Pre-painted steel sheet
Patent Information
- Application Number
- MYPI2025008081
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-03
- Filing Date
- 2024-07-03
- Publication Date
- 2025-01-03
AI Technical Summary
Zinc-based plated steel sheets with organic coatings containing large beads face issues with bead detachment during coil winding or press processes, leading to contamination and design deterioration, and existing solutions do not adequately address productivity and scratch resistance concerns.
A prepainted steel sheet with a coating layer containing resin particles larger than the film thickness, where the particles are partially covered with a binder resin, maintaining a specific area ratio, thickness, and particle distribution to prevent detachment and deformation, while ensuring the coating's design and productivity.
The solution effectively prevents resin particle detachment and deformation, maintaining the coating's design quality and improving productivity by ensuring the coating's integrity and scratch resistance.
Smart Images

Figure PI2025008081_DRAWING_001 
Figure PI2025008081_DRAWING_002 
Figure PI2025008081_DRAWING_003
Abstract
Description
Pre-coated steel sheet
[0001] The present invention relates to a pre-coated steel sheet.
[0002] Metal sheets with high designability have come to be used for applications such as home appliances, building materials, and automobiles. Examples of such metal sheets with high designability include metal sheets with colored organic coatings and metal sheets with highly glossy surfaces. Among such metal sheets with designability, when a zinc-based plated steel sheet having various zinc-based plating layers is used as the material for the metal sheet, it is possible to realize a steel sheet that combines the excellent corrosion resistance inherent to zinc-based plated steel sheets with excellent designability.
[0003] In metal sheets or steel sheets having such high designability, the scratch resistance of the outermost surface of the metal sheets or steel sheets having such designability is important in order to maintain the excellent designability. Therefore, many proposals have been made so far regarding the scratch resistance of metal sheets or steel sheets having such designability.
[0004] For example, Patent Document 1 below proposes a technology for improving the scratch resistance of an organic coating on a zinc-based plated steel sheet having an organic coating by incorporating beads (hereinafter also referred to as "large particle size beads") having a particle size larger than the film thickness of the organic coating into the organic coating.
[0005] International Publication No. 2014 / 112544
[0006] However, when a zinc-based plated steel sheet having an organic coating containing large beads as proposed in Patent Document 1 is wound into a coil or subjected to a predetermined press processing, the large beads may fall off from the organic coating, thereby reducing the design quality of the organic coating. Furthermore, there is a concern that the large beads that fall off from the organic coating may contaminate various equipment used for winding into a coil or performing press processing, thereby hindering the processing. For these reasons, when handling an organic coating containing large beads, sufficient care must be taken, and there is room for further improvement in terms of improving productivity.
[0007] Furthermore, even if the large beads do not fall off when wound into a coil or subjected to a predetermined press processing, they may be deformed due to the coil winding tension or the pressure during press processing. If such deformation occurs, the organic coating in the deformed area becomes relatively flat, resulting in a partial change in gloss and a loss of the desired design. This loss of design due to a change in gloss is also known as pressure marks. As such, there is still room for further improvement in organic coatings containing large beads, even from the perspective of maintaining design.
[0008] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a pre-coated steel sheet that has a coating layer containing resin particles whose particle diameter is larger than the film thickness, while still being capable of further improving design and productivity.
[0009] In order to solve the above problems, the present inventors conducted extensive research and came up with the idea that if the surfaces of resin particles contained in a coating layer, which have a particle size larger than the average film thickness, could be coated to some extent with a binder resin, the resin particles could be prevented from falling off or deforming. Based on this idea, the present inventors conducted detailed research on the conditions for resin particles having a particle size larger than the average film thickness. As a result, the present inventors found that when the average particle size of the resin particles, the average film thickness of the coating layer, the thickness of the binder resin coating the surfaces of the resin particles, etc., satisfy certain conditions, it is possible to prevent the resin particles from falling off or deforming from the coating layer, thereby further improving the design and productivity of pre-coated steel sheets. The gist of the present invention, which was completed based on this finding, is as follows.
[0010] (1) A precoated steel sheet having a zinc-based plated steel sheet having a zinc-based plating layer, which is a plating layer containing at least zinc, located on the surface of a base steel sheet, and a coating layer located on the surface of the zinc-based plating layer, wherein the coating layer contains resin particles and a binder resin and a color pigment as film-forming components, and in a cross section obtained by cutting the coating layer at an arbitrary position in the thickness direction, the average value of the area ratio, which is the area ratio occupied by the resin particles, is within a range of 5 to 40%, and the average film thickness dA of the coating layer in a portion not containing the resin particles is within a range of 10 to 40 μm, and the average particle diameter φ of the resin particles is within a range of 10 to 40 μm. (2) A precoated steel sheet according to (1), wherein, in the cross section, 80% or more of the length along the outer periphery of the exposed resin particles is covered with the film-forming component. (3) Before and after applying a 30% tensile elongation to the pre-coated steel sheet, the surface of the coating layer is measured for the 60-degree specular gloss G defined in JIS Z 8741:1997. S (60 °) before and after the tensile elongation is applied. S(4) The precoated steel sheet according to (1) or (2), wherein the compressive modulus of the binder resin at 25° C. is in the range of 60 to 150 MPa, the compressive modulus of the resin particles at 25° C. is in the range of 60 to 250 MPa, and the compressive modulus of the binder resin at 25° C. is equal to or less than the compressive modulus of the resin particles at 25° C. (5) The precoated steel sheet according to claim 1 or 2, wherein the coating layer contains, as the resin particles, small-sized resin particles having an average particle size of 9 to 26 μm that gives a peak in a particle size range of 17±8 μm, and large-sized resin particles having an average particle size of 40 to 70 μm that gives a peak in a particle size range of 55±10 μm, when a particle size distribution is measured. (6) The precoated steel sheet according to (5), wherein the proportion CL of the small-particle resin particles is in the range of 5 to 30 mass% relative to the total solid mass of the coating layer, and the proportion CH of the large-particle resin particles is in the range of 5 to 30 mass% relative to the total solid mass of the coating layer. (7) The precoated steel sheet according to (5), wherein the ratio (CL / CH) of the proportion CL of the small-particle resin particles to the proportion CH of the large-particle resin particles is in the range of 0.5 to 1.5. (8) The precoated steel sheet according to (5), wherein the ratio (φL / φH) of the average particle diameter φL of the small-particle resin particles to the average particle diameter φH of the large-particle resin particles is in the range of 0.14 to 0.58. (9) The precoated steel sheet according to (5), wherein the compressive modulus of the small-diameter resin particles at 25°C is in the range of 60 to 250 MPa, and the compressive modulus of the large-diameter resin particles at 25°C is in the range of 60 to 250 MPa.
[0011] As described above, according to the present invention, it is possible to prevent resin particles from falling off from the coating layer and deformation, thereby further improving the design and productivity of the precoated steel sheet.
[0012] Fig. 1 is a schematic diagram for explaining an example of the structure of a pre-coated steel sheet according to an embodiment of the present invention. Fig. 2 is a schematic diagram for explaining an example of the structure of a pre-coated steel sheet according to the same embodiment. Fig. 3 is a schematic diagram for explaining an example of the structure of a pre-coated steel sheet according to the same embodiment. Fig. 4 is a schematic diagram for explaining an example of the structure of a pre-coated steel sheet according to the same embodiment. Fig. 5 is a schematic diagram for explaining a coating layer in the pre-coated steel sheet according to the same embodiment.
[0013] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and drawings, components having substantially the same functional configurations are designated by the same reference numerals, and redundant explanations will be omitted.
[0014] (Regarding Pre-painted Steel Sheet) <Structure of Pre-painted Steel Sheet> First, the structure of a pre-painted steel sheet according to an embodiment of the present invention will be described below with reference to Figures 1A to 1D. Figures 1A to 1D are schematic diagrams for explaining an example of the structure of a pre-painted steel sheet according to this embodiment. Here, in this embodiment, the pre-painted steel sheet means a plated steel sheet having a coating layer on its surface.
[0015] 1A , the pre-coated steel sheet 1 according to this embodiment includes a zinc-based plated steel sheet 10 and a coating layer 20 located on one surface of the zinc-based plated steel sheet 10. Here, the zinc-based plated steel sheet 10 includes a base steel sheet 11 serving as a substrate, and a zinc-based plating layer 13 located on the surface of the base steel sheet 11. Furthermore, the coating layer 20 according to this embodiment contains resin particles 201 in a dispersed state.
[0016] As shown schematically in FIG. 1B , in the precoated steel sheet 1 according to this embodiment, a coating layer 20 containing resin particles 201 is provided on one surface of a zinc-based plated steel sheet 10 serving as a substrate, and a coating layer 25 not containing resin particles 201 may be provided on the other surface of the zinc-based plated steel sheet 10.
[0017] As shown schematically in FIG. 1C , in the precoated steel sheet 1 according to this embodiment, a coating layer 20 containing resin particles 201 may be provided on both surfaces of a zinc-based plated steel sheet 10 serving as a substrate.
[0018] Furthermore, as schematically shown in FIG. 1D , the precoated steel sheet 1 according to this embodiment may further include, as necessary, an anti-rust coating layer 30 as an example of a coating layer containing an anti-rust pigment and a resin between the zinc-based plated steel sheet 10 and the coating layer 20.
[0019] While FIG. 1D illustrates a case in which a rust-preventive coating layer 30 is provided on the pre-coated steel sheet 1 having the structure shown in FIG. 1A , a rust-preventive coating layer 30 may also be provided at least between the zinc-based plated steel sheet 10 and the coating layer 20 or between the zinc-based plated steel sheet 10 and the coating layer 25 on the pre-coated steel sheet 1 having the structure shown in FIG. 1B or 1C .
