teeth-600 teeth (the turntable schematic diagram of the high-speed rotary sprayer is shown in Figure 4), and the distance from the turntable to the membrane surface is 20cm-50cm;

[0107] S03, drying the membrane substrate and the polymer coating to obtain a polymer-coated membrane having secondary aggregates.

[0108] In an embodiment of the present invention, step S01 in the above preparation method may further include:

[0109] S011, mixing water and a dispersant uniformly to obtain a first mixed solution;

[0110] S012. Adding a polymer to the first mixed solution in a times, each time adding 1 / a of the total amount of the polymer, performing a first stage dispersion after each addition: stirring at a speed of 100 rpm-600 rpm, stirring for 10 min-50 min; then performing a second stage dispersion: stirring at a speed of 1000 rpm-2000 rpm, stirring for 30 min-180 min, and finally performing a third stage dispersion: stirring at a speed of 100 rpm-600 rpm, stirring for 10 min-50 min; until all the polymers are added, to obtain a second mixed solution;

[0111] S013. Add a binder to the second mixed solution and stir evenly, then filter through a 40-300 mesh filter (undispersed large PVDF particles can be screened out by filtering) to obtain a polymer slurry.

[0112] Adding in batches can make the PVDF resin better dispersed. Stir slowly first to prevent the PVDF powder from flying during the mixing process, and then stir quickly to accelerate the mixing of PVDF in water. By controlling the number of times the PVDF resin is added, the speed and time of slow and fast stirring, and the size of the filter, the desired PVDF slurry (secondary particles) size can be obtained, thereby adjusting the A / B range.

[0113] In some embodiments, the obtained polymer slurry has a particle size D10 of 1 μm to 4 μm and a particle size D90 of 6 μm to 20 μm (controlling the A value range). The particle sizes D10 and D90 of the slurry can be measured using a laser particle size analyzer.

[0114] The size of C, and thus the size of C / A, can be adjusted by adjusting the spraying speed, slurry flow, the number of teeth on the spraying turntable, and the distance from the turntable to the membrane surface.

[0115] The effective bonding area n×∑A / S can be adjusted by adjusting the size of A and the flow rate of spraying slurry.

[0116] In some embodiments, the obtained spray point D10 is 100 μm-300 μm, and D90 is 800 μm-1000 μm.

[0117] The test method for D10 and D90 of the spraying point can be as follows: place the finished diaphragm under a static CCD lens, take a photo at a 3x magnification field of view, use image processing software to calculate the number n of spraying points in the photo and the size of each spraying point, and thus calculate the D10 and D90 of the spraying point.

[0118] In the embodiment of the present invention, the membrane substrate and the PVDF coating are dried in a conventional manner.

[0119] In the embodiment of the present invention, the temperature of the drying process is 50°C-90°C.

[0120] According to the method provided in the second aspect of the embodiment of the present invention, a polymer-coated separator having secondary aggregates according to any embodiment of the first aspect of the present invention can be obtained.

[0121] Figures 1 to 3 show scanning electron micrographs of the PVDF coating of the coated diaphragm at different magnifications (accelerating voltage EHT = 1 kV, working distance WD = 5.8-6.1 mm, SE2 detector).

[0122] In a third aspect, the present invention provides a battery comprising the polymer-coated diaphragm with secondary aggregates provided in the first aspect of the embodiment of the present invention or the polymer-coated diaphragm with secondary aggregates prepared by the preparation method provided in the second aspect of the embodiment of the present invention.

[0123] In an embodiment of the present invention, the battery is a lithium-ion secondary battery or a sodium-ion secondary battery.

[0124] The present invention is described below with reference to specific examples. It should be noted that these examples are merely illustrative and do not limit the present invention in any way.

[0125] Unless otherwise specified, the raw materials, reagents, methods, etc. used in the examples are conventional raw materials, reagents, and methods in the art.

[0126] The high-speed rotary spraying machine is a DS-800-01 PCS isolation film spraying machine manufactured by Yuanbiao in Hong Kong, China.

