Electrode for oxygen evolution and method for producing same

MYPI2025007813A0Undetermined Publication Date: 2025-04-11INDUSTRIE DE NORA SPA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025007813
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-11
Filing Date
2024-10-07
Publication Date
2025-04-11

AI Technical Summary

Technical Problem

The existing oxygen-generating electrode has a short service life during electrolysis, especially the precious element erbium (Ir) used in the catalytic layer is not efficient, resulting in insufficient service life of the electrode.

Method used

A substrate made of titanium (Ti) or titanium alloy is used to cover the first intermediate layer and the catalytic layer. The first intermediate layer is composed of mixed metal oxide (MMO) formed by titanium and tantalum (Ta). The catalytic layer is composed of MMO formed by erbium and tantalum. A tantalum oxide layer is added between the catalytic layer, with a content of between 1.2 and 2.5 grams/square meter. At the same time, a platinum (Pt) coating can be optionally added, with a platinum content of between 0.5 and 3.0 grams/square meter.

Benefits of technology

By optimizing the electrode structure and material composition, the service life of the oxygen-generating electrode is extended, the efficiency of erbium is improved, and the energy consumption of the electrode during the electrolysis process is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025007813_DRAWING_001
    Figure PI2025007813_DRAWING_001
  • Figure PI2025007813_DRAWING_002
    Figure PI2025007813_DRAWING_002
  • Figure PI2025007813_DRAWING_003
    Figure PI2025007813_DRAWING_003
Patent Text Reader

Abstract

An electrode for oxygen evolution that can be used for electrolysis over a long period of time by efficiently consuming iridium used as an active element is provided. An electrode for oxygen evolution (10) includes a substrate (2) made of titanium or a titanium alloy; a first intermediate layer (4) disposed on the substrate (2) and made of a first mixed metal oxide containing titanium and tantalum; a catalyst layer (6) disposed above the first intermediate layer (4) and made of a second mixed metal oxide containing iridium and tantalum; and a second intermediate layer (5) disposed between the first intermediate layer (4) and the catalyst layer (6), made of a tantalum oxide, and having a tantalum content of 1.2 to 2.5 g / m2. Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Oxygen generating electrode and method of manufacturing the same

[0001] The present invention relates to an electrode for oxygen generation and a method for producing the same.

[0002] In the process of electrowinning non-ferrous metals such as copper, nickel, and zinc, sulfuric acid or strong acid electrolyte is generally used.And, as the counter electrode, the anode is used as an oxygen generating electrode that causes oxygen generating reaction.Titanium electrode with a coating layer containing mixed metal oxide (MMO) as a catalyst layer on its surface has a lower overvoltage characteristic for oxygen generating reaction, so it has been proposed as an anode for electrowinning process that can replace the lead alloy electrode that has been used as the oxygen generating electrode and can reduce energy consumption.

[0003] The mixed metal oxide for forming the catalyst layer is usually a composite oxide of iridium (Ir) as an active element and a valve metal such as tantalum (Ta), tin (Sn), titanium (Ti), zirconium (Zr), or niobium (Nb) as a binder element. 2 -Ta 2 O 5 and an electrode for electrolysis provided with a coating layer containing a composite oxide of iridium and tantalum and platinum (Pt) (Patent Document 1).

[0004] Also, an electrode for electrolysis has been proposed in which a base layer containing titanium and tantalum formed by an arc ion plating (AIP) method and a catalyst layer formed of a mixed metal oxide containing iridium and tantalum are provided on a titanium electrode substrate (Patent Document 2).

[0005] Japanese Unexamined Patent Publication No. 5-59580 Japanese Unexamined Patent Publication No. 2009-263770

[0006] Journal of Applied Electrochemistry, 1991, 21, p. 335-345

[0007] A catalytic layer formed from a mixed metal oxide is gradually consumed by repeated electrolysis. In particular, iridium, which is used as an active element, is one of the most expensive and rare elements, so there has been a strong demand for an electrolysis electrode having an iridium-based catalytic layer that can efficiently consume iridium and thereby extend its service life.

[0008] However, even with the electrolysis electrodes proposed in Patent Documents 1 and 2, Non-Patent Document 1, etc., the service life of the catalyst layer using iridium is not necessarily sufficient, and there is room for further improvement.

[0009] The present invention has been made in view of the problems of the prior art, and an object of the present invention is to provide an oxygen generating electrode that can be used for electrolysis over a long period of time by efficiently consuming iridium used as an active element. Another object of the present invention is to provide a method for manufacturing an oxygen generating electrode that can be used for electrolysis over a long period of time by efficiently consuming iridium used as an active element.