[0020] Hereinafter, each configuration of the pre-coated steel sheet 1 as shown in FIGS. 1A to 1D will be described in detail.
[0021] [Regarding the zinc-based plated steel sheet 10] As described above, the zinc-based plated steel sheet 10 used as the substrate of the pre-coated steel sheet 1 according to this embodiment has a base steel sheet 11 and a zinc-based plating layer 13 located on the surface of the base steel sheet 11.
[0022] As the base steel plate 11, various steel plates can be used, such as Al-killed steel, ultra-low carbon steel containing Ti, Nb, etc., and high-strength steel in which ultra-low carbon steel further contains strengthening elements such as P, Si, Mn, etc.
[0023] Examples of the zinc-based plating layer 13 include zinc-based platings such as zinc plating, zinc-nickel plating, zinc-iron plating, zinc-chromium plating, zinc-aluminum plating, zinc-titanium plating, zinc-magnesium plating, zinc-manganese plating, zinc-aluminum-magnesium plating, and zinc-aluminum-magnesium-silicon plating. The zinc-based plating may contain small amounts of dissimilar metal elements or impurities, such as cobalt, molybdenum, tungsten, nickel, titanium, chromium, aluminum, manganese, iron, magnesium, lead, bismuth, antimony, tin, copper, cadmium, or arsenic, or may have inorganic substances such as silica, alumina, or titania dispersed therein. The zinc-based plating may also be a multi-layer plating that combines the above-mentioned plating with other types of plating (e.g., iron plating, iron-phosphorus plating, nickel plating, cobalt plating, etc.). The plating method is not particularly limited, and various known plating methods, such as electroplating, hot-dip plating, vapor deposition plating, dispersion plating, and vacuum plating, may be used.
[0024] Among such zinc-based platings, it is particularly preferable to use a zinc-aluminum-magnesium alloy plating as the zinc-based plating layer 13, and it is more preferable to use a zinc-aluminum-magnesium-silicon alloy plating layer containing 4 to 22 mass % of Al, 1 to 10 mass % of Mg, 0.0001 to 2.0000 mass % of Si, with the balance being Zn and impurities.
[0025] [Al: 4 to 22 mass%] By setting the Al content to 4 mass% or more, it is possible to further improve the corrosion resistance of the steel sheet. The Al content is more preferably 5 mass% or more. On the other hand, by setting the Al content to 22 mass% or less, it is possible to further improve the corrosion resistance of the steel sheet while suppressing saturation of the corrosion resistance improvement effect as described above. The Al content is more preferably 16 mass% or less.
[0026] [Mg: 1 to 10 mass%] By adjusting the Mg content to 1 mass% or more, the corrosion resistance of the steel sheet can be further improved. The Mg content is more preferably 2 mass% or more. Meanwhile, by adjusting the Mg concentration in the coating bath used to form the coating layer so that the Mg content in the zinc-based coating layer 13 after production is 10 mass% or less, it is possible to stabilize the generation of dross in the coating bath and stably produce coated steel sheets. It is more preferable to adjust the Mg concentration in the coating bath used to form the zinc-based coating layer 13 so that the Mg content in the zinc-based coating layer 13 after production is 5 mass% or less.
[0027] [Si: 0.0001 to 2.0000 mass%] By setting the Si content to 0.0001 mass% or more, it is possible to further improve the adhesion of the zinc-based plating layer 13 (more specifically, the adhesion between the base steel sheet 11 and the zinc-based plating layer 13). On the other hand, by setting the Si content to 2.0000 mass% or less, it is possible to further improve the adhesion of the zinc-based plating layer 13 while suppressing saturation of the adhesion-improving effect of the zinc-based plating layer 13. The Si content is more preferably 1.6000 mass% or less.
[0028] Furthermore, the zinc-based plating layer 13 according to this embodiment may contain 1 mass % or less of elements such as Fe, Sb, Pb, or the like, either singly or in combination, in place of a portion of the remaining Zn.
[0029] Examples of the zinc-based plated steel sheet 10 provided with the zinc-based plating layer 13 having the above-described chemical composition include a hot-dip zinc-aluminum-magnesium alloy plated steel sheet having a Zn-6%Al-3%Mg alloy plating layer and a hot-dip zinc-aluminum-magnesium-silicon alloy plated steel sheet (for example, "Superdyma (registered trademark)" manufactured by Nippon Steel Corporation) such as a plated steel sheet having a Zn-11%Al-3%Mg-0.2%Si alloy plating layer.
[0030] The coating weight of the zinc-based coating layer 13 as described above is 30 g / m in total on both sides of the steel sheet. 2 or more (i.e., 15 g / m per side) 2It is preferable that the coating amount is 30 g / m or more. 2 By setting the coating weight at or above this level, it is possible to reliably ensure the corrosion resistance of the zinc-based plated steel sheet 10. More preferably, the coating weight is 40 g / m in total on both sides of the steel sheet. 2 On the other hand, the coating weight on both sides of the steel sheet is 600 g / m 2 or less (i.e., 300 g / m per side) 2 It is preferable that the coating amount is 600 g / m or less. 2 By setting the coating weight to 550 g / m or less, it is possible to further improve corrosion resistance while ensuring the smoothness of the surface of the zinc-based coating layer 13. More preferably, the coating weight is 550 g / m in total on both sides of the steel sheet. 2 The following is the result.
[0031] Here, the thickness of the zinc-based plated steel sheet 10 as described above is not particularly limited, and may be set appropriately depending on the mechanical strength (e.g., tensile strength, etc.) and workability required of the pre-coated steel sheet 1 according to this embodiment.
[0032] [Regarding the Coating Layer 20] Next, the coating layer 20 of the precoated steel sheet 1 according to this embodiment will be described. The coating layer 20 according to this embodiment is provided on at least one surface of the zinc-based plated steel sheet 10. As illustrated in FIGS. 1A to 1D , the coating layer 20 according to this embodiment is a coating layer in which resin particles 201 are present in a dispersed state in a binder resin and a color pigment as film-forming components 203. Furthermore, the coating layer 20 according to this embodiment may further contain various additives such as a crosslinking agent in addition to the resin particles 201 and film-forming components 203 described above.
[0033] In the pre-coated steel sheet 1 according to this embodiment, resin particles 201 are dispersed in the film-forming component 203 in the coating layer 20, and in addition, these resin particles 201 satisfy the conditions described in detail below. As a result, in the pre-coated steel sheet 1 according to this embodiment, the binder resin as the film-forming component 203 achieves predetermined corrosion resistance and scratch resistance. Furthermore, in the pre-coated steel sheet 1 according to this embodiment, the pre-coated steel sheet 1 as a whole achieves excellent design that combines a grained appearance and a matte appearance, while making it possible to prevent the occurrence of pressure marks caused by the coating layer in deformed portions becoming relatively flat.
[0034] <Regarding the Resin Particles 201> In the coating layer 20 according to this embodiment, it is more preferable that the resin particles 201 have predetermined toughness and ductility. The resin particles 201 having predetermined toughness and ductility can mitigate impacts applied to the coating layer 20. As a result, in the pre-coated steel sheet 1 according to this embodiment, the scratch resistance of the coating layer 20 can be further improved. Furthermore, the resin particles 201 having predetermined toughness and ductility can more effectively prevent the occurrence of pressure marks caused by the binder resin in deformed areas becoming relatively flat. Furthermore, even if the coating layer 20 is scratched, the scratch can be prevented from reaching the zinc-based plated steel sheet 10, thereby maintaining the corrosion resistance of the pre-coated steel sheet 1.
[0035] In the coating layer 20 according to this embodiment, particles made of various materials can be used as the resin particles 201 as long as they have predetermined toughness and ductility. However, from the viewpoint of having better toughness and ductility, it is more preferable to use organic resin particles made of an organic resin.
[0036] Examples of organic resin particles used as the particles 201 include resin particles made of acrylic resin, resin particles made of polyester resin, resin particles made of urethane resin, resin particles made of fluorine resin, resin particles made of silicone resin, and resin particles made of polyolefin resin. Among these, it is more preferable to use resin particles made of urethane resin or resin particles made of acrylic resin as the resin particles 201, from the viewpoint of more easily achieving the desired toughness and ductility.
[0037] Furthermore, when resin particles made of urethane-based resin or acrylic-based resin as described above are used as the resin particles 201, it is preferable that the resin constituting these resin particles exhibits a predetermined glass transition temperature Tg.
[0038] More specifically, when resin particles made of a urethane resin are used as the resin particles 201, the glass transition temperature Tg of the urethane resin is preferably within a range of −40° C. to 40° C. When resin particles made of an acrylic resin are used as the resin particles 201, the glass transition temperature Tg of the acrylic resin is preferably within a range of 40° C. to 160° C.
[0039] When the constituent resin of the resin particles used as the resin particles 201 has the above-mentioned glass transition temperature Tg, the resin particles 201 exhibit even more preferable toughness and ductility, and even if an external force is applied to the resin particles 201 and the resin particles 201 are deformed, the resin particles 201 can quickly restore their shape before the impact was applied. This makes it possible to further prevent the occurrence of pressure marks caused by the binder resin in the deformed portion becoming relatively flat.
[0040] Furthermore, by using resin particles made of an acrylic resin having the above-mentioned glass transition temperature Tg as the resin particles 201, it is possible to prevent the occurrence of pressure marks as described above at a lower cost than when using resin particles made of a urethane resin having the above-mentioned glass transition temperature Tg.