[0127] Example 1: Preparation of PVDF aqueous spray slurry: 57 kg of water and 0.025 kg of dispersant were weighed and stirred at 500 rpm for 30 min to obtain a first mixed solution; 5 kg of PVDF-HFP resin (East Sunshine HEVER2601 primary particle size is 0.1-0.3 μm) was added to the first mixed solution in two times, each adding amount was 2.5 kg, and after each addition of PVDF-HFP resin, it was first stirred slowly at 300 rpm for 30 min, then stirred quickly at 1000 rpm for 60 min, and finally stirred slowly at 300 rpm for 20 min to obtain a second mixed solution after all were added; then 0.25 kg of polyacrylic acid binder was added to the second mixed solution, stirred at 50 rpm for 30 min to obtain a third mixed solution, and finally filtered through a 200 mesh filter to obtain PVDF spray slurry, the D10 of the PVDF spray slurry was 2.1 μm and the D90 was 7.6 μm.

[0128] Coating: The prepared PVDF spray slurry is fed into the feeding tank of a high-speed rotary sprayer through an automatic feeding system, and then coated on one side of a 9μm, 50% porosity polyethylene wet-process base membrane by rotary spraying. The coating speed is 150m / min, the number of teeth on the spray turntable is 360, the distance from the turntable to the membrane surface is 25cm, the spray slurry flow rate is 5000mL / min, and the spraying speed is 9000rpm; after drying at 60℃, a water-based PVDF coated diaphragm is obtained.

[0129] The spray point obtained after coating had a D10 of 200 μm and a D90 of 800 μm.

[0130] The PVDF secondary agglomerate accumulation state A / B, spray point accumulation state C / A, effective bonding area, and diaphragm performance and parameters of the coated diaphragm are shown in Table 1-1 below.

[0131] Example 2: Preparation of PVDF aqueous spray slurry: 57 kg of water and 0.0025 kg of dispersant were weighed and stirred at 500 rpm for 30 min to obtain a first mixed solution; 5 kg of PVDF-HFP resin (manufacturer Arkema LBG primary particle size is 0.15-0.2 μm) was added to the first mixed solution in 3 times, each addition amount was 1.667 kg, and after each addition of PVDF-HFP resin, it was first stirred slowly at 500 rpm for 30 min, then stirred quickly at 1500 rpm for 90 min, and finally stirred slowly at 500 rpm for 30 min to obtain a second mixed solution after all were added; then 0.25 kg of polyacrylic acid binder was added to the second mixed solution, and stirred at 50 rpm for 30 min to obtain a third mixed solution, which was finally filtered through a 300 mesh filter to obtain a PVDF spray slurry. The D10 of the PVDF spray slurry was 1.6 μm and the D90 was 7.2 μm.

[0132] Coating: The prepared PVDF spray slurry is poured into the spray feeding tank through the automatic feeding system, and is coated on one side of the polyethylene wet-process base membrane with a thickness of 9 μm and a porosity of 50% by rotary spraying. The coating speed is 200 m / min, the number of teeth of the spray dispersion disk is 450, the distance from the turntable to the diaphragm substrate is 25 cm, the spray slurry flow rate is 7500 mL / min, the spraying speed is 9000 rpm, and the water-based PVDF coated diaphragm is obtained after drying at 85°C.

[0133] The spray point D10 obtained after coating was 150 μm and D90 was 850 μm.

[0134] The PVDF secondary agglomerate accumulation state A / B, spray point accumulation state C / A, effective bonding area, and diaphragm performance and parameters of the coated diaphragm are shown in Table 1-1 below.

[0135] Example 3: Preparation of PMMA aqueous spray slurry: 82.75 kg of water and 0.009 kg of dispersant were weighed and stirred at 300 rpm for 30 min to obtain a first mixed solution; 15 kg of PMMA powder (manufacturer Yindi Le, primary particle size of 0.2-0.5 μm) was added to the first mixed solution in 3 times, each addition amount was 5 kg, and after each addition of PMMA powder, it was first stirred slowly at 400 rpm for 30 min, then stirred quickly at 1200 rpm for 80 min, and finally stirred slowly at 500 rpm for 30 min to obtain a second mixed solution after all were added; then 2.25 kg of polyacrylic acid binder (binder solid content of 40%) was added to the second mixed solution, stirred at 20 rpm for 30 min to obtain a third mixed solution, and finally filtered through a 150 mesh filter to obtain PMMA aqueous spray slurry, the D10 of the PMMA spray slurry was 1.7 μm, and the D90 was 14.1 μm.