[0010] That is, according to the present invention, the following oxygen generating electrode is provided: [1] An electrode comprising: a substrate made of titanium or a titanium alloy; a first intermediate layer formed of a first mixed metal oxide containing titanium and tantalum and disposed on the substrate; and a catalyst layer formed of a second mixed metal oxide containing iridium and tantalum and disposed above the first intermediate layer, wherein the second mixed metal oxide is formed of tantalum oxide and has a tantalum content of 1.2 to 2.5 g / m and is disposed between the first intermediate layer and the catalyst layer. 2 [2] The oxygen generating electrode according to the above [1], further comprising a coating layer containing platinum, which is disposed on the catalyst layer. [3] The platinum content in the coating layer is 0.5 to 3.0 g / m 2 [4] The electrode for oxygen generation according to any one of [1] to [3], wherein the first intermediate layer is a layer formed by an arc ion plating method.

[0011] The present invention also provides the following method for producing an electrode for oxygen generation: [5] A method for producing an electrode for oxygen generation, comprising the steps of: disposing a first intermediate layer formed of a first mixed metal oxide containing titanium and tantalum on a substrate formed of titanium or a titanium alloy by arc ion plating; applying a coating liquid containing tantalum but not iridium onto the first intermediate layer, and then heat-treating the coating liquid to form an electrode for oxygen generation, the electrode having a tantalum content of 1.2 to 2.5 g / m2. 2 and a step of applying a catalyst precursor solution containing iridium and tantalum onto the second intermediate layer, followed by heat treatment to form a catalyst layer formed of a second mixed metal oxide containing iridium and tantalum. [6] A method for producing an oxygen generating electrode according to item [5] above, further comprising a step of applying a coating solution containing platinum onto the catalyst layer, followed by heat treatment to form a coating layer containing platinum on the catalyst layer.

[0012] According to the present invention, an oxygen generating electrode that can be used for electrolysis over a long period of time by efficiently consuming iridium used as an active element can be provided. Also, according to the present invention, a method for manufacturing an oxygen generating electrode that can be used for electrolysis over a long period of time by efficiently consuming iridium used as an active element can be provided.

[0013] FIG. 1 is a schematic diagram showing one embodiment of the oxygen generating electrode of the present invention; FIG. 2 is a schematic diagram showing another embodiment of the oxygen generating electrode of the present invention; FIG. 3 is a schematic diagram showing an example of a conventional oxygen generating electrode; FIG. 4 is a schematic diagram showing an example of an oxygen generating electrode used to verify the amount of Pt in the coating layer; 2 ) is a graph plotting the predicted electrode life (h) against the Pt amount (g / m 2 ) with respect to the initial Ir reduction amount (g / m 2 ) is a graph plotting

[0014] <Oxygen Evolution Electrode> Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments. One embodiment of the oxygen evolution electrode of the present invention comprises a substrate made of titanium or a titanium alloy, a first intermediate layer formed of a first mixed metal oxide containing titanium and tantalum and disposed on the substrate, and a catalyst layer formed of a second mixed metal oxide containing iridium and tantalum and disposed on the first intermediate layer. The oxygen evolution electrode of this embodiment comprises a catalyst layer formed of tantalum oxide and having a tantalum content of 1.2 to 2.5 g / m, which is disposed between the first intermediate layer and the catalyst layer. 2 The oxygen generating electrode of the present invention is described in detail below.

[0015] (Substrate) Fig. 1 is a schematic diagram showing one embodiment of the oxygen generating electrode of the present invention. The oxygen generating electrode 10 of the embodiment shown in Fig. 1 includes a substrate 2, a first intermediate layer 4 disposed on the substrate 2, and a catalyst layer 6 disposed above the first intermediate layer 4. The substrate 2 is formed of titanium or a titanium alloy. The overall shape of the substrate 2 is not particularly limited and can be appropriately designed depending on the application. Examples of the overall shape of the substrate include a plate shape, a rod (column) shape, and a mesh shape.

[0016] (First Intermediate Layer) The first intermediate layer 4 disposed on the substrate 2 is formed of a first mixed metal oxide ( FIG. 1 ). By providing such a first intermediate layer between the substrate and the catalyst layer, passivation of the titanium or titanium alloy substrate due to electrolysis can be suppressed and the substrate can be protected from corrosion. This improves durability and allows for an oxygen generating electrode capable of electrolysis for a longer period of time.

[0017] The first mixed metal oxide forming the first intermediate layer 4 is a mixed oxide of metals containing titanium (Ti) and tantalum (Ta). It is preferable that the metal elements constituting the first mixed metal oxide are substantially only titanium and tantalum. The thickness of the first intermediate layer is not particularly limited and can be set as desired. The thickness of the first intermediate layer may be, for example, 0.2 to 5 μm.