[0041] When resin particles made of a urethane-based resin are used as the resin particles 201, the glass transition temperature Tg of the urethane-based resin is more preferably −10° C. or higher. Furthermore, the glass transition temperature Tg of the urethane-based resin is more preferably 20° C. or lower. Furthermore, when resin particles made of an acrylic-based resin are used as the resin particles 201, the glass transition temperature Tg of the acrylic-based resin is more preferably 40° C. or higher. Furthermore, the glass transition temperature Tg of the acrylic-based resin is more preferably 120° C. or lower.
[0042] The glass transition temperature Tg can be determined, for example, by thermomechanical analysis (TMA), in which a needle is inserted into the surface of a particle to be measured, a certain temperature change is applied, and a change in thermal expansion of the particle to be measured is measured.
[0043] In the pre-coated steel sheet 1 according to this embodiment, the content of the resin particles 201 in the coating layer 20 is 1.0 to 15.0 mass% per side, relative to the total solid mass of the coating layer 20. If the content of the resin particles 201 in the coating layer 20 is less than 1.0 mass% per side, the content of the resin particles 201 is too low to achieve the desired design, which is to combine a grained appearance and a matte appearance. If the content of the resin particles 201 in the coating layer 20 is 1.0 mass% or more per side, the desired design can be achieved as a pre-coated steel sheet 1. The content of the resin particles 201 in the coating layer 20 per side is preferably 2.0 mass% or more, and more preferably 3.0 mass% or more.
[0044] On the other hand, if the content of the resin particles 201 in the coating layer 20 exceeds 15.0% by mass per side, the content of the resin particles 201 becomes too high, and as a result, it is not possible to achieve the scratch resistance required of the coating layer 20. By making the content of the resin particles 201 in the coating layer 20 15.0% by mass or less per side, it becomes possible to achieve the desired design while ensuring the scratch resistance required of the coating layer 20. The content of the resin particles 201 in the coating layer 20 per side is preferably 12.0% by mass or less, and more preferably 9.0% by mass or less.
[0045] <<Film-forming component 203>> The coating layer 20 according to this embodiment contains a binder resin and a color pigment as film-forming components in addition to the resin particles 201. The film-forming component 203 will be described in detail below.
[0046] Binder Resin The binder resin, which is one of the film-forming components 203 contained in the coating layer 20 according to this embodiment, can be any material that functions as a binder for the resin particles 201. However, from the viewpoints of ease and cost of production, as well as corrosion resistance and scratch resistance, it is preferable to use various organic resins as the binder resin. Examples of such binder resins include acrylic resins, polyester resins, urethane resins, and fluorine-based resins.
[0047] Furthermore, in the coating layer 20 according to this embodiment, it is more preferable to select, as the binder resin, the same type of resin as that of the resin particles 201 used. This further improves the affinity between the resin particles 201 and the binder resin, and makes it possible to further improve the adhesion and barrier properties of the coating layer 20.
[0048] Coloring Pigment The coloring pigment contained in the coating layer 20 according to this embodiment, which serves as one type of film-forming component 203, is not particularly limited, and various known coloring agents can be used depending on the color tone desired for the coating layer 20. Examples of such coloring agents include aluminum pigment, titanium oxide, zinc oxide, zirconium oxide, calcium carbonate, barium sulfate, kaolin clay, carbon black, iron oxide, Hansa Yellow, pyrazolone orange, phthalocyanine, and azo pigment carbon black. The content thereof can also be set appropriately, and may be, for example, about 3 to 60 mass %.
[0049] ◇Other Components The coating layer 20 according to this embodiment may contain various additives such as a crosslinking agent, as needed, in addition to the resin particles 201 described above and the binder resin and coloring pigment as the film-forming components 203.
[0050] Furthermore, the organic resin coating layer 20 according to this embodiment may further contain additives such as anti-rust pigments, extender pigments, surface-modified metal powders or glass powders, dispersants, leveling agents, waxes, aggregates, or dilution solvents, as needed, within the range that does not impair the above-described effects.
[0051] When the coating layer 20 contains an anti-rust pigment, the content thereof is preferably, for example, about 1 to 15 mass %. The anti-rust pigment used may be any of various known anti-rust pigments.
[0052] <Compressive modulus of resin particles 201 and binder resin> In the coating layer 20 according to this embodiment, it is preferable that the compressive modulus of the resin particles 201 at 25°C is in the range of 60 to 250 MPa, the compressive modulus of the binder resin at 25°C is in the range of 60 to 150 MPa, and the compressive modulus of the binder resin at 25°C is equal to or less than the compressive modulus of the resin particles 201 at 25°C.
[0053] When the compressive moduli at 25°C of the resin particles 201 and the binder resin satisfy all of the above relationships, when an external force is applied to the resin particles 201 and the resin particles are deformed, the binder resin can more easily follow the deformation of the resin particles 201 (in other words, the binder resin can more easily deform in accordance with the deformation of the resin particles 201). As a result, the formation of excess voids between the resin particles 201 and the binder resin is prevented, and the adhesion and barrier properties of the coating layer 20 are further improved.
[0054] Here, the compressive elastic modulus of the resin particles 201 at 25°C is more preferably 90 MPa or more. The compressive elastic modulus of the resin particles 201 at 25°C is more preferably 210 MPa or less. The compressive elastic modulus of the binder resin at 25°C is more preferably 80 MPa or more. The compressive elastic modulus of the binder resin at 25°C is more preferably 130 MPa or less.
[0055] The compressive modulus of elasticity at 25°C of the resin particles 201 and the binder resin can be determined by focusing on a cross section obtained by cutting the coating layer 20 according to this embodiment in the thickness direction and measuring the compressive stress-strain curves for each of the resin particles 201 and the binder resin. More specifically, in accordance with JIS K 7181:2011, a nanoindenter is pressed into the section of interest at a location corresponding to the resin particles 201 and a location corresponding to the binder resin, and the load and displacement are measured. The measurement temperature is 25°C. From this measurement, compressive stress-strain curves can be obtained for each of the resin particles 201 and the binder resin. From the obtained compressive stress-strain curves, the compressive modulus of elasticity of the resin particles 201 and the binder resin can be calculated in accordance with JIS K 7181:2011.
[0056] The above-described measurements are carried out at least 10 locations for each of the resin particles 201 and the binder resin, and the average value of the obtained multiple compressive elastic moduli is taken as the compressive elastic modulus of the resin particles 201 and the binder resin of interest.
[0057] <Regarding the state of presence of resin particles 201 in coating layer 20> Next, the distribution state of the resin particles 201 in the coating layer 20 according to this embodiment will be described in detail with reference to Fig. 2. Fig. 2 is an explanatory diagram for explaining the coating layer in the pre-coated steel sheet according to this embodiment.
[0058] As mentioned previously, in the precoated steel sheet 1 according to this embodiment, resin particles 201 are present in a dispersed state in film-forming components 203, such as binder resins and color pigments, that constitute the coating layer 20. In discussing the state of existence of these resin particles 201, attention will be focused below on a cross section obtained by cutting the coating layer 20 according to this embodiment at an arbitrary position in the thickness direction, as schematically shown in FIG. 2. Then, this cross section will be observed with an electron microscope (more specifically, with a field emission scanning electron microscope (FE-SEM)) to discuss the state of existence of the resin particles 201.
[0059] More specifically, in a cross section obtained by cutting the coating layer 20 at an arbitrary position in the thickness direction, a region having a length of 400 μm in a direction perpendicular to the thickness direction (hereinafter also referred to as the width direction) is defined as the observation field region for one microscope observation, and 10 such observation field regions are arbitrarily set within the cross section of interest. Then, based on the measurement results obtained at the 10 positions, a feature quantity representing the state of existence of the resin particles 201 is calculated as described below.
[0060] ◇Average area ratio of resin particles 201 in cross section In the cross section described above in the coating layer 20 according to this embodiment, the average value of the area ratio (i.e., the average area ratio), which is the area proportion occupied by the resin particles 201, is in the range of 5 to 40%.
[0061] Here, the average area ratio is calculated as follows. That is, in the cross section of interest, a certain observation field region (length in the width direction: 400 μm) is focused on. In this case, the magnification of the FE-SEM may be set to an appropriate magnification (for example, about 300x) so that a coating layer 400 μm long in the width direction fits within one field of view. Then, the area ratio of the resin particles 201 to the total area of the coating layer in the observation field region of this size (i.e., area ratio) is calculated using various functions implemented in the electron microscope, image processing, etc. In this case, if only a portion of a certain resin particle 201 is present in the field of view, rather than the entire particle, the area ratio of the particle portion present in the field of view is calculated. By performing this observation on 10 arbitrary observation field regions, 10 measured values of the area ratio of the resin particles 201 can be obtained. The average of the 10 measured values obtained in this way is calculated to be the average area ratio of the resin particles 201 in the cross section. Thus, the average area ratio is the average value of the area ratio of the resin particles to the total area of the coating layer in the 10 observation field regions.
[0062] If the average area ratio of the resin particles 201 in the cross section is less than 5%, the presence ratio of the resin particles 201 is too low and the desired design cannot be achieved. If the average area ratio of the resin particles 201 is 5% or more, it becomes possible to achieve an excellent design that combines a grained appearance and a matte appearance. The average area ratio of the resin particles 201 in the cross section is preferably 8% or more, and more preferably 10% or more.