[0136] Coating: The prepared spray slurry is poured into the spray feeding tank through the automatic feeding system, and coated on one side of the polyethylene wet-process base membrane with a thickness of 9 μm and a porosity of 50% by rotary spraying. The coating speed is 150 m / min, the number of teeth of the spray dispersion disk is 360, the distance from the turntable to the diaphragm substrate is 25 cm, the spray slurry flow rate is 4000 mL / min, the spraying speed is 9000 rpm, and the water-based PMMA coated diaphragm is obtained after drying at 80°C.

[0137] The spray point D10 obtained after coating was 210 μm and D90 was 800 μm.

[0138] The PMMA secondary agglomerate stacking state A / B, spray point stacking state C / A, effective bonding area, and diaphragm performance and parameters of the coated diaphragm are shown in Table 1-1 below.

[0139] Example 4: Preparation of PVDF-PMMA copolymer aqueous spray slurry: 45 kg of water and 0.015 kg of dispersant were weighed and stirred at 500 rpm for 30 min to obtain a first mixed solution; 5 kg of PVDF-PMMA powder (primary particle size of 0.2-0.4 μm) was added to the first mixed solution in two times, each adding amount was 2.5 kg, and after each addition of PMMA powder, it was first stirred slowly at 600 rpm for 30 min, then stirred quickly at 1800 rpm for 100 min, and finally stirred slowly at 600 rpm for 30 min to obtain a second mixed solution after all were added; then 1.25 kg of polyacrylic acid binder (binder solid content of 40%) was added to the second mixed solution, stirred at 20 rpm for 30 min to obtain a third mixed solution, and finally filtered through a 100 mesh filter to obtain a PVDF-PMMA aqueous spray slurry, the D10 of the spray slurry was 2.3 μm, and the D90 was 12.5 μm.

[0140] Coating: The prepared spray slurry is pumped into the spray feeding tank through an automatic feeding system, and coated on the ceramic membrane surface of the 7+2 ceramic coating membrane by rotary spraying, where 7 is a 7μm polyethylene wet base membrane with a porosity of 40%, 2 is a 2μm ceramic coating, the coating speed is 100m / min, the number of teeth of the spray dispersion disk is 360, the distance from the turntable to the diaphragm substrate is 25cm, the spray slurry flow rate is 2200mL / min, the spraying speed is 8500rpm, and after drying at 65℃, a water-based PVDF-PMMA coated diaphragm is obtained.

[0141] The spray point D10 obtained after coating was 230 μm and D90 was 820 μm.

[0142] The stacking state A / B of the PVDF-PMMA secondary agglomerates in the coated diaphragm, the stacking state C / A of the spraying points, the effective bonding area, and the performance and parameters of the diaphragm are shown in Table 1-1 below.

[0143] Example 5: Preparation of PVDF-PMMA copolymer aqueous spray slurry: same as Example 4.

[0144] Coating: The prepared spray slurry is pumped into the spray feeding tank through an automatic feeding system, and coated on both sides of the 7+2 ceramic coating membrane by rotary spraying, where 7 is a 7μm polyethylene wet base membrane with a porosity of 40%, and 2 is a 2μm ceramic coating. The coating speed is 100m / min, the number of teeth of the spray dispersion disk is 360, the distance from the turntable to the diaphragm substrate is 25cm, the spray slurry flow rate is 2200mL / min, the spraying speed is 8500rpm, and after drying at 65℃, a water-based PVDF-PMMA coated diaphragm is obtained.

[0145] The spray point D10 obtained after coating was 230 μm and D90 was 820 μm.

[0146] The stacking state A / B of the PVDF-PMMA secondary agglomerates in the coated diaphragm, the stacking state C / A of the spraying points, the effective bonding area, and the performance and parameters of the diaphragm are shown in Table 1-1 below.