[0018] The first intermediate layer 4 can be formed, for example, by applying a coating liquid containing titanium, tantalum, and their salts in a desired ratio to the surface of a substrate to form a coating layer, followed by baking under appropriate temperature conditions (so-called pyrolysis). Alternatively, a desired first intermediate layer can be formed on a substrate by arc ion plating (AIP), sputtering, plasma spraying, or the like. Among these, the first intermediate layer is preferably a layer formed by arc ion plating (AIP). It is believed that a first intermediate layer formed by the AIP method has a smaller proportion of voids formed therein than a first intermediate layer 4 formed by other methods, and is more likely to have a relatively dense structure. Therefore, by providing a first intermediate layer formed by the AIP method, an oxygen generating electrode with further improved electrode performance can be obtained. It is practically difficult to identify the fine structure (shape, size, proportion, distribution, etc. of voids) of a first intermediate layer formed by the AIP method.

[0019] (Second Intermediate Layer) The oxygen generating electrode 10 of this embodiment further includes a second intermediate layer 5 formed of tantalum oxide, which is disposed between the first intermediate layer 4 and the catalytic layer 6 ( FIG. 1 ). In the case of a conventional electrode in which a catalytic layer formed of a mixed metal oxide containing iridium and tantalum is disposed directly on a substrate or an underlayer formed of a mixed metal oxide containing titanium and tantalum, iridium tends to segregate toward the substrate in the catalytic layer, while tantalum tends to segregate toward the electrode surface. That is, iridium, which is an active element, is distributed closer to the substrate in the catalytic layer, while tantalum is distributed closer to the electrode surface.

[0020] In contrast, when a second intermediate layer 5 formed of tantalum oxide is disposed between the first intermediate layer 4 and the catalytic layer 6, segregation of iridium toward the substrate side in the catalytic layer 6 is suppressed, and segregation of tantalum toward the electrode surface side is also suppressed. Consumption of iridium in the catalytic layer tends to proceed from the electrode surface side. Therefore, when focusing on the remaining amount of iridium in the catalytic layer 6 upon electrode degradation (e.g., when the catalytic activity is gradually lost and the electrode potential exceeds a desired value), it is expected that an electrode having a second intermediate layer 5 in which segregation of iridium toward the substrate side is suppressed will have a lower remaining amount of iridium than a conventional electrode in which iridium segregates toward the substrate side. In other words, an electrode having a second intermediate layer 5 consumes more iridium before electrode degradation than a conventional electrode, and therefore consumes iridium more efficiently. Therefore, when predicting the lifespan of an electrode having a second intermediate layer 5, the threshold value for the remaining amount of iridium upon electrode degradation can be set lower than that of a conventional electrode. This makes it possible to provide an oxygen generating electrode with a longer life that can be used for electrolysis over a long period of time.

[0021] The content of tantalum in the second intermediate layer 5 is 1.2 to 2.5 g / m 2 The content of tantalum in the second intermediate layer 5 is 1.2 to 2.3 g / m 2 It is preferable that the density is 1.5 to 2.3 g / m 2 More preferably, it is 1.5 to 2.0 g / m or more. 2 More preferably, it is 1.6 to 2.0 g / m 2 It is particularly preferable that the content of tantalum in the second intermediate layer is 1.2 g / m 2 On the other hand, if the content of tantalum in the second intermediate layer is less than 2.5 g / m, it becomes difficult to sufficiently extend the life of the oxygen generating electrode. 2 If it exceeds this value, the life of the oxygen generating electrode may be shortened.

[0022] (Catalyst Layer) The catalyst layer 6 is formed of a second mixed metal oxide containing iridium and tantalum ( FIG. 1 ). That is, the catalyst layer is formed of a second mixed metal oxide, which is a composite oxide containing iridium as an active element and tantalum as a polyvalent metal element. It is preferable that the metal elements constituting the second mixed metal oxide are essentially iridium and tantalum only. The coexistence of tantalum as a polyvalent metal element in the catalyst layer makes it possible to increase the conductivity, resulting in an oxygen generating electrode with a lower electrode potential. Furthermore, the use of tantalum makes it difficult for iridium as an active element to be consumed even when electrolysis is performed under acidic conditions such as sulfuric acid acidity, resulting in a catalyst layer with a long life and excellent durability.

[0023] The content of iridium in the catalyst layer is 3.0 to 30 g / m 2 It is preferable that the density is 5 to 20 g / m 2 It is more preferable that the content of iridium in the catalyst layer is within the above range, thereby achieving higher catalytic activity. Furthermore, the content of iridium in the catalyst layer is preferably 50 to 80 mass% based on the total amount of metal elements in the catalyst layer. By setting the content of iridium in the catalyst layer within the above range, it is possible to achieve higher catalytic activity. The type and content of metal elements in each layer, including the catalyst layer, can be measured and calculated by an analytical method such as X-ray fluorescence (XRF) analysis.