[0063] On the other hand, if the average area ratio of the resin particles 201 in the cross section exceeds 40%, the presence ratio of the resin particles 201 is too high, and as a result, not only cannot the scratch resistance required of the coating layer 20 be realized, but also the desired design (particularly, a matte appearance) cannot be realized. By making the average area ratio of the resin particles 201 40% or less, it becomes possible to realize the scratch resistance required of the coating layer 20 while also achieving the desired design. The average area ratio of the resin particles 201 in the cross section is preferably 38% or less, and more preferably 35% or less.
[0064] Average film thickness dA of the coating layer 20 in portions not containing resin particles 201 In the coating layer 20 according to this embodiment, the average film thickness dA of the coating layer 20 in portions not containing resin particles 201 in the cross section described above is within the range of 10 to 40 μm. If the average film thickness dA of the coating layer 20 in portions not containing resin particles 201 in the cross section is less than 10 μm, the thickness of the coating layer 20 is too thin and the desired corrosion resistance cannot be achieved. By making the average film thickness dA 10 μm or more, the corrosion resistance required for the pre-coated steel sheet 1 according to this embodiment can be achieved. The average film thickness dA is preferably 13 μm or more, and more preferably 15 μm or more.
[0065] On the other hand, if the average film thickness dA of the coating layer 20 in the cross section not containing the resin particles 201 exceeds 40 μm, the thickness of the coating layer 20 becomes too thick, which is undesirable as it reduces the adhesion of the coating layer 20. By setting the average film thickness dA to 40 μm or less, it is possible to achieve the desired corrosion resistance while ensuring the adhesion of the coating layer 20. The average film thickness dA is preferably 30 μm or less, and more preferably 25 μm or less.
[0066] The average film thickness dA of the coating layer 20 in the cross section not containing the resin particles 201 is determined by the following procedure. First, in one observation field of view of interest, the thickness of the coating layer 20 in the portion not containing the resin particles 201 is measured at 10 locations. In this case, the thickness of the coating layer 20 in the portion not containing the resin particles 201 may be measured using a length measurement function or the like implemented in the FE-SEM. The average value of the obtained 10 measurements is then calculated and used as the average thickness of the coating layer 20 in the observation field of view of interest. The above-mentioned operation is performed for 10 arbitrary observation field of view areas, and the average values obtained from each observation field of view area are further averaged by the number of fields of view. The value obtained in this manner is used as the average film thickness dA of the coating layer 20 in the portion not containing the resin particles 201.
[0067] In one observation field of view of interest, as illustrated in FIG. 2, at four locations where the resin particles 201 are not present, the thickness dA 1 , dA2 , dA 3 , dA 4 In this case, the average thickness of the coating layer 20 in one observation field of view area of interest is (1 / 4) × (dA 1 +dA 2 +dA 3 +dA 4 Such observation is performed for any 10 observation field regions, and the obtained average values are further averaged by the number of fields, thereby obtaining the average film thickness dA of the coating layer 20 in the portion not containing the resin particles 201.
[0068] Relationship between the average particle diameter φ of the resin particles 201 and the average film thickness dA of the coating layer 20 In the above-described cross section of the coating layer 20 according to this embodiment, the average particle diameter φ of the resin particles 201 is 4.0 times or less the average film thickness dA determined as described above. In other words, in the coating layer 20 according to this embodiment, the relationship φ≦4.0×dA holds.
[0069] In the coating layer 20 according to this embodiment, if the average particle size φ of the resin particles 201 in the cross section described above is more than 4.0 times the average film thickness dA of the coating layer 20, the average particle size φ of the resin particles 201 will be too large relative to the average film thickness dA, making it difficult for the resin particles 201 to be stably held by the coating layer 20. As a result, the resin particles 201 will be prone to falling off, making it impossible to achieve the desired design. The ratio (φ / dA) of the average particle size φ to the average film thickness dA is preferably 3.8 or less, and more preferably 3.5 or less.
[0070] In the coating layer 20 according to this embodiment, the average particle size φ of the resin particles 201 is preferably within the range of 9 to 70 μm. By setting the average particle size φ of the resin particles 201 within the range of 9 to 70 μm, the scratch resistance required for the coating layer 20 can be more preferably achieved, and the desired design can be more preferably achieved.
[0071] The average particle diameter φ of the resin particles 201 is more preferably 13 μm or more, and even more preferably 17 μm or more. The average particle diameter φ of the resin particles 201 is more preferably 60 μm or less, and even more preferably 55 μm or less.
[0072] The average particle size φ of the resin particles 201 in the cross section as described above is determined by the following procedure. First, in a cross section obtained by cutting the coating layer 20 at an arbitrary position, focus is placed on one arbitrary observation area as described above. In the observation area, the circle-equivalent diameters of the resin particles 201 present in the area are measured. Then, the average value of the measured circle-equivalent diameters in the observation area of interest is calculated. This measurement is performed on 10 arbitrary observation field areas, and the average values obtained from each observation field area are further averaged by the number of fields of view. The value obtained in this way is the average particle size φ of the resin particles 201.
[0073] In one observation field of view of interest, as shown in FIG. 2, three resin particles 201 are present in the field of view, and the equivalent circle diameter of each resin particle 201 is φ 1 , φ 2 , φ 3 In this case, the average value of the circle-equivalent diameter of the resin particles 201 in the observation field of view is (1 / 3)×(φ 1 +φ 2 +φ 3 Such measurements are performed on 10 arbitrary observation field regions in the specified cross section, and the obtained average values are further averaged by the number of fields, thereby obtaining the average particle diameter φ of the resin particles 201.
[0074] The value of the ratio (φ / dA) of the average particle diameter φ to the average film thickness dA is preferably 0.2 or more, more preferably 0.3 or more, even more preferably 1.0 or more, and even more preferably more than 1.0. This is because, when the average particle diameter φ is less than 0.2 of the average film thickness dA of the coating layer 20, the average particle diameter φ of the resin particles 201 is too small relative to the average film thickness dA, so that the resin particles 201 are completely buried in the coating layer 20, making it difficult for the resin particles 201 to contribute to the surface unevenness, and as a result, the desired design cannot be achieved.
[0075] Average Substantial Film Thickness dB of Coating Layer 20 In the above-described cross section of the coating layer 20 according to this embodiment, attention is focused on the portion containing the resin particles 201. In the portion of the coating layer 20 containing the resin particles 201, the thickness obtained by subtracting the thickness of the portion corresponding to the resin particles 201 from the total thickness of the coating layer 20 including the resin particles 201 will be referred to as the substantive film thickness of the coating layer 20 in the portion containing the resin particles 201.
[0076] Here, the total thickness of the coating layer 20 containing the resin particles 201 is defined as the length from the interface of the coating layer 20 on the zinc-based plated steel sheet 10 side to the surface of the coating layer 20 at the position of the portion containing the resin particles 201 in the cross section (the length to the surface of the coating layer 20 in a direction parallel to the surface normal of the zinc-based plated steel sheet 10). The thickness of the portion corresponding to the resin particles 201 is defined as the sum of the lengths of the portions corresponding to the resin particles 201 in a direction parallel to the surface normal of the zinc-based plated steel sheet 10 at the location of interest in the total thickness as described above.
[0077] When the average value of the substantial film thickness in the portion containing the resin particles 201 as defined above is referred to as the average substantial film thickness dB, this average substantial film thickness dB is within the range of 4 to 30 μm.
[0078] In the coating film layer 20 according to this embodiment, if the average substantial film thickness dB of the coating film layer 20 is less than 4 μm in the cross section described above, the amount of film-forming component 203 present in the portion where the resin particles 201 are present will be too small, resulting in the resin particles 201 being prone to falling off and the desired design properties not being achieved. Furthermore, if the amount of film-forming component 203 present is too small, the corrosion resistance and scratch resistance required of the coating film layer 20 will not be achieved. By ensuring that the average substantial film thickness dB of the coating film layer 20 is 4 μm or more, it is possible to achieve the desired design properties while also achieving the corrosion resistance and scratch resistance required of the coating film layer 20. The average substantial film thickness dB of the coating film layer 20 is preferably 5 μm or more, and more preferably 7 μm or more.
[0079] On the other hand, in the cross section of the coating film layer 20 according to this embodiment, if the average substantial film thickness dB of the coating film layer 20 exceeds 30 μm, the amount of film-forming component 203 present in the portion where the resin particles 201 are present will be too large, making it impossible to achieve the desired design (particularly, a matte appearance). By ensuring that the average substantial film thickness dB of the coating film layer 20 is 30 μm or less, it becomes possible to achieve the desired design. The average substantial film thickness dB of the coating film layer 20 is preferably 28 μm or less, and more preferably 25 μm or less.
[0080] The above-described average substantial film thickness dB in a cross section is determined by the following procedure. First, in a cross section obtained by cutting the coating layer 20 at an arbitrary position, attention is paid to one arbitrary observation region as described above. In the observation region, attention is paid to an arbitrary position where a resin particle 201 is present, and the total thickness of the coating layer 20 and the thickness of the portion corresponding to the resin particle 201 are measured. The two obtained measurements are used to perform a subtraction of (total thickness of the coating layer 20 - thickness of the portion corresponding to the resin particle 201), thereby obtaining the substantial film thickness of the coating layer 20 at the position of interest. Such measurements and calculations are performed at 10 arbitrary positions in the observation region of interest. The obtained multiple substantial film thickness measurements are averaged by the number of observation positions to obtain the average substantial film thickness in the observation region of interest. Such measurements are performed at 10 arbitrary observation field regions, and the average values obtained from each observation field region are further averaged by the number of fields of view. The value obtained in this manner is designated as the average substantial film thickness dB of the coating layer 20.