[0147] Comparative Example 1: Preparation of PVDF aqueous spray slurry: 52 kg of water and 0.3 kg of dispersant were weighed and stirred for 30 min to obtain a first mixed solution; 20 kg of PVDF-HFP emulsion (primary particle size of 0.15-0.2 μm) was added to the first mixed solution, the solid content of the emulsion was 30%, and the mixture was stirred at 200 rpm for 30 min to obtain a second mixed solution; 0.5 kg of polyacrylic acid binder was added to the second mixed solution, and the mixture was stirred for 30 min to obtain a PVDF spray slurry; the D10 of the PVDF spray slurry was 0.15 μm, and the D90 was 0.6 μm.

[0148] Coating: The prepared PVDF spray slurry is pumped into the spray feeding tank through the automatic feeding system, and is coated on one side of the polyethylene wet-process base membrane with a thickness of 12 μm and a porosity of 50% by rotary spraying. The coating speed is 100 m / min, the number of teeth of the spray dispersion disk is 450, the distance from the turntable to the diaphragm substrate is 30 cm, the spray slurry flow rate is 3200 mL / min, the spraying speed is 7200 rpm, and the water-based PVDF coated diaphragm is obtained after drying at 85°C.

[0149] The spray point obtained after coating had a D10 of 100 μm and a D90 of 600 μm.

[0150] The stacking state A / B of the PVDF secondary agglomerates in the coated diaphragm, the stacking state C / A of the spraying points, the effective bonding area, and the performance and parameters of the diaphragm are shown in Table 1-2 below.

[0151] Comparative Example 2: Preparation of PVDF aqueous spray slurry: Weigh 57 kg of water and 0.0025 kg of dispersant, stir for 30 minutes to obtain a first mixed solution; add 5 kg of PVDF resin powder (primary particle size is 0.15-0.2 μm) to the first mixed solution, first stir slowly at 200 rpm for 50 minutes, then stir at 600 rpm for 60 minutes, and finally stir at 200 rpm for 30 minutes to mix evenly to obtain a second mixed solution, then add 0.25 kg of polyacrylic acid binder to the second mixed solution, stir at 50 rpm for 30 minutes to obtain a third mixed solution, no filtration is required, the D10 of the PVDF spray slurry is 3.8 μm, and D90 is 35 μm.

[0152] Coating: The prepared PVDF spray slurry is poured into the spray feeding tank through the automatic feeding system, and is coated on one side of the polyethylene wet-process base membrane with a thickness of 9 μm and a porosity of 50% by rotary spraying. The coating speed is 150 m / min, the number of teeth of the spray dispersion disk is 450, the distance from the turntable to the diaphragm substrate is 25 cm, the spray slurry flow rate is 5000 mL / min, and the spraying speed is 12000 rpm.

[0153] The spray point D10 is 80 μm and D90 is 600 μm.

[0154] The stacking state A / B of the PVDF secondary agglomerates in the coated diaphragm, the stacking state C / A of the spraying points, the effective bonding area, and the performance and parameters of the diaphragm are shown in Table 1-2 below.

[0155] Comparative Example 3: Preparation of PVDF aqueous spray slurry: same as Example 1.

[0156] Coating: The prepared PVDF spray slurry is coated on one side of a 9μm, 50% porosity polyethylene wet-process base membrane by rotary spraying. The coating speed is 200m / min, the number of teeth of the spray dispersion disk is 800, the distance from the turntable to the diaphragm substrate is 25cm, the spray slurry flow rate is 9000mL / min, the spray speed is 17000rpm, and after drying at 85℃, a polymer-coated diaphragm with secondary agglomerates is obtained.

[0157] The spray point obtained after coating had a D10 of 50 μm and a D90 of 300 μm.

[0158] The stacking state A / B of the PVDF secondary agglomerates in the coated diaphragm, the stacking state C / A of the spraying points, the effective bonding area, and the performance and parameters of the diaphragm are shown in Table 1-2 below.