[0024] (Coating Layer) FIG. 2 is a schematic diagram showing another embodiment of the oxygen generating electrode of the present invention. The oxygen generating electrode 30 of the embodiment shown in FIG. 2 includes a substrate 2, a first intermediate layer 4 disposed on the substrate 2, and a catalytic layer 6 disposed above the first intermediate layer 4. The oxygen generating electrode 30 of this embodiment further includes a second intermediate layer 5 formed of tantalum oxide and disposed between the first intermediate layer 4 and the catalytic layer 6, and a coating layer 7 containing platinum (Pt) and disposed on the catalytic layer 6. Preferably, the metal element in the coating layer is substantially platinum alone. By providing such a coating layer on the catalytic layer, it is possible to reduce the consumption of iridium in the catalytic layer in the early stage of electrolysis, resulting in an oxygen generating electrode with a longer life that can be used for electrolysis over a long period of time.

[0025] The platinum content in the coating layer is 0.5 to 3.0 g / m 2 The platinum content in the coating layer is preferably 2.0 to 3.0 g / m 2 More preferably, it is 2.3 to 2.9 g / m 2 It is particularly preferable that the platinum content is 0.5 g / m 2 If the platinum content is less than 3.0 g / m, it may be difficult to sufficiently extend the life of the oxygen generating electrode. 2 If the thickness exceeds 1 μm, the effect obtained by providing the coating layer will reach a plateau and the cost will tend to be somewhat disadvantageous (see Figure 6). The thickness of the coating layer is not particularly limited and can be set arbitrarily. The thickness of the coating layer may be, for example, 0.5 to 5 μm.

[0026] (Use of oxygen generating electrode) The oxygen generating electrode of this embodiment has high conductivity, and even when electrolyzing acidic electrolyte such as sulfuric acid, the iridium in catalytic layer is not easily consumed, and has durability suitable for long-term electrolysis.Therefore, the oxygen generating electrode of this embodiment is useful as the anode (electrowinning anode) for the electrowinning process of non-ferrous metal such as copper (Cu), which is used in combination with the cathode (electrowinning cathode) for non-ferrous metal such as copper (Cu).Furthermore, when the applied current density is 10 kA / m 2It is useful as an oxygen generating electrode used in the following electrolytic processes.

[0027] <Method for manufacturing an electrode for oxygen generation> One embodiment of the method for manufacturing an electrode for oxygen generation of the present invention is a suitable method for manufacturing the above-mentioned electrode for oxygen generation. That is, the method for manufacturing an electrode for oxygen generation of this embodiment includes the steps of: disposing a first intermediate layer formed of a first mixed metal oxide containing titanium and tantalum on a substrate formed of titanium or a titanium alloy by arc ion plating; applying a coating liquid containing tantalum onto the first intermediate layer, and then performing heat treatment to form a first intermediate layer formed of a tantalum oxide and having a tantalum content of 1.2 to 2.5 g / m 2 and applying a catalyst precursor solution containing iridium and tantalum onto the second intermediate layer, followed by heat treatment to form a catalyst layer formed of a second mixed metal oxide containing iridium and tantalum. Hereinafter, the method for producing an oxygen generating electrode of the present invention will be described in detail.

[0028] A first intermediate layer formed of a first mixed metal oxide is disposed on a substrate by arc ion plating (AIP). The substrate may be subjected to a surface treatment such as blasting or etching, if necessary. By providing the first intermediate layer by AIP, as described above, it is possible to form a first intermediate layer having a relatively dense structure with a small proportion of voids formed therein.

[0029] To form a second intermediate layer on a first intermediate layer, a coating liquid containing tantalum or a tantalum salt, but not iridium, is first applied to the surface of the first intermediate layer to form a coating layer. Then, by baking under appropriate temperature conditions, a second intermediate layer formed of tantalum oxide can be formed. By repeating the application and baking of the coating liquid, the thickness of the second intermediate layer and the content of the metal element (Ta) can be controlled. The baking temperature is typically 400 to 600°C, preferably 450 to 550°C. The coating liquid does not contain titanium, and essentially contains only tantalum as a metal useful for oxygen generating electrodes.

[0030] To dispose a catalyst layer on the second intermediate layer, a coating liquid containing iridium, tantalum, and salts of these metals in the desired ratio is first applied to the surface of the second intermediate layer to form a coating layer. Then, the coating is baked under appropriate temperature conditions to form a catalyst layer formed from the second mixed metal oxide. The thickness and metal element content of the catalyst layer can be controlled by repeating the application and baking of the coating liquid. The baking temperature is typically 400 to 600°C, preferably 450 to 550°C.