[0081] In one observation field of view of interest, it is assumed that three resin particles 201 are present in the field of view, as shown in Fig. 2. When focusing on the spherical resin particle 201 located on the far left, the thickness corresponding to the resin particle 201 is φ, which is the particle diameter of the resin particle 201. 1 At this time, the total thickness of the coating layer 20 is dT 1 If so, the actual film thickness dB 1 is dT 1 -φ 1 Similarly, when attention is paid to the spherical resin particle 201A located in the center of FIG. 2, the thickness corresponding to the resin particle 201A is calculated by multiplying the particle diameter φ of the resin particle 201A by 1 / 2. 2 At this time, the total thickness of the coating layer 20 is dT 2 If so, the actual film thickness dB 2 is dT 2 -φ 2 Similarly, when attention is paid to the spherical resin particle 201B located at the rightmost side of FIG. 2, the thickness corresponding to the resin particle 201B is φ, which is the particle diameter of the resin particle 201B. 3At this time, the total thickness of the coating layer 20 is dT 3 If so, the actual film thickness dB 3 is dT 3 -φ 3 By performing such measurements at any 10 points in the observation area, it is possible to obtain the average value of the substantial membrane thickness in the observation area of interest.
[0082] ◇Average number ratio of exposed resin particles In the cross section of the coating film layer 20 according to this embodiment, among the resin particles 201, those having a portion on the outer periphery that is not covered with a film-forming component 203 having a thickness of 1 μm or more are referred to as exposed resin particles.
[0083] Such exposed resin particles include not only resin particles in which a portion of the resin particle is exposed and not covered with the film-forming component 203, such as the resin particle 201B illustrated on the far right side of Figure 2, but also resin particles in which the outer periphery of the resin particle is covered with the film-forming component 203, but the thickness of the film-forming component 203 covering the outer periphery is less than 1 μm, such as the resin particle 201A illustrated in the center of Figure 2.
[0084] In the coating layer 20 according to this embodiment, the average value of the number ratio of exposed resin particles (hereinafter referred to as the average number ratio) in the cross section described above is 5 to 50%. If the average number ratio of exposed resin particles is less than 5%, the surface appearance will lack a grained texture, making it impossible to achieve the desired design, which is undesirable. If the average number ratio of exposed resin particles is 5% or more, it is possible to impart a grained texture, which makes it possible to achieve the desired design, which is preferable. The average number ratio of exposed resin particles is preferably 8% or more, and more preferably 10% or more.
[0085] On the other hand, if the average number ratio of exposed resin particles exceeds 50%, the proportion of resin particles 201 exposed on the surface of the coating layer 20 becomes too high, resulting in the resin particles 201 being prone to falling off and making it impossible to achieve the desired scratch resistance. Also, if the average number ratio of exposed resin particles exceeds 50%, the proportion of resin particles 201 exposed on the surface of the coating layer 20 becomes too high, making it impossible to achieve the desired design (particularly, a matte appearance). By keeping the average number ratio of exposed resin particles at 50% or less, it is possible to achieve the desired design while ensuring the scratch resistance required of the coating layer 20. The average number ratio of exposed resin particles is preferably 47% or less, and more preferably 45% or less.
[0086] Furthermore, in the cross section of the coating layer 20 according to this embodiment, it is preferable that 80% or more of the length of the exposed resin particles along the periphery is covered with the film-forming component 203. When 80% or more of the length of the exposed resin particles along the periphery is covered with the film-forming component 203, even the exposed resin particles are less likely to fall off the coating layer 20, making it possible to further prevent deterioration in scratch resistance and design. It is more preferable that 85% or more of the length of the exposed resin particles along the periphery is covered with the film-forming component 203.
[0087] The average number ratio of exposed resin particles in a cross section, as described above, is determined by the following procedure. First, in a cross section obtained by cutting the coating layer 20 at an arbitrary position, a single observation region as described above is focused on. In the observation region, the number of all resin particles 201 present in the region is counted, and exposed resin particles are identified and counted to determine their number ratio. In this case, if only a portion of a particle, rather than the entire particle, is present in the field of view, the particle is counted to one decimal place, for example, 0.1 to 0.9, depending on the area ratio of the particle present in the field of view. This measurement is performed for 10 arbitrary observation field regions, and the number ratio measurement results obtained from each observation field region are further averaged by the number of fields of view. The value obtained in this manner is the average number ratio of exposed resin particles. Here, when calculating the average number ratio, if the obtained value contains a decimal point, the decimal point is rounded down.
[0088] When calculating the average number ratio of exposed particles, attention is focused on one observation field area (length in the width direction: 400 μm) in the cross section of interest. In this case, the magnification of the FE-SEM may be set to an appropriate magnification (for example, about 300 times) so that the coating layer having a length of 400 μm in the width direction fits into one field of view.
[0089] Furthermore, the extent to which the film-forming component 203 covers the length along the periphery of the resin particle 201 can be calculated by measuring the length of the periphery of each exposed resin particle and the length of the portion exposed from the coating layer 20 using a length measurement function or the like implemented in the FE-SEM. Such measurements are performed for all exposed resin particles present in the observation area of interest, and the average value of the obtained proportions is calculated. This operation is performed for 10 arbitrary observation field areas, and the average values of the proportions obtained from each observation field area are further averaged by the number of fields of view. The value obtained in this way can be used as the proportion of the periphery of the exposed resin particle.
[0090] <Use of Two Types of Resin Particles 201> In the coating layer 20 according to this embodiment, it is preferable to use two types of resin particles having different average particle sizes as the previously described resin particles 201. Hereinafter, resin particles having a relatively large average particle size will be referred to as large-particle-size resin particles, and resin particles having a relatively small average particle size will be referred to as small-particle-size resin particles.
[0091] In the coating layer 20 according to this embodiment, by using the above-described large-diameter resin particles as the resin particles 201, it is possible to realize significant unevenness on the surface of the coating layer 20, and as described above, it is possible to realize high designability (grained appearance and matte appearance). Furthermore, by using the above-described small-diameter resin particles as the resin particles 201, it is possible to realize unevenness with a gentler degree of protrusion than the unevenness formed by large-diameter resin particles, and it is also possible to form surface undulations that smoothly connect the unevenness formed by the large-diameter resin particles. As a result, it is possible to further improve the designability of the pre-coated steel sheet 1 according to this embodiment.
[0092] Incidentally, previously, the coating layer 20 has been referred to as a "portion containing resin particles 201" and a "portion not containing resin particles 201." When the large-diameter resin particles and small-diameter resin particles described above are used as the resin particles 201, the "portion not containing resin particles 201" refers to a portion that does not contain either large-diameter resin particles or small-diameter resin particles.
[0093] In the coating layer 20 according to this embodiment, the large-diameter resin particles preferably have an average particle size in the range of 40 to 70 μm, which gives a peak in the particle size range of 55±10 μm when the particle size distribution is measured, and the small-diameter resin particles preferably have an average particle size in the range of 9 to 26 μm, which gives a peak in the particle size range of 17±8 μm when the particle size distribution is measured. By using such large-diameter resin particles and small-diameter resin particles, it is possible to further improve the design properties of the precoated steel sheet 1.
[0094] Furthermore, it is more preferable that the large-sized resin particles have a peak particle size within a particle size range of 55±5 μm and an average particle size within a range of 45 to 65 μm, and it is more preferable that the small-sized resin particles have a peak particle size within a particle size range of 17±5 μm and an average particle size within a range of 12 to 22 μm.
[0095] Here, the ratio (φL / φH) of the average particle size φL of the small-particle resin particles to the average particle size φH of the large-particle resin particles is preferably within a range of 0.14 to 0.58. By ensuring that the average particle size ratio (φL / φH) is within the above range, it is possible to further improve the design of the precoated steel sheet 1 according to this embodiment. The average particle size ratio (φL / φH) is more preferably 0.20 or more. Furthermore, the average particle size ratio (φL / φH) is more preferably 0.50 or less.
[0096] Furthermore, in the coating layer 20 according to this embodiment, the content ratio CL of the small-diameter resin particles is preferably within a range of 5 to 30 mass % relative to the total solid mass of the coating layer 20, and the content ratio CH of the large-diameter resin particles is preferably within a range of 5 to 30 mass % relative to the total solid mass of the coating layer 20. When the content ratio CL of the small-diameter resin particles and the content ratio CH of the large-diameter resin particles are within the above ranges, the design properties of the precoated steel sheet 1 can be further improved.
[0097] The proportion CL of small-sized resin particles is more preferably 7% by mass or more, relative to the total solid mass of the coating layer 20. The proportion CL of small-sized resin particles is more preferably 25% by mass or less, relative to the total solid mass of the coating layer 20. The proportion CH of large-sized resin particles is more preferably 7% by mass or more, relative to the total solid mass of the coating layer 20. The proportion CH of large-sized resin particles is more preferably 25% by mass or less, relative to the total solid mass of the coating layer 20.
[0098] In the coating layer 20 according to this embodiment, the ratio (CL / CH) of the content proportion of small-sized resin particles CL to the content proportion of large-sized resin particles CH is preferably within the range of 0.5 to 1.5. When the content proportion ratio (CL / CH) is within the above range, it is possible to further improve the design of the precoated steel sheet 1. The content proportion ratio (CL / CH) is more preferably 0.7 or more. Furthermore, the content proportion ratio (CL / CH) is more preferably 1.3 or less.
