Conductive paste, electronic component, and multilayered ceramic capacitor

MYPI2025008364A0Undetermined Publication Date: 2025-01-04SUMITOMO METAL MINING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025008364
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-04
Filing Date
2024-07-02
Publication Date
2025-01-04

AI Technical Summary

Technical Problem

The challenge in manufacturing smaller, high-capacity multilayer ceramic capacitors is the occurrence of delamination and cracking during the firing process due to differences in thermal contraction rates between conductive films and dielectric layers, which affects the electrical characteristics and increases manufacturing costs.

Method used

A conductive paste composition containing conductive powder, ceramic powder, phosphoric acid additive, binder resin, and organic solvent, which reduces the difference in thermal shrinkage between the conductive film and dielectric layer without special treatment of the conductive powder, thereby suppressing delamination and cracking.

Benefits of technology

The conductive paste composition ensures a gradual sintering process, reducing thermal shrinkage differences and preventing delamination and cracking, leading to improved electrical characteristics and reduced manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025008364_DRAWING_001
    Figure PI2025008364_DRAWING_001
  • Figure PI2025008364_DRAWING_002
    Figure PI2025008364_DRAWING_002
  • Figure PI2025008364_DRAWING_003
    Figure PI2025008364_DRAWING_003
Patent Text Reader

Abstract

Provided is a conductive paste that can reduce a difference in thermal shrinkage during a firing process. The conductive paste contains conductive powder, ceramic powder, an additive, a binder resin, and an organic solvent. The additive contains a phosphoric acid-based additive having a structure represented by a structural formula (1) below in a content of 0.03% by mass or more and 1.5% by mass or less with respect to an entire amount of the conductive paste. The organic solvent contains a terpene-based solvent (a) and at least one solvent (b) selected from a hydrocarbon-based solvent, an acetate-based solvent, an ether-based solvent, and a ketone-based solvent. The binder resin contains at least one of a cellulose-based resin and an acetal-based resin. [Chem. 1] R1 includes at least one of alkyl groups having 6 or more carbon atoms, ether groups having 6 or more carbon atoms, polyether groups, and polyester groups; and R2 and R3 are each independently hydrogen or an ammonium base, or include at least one of alkyl groups, ester groups, and ether groups.
Need to check novelty before this filing date? Find Prior Art

Description

Conductive paste, electronic components, and multilayer ceramic capacitors

[0001] The present invention relates to a conductive paste, an electronic component, and a multilayer ceramic capacitor.

[0002] As electronic devices such as mobile phones and digital devices become smaller and more powerful, there is a demand for smaller and higher-capacity electronic components, including multilayer ceramic capacitors. Multilayer ceramic capacitors have a structure in which multiple dielectric layers and multiple internal electrode layers are alternately stacked, and by reducing the thickness of these dielectric layers and internal electrode layers, miniaturization and higher capacitance are achieved.

[0003] For example, a multilayer ceramic capacitor is manufactured as follows: First, barium titanate (BaTiO 3 A conductive paste for internal electrodes is printed in a predetermined electrode pattern on the surface of a green sheet (substrate) containing a dielectric powder such as nickel and a binder resin, and then dried to form a dry film (conductive film). The conductive paste contains a conductive powder such as nickel. Next, the conductive film and the green sheet are alternately stacked to obtain a laminate. Next, this laminate is integrated by heat and pressure bonding to form a pressed body. This pressed body is cut, subjected to an organic binder removal treatment in an oxidizing or inert atmosphere, and then fired to obtain fired chips. Next, a paste for external electrodes is applied to both ends of the fired chip, and after firing, the surfaces of the external electrodes are nickel-plated or the like to obtain a multilayer ceramic capacitor.

[0004] In the above-described firing process to obtain a fired chip, if there is a large difference in the thermal shrinkage rate between the conductive film and the green sheet adjacent to the conductive film, the conductive film may delaminate from the green sheet or cracks may occur in the pressure-bonded laminate (conductive film or green sheet). In this case, the resulting multilayer ceramic capacitor may not have the desired electrical characteristics.

[0005] For example, Patent Document 1 discloses a paste-like conductor-forming composition containing core-shell particles having a particle size of 100 nm to 1000 nm based on SEM observation, each of which is composed of nickel particles as core particles and a shell in which the surface of the nickel particles is coated with barium titanate, and a dispersion medium. Patent Document 1 states that thermal shrinkage can be suppressed by using a shell in which the surface of the nickel particles as core particles is coated with barium titanate.

[0006] Patent Document 2 discloses a nickel microparticle-containing composition containing the following components A and B: A) first nickel microparticles having an average particle size within the range of 60 to 150 nm as measured by scanning electron microscopy and a coefficient of variation of the particle size of 0.2 or less, and B) second nickel microparticles having an average particle size within the range of 10 to 60 nm as measured by scanning electron microscopy and a coefficient of variation of the particle size of 0.2 or less and a 5% heat shrinkage temperature that is 50°C or more higher than the 5% heat shrinkage temperature of the first nickel microparticles. Patent Document 2 aims to suppress thermal shrinkage by mixing the first nickel particles with second nickel particles having a small particle size and a high heat shrinkage temperature, and further coating the particles with elemental sulfur or by containing elemental phosphorus or nickel carbide.

[0007] JP 2016-014194 A JP 2014-145117 A

[0008] However, Patent Document 1 includes a process of coating nickel particles with barium titanate, a process of adjusting the pH of the fine particles, and a process of evaporating the dispersion medium by heat treatment, which may result in the nickel particles linking or agglomerating during the manufacturing process. If the nickel particles aggregate, the agglomerates may penetrate the green sheet during compression bonding, causing a short circuit. In addition, the barium titanate may not be uniformly dispersed, resulting in a lower dielectric constant. Furthermore, if customization is required, such as changing the amount of barium titanate to match the thermal shrinkage rate of the green sheet, the manufacturing cost will increase.

[0009] Furthermore, in Patent Document 1, the behavior of the thermal shrinkage rate of nickel particles coated with barium titanate, measured based on thermomechanical analysis (TMA), is made similar to the thermal shrinkage behavior of barium titanate particles (dielectric powder), thereby suppressing the occurrence of cracks that occur when firing the internal electrode layers.

[0010] In Patent Document 2, two types of nickel particles are required, which increases the manufacturing cost. In addition, when the particles are coated with elemental sulfur or treated to contain elemental phosphorus or nickel carbide in order to increase the sintering initiation temperature, the surface condition changes, which causes a problem of changing the dispersion behavior.

[0011] Furthermore, in Patent Document 2, the occurrence of defects such as delamination and cracks during sintering can be prevented by reducing the thermal shrinkage of mixed particles obtained by mixing two types of nickel particles with different average particle sizes and increasing the sintering start temperature (5% thermal shrinkage temperature measured by TMA).

[0012] In recent years, in response to the trend toward smaller and higher capacity multilayer ceramic capacitors, thinning of both the dielectric layer and the internal electrode layer has been studied. 3 The diameters of powders and conductive powders (e.g., nickel powder) are becoming smaller. In particular, when the particle size of conductive powder is reduced, the difference in thermal contraction between the conductive powder and the dielectric layer during the sintering process during manufacturing tends to be larger than when nickel powder with a larger particle size is used. Therefore, there is a need to further reduce the occurrence of delamination and cracks during the sintering process.

[0013] The inventors conceived the idea that one of the causes of delamination and cracking during the firing process is a sudden increase in thermal shrinkage of the conductive film during firing, and as a result of extensive research, they discovered that by using a conductive paste having a specific composition, the difference between the thermal shrinkage behavior of the conductive film and the thermal shrinkage behavior of the dielectric layer can be reduced, and the sudden thermal shrinkage of the conductive film during sintering can be suppressed, i.e., the difference in thermal shrinkage of the conductive film per temperature difference during sintering (e.g., difference in thermal shrinkage rate) can be reduced, thereby suppressing the occurrence of delamination and cracking, and thus completed the present invention.

[0014] In view of the above circumstances, the present invention aims to provide a conductive paste that can reduce the difference in thermal shrinkage (difference in dimensional change rate) during sintering of a conductive film containing conductive powder, without requiring any special treatment of the conductive powder.

[0015] In a first aspect of the present invention, there is provided a conductive paste comprising a conductive powder, a ceramic powder, an additive, a resin, and an organic solvent, wherein the additive comprises a phosphoric acid-based additive having a structure represented by the following structural formula (1) in an amount of 0.05 mass% or more and 1.5 mass% or less relative to the total amount of the conductive paste, the organic solvent comprises a terpene-based solvent (a) and one or more solvents (b) selected from a hydrocarbon-based solvent, an acetate-based solvent, an ether-based solvent, and a ketone-based solvent, and the resin comprises at least one of a cellulose-based resin and an acetal-based resin.

[0016]

[0017] (However, R 1 contains at least one of an alkyl group having 6 or more carbon atoms, an ether group having 6 or more carbon atoms, a polyether group, and a polyester group, and R 2 , R 3 are each independently hydrogen or an ammonium salt group, or contain at least one of an alkyl group, an ether group, and an ester group.

[0018] The conductive powder preferably has an average particle size of 0.05 μm or more and 1.0 μm or less. The conductive powder preferably contains at least one metal powder selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof. The ceramic powder is preferably contained in an amount of 1 mass% or more relative to the total amount of the conductive paste. The ceramic powder preferably contains barium titanate. The ceramic powder preferably has an average particle size of 0.01 μm or more and 0.5 μm or less. The conductive paste preferably further contains an acid dispersant and / or a basic dispersant. The conductive paste is preferably for use in internal electrodes of multilayer ceramic components.

[0019] In a second aspect of the present invention, there is provided an electronic component formed using the conductive paste.

[0020] In a third aspect of the present invention, there is provided a multilayer ceramic capacitor having at least a laminate in which dielectric layers and internal electrode layers are laminated, the internal electrode layers being formed using the above-mentioned conductive paste.

[0021] The conductive paste of the present invention can reduce the difference in thermal shrinkage of a conductive film manufactured using the conductive paste during firing without any special treatment of the conductive powder.Furthermore, the multilayer ceramic capacitor of the present invention can suppress the occurrence of delamination and cracks during firing by forming internal electrodes using the conductive paste.

[0022] Fig. 1 is a perspective view and a cross-sectional view showing a multilayer ceramic capacitor according to an embodiment. Fig. 2 is a graph showing a thermal shrinkage curve obtained by thermomechanical analysis (TMA) measurement of Example 1. Fig. 3 is a photograph, substitute for a drawing, showing an image of a cross section of an evaluation pellet of Example 1 taken by a scanning electron microscope (SEM) at 800°C when fired. Fig. 4 is a photograph, substitute for a drawing, showing an image of a cross section of an evaluation pellet of Comparative Example 1 taken by a SEM at 800°C when fired.

[0023] [Conductive Paste] The conductive paste of the embodiment contains a conductive powder, a ceramic powder, an additive, a binder resin, and an organic solvent. Each component will be described in detail below.

[0024] (Conductive Powder) The conductive powder is not particularly limited, and metal powders can be used. For example, powders of one or more elements selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof can be used. Among these, powders of Ni or its alloys (hereinafter sometimes referred to as "nickel powder") are preferred from the viewpoints of conductivity, corrosion resistance, and cost. As the Ni alloy, for example, an alloy of Ni and at least one element selected from the group consisting of Mn, Cr, Co, Al, Fe, Cu, Zn, Ag, Au, Pt, and Pd can be used. The Ni content in the Ni alloy is, for example, 50% by mass or more, preferably 80% by mass or more. Furthermore, the nickel powder may contain several hundred ppm of element S to suppress rapid gas generation due to partial thermal decomposition of the binder resin during debinding.

[0025] Furthermore, when nickel powder is used as the conductive powder, the manufacturing method is not particularly limited, and it can be manufactured using a conventionally known wet method, dry method, or the like. For example, the nickel powder may be nickel powder produced by a so-called dry method, such as a CVD method, an evaporation quenching method, or a hydrogen reduction method using nickel salt or nickel hydroxide, or may be nickel powder produced by a so-called wet method, such as a wet reduction method using a nickel salt solution with a reducing agent such as hydrazine. Among these, it is preferable to use nickel powder produced by a so-called wet method, such as a wet reduction method. Furthermore, in the conductive paste of this embodiment, the nickel powder does not need to have a coating layer, as in Patent Document 1.

[0026] The average particle size of the conductive powder is preferably 0.01 μm or more and 1.0 μm or less, more preferably 0.01 μm or more and 0.5 μm or less, and even more preferably 0.05 μm or more and 0.4 μm or less. When the average particle size of the conductive powder is within the above range, it can be suitably used as a paste for internal electrodes of thin-film multilayer ceramic capacitors (multilayer ceramic components). Furthermore, the average particle size of the conductive powder may be, for example, 0.3 μm or less, 0.25 μm or less, or 0.2 μm or less. In the conductive paste of this embodiment, even when the average particle size of the conductive powder is within the above range, the difference in thermal shrinkage during firing can be sufficiently reduced.

[0027] The average particle size is a value determined by observation with a scanning electron microscope (SEM), and is the average value (SEM average particle size, number average) obtained by measuring the particle size of each of a plurality of particles from an image observed with an SEM at a magnification of 10,000 times.

[0028] The content of the conductive powder is preferably 30% by mass or more and less than 70% by mass, more preferably 40% by mass or more and 60% by mass or less, based on the total amount of the conductive paste. When the content of the conductive powder is within the above range, the conductive paste has excellent conductivity and dispersibility.

[0029] (Ceramic Powder) The ceramic powder is not particularly limited, and for example, in the case of a paste for an internal electrode of a multilayer ceramic capacitor, a known ceramic powder is appropriately selected depending on the type of multilayer ceramic capacitor to be applied. As the ceramic powder, for example, a perovskite oxide containing Ba and Ti can be used, and preferably barium titanate (BaTiO 3 ) is included.

[0030] The ceramic powder may be a ceramic powder containing barium titanate as a main component and an oxide as a secondary component. Examples of the oxide include oxides of Mn, Cr, Si, Ca, Ba, Mg, V, W, Ta, Nb, and one or more rare earth elements. Examples of the ceramic powder include barium titanate (BaTiO 3Alternatively, a ceramic powder of a perovskite-type oxide ferroelectric may be used in which the Ba atoms or Ti atoms of the above-mentioned alloy are substituted with other atoms such as Sn, Pb, or Zr.

[0031] When used as a conductive paste for internal electrodes, the ceramic powder may have the same composition as the dielectric ceramic powder constituting the green sheet of a multilayer ceramic capacitor (electronic component). This further suppresses cracking due to the difference in thermal contraction at the interface between the dielectric layer and the conductive film during the sintering process. Examples of such ceramic powders include, in addition to those mentioned above, ZnO, ferrite, PZT, BaO, and Al. 2 O 3 , Bi 2 O 3 , R (rare earth element) 2 O 3 , TiO 2 , Nd 2 O 3 The ceramic powder may be one type or two or more types.

[0032] The average particle size of the ceramic powder is, for example, 0.01 μm or more and 0.5 μm or less, preferably 0.01 μm or more and 0.3 μm or less. When the average particle size of the ceramic powder is in the above range, when used as an internal electrode paste, a sufficiently fine, thin, and uniform internal electrode can be formed. The average particle size is a value determined by observation with a scanning electron microscope (SEM), and is the average value (SEM average particle size, number average) obtained by measuring the particle size of each of multiple particles from an image observed with the SEM at a magnification of 50,000 times.

[0033] The content of the ceramic powder is, for example, 1 mass % or more relative to the entire conductive paste. By including a large amount of ceramic powder, the thermal shrinkage behavior of the conductive film can be made closer to that of the green sheet. The upper limit of the ceramic powder content may be 20 mass % or less, 10 mass % or less, 6 mass % or less, 4 mass % or less, 3 mass % or less, or 2 mass % or less. The lower the ceramic powder content, the more improved the continuity of the conductive film, thereby increasing the capacitance of the capacitor. Even if the content of ceramic powder is reduced, the conductive paste of this embodiment can reduce the difference in thermal shrinkage of the conductive film during sintering and reduce the difference in thermal shrinkage behavior with the green sheet.

[0034] The content of the ceramic powder is preferably 2 parts by mass or more relative to 100 parts by mass of the conductive powder, and may be 20 parts by mass or less, 12 parts by mass or less, 8 parts by mass or less, 6 parts by mass or less, or 4 parts by mass or less relative to 100 parts by mass of the conductive powder.

[0035] (Binder Resin) The binder resin contains at least one of a cellulose-based resin and an acetal-based resin. When used as an internal electrode paste, from the viewpoint of improving adhesive strength with the green sheet, an acetal-based resin may be contained, or the acetal-based resin may be used alone. The acetal-based resin preferably contains a butyral-based resin, and more preferably contains polyvinyl butyral (PVB). When the conductive paste contains an acetal-based resin, the difference in thermal shrinkage behavior with the green sheet can be further reduced.

[0036] The content of the acetal resin may be, for example, 20% by mass or more, 40% by mass or more, or 60% by mass or more, based on the total amount of the binder resin. When the content of the acetal resin is within the above range, the adhesiveness is further improved, and the adhesive strength between the dried film and the green sheet (substrate) is improved.

[0037] The upper limit of the acetal resin content is not particularly limited, but may be, for example, 90% by mass or less, 80% by mass or less, or 50% by mass or less, based on the total amount of the binder resin. When the acetal resin content is within the above range, the conductive paste has an appropriate hardness, and therefore, problems such as the printed film not peeling off from the support film and the electrodes being crushed during thermocompression bonding are less likely to occur.

[0038] The weight-average molecular weight (Mw) of the acetal resin may be 30,000 or more and 300,000 or less, 50,000 or more and 200,000 or less, or 100,000 or more and 150,000 or less. The glass transition temperature Tg of the acetal resin may be 50°C or more and 90°C or less, or 60°C or more and 80°C or less. By including the additives described below in addition to the acetal resin having the above properties, a conductive paste with improved adhesion can be obtained. The acetal resins may be used alone or in combination of two or more.

[0039] Examples of cellulose-based resins include methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, and nitrocellulose. When a cellulose-based resin is contained, the solubility in a solvent and the decomposition property by combustion are good. Among the cellulose-based resins, ethyl cellulose is preferred.

[0040] For example, when a cellulose-based resin is contained as the binder resin, the weight-average molecular weight (Mw) may be 10,000 or more and 300,000 or less, 30,000 or more and 250,000 or less, or 50,000 or more and 200,000 or less. The hydroxyl value of the cellulose-based resin is not particularly limited, but is preferably 0.1 mgKOH / g or more and 15 mgKOH / g or less, more preferably 0.5 mgKOH / g or more and 7 mgKOH / g or less, and even more preferably 1.5 mgKOH / g or more and 3 mgKOH / g or less. The cellulose-based resin may be contained alone or in combination of two or more types.

[0041] The content of the cellulose-based resin is not particularly limited, but may be, for example, 20% by mass or more, 40% by mass or more, or 60% by mass or more relative to the total binder resin. Furthermore, when the binder resin contains a cellulose-based resin and an acetal-based resin, the cellulose-based resin may be contained in an amount of 20% by mass or more, 40% by mass or more, or 60% by mass or more relative to the total content (100% by mass) of the cellulose-based resin and the acetal-based resin. When the contents of both resins are within the above ranges, the conductive paste can have an appropriate hardness, and defects such as the printed film not peeling off from the support film or the electrode being crushed during thermocompression bonding are less likely to occur. Furthermore, the thermal shrinkage of the conductive film during firing can be moderated, and the adhesion between the conductive film and the green sheet and the dispersibility of the conductive powder can be improved in a balanced manner. Furthermore, the upper limit of the cellulose-based resin content is not particularly limited, and may be less than 100% by mass, 90% by mass or less, or 80% by mass or less.

[0042] The binder resin may contain other resins such as acrylic resins in addition to the cellulose-based resins and acetal-based resins.

[0043] The content of the binder resin is preferably 0.5% by mass