[0031] By forming a catalytic layer on the second intermediate layer made of tantalum oxide in this way, segregation of iridium in the catalytic layer toward the substrate side is suppressed, as described above, and segregation of tantalum toward the electrode surface side is also suppressed. This is thought to be because, since the second intermediate layer does not contain iridium immediately after formation, even if a catalytic layer containing iridium is formed on it, distribution of iridium toward the substrate side within the catalytic layer is suppressed.

[0032] The method for producing an oxygen generating electrode according to this embodiment preferably further includes a step of applying a platinum-containing coating liquid onto the catalyst layer, followed by heat treatment to form a platinum-containing coating layer on the catalyst layer. To form a coating layer on the catalyst layer, a coating liquid containing platinum or a platinum salt is first applied to the surface of the catalyst layer, similar to the formation of the catalyst layer described above, to form a coating layer. The coating layer can then be formed on the catalyst layer by firing under appropriate temperature conditions. Repeated application and firing of the coating liquid can control the thickness of the formed coating layer and the content of the metal element (Pt). The firing temperature is typically 400 to 600°C, preferably 450 to 550°C.

[0033] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are by mass unless otherwise specified.

[0034] <Pretreatment of substrate and formation of first intermediate layer> A JIS Class I titanium plate was prepared. The surface of the titanium plate was dry-blasted using an iron grid (G120 size) and then annealed at 590°C for 60 minutes. The titanium plate was etched using 20% ​​hydrochloric acid at boiling temperature for 20 minutes and then washed to obtain a substrate. The obtained substrate was placed in an arc ion plating device using a Ti-Ta alloy target as the evaporation source, and a base layer (first intermediate layer) containing titanium and tantalum was formed on the surface of the substrate. The coating conditions are shown in Table 1.

[0035]

[0036] <Production of Oxygen Evolution Electrode> (Comparative Example 1) The substrate on which the first intermediate layer was formed was placed in an air-circulating electric furnace and heat-treated at 530°C for 180 minutes. 4 ) and tantalum pentachloride (TaCl 5 ) was dissolved in 10% hydrochloric acid to prepare a coating solution for the catalyst layer (Ir 65%-Ta 35%). The prepared coating solution for the catalyst layer was applied to the first intermediate layer and then dried at 60°C for 10 minutes. The product was placed in an air-circulating electric furnace and subjected to a pyrolysis treatment by heating at 520°C for 10 minutes, and then cooled in air. The cycle from application of the coating solution to cooling was repeated until the desired iridium content was achieved to form a catalyst layer, and an oxygen generating electrode having the layer structure shown in FIG. 3 was obtained.

[0037] (Examples 1 to 6, Comparative Examples 2 to 5) The substrate on which the first intermediate layer was formed was placed in an air-circulating electric furnace and heat-treated at 530°C for 180 minutes. 5 A coating solution for the second intermediate layer, obtained by dissolving 1.2 g / m² of tantalum in 10% hydrochloric acid, was applied onto the first intermediate layer, followed by drying at 60°C for 10 minutes. The first intermediate layer was placed in an air-circulating electric furnace, where it was subjected to a pyrolysis treatment by heating at 520°C for 10 minutes, and then cooled in air. The cycle from application of the coating solution to cooling was repeated until the desired tantalum content was achieved, thereby forming the second intermediate layer. Specifically, the tantalum content of the second intermediate layer in Examples 1 to 6 was 1.2 g / m². 2 , 1.5 g / m 2 , 1.8 g / m 2 , 2.0 g / m2 , 2.2 g / m 2 , 2.3 g / m 2 The tantalum content of the second intermediate layer in Comparative Examples 2 to 5 was 1.0 g / m 2 , 2.6 g / m 2 , 2.7 g / m 2 , 3.0 g / m 2 (All figures are target values.)

[0038] The coating liquid for the catalyst layer was applied to the second intermediate layer, and then dried at 60° C. for 10 minutes. The product was placed in an air-circulating electric furnace and subjected to a pyrolysis treatment by heating at 520° C. for 10 minutes, and then cooled in air. The cycle from application of the coating liquid to cooling was repeated until the desired iridium content was achieved, thereby forming a catalyst layer and obtaining an oxygen generating electrode having the layer structure shown in FIG.

[0039] (Example 7, Comparative Examples 6 and 7) The substrate on which the first intermediate layer was formed was placed in an air-circulating electric furnace and heat-treated at 530°C for 180 minutes. Next, the coating liquid for the second intermediate layer described above was applied onto the first intermediate layer, and then dried at 60°C for 10 minutes. The substrate was placed in an air-circulating electric furnace and subjected to a pyrolysis treatment by heating at 520°C for 10 minutes, and then cooled in air. The cycle from application of the coating liquid to cooling was repeated until the desired tantalum content was achieved, thereby forming a second intermediate layer. Specifically, the tantalum content of the second intermediate layer in Comparative Example 6, Example 7, and Comparative Example 7 was 1.0 g / m 2 , 2.0 g / m 2 , 3.0 g / m 2 (All figures are target values.)