[0099] Furthermore, in the coating layer 20 according to this embodiment, it is preferable that the compressive modulus of the small-sized resin particles at 25°C is in the range of 60 to 250 MPa, and the compressive modulus of the large-sized resin particles at 25°C is in the range of 60 to 250 MPa. By ensuring that the compressive moduli of the small-sized resin particles and the large-sized resin particles are within the above ranges, when an external force is applied to the resin particles, the applied force can be dispersed more efficiently, making it possible to further prevent a decrease in the design of the precoated steel sheet 1. The compressive modulus of the small-sized resin particles at 25°C is more preferably 90 MPa or more. The compressive modulus of the small-sized resin particles at 25°C is more preferably 210 MPa or less. The compressive modulus of the large-sized resin particles at 25°C is more preferably 90 MPa or more. The compressive modulus of the large-sized resin particles at 25°C is more preferably 210 MPa or less.
[0100] Here, when determining the average particle size and content of the large-diameter resin particles and the small-diameter resin particles by cross-sectional observation, the method is not particularly limited, but may be, for example, as follows. First, in a cross-section obtained by cutting the coating layer 20 at an arbitrary position, focus is placed on one arbitrary observation region as described above. In the observation region, the circle-equivalent diameters of the resin particles 201 present in the region are measured. The average value of the measured circle-equivalent diameters in the observation region of interest is then calculated. This measurement is performed on 10 arbitrary observation regions, and a particle size distribution is obtained from each observation region. In this case, resin particles having a particle size of 40 μm or more are defined as large-diameter resin particles, and their average is defined as the average particle size of the large-diameter resin particles. Meanwhile, resin particles having a particle size of 30 μm or less are defined as small-diameter resin particles, and their average is defined as the average particle size of the small-diameter resin particles.
[0101] The content of resin particles can be measured as follows. First, the total mass per unit volume of the coating film, including resin particles, is calculated from the difference between the volume of the coating film calculated from the average film thickness dA of the coating film determined by cross-sectional observation and the mass of the coating film removed from the steel sheet using an organic solvent or remover. Similarly, the average particle diameter of the resin particles determined by cross-sectional observation is converted into the volume of the resin particles, and the total mass of the resin particles contained in the coating film layer per unit volume is calculated when the specific gravity of the resin particles is 1.2. The content of resin particles can be calculated from the total mass per unit volume of the coating film and the total mass of the resin particles per unit volume.
[0102] The compressive modulus of elasticity at 25° C. of the large-diameter resin particles and the small-diameter resin particles may be measured in accordance with the method for measuring the compressive modulus of elasticity of the resin particles and the binder resin described above.
[0103] The coating layer 20 according to this embodiment has been described in detail above with reference to FIG.
[0104] [Regarding the Coating Layer 25] The coating layer 25 that the precoated steel sheet 1 according to this embodiment may have may have the same configuration as the coating layer 20, except that it does not contain the resin particles 201 as described above. That is, the coating layer 25 contains at least a binder resin as the film-forming component 205, and may further contain various color pigments and additives that the coating layer 20 may contain as described above. Therefore, a detailed description of the coating layer 25 according to this embodiment will be omitted below.
[0105] [Regarding the Rust-Preventive Coating Layer 30] Next, a brief description will be given of the rust-preventive coating layer 30 that is provided as needed between the zinc-based plated steel sheet 10 and the coating layer 20 in the pre-coated steel sheet 1 according to this embodiment. The rust-preventive coating layer 30 is a coating layer that contains an anti-rust pigment and a resin.
[0106] The resin contained in the rust-preventive coating layer 30 functions as a film-forming component, and any material can be used. However, from the viewpoints of ease and cost of production, as well as corrosion resistance and scratch resistance, it is preferable to use various organic resins as the resin. Examples of such resins include acrylic resins, polyester resins, urethane resins, and fluorine-based resins.
[0107] The rust-preventive coating layer 30 according to this embodiment may contain various known rust-preventive pigments as the rust-preventive pigment, but preferably contains a pigment containing at least one of the elements P, V, Si, and Mg as the rust-preventive pigment.
[0108] Examples of pigments containing at least one of the elements P, V, Si, and Mg include zinc phosphate, zinc phosphite, zinc magnesium phosphate, magnesium phosphate, magnesium phosphite, silica, calcium ion-exchanged silica, zirconium phosphate, aluminum dihydrogen tripolyphosphate, zinc oxide, zinc phosphomolybdate, barium metaborate, and strontium chromate.
[0109] The average thickness of the anticorrosive coating layer 30 is not particularly limited, and may be, for example, about 3.0 to 12.0 μm.
[0110] Furthermore, when a coating layer such as the rust-preventive coating layer 30 exists between the zinc-based plated steel sheet 10 and the coating layer 20, the average film thickness dA in the portions of the coating layer 20 that do not contain resin particles and the average actual film thickness dB, which is the average value of the actual film thickness in the portions that contain resin particles, also include the thickness of the coating layer between the zinc-based plated steel sheet 10 such as the rust-preventive coating layer 30 and the coating layer 20.
[0111] <Glossiness of Pre-painted Steel Sheet 1> One of the properties corresponding to the high designability exhibited by the pre-painted steel sheet 1 according to this embodiment is glossiness that gives a matte appearance. Hereinafter, such glossiness will be described in detail.
[0112] In the precoated steel sheet 1 according to this embodiment, the surface of the coating layer 20 containing the resin particles 201 has a 60-degree specular gloss G defined in JIS Z 8741:1997. S (60°), the 60° specular gloss G S The value of the 60° specular gloss G is preferably in the range of 3 or more and 30 or less. In the pre-coated steel sheet 1 according to this embodiment, when the surface of the coating layer 20 exhibits a gloss within the above range, the pre-coated steel sheet 1 according to this embodiment exhibits a more excellent matte appearance (and thus more excellent design). S The value of (60°) is more preferably 3 or more. S The value of (60°) is more preferably 25 or less.
[0113] [Change in gloss before and after tensile elongation] In the pre-coated steel sheet 1 according to this embodiment, the 60-degree specular gloss G defined in JIS Z 8741:1997 of the surface of the coating layer 20 was measured before and after imparting a 30% tensile elongation to the pre-coated steel sheet. S (60 °) was measured, the 60 ° specular gloss G SThe rate of change of the angle (60°) is preferably 60% or less. Here, the tensile elongation of the pre-coated steel sheet 1 may be imparted by taking No. 5 test pieces from the pre-coated steel sheets 1 in accordance with JIS Z2241:2011 and using a tensile tester.
[0114] 60° specular gloss G before and after applying 30% tensile elongation S By making the rate of change of the gloss (60°) 60% or less, even if various processes are performed on the pre-coated steel sheet 1 according to this embodiment, the change in gloss before and after the processing is suppressed. As a result, it is possible to maintain the design properties of the pre-coated steel sheet 1 even after various processes are performed.
[0115] 60° specular gloss G before and after applying 30% tensile elongation S The rate of change of (60°) is more preferably 50% or less.
[0116] In addition, the 60-degree specular gloss G S (60°) can be measured using various gloss meters in accordance with JIS Z 8741:1997.
[0117] The pre-coated steel sheet 1 according to this embodiment has been described in detail above with reference to FIGS. 1A to 2.
[0118] (Regarding Manufacturing Method of Pre-painted Steel Sheet) Next, an example of a manufacturing method of the pre-painted steel sheet 1 according to this embodiment will be described. First, a steel sheet serving as a base material is subjected to various pretreatments, including alkaline degreasing treatment, water washing treatment, and pickling treatment, to obtain a clean steel sheet surface. Then, a zinc-based plating layer is formed on the surface of this base steel sheet. In this plating step, a plating bath containing components capable of realizing the desired plating composition is prepared, and the zinc-based plating layer is formed by various known methods. In this way, a zinc-based plated steel sheet 10 serving as the substrate of the pre-painted steel sheet 1 according to this embodiment can be manufactured.
[0119] Thereafter, various known anti-rust paints for forming the anti-rust coating layer 30 are applied to the zinc-based plated steel sheet as necessary, and then dried. The application of the anti-rust paint can be carried out by a generally known application method, such as roll coating, curtain flow coating, air spraying, airless spraying, immersion, bar coating, or brush coating. The method for heating the anti-rust paint is not particularly limited, and any method may be used, such as hot air, near infrared rays, far infrared rays, induction heating, or a combination of these.
[0120] Next, a coating liquid for forming the coating layer 20 is applied to the surface of the zinc-based plated steel sheet 10 on which the rust-preventive coating layer has been formed as needed, and the coating liquid is dried by heating to form the coating layer. Here, the coating liquid is prepared by adding the above-mentioned resin particles, film-forming components including a binder resin and a coloring pigment, and various additives as needed, to a solvent.
[0121] It is also important to use a curtain flow coater to apply the prepared coating solution. By using a curtain flow coater to apply a coating solution containing particles, it is possible to apply the coating solution without causing the particles to settle or causing coating defects (roping).
[0122] After applying the coating liquid to the surface of the zinc-based plating layer (or rust-preventive coating layer), the coating liquid is heat-cured. The heating temperature can be set depending on the solvent used, but is preferably within the range of 180 to 250°C, for example. When heat-curing the coating liquid, attention must be paid to the rate of temperature rise. More specifically, it is important to set the rate of temperature rise within the range of 5 to 50°C / sec. By applying the coating liquid having the above-described surface tension and viscosity using a curtain flow coater and then heat-curing it under the above-described heating rate, a coating layer 20 having the particle state described above can be formed. The heating rate is more preferably within the range of 10 to 30°C / sec.
[0123] The method for heating the coating liquid is not particularly limited, and any method may be used, such as hot air, near infrared rays, far infrared rays, induction heating, or a combination of these.
[0124] The method for manufacturing a pre-coated steel sheet according to this embodiment has been described above.