[0159] Comparative Example 4: Preparation of PVDF aqueous spray slurry: 57 kg of water and 0.0025 kg of dispersant were weighed and stirred at 500 rpm for 30 min to obtain a first mixed solution; 5 kg of PVDF-HFP resin (primary particle size of 0.15-0.2 μm) was added to the first mixed solution in 5 times, with an addition amount of 1 kg each time. After each addition of PVDF-HFP resin, the mixture was slowly stirred at 500 rpm for 30 min, then quickly stirred at 2500 rpm for 100 min, and finally slowly stirred at 500 rpm for 30 min. The above operation was repeated until the PVDF-HFP resin was completely mixed to obtain a second mixed solution; then 0.25 kg of polyacrylic acid binder was added to the second mixed solution, and the mixture was stirred at 50 rpm for 30 min to obtain a third mixed solution, which was finally filtered through a 300 mesh filter to obtain a PVDF spray slurry. The D10 of the PVDF spray slurry was 1.2 μm and the D90 was 5.6 μm.

[0160] Coating: The prepared PVDF spray slurry was rotary sprayed onto one side of a 9μm, 50% porosity polyethylene wet-process base membrane. The coating speed was 200 m / min, the spray dispersion disc had 280 teeth, the distance between the disc and the membrane substrate was 25 cm, the spray slurry flow rate was 6000 mL / min, and the spray speed was 4000 rpm. After drying at 85°C, the resulting polymer-coated membrane with secondary aggregates had a spray point D10 of 350 μm and a D90 of 1500 μm.

[0161] The stacking state A / B of the PVDF secondary agglomerates in the coated diaphragm, the stacking state C / A of the spraying points, the effective bonding area, and the performance and parameters of the diaphragm are shown in Table 1-2 below.

[0162] Comparative Example 5: Preparation of PVDF aqueous spray slurry: same as Comparative Example 2.

[0163] Coating: Same as Comparative Example 3.

[0164] The stacking state A / B of the PVDF secondary agglomerates in the coated diaphragm, the stacking state C / A of the spraying points, the effective bonding area, and the performance and parameters of the diaphragm are shown in Table 1-2 below.

[0165] Comparative Example 6: Preparation of PVDF aqueous spray slurry: same as Comparative Example 4.

[0166] Coating: The prepared PVDF spray slurry was rotary sprayed onto one side of a 9μm, 50% porosity polyethylene wet-process base membrane. The coating speed was 300 m / min, the spray dispersion disc had 180 teeth, the distance between the disc and the membrane substrate was 15 cm, the spray slurry flow rate was 16,000 mL / min, and the spray speed was 4,500 rpm. After drying at 85°C, the resulting polymer-coated membrane with secondary aggregates had a spray point D10 of 450 μm and a D90 of 2,000 μm.

[0167] The stacking state A / B of the PVDF secondary agglomerates in the coated diaphragm, the stacking state C / A of the spraying points, the effective bonding area, and the performance and parameters of the diaphragm are shown in Tables 1-3 below.

[0168] Comparative Example 7: Preparation of PVDF aqueous spray slurry: same as Comparative Example 2.

[0169] Coating: The prepared PVDF spray slurry was rotary sprayed onto one side of a 9μm, 50% porosity polyethylene wet-process base membrane. The coating speed was 150 m / min, the spraying disc had 300 teeth, the distance between the disc and the membrane substrate was 15 cm, the spray slurry flow rate was 1000 mL / min, and the spraying speed was 6000 rpm. After drying at 80°C, the resulting polymer-coated membrane with secondary aggregates had a spray point D10 of 220 μm and a D90 of 1000 μm.

[0170] The stacking state A / B of the PVDF secondary agglomerates in the coated diaphragm, the stacking state C / A of the spraying points, the effective bonding area, and the performance and parameters of the diaphragm are shown in Tables 1-3 below.

[0171] Test section

[0172] Relevant performance tests were performed on the PVDF coatings and battery separators in Examples 1 to 5 and Comparative Examples 1 to 7. The test results are shown in Tables 1-1, 1-2, and 1-3 below.