[0040] The coating solution for the catalyst layer was applied to the second intermediate layer, and then dried at 60° C. for 10 minutes. The resulting product was placed in an air-circulating electric furnace and subjected to a pyrolysis treatment by heating at 520° C. for 10 minutes, followed by cooling in air. The cycle from application of the coating solution to cooling was repeated until the desired iridium content was achieved, thereby forming a catalyst layer.

[0041] Dinitrodiammineplatinum (Pt(NH 3 ) 2 (NO 2 ) 2) was dissolved in a 16 to 40% aqueous solution of nitric acid to prepare a coating solution for the coating layer. The prepared coating solution was applied to the catalyst layer and then dried at 60°C for 10 minutes. The catalyst layer was placed in an air-circulating electric furnace and subjected to a pyrolysis treatment by heating at 520°C for 10 minutes, followed by cooling in air. The cycle from application of the coating solution to cooling was repeated until the desired platinum content was achieved to form a coating layer, thereby obtaining an oxygen generating electrode having the layer structure shown in Figure 2. The platinum content of the coating layer was 1.1 g / m in all of Example 7 and Comparative Examples 6 and 7. 2 (All figures are target values.)

[0042] (Reference Examples 1 to 3) The substrate on which the first intermediate layer was formed was placed in an air-circulating electric furnace and heat-treated at 530°C for 180 minutes. The above-mentioned coating liquid for the catalyst layer was applied onto the first intermediate layer, and then dried at 60°C for 10 minutes. The substrate was placed in an air-circulating electric furnace and subjected to a pyrolysis treatment by heating at 520°C for 10 minutes, and then cooled in air. The cycle from application of the coating liquid to cooling was repeated until the desired iridium content was achieved to form a catalyst layer.

[0043] The coating solution for the coating layer was applied onto the catalyst layer, and then dried at 60°C for 10 minutes. The catalyst layer was placed in an air-circulating electric furnace, where it was subjected to a pyrolysis treatment by heating at 520°C for 10 minutes, and then cooled in air. The cycle from application of the coating solution to cooling was repeated until the desired platinum content was achieved, forming a coating layer, and an oxygen generating electrode having the layer structure shown in Figure 4 was obtained. Specifically, the platinum content in Reference Examples 1, 2, and 3 was 1.1 g / m, respectively. 2 , 2.3 g / m 2 , 2.9 g / m 2 (All figures are target values.)

[0044] The details of the oxygen generating electrodes obtained in Experimental Examples 1 to 7, Comparative Examples 1 to 7, and Reference Examples 1 to 3 are summarized in Table 2.

[0045]

[0046] <Evaluation 1> The cross sections of the oxygen generating electrodes obtained in Comparative Examples 1 to 5 and Examples 1 to 6 were analyzed using an electron probe microanalyzer (EPMA) to measure the distribution states of iridium and tantalum in the formed catalytic layers. As a result, it was confirmed that in the catalytic layer of the oxygen generating electrode obtained in Comparative Example 1 as a conventional example, iridium segregated toward the substrate side and tantalum segregated toward the electrode surface side. In contrast, it was confirmed that in the catalytic layers of the oxygen generating electrodes obtained in Comparative Examples 2 to 5 and Experimental Examples 1 to 6 in which a second intermediate layer was disposed, segregation of iridium and tantalum was suppressed, and in particular, segregation of iridium toward the substrate side was suppressed.

[0047] <Evaluation 2> Electrolysis was performed under the test conditions shown below using the oxygen generating electrodes obtained in Comparative Examples 1 to 5 and Examples 1 to 6 as anodes. The amount of iridium (Ir) in the electrode (catalytic layer) before and during the test was measured to determine the initial Ir consumption amount between 0 and 1,000 hours after the start of the test, and the Ir consumption rate between 1,000 and 4,000 hours after the start of the test was calculated. The initial Ir consumption amount was determined separately because the consumption rate up to approximately 1,000 hours after the start of the test differs from the consumption rate thereafter. Furthermore, using the obtained data, the predicted electrode life (0 hours to the time of electrode degradation) (h) of each anode was calculated using the following formula:

[0048] Electrode life (0 hours to electrode deterioration) (h) = (initial Ir amount - remaining Ir amount - initial Ir consumption amount) / Ir consumption rate + 1,000 Here, for comparison, the "initial Ir amount" of each anode is 7 g / m 2 Regarding the "initial Ir consumption amount," since the outermost layer in each of Comparative Examples 1 to 5 and Examples 1 to 6 is a catalyst layer containing iridium and tantalum, the average initial Ir consumption amount of each anode (0.71 g / m) was used for comparison. 2 In Comparative Examples 6 and 7 and Example 7, in which the outermost layer was a coating layer, the initial Ir consumption was suppressed by the coating layer, as will be described later, and therefore the measured initial Ir consumption was used as is.