[0125] The pre-coated steel sheet according to this embodiment will be specifically described below with reference to examples and comparative examples. Note that the examples shown below are merely examples of the pre-coated steel sheet according to this embodiment, and the pre-coated steel sheet according to this embodiment is not limited to the examples below.
[0126] <1. Preparation of top coating paint> Amorphous polyester resins manufactured by Toyobo Co., Ltd., "Vylon (registered trademark) 500 (Tg 4°C)," "Vylon (registered trademark) 270 (Tg 50°C)," and "Vylon (registered trademark) UR-6100 (Tg -30°C)," were dissolved in an organic solvent (a mixture of cyclohexanone and Solvesso 150 (trade name) in a mass ratio of 1:1). The mixing ratio of these polyester resins was then adjusted.
[0127] Next, melamine resin "Cymel (registered trademark) 303" manufactured by Allnex Japan Co., Ltd. and melamine resin "Super Beckamine (registered trademark)" manufactured by DIC Corporation were added to the above solution as curing agents. The amount of melamine resin added was such that the mass ratio of polyester resin solids to melamine resin solids was 70:30. Furthermore, 0.5 mass% of acid catalyst "Catalyst 600" manufactured by Allnex Japan Co., Ltd. was further added to this mixed solution of polyester resin and melamine resin. A varnish paint was obtained by stirring this mixed solution. The polyester resin and melamine resin contained in this varnish paint mainly function as binder resins. The compressive modulus of the binder resin was adjusted by adjusting the ratio of the polyester resin and the ratio of the melamine resin.
[0128] 2. Preparation of Resin Particle-Containing Paints Resin particles were prepared using "Art Pearl (registered trademark)," a urethane resin manufactured by Negami Chemical Industries, Ltd., or "MBX," an acrylic bead manufactured by Sekisui Chemical Co., Ltd. (different particle size distributions). These resin particles were combined and dispersed in the top coat to prepare a resin particle-containing paint. In addition, in some cases, carbon black "Touka Black #7300" manufactured by Tokai Carbon Co., Ltd. and titanium oxide "R-820" manufactured by Ishihara Sangyo Kaisha, Ltd. were added as coloring pigments. The coloring pigments were used such that the mass ratio of the carbon black to titanium oxide (carbon black:titanium oxide) was 20:80. The amount of coloring pigment added was such that the mass ratio of the solid content of the varnish to the colorant (varnish solid content:colorant) was 92:8. The resulting mixture was stirred to prepare a resin particle-containing paint.
[0129] In the examples and comparative examples shown below, examples in which the particle size distribution of resin particles has two peaks, one for large-sized resin particles and one for small-sized resin particles, correspond to cases in which a resin particle-containing paint was prepared using a combination of two types of resin particles in which one peak is observed in the particle size distribution.
[0130] <3. Preparation of Backside Paint> For the backside paint, "Flexicoat 100," a polyester / melamine paint manufactured by Nippon Paint Industrial Coatings Co., Ltd., was used. The paint was colored beige using white pigments, yellow pigments, etc. The gloss level was adjusted by adding silica fine particles as a gloss adjuster to the paint. The dry film thickness was set to 5 μm.
[0131] <4. Preparation of Anti-Rust Paint> Amorphous polyester resins "Vylon (registered trademark) 500 (Tg 4°C)" and "Vylon (registered trademark) 270 (Tg 50°C)" manufactured by Toyobo Co., Ltd. were mixed in a mass ratio of 1:1. Next, these polyester resin mixtures were dissolved in an organic solvent (a mixture of cyclohexanone and Solvesso 150 (trade name) in a mass ratio of 1:1 was used) to prepare a primer varnish. To this primer varnish, an isocyanate "Coronate HX" manufactured by Tosoh Corporation was added. The amount of isocyanate added was such that the solid content of the varnish:isocyanate ratio was 95:5 by mass. Furthermore, as anti-rust pigments, condensed aluminum "K-WHITE #450H" manufactured by Teika Corporation, calcium-modified silica "SHIELDEX C303" manufactured by GRACE Corporation, calcium vanadate apatite (reagent manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and magnesium hydroxide (reagent manufactured by Kanto Chemical Co., Ltd.) were used. Each was added so that the concentration in the dried film would be 50 mass %, and the mixture was stirred to prepare an anti-rust paint.
[0132] <5. Preparation of Test Materials> Next, as zinc-based plated steel sheets serving as substrates, a Zn-0.2 mass% Al-plated steel sheet (GI), a Zn-11 mass% Al-3 mass% Mg-0.2 mass% Si-plated steel sheet (SD), and a Zn-6 mass% Al-3 mass% Mg-plated steel sheet (ZAM) (all manufactured by Nippon Steel Corporation) were used. The thickness of each zinc-based plated steel sheet was 0.6 mm.
[0133] Here, in order to improve adhesion between the zinc-based plated steel sheet and the paint film, a chemical conversion coating was formed on the surface of the zinc-based plated steel sheet prior to the application of the paint. The chemical conversion coating was formed by applying a chromate-free chemical conversion treatment solution "CT-E300N" manufactured by Nihon Parkerizing Co., Ltd., with a coating weight of 100 mg / m2 after drying. 2 The coating was then dried at a steel sheet temperature of 60°C to form a chemical conversion coating.
[0134] Two layers, the anti-rust coating and the resin particle-containing coating, were applied to one side of the above zinc-plated steel sheet, and a backside coating was applied to the other side, followed by heating and baking. The maximum thickness temperatures were 210°C for the anti-rust coating layer and 230°C for the coating layer containing resin particles, with a heating rate of 5°C / sec. A curtain flow coater was used to apply the coating. Test specimens were prepared in this manner. Multiple test specimens were prepared for each level.
[0135] For each of the obtained test materials, the average film thickness dA, the actual film thickness dB, various indices for the resin particles, the number ratio of exposed resin particles, the coverage rate, etc. were measured according to the methods previously described. The obtained results are summarized in Table 1 below.
[0136]
[0137] Each test material obtained as described above was evaluated from the viewpoints of grain appearance, corrosion resistance, gloss change rate before and after tensile elongation, processing adhesion, and scratch resistance. The evaluation methods are as follows.
[0138] (Grain appearance) In addition to the surface of the test material, a resin molded product (with a grained appearance, resin used: exterior material of the multifunction printer iR ADVC5250F manufactured by Canon Inc.) was used. Each of the test material and the resin molded product was evaluated by visual observation from a distance of 20 cm to investigate whether they could be distinguished from the test material. The evaluators were 10 random people with a visual acuity of 1.0 or higher. The percentage of the 10 evaluators who were able to distinguish was calculated as the distinguishability rate, which was used to evaluate the design. The evaluation criteria were as follows. The pass level was 2 or higher. <Evaluation criteria> Rating 3: distinguishability rate is 30% or less 2: distinguishability rate is more than 30% to 60% or less 1: distinguishability rate is more than 60%
[0139] (Corrosion Resistance) An X-shaped cut was made on the surface of the test material using an NT cutter. At this time, the cut was made so that the cut reached the metal plate, which was the substrate. Thereafter, a combined cyclic corrosion test (CCT JASO M609) in accordance with JIS K 5600-7-9:2006 was performed for 60 cycles. After the test, the test material was washed and dried, and the maximum blister width from the X-shaped cut was measured. Of the blisters that occurred on both sides of the scratch, the maximum blister width on one side was measured. A 10x magnifying glass was used for observation. The corrosion resistance was evaluated according to the following evaluation criteria. A pass level was 2 or higher. <Evaluation Criteria> Rating 3: Maximum blister width is less than 2 mm 2: Maximum blister width is 2 mm or more but less than 5 mm 1: Maximum blister width is 5 mm or more
[0140] (Change in glossiness before and after tensile elongation) Before tensile elongation, each test material was measured for 60-degree specular glossiness G defined in JIS Z 8741:1997. S The gloss meter used conforms to JIS Z 8741:1997. Then, using a tensile tester, the surface of the test material was stretched to a tensile elongation of 30%, and the 60-degree specular gloss G defined in JIS Z 8741:1997 was measured for the part that had reached a tensile elongation of 30%. S The 60-degree specular gloss G (G) was measured using the obtained measurement values before and after the application of tensile elongation. S The rate of change in gloss (60°) was calculated. The evaluation criteria are as follows. A pass level was 2 or higher. <Evaluation criteria> Rating 4: The rate of change in gloss is 40% or less. 3: The rate of change in gloss is more than 40% and 50% or less. 2: The rate of change in gloss is more than 50% and 60% or less. 1: The rate of change in gloss is more than 60%.
[0141] (Processing Adhesion) The surface of the test material was bent at 180 degrees 0T in accordance with JIS K 5600:1999 so that the evaluation surface was on the outside, and the cross section of the coating film in a 5 mm area centered on the top of the bent part was observed to measure whether resin particles had fallen off. The cross section of the coating film was observed with a scanning electron microscope (JSM-7200F manufactured by JEOL Ltd.). The corrosion resistance was evaluated according to the following evaluation criteria. A pass level was 2 or higher. <Evaluation Criteria> Rating 3: No resin particles were observed to have fallen off from the coating film. 2: 5 or fewer resin particles were observed to have fallen off from the coating film. 1: 6 or more resin particles were observed to have fallen off from the coating film.
[0142] (Scratch Resistance) The surface of the test material was scratched 5 mm along the coating surface with a 5H pencil in accordance with JIS K 5600:1999, and the presence or absence of large resin particles was measured. The scratched surface was observed under an optical microscope. The corrosion resistance was evaluated according to the following evaluation criteria. A pass level was 2 or higher. <Evaluation Criteria> Rating 3: No resin particles were observed to have fallen off from the coating. 2: 5 or fewer resin particles were observed to have fallen off from the coating. 1: 6 or more resin particles were observed to have fallen off from the coating.
[0143] The results obtained are summarized in Table 2 below.
[0144]
[0145] As is clear from Table 2 above, the test materials corresponding to the examples of the present invention exhibited excellent grain appearance, corrosion resistance, gloss change rate before and after tensile elongation, processing adhesion, and scratch resistance, while the test materials corresponding to the comparative examples of the present invention failed in at least one of the grain appearance, corrosion resistance, gloss change rate before and after tensile elongation, processing adhesion, or scratch resistance.
[0146] Separately, the particle-containing coating material No. 20 shown in Table 1 above was used to compare productivity when the coating material was applied using a curtain flow coater and a roll coater commonly used in the manufacture of pre-coated steel sheets. The roll coater used was a two-roll coater consisting of a pickup roll and an applicator roll. The substrate speed was changed in 10 mpm increments between 10 mpm and 80 mpm.
[0147] In the case of the curtain flow coater, a beautiful appearance was obtained at a plate speed in the range of 50 to 80 mpm, and the performance was also equivalent to that of No. 20 shown in Table 1 above. On the other hand, in the case of the roll coater, roping occurred at a plate speed in the range of 20 to 80 mpm, but at a plate speed of 10 mpm, a beautiful appearance similar to that obtained with the curtain flow coater was obtained. From these results, it can be said that painting with a curtain flow coater is 5 to 8 times more productive than using a roll coater, which is a commonly used painting method.
[0148] Although the preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to these examples. It is clear that a person skilled in the art to which the present invention pertains can conceive of various modifications and alterations within the scope of the technical ideas set forth in the claims, and it is understood that these also naturally fall within the technical scope of the present invention.
[0149] The embodiments disclosed herein are illustrative in all respects and are not limiting. The above-described embodiments may be omitted, substituted, or modified in various ways without departing from the scope of the appended claims, the technical scope of the present invention as described below, and the spirit thereof. For example, the components of the above-described embodiments may be arbitrarily combined within the scope that does not impair the effects of the components. Furthermore, such an arbitrary combination naturally provides the functions and effects of each of the components involved in the combination, and also provides other functions and effects that are apparent to those skilled in the art from the description of this specification.
[0150] Furthermore, the effects described in this specification are merely descriptive or exemplary and are not limiting. In other words, the technology according to the present invention may achieve other effects that will be apparent to those skilled in the art from the description of this specification, in addition to or in place of the above-described effects.
[0151] The following configurations also fall within the technical scope of the present invention. (1) A precoated steel sheet having a zinc-based plated steel sheet having a zinc-based plating layer, which is a plating layer containing at least zinc, located on the surface of a base steel sheet, and a coating layer located on the surface of the zinc-based plating layer, wherein the coating layer contains resin particles and a binder resin and a color pigment as film-forming components, and in a cross section of the coating layer cut at an arbitrary position in the thickness direction, the average value of the area ratio, which is the area ratio occupied by the resin particles, is within a range of 5 to 40%, the average film thickness dA in a portion of the coating layer not containing the resin particles is within a range of 10 to 40 μm, the average particle diameter φ of the resin particles is 4.0 times or less the average film thickness dA, and when the thickness obtained by subtracting the thickness of a portion corresponding to the resin particles from the total thickness of the coating layer containing the resin particles is referred to as the actual film thickness of the coating layer in the portion containing the resin particles, the average actual film thickness dB, which is the average value of the actual film thickness in the portion containing the resin particles, is within a range of 4 to 30 μm, (2) A precoated steel sheet according to (1), wherein, when the resin particles among the resin particles have a portion of the outer periphery that is not covered with the film-forming component to a thickness of 1 μm or more, and the average number ratio of the exposed resin particles is 5 to 50%, the exposed resin particles are covered with the film-forming component over 80% or more of the length along the outer periphery in the cross section. (3) A precoated steel sheet according to (1), wherein, before and after imparting a 30% tensile elongation to the precoated steel sheet, the 60-degree specular gloss G defined in JIS Z 8741:1997 of the surface of the coating layer is measured. S (60 °) before and after the tensile elongation is applied. S(4) The precoated steel sheet according to any one of (1) to (3), wherein the compressive modulus of the binder resin at 25°C is in the range of 60 to 150 MPa, the compressive modulus of the resin particles at 25°C is in the range of 60 to 250 MPa, and the compressive modulus of the binder resin at 25°C is equal to or less than the compressive modulus of the resin particles at 25°C. (5) The precoated steel sheet according to any one of (1) to (4), wherein the coating layer contains, as the resin particles, small-sized resin particles having an average particle size in the range of 9 to 26 μm that gives a peak in a particle size range of 17±8 μm, and large-sized resin particles having an average particle size in the range of 40 to 70 μm that gives a peak in a particle size range of 55±10 μm, when a particle size distribution is measured. (6) The precoated steel sheet according to (5), wherein the content percentage CL of the small-particle resin particles is within a range of 5 to 30 mass% relative to the total solid mass of the coating layer, and the content percentage CH of the large-particle resin particles is within a range of 5 to 30 mass% relative to the total solid mass of the coating layer. (7) The precoated steel sheet according to (5) or (6), wherein the ratio (CL / CH) of the content percentage CL of the small-particle resin particles to the content percentage CH of the large-particle resin particles is within a range of 0.5 to 1.5. (8) The precoated steel sheet according to any one of (5) to (7), wherein the ratio (φL / φH) of the average particle diameter φL of the small-particle resin particles to the average particle diameter φH of the large-particle resin particles is within a range of 0.14 to 0.58. (9) The precoated steel sheet according to any one of (5) to (8), wherein the small-particle-size resin particles have a compressive modulus of elasticity at 25°C in the range of 60 to 250 MPa, and the large-particle-size resin particles have a compressive modulus of elasticity at 25°C in the range of 60 to 250 MPa.
[0152] REFERENCE SIGNS LIST 1 Pre-coated steel sheet 10 Zinc-based plated steel sheet 11 Base steel sheet 13 Zinc-based plated layer 20, 25 Coating layer 30 Anti-rust coating layer 201 Resin particles 201a Small particle size resin particles 201b Large particle size resin particles 203, 205 Film-forming component
Claims
1. A precoated steel sheet having a zinc-based plated steel sheet having a zinc-based plated layer which is a plated layer containing at least zinc and located on the surface of a base steel sheet, and a coating layer located on the surface of the zinc-based plated layer, wherein the coating layer contains resin particles and a binder resin and a color pigment as film-forming components, and in a cross section of the coating layer cut in the thickness direction at an arbitrary position, the average area ratio which is the area ratio occupied by the resin particles is within a range of 5 to 40%, the average film thickness dA in the portion of the coating layer which does not contain the resin particles is within a range of 10 to 40 μm, the average particle diameter φ of the resin particles is 4.0 times or less the average film thickness dA, and when the thickness obtained by subtracting the thickness of the portion corresponding to the resin particles from the total thickness of the coating layer including the resin particles is referred to as the actual film thickness of the coating layer in the portion including the resin particles, the average actual film thickness dB which is the average value of the actual film thickness in the portion including the resin particles is within a range of 4 to 30 μm, When the resin particles, among the resin particles, have a portion whose outer periphery is not covered with the film-forming component to a thickness of 1 μm or more, and are referred to as exposed resin particles, the average number ratio of the exposed resin particles is 5 to 50%.
2. The precoated steel sheet according to claim 1, wherein in the cross section, 80% or more of the length of the exposed resin particle along the outer periphery is covered with the film-forming component.
3. Before and after applying a 30% tensile elongation to the precoated steel sheet, the surface of the coating layer is measured for the 60 degree specular gloss G defined in JIS Z 8741:1997. S (60°) was measured, the 60° specular gloss G S The precoated steel sheet according to claim 1 or 2, wherein a rate of change in (60°) is 60% or less.
4. A precoated steel sheet as described in claim 1 or 2, wherein the compressive modulus of the binder resin at 25°C is within the range of 60 to 150 MPa, the compressive modulus of the resin particles at 25°C is within the range of 60 to 250 MPa, and the compressive modulus of the binder resin at 25°C is equal to or lower than the compressive modulus of the resin particles at 25°C.
5. A precoated steel sheet according to claim 1 or 2, wherein the coating layer contains, as the resin particles, small-sized resin particles having an average particle size in the range of 9 to 26 μm which gives a peak in the particle size range of 17±8 μm when particle size distribution is measured, and large-sized resin particles having an average particle size in the range of 40 to 70 μm which gives a peak in the particle size range of 55±10 μm.
6. A precoated steel sheet as described in claim 5, wherein the content ratio CL of the small-diameter resin particles is within the range of 5 to 30 mass % relative to the total solid mass of the coating layer, and the content ratio CH of the large-diameter resin particles is within the range of 5 to 30 mass % relative to the total solid mass of the coating layer.
7. The precoated steel sheet according to claim 5, wherein the ratio (CL / CH) of the content proportion CL of the small-diameter resin particles to the content proportion CH of the large-diameter resin particles is within the range of 0.5 to 1.
5.
8. The precoated steel sheet according to claim 5, wherein the ratio (φL / φH) of the average particle size φL of the small resin particles to the average particle size φH of the large resin particles is within the range of 0.14 to 0.
58.
9. The precoated steel sheet according to claim 5, wherein the small resin particles have a compressive elastic modulus at 25°C in the range of 60 to 250 MPa, and the large resin particles have a compressive elastic modulus at 25°C in the range of 60 to 250 MPa.