[0173] Table 1-1

[0174] Table 1-2

[0175] Table 1-3

[0176] From the results of the embodiments and comparative examples, it can be seen that in Examples 1-5, A / B, C / A, and n×∑A / S are all within the given range, and their bonding performance and ionic conductivity, liquid absorption / liquid retention rate, and powder loss can be effectively balanced to achieve the optimal effect; Comparative Example 1 uses emulsion PVDF-HFP without secondary aggregate structure, A / B is small, C / A is large, and although the bonding performance is high, the ionic conductivity and liquid absorption and liquid retention performance are poor; Comparative Example 2 is a one-time feeding and dispersion process for preparing the slurry, and the stirring speed is too low, the powder has poor dispersion performance in water, and the slurry is not filtered. Therefore, the PVDF particle size in the slurry is large and the distribution range is wide, A / B is large, C / A is normal, the bonding performance and ion permeability are poor, the powder loss rate is significantly increased, and the coating loses powder seriously; Comparative Example 3 has normal secondary aggregates, uses an 800-tooth dispersion disk, and the spraying speed is 17000rpm, so The spray point is too small, A / B is normal, C / A is small, the spray point accumulation is high, the bonding strength has no obvious change, but the ionic conductivity is significantly reduced, and the powder removal rate increases; in comparative example 4, PVDF powder is added 5 times during the pulping process, and the stirring is performed at ultra-high speed. The PVDF secondary agglomerates, the speed is low, the number of turntable teeth is small, the spray point is large, A / B is small, C / A is large, the bonding and ionic conductivity are reduced, and the liquid absorption and liquid retention rate is significantly reduced; in comparative example 5 , the secondary agglomerates are too large, the spraying points are small, A / B is too large, C / A is too small, the bonding and ionic conductivity are deteriorated, and the powder removal rate is significantly improved; in comparative example 6, the spraying flow rate is too large, the number of turntable teeth is too small, the coating amount is high, and the spraying point is too large, which makes n×∑A / S too large and the ionic conductivity decreases significantly; in comparative example 7, the spraying flow rate is too small, the slurry particle size is too large, and the coating amount is small, which makes n×∑A / S too small, and the bonding strength between the coating and the positive and negative electrodes is significantly reduced.

[0177] From the results of the embodiments and comparative examples, it can be seen that only when A / B, C / A and n×∑A / S are all within the given ranges can high adhesion, high ion permeability, high liquid absorption and retention performance and low powder loss rate be achieved.

[0178] Although the embodiments of the present invention have been shown and described above, it will be understood that the above embodiments are illustrative and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A polymer-coated separator having secondary aggregates, It is characterized in that include: a diaphragm substrate, and A polymer coating applied on at least one surface of the diaphragm substrate, The polymer coating comprises a plurality of randomly distributed spraying points, and the spraying points comprise a plurality of polymer secondary agglomerates formed by agglomeration of polymer primary particles; Any spraying point in the polymer coating satisfies the following conditions: 25≤A / B≤40000, 100≤C / A≤10 6 ,in, A represents the projected area of ​​the polymer secondary aggregates within the spraying point on the diaphragm substrate; B represents the projected area of ​​the polymer primary particles on the diaphragm substrate within the spraying point; C represents the projected area of ​​the spray point on the diaphragm substrate; The effective bonding area ratio of the polymer coating n×∑A / S satisfies: 4%≤n×∑A / S≤50%, where: S represents the surface area of ​​the diaphragm substrate; ∑A represents the sum of the projected areas of all polymer secondary aggregates within the spraying point on the diaphragm substrate; n represents the number of spraying points within area S.

2. The polymer-coated separator having secondary aggregates according to claim 1, It is characterized in that 25≤A / B≤10000,2500≤C / A≤5×10 5 ; 6%≤n×∑A / S≤30%。 3. The polymer-coated separator having secondary aggregates according to claim 1, It is characterized in that The bonding strength of the polymer coated separator to the ternary positive electrode is ≥1N / m, and the bonding strength to the graphite negative electrode is ≥0.5N / m; and / or The ionic conductivity of the polymer coated membrane is 80% to 110% of the ionic conductivity of the membrane substrate; and / or The liquid absorption rate of the polymer coated diaphragm is ≥70%, and the liquid retention rate is ≥70%; and / or The powder removal rate of the polymer coated diaphragm is ≤5%.