[0049] The "Ir remaining amount" is the threshold for the amount of iridium remaining when the electrode has deteriorated (it can also be considered a deterioration determination value). As described above, the threshold for the Ir remaining amount in Examples 1 to 6 and Comparative Examples 2 to 5, which have a second intermediate layer, can be set lower than the threshold for Comparative Example 1, which does not have a second intermediate layer. Taking field data into consideration, the threshold for the electrode of Comparative Example 1 was set to 20% of the initial Ir amount (initial Ir amount was 7 g / m 2 Therefore, the remaining amount of Ir is 1.4 g / m 2 ), and the threshold voltage of the electrodes of Examples 1 to 6 and Comparative Examples 2 to 5 was set to 10% of the initial Ir amount (initial Ir amount was 7 g / m 2 Therefore, the remaining amount of Ir is 0.7 g / m 2 ), the predicted value of the electrode life (0 hours to electrode deterioration) (h) was calculated. The calculated predicted value was rounded to the nearest tenth. The calculation results of the predicted values ​​are shown in Table 3. In addition, the Ta amount (g / m 2 5 is a graph plotting predicted values ​​of electrode life (0 hours to electrode deterioration) (h) against the time of electrode deterioration.

[0050] As shown in Table 3, in Examples 1 to 6 and Comparative Examples 2 to 5 in which the second intermediate layer 5 was disposed, the tantalum content of the second intermediate layer was 1.2 g / m 2 , 1.5 g / m 2 , 1.8 g / m 2 , 2.0 g / m 2 , 2.2 g / m 2 , 2.3 g / m 2 The predicted electrode life values ​​of Examples 1 to 6, in which the tantalum content was about 1.8 g / m, clearly exceeded the predicted electrode life value of Comparative Example 1, which was a conventional example. As shown in the approximation curve of FIG. 5 based on the predicted electrode life values ​​of Examples 1 to 6 and Comparative Examples 2 to 5, 2 Above 2.5 g / m, the predicted electrode life value starts to decrease. 2 It can be said that the values ​​up to this point clearly exceed the predicted values ​​of Comparative Example 1. Therefore, when the tantalum content of the second intermediate layer 5 is 1.2 to 2.5 g / m 2 It was confirmed that the oxygen generating electrode having the above structure can be used for electrolysis for a longer period of time than the conventional electrode. [Test conditions] Electrolyte: 150 g / L sulfuric acid (H 2 SO 4) Aqueous solution Electrolysis temperature: 60°C Current density applied to anode: 10 kA / m 2

[0051] <Evaluation 3> Electrolysis was carried out under the test conditions shown below, using the oxygen generating electrodes obtained in Comparative Examples 1, 6, and 7 and Example 7 as anodes. The amount of iridium (Ir) in the electrode (catalytic layer) before and during the test was measured, and the predicted value of the electrode life (0 hours to when the electrode has deteriorated) (h) was calculated using the same method as in the above-mentioned evaluation (2). The calculated predicted value was rounded to the nearest ten. The calculation results of the predicted values ​​are shown in Table 3. As shown in Table 3, in Example 7 and Comparative Examples 6 and 7, in which a coating layer 7 was further disposed, the tantalum content of the second intermediate layer was 2.0 g / m 2 , 3.0 g / m 2 The predicted electrode life values ​​of Example 6 and Comparative Example 7, in which the tantalum content of the second intermediate layer was 1.2 to 2.5 g / m, exceeded the predicted electrode life values ​​of Example 4 and Comparative Example 5, in which the tantalum content of the second intermediate layer was equivalent but no coating layer 7 was provided. Note that the predicted electrode life values ​​of Comparative Example 6, Example 6, and Comparative Example 7 increased and then decreased as the tantalum content increased. Therefore, even for the oxygen generating electrode further provided with the coating layer 7, the predicted electrode life values ​​of Example 6 and Comparative Example 7 increased and then decreased as the tantalum content of the second intermediate layer 5 increased and then decreased. 2 It can be inferred that an electrode having such a coating layer can be used for electrolysis for a longer period of time than an electrode without a coating layer. [Test conditions] Electrolyte: 150 g / L sulfuric acid (H 2 SO 4 ) Aqueous solution Electrolysis temperature: 60°C Current density applied to anode: 10 kA / m 2

[0052]

[0053] <Evaluation 4> Electrolysis was carried out under the test conditions shown below, using the oxygen generating electrodes obtained in Comparative Example 1 and Reference Examples 1 to 3 as anodes. The amount of iridium (Ir) in the catalyst layer before and during the test was measured, and the initial reduction amount for each experimental example was calculated. Specifically, the reduction amounts were calculated after 500 hours and 1,000 hours from the start of the test, and the larger value was taken as the initial reduction amount, taking into account measurement errors. The results are shown in Table 4. In addition, the amount of Pt in the coating layer (g / m2 ) with respect to the initial Ir reduction amount (g / m 2 ) is plotted in a graph shown in Figure 6. As shown in Table 4, the initial loss of iridium in all of Reference Examples 1 to 3 in which coating layer 7 was provided was lower than the initial loss of iridium in Comparative Example 1, which was a conventional example. Note that, as shown in Figure 6, when the platinum content in coating layer 7 was about 0.5 g / m 2 If the initial platinum content is less than about 3.0 g / m, the initial loss of iridium is still large, and the effect of providing the coating layer 7 tends to be insufficient. 2 When the platinum content in the coating layer 7 exceeds 0.5 to 3.0 g / m, the increase in the initial decrease in the amount of iridium becomes slow, and the effect of providing the coating layer 7 reaches a plateau. 2 The initial loss of iridium can be more effectively reduced when the coating layer 7 is in the range of 0.5 to 3.0 g / m. The effect of the coating layer 7 is also considered to be exerted in an electrode in which the catalyst layer 6 is disposed on the second intermediate layer 5. Therefore, for an oxygen generating electrode further provided with the coating layer 7, when the platinum content in the coating layer 7 is 0.5 to 3.0 g / m, 2 It was confirmed that the electrode having the above platinum content can enjoy the effect of the coating layer 7 more effectively than the electrodes having different platinum contents.

[0054] In Reference Examples 1 to 3, the effect of reducing the initial loss of iridium in the catalyst layer 6 was confirmed when the coating layer 7 was provided without providing the second intermediate layer 5 between the first intermediate layer 4 and the catalyst layer 6. Even when the second intermediate layer 5 was provided between the first intermediate layer 4 and the catalyst layer 6, the effect of reducing the initial loss of iridium in the catalyst layer 6 was obtained by providing the coating layer 7 on the catalyst layer 6, similar to Reference Examples 1 to 3. [Test conditions] Electrolyte: 150 g / L sulfuric acid (H 2 SO 4 ) Aqueous solution Electrolysis temperature: 60°C Current density applied to anode: 10 kA / m 2

[0055]

[0056] The oxygen generating electrode of the present invention is suitable for applications where the current density applied in, for example, electrolytic copper foil manufacturing is 10 kA / m 2It is useful as an anode for use in the following electrowinning process:

[0057] 10, 20, 30, 40: Oxygen generating electrode 2: Substrate 4: First intermediate layer 5: Second intermediate layer 6: Catalyst layer 7: Coating layer

Claims

1. A substrate made of titanium or a titanium alloy; a first intermediate layer formed of a first mixed metal oxide containing titanium and tantalum, which is disposed on the substrate; and a catalyst layer formed of a second mixed metal oxide containing iridium and tantalum, which is disposed above the first intermediate layer. A catalyst layer formed of an oxide of tantalum, which has a tantalum content of 1.2 to 2.5 g / m, which is disposed between the first intermediate layer and the catalyst layer. 2 The oxygen evolution electrode further comprises a second intermediate layer comprising:

2. The oxygen generating electrode according to claim 1, further comprising a coating layer containing platinum, disposed on the catalyst layer.

3. The platinum content in the coating layer is 0.5 to 3.0 g / m 2 3. The electrode for oxygen evolution according to claim 2, wherein 4. The electrode for generating oxygen according to any one of claims 1 to 3, wherein the first intermediate layer is a layer formed by an arc ion plating method.

5. A process of disposing a first intermediate layer formed of a first mixed metal oxide containing titanium and tantalum on a substrate formed of titanium or a titanium alloy by arc ion plating; applying a coating solution containing tantalum but not containing iridium on the first intermediate layer, and then heat-treating the coating solution to form a tantalum oxide having a tantalum content of 1.2 to 2.5 g / m 2 and applying a catalyst precursor solution containing iridium and tantalum onto the second intermediate layer, followed by heat treatment to thereby form a catalyst layer formed of a second mixed metal oxide containing iridium and tantalum.

6. The method for producing an oxygen generating electrode according to claim 5, further comprising a step of applying a coating liquid containing platinum onto the catalyst layer, followed by heat treatment to place a coating layer containing platinum on the catalyst layer.