4. The polymer-coated separator having secondary aggregates according to any one of claims 1 to 3, It is characterized in that Polymer coatings include: Polymer with secondary aggregates, 80 to 100 parts by mass; Binder, 2 to 20 parts by weight; Dispersant: 0.01 to 3 parts by mass.

5. The polymer-coated separator having secondary aggregates according to claim 4, It is characterized in that The polymer having secondary aggregates includes at least one of polyvinylidene fluoride homopolymer, polyvinylidene fluoride-trifluoroethylene copolymer, polyvinylidene fluoride-methyl methacrylate copolymer, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-acrylic acid copolymer, polymethyl methacrylate, polyethylene, and acrylate polymer; and / or The binder comprises at least one of carboxymethyl cellulose, hydroxyethyl cellulose, polyacrylic acid, polymethacrylic acid, polymethyl methacrylate, and acrylonitrile multipolymer; and / or The dispersant includes at least one of ethylene-acrylic acid copolymer, ethylene-vinyl acetate copolymer, acrylic acid-polyurethane and polyethylene glycol.

6. The polymer-coated separator having secondary aggregates according to any one of claims 1 to 3, It is characterized in that The thickness of the diaphragm substrate is 3 μm to 25 μm, and the porosity is 20% to 80%; and / or The thickness of the polymer coating is 0.5 μm-10 μm.

7. A method for preparing the polymer-coated diaphragm having secondary aggregates according to claim 1, It is characterized in that include: S01, mixing the dispersant and water evenly, then adding the polymer in a times, the mass of the polymer added each time is 1 / a of the total amount, stirring slowly first, then quickly, and then slowly again after adding the polymer each time, until all the polymer is added, wherein a≥2, finally adding the binder, mixing evenly, and filtering to obtain the polymer slurry; Step S01 includes: S011, mixing water and a dispersant uniformly to obtain a first mixed solution; S012, adding polymer to the first mixed solution in a times, each time the amount of polymer added is 1 / a of the total amount, and performing the first stage dispersion after each addition: the stirring speed is 100rpm-600rpm, the stirring time is 10min-50min, and then the second stage dispersion is performed: the stirring speed is 1000rpm-2000rpm, the stirring time is 30min-180min, and finally the third stage dispersion is performed: the stirring speed is 100rpm-600rpm, the stirring time is 10min-50min until all the polymers are added, to obtain a second mixed solution; S013, adding a binder to the second mixed solution and stirring the mixture evenly, filtering the mixture through a 40-300 mesh filter to obtain a polymer slurry; S02, coating the polymer slurry onto the surface of at least one side of the diaphragm substrate by rotary spraying to obtain a polymer coating, wherein the rotary spraying parameters are: coating speed 100m / min-300m / min, spraying slurry flow rate 1500mL / min-15000mL / min, spraying speed 5000rpm-15000rpm, the number of teeth of the spraying turntable is 200 teeth-600 teeth, and the distance from the turntable to the membrane surface is 20cm-50cm; S03, drying the membrane substrate and the polymer coating to obtain a polymer-coated membrane having secondary aggregates.

8. The method for preparing a polymer-coated diaphragm having secondary aggregates according to claim 7, It is characterized in that The particle size D10 of the polymer slurry is 1 μm-4 μm, and D90 is 6 μm-20 μm.

9. The method for preparing a polymer-coated diaphragm having secondary aggregates according to claim 7, It is characterized in that The polymer coating amount is 0.05g / m 2 -1.5g / m 2 .

10. The method for preparing a polymer-coated diaphragm having secondary aggregates according to claim 7, It is characterized in that After all the polymers in step S01 are added, grinding treatment is performed, and finally a binder is added, mixed evenly, and filtered to obtain a polymer slurry.

11. A battery, It is characterized in that A polymer-coated separator having secondary agglomerates according to any one of claims 1 to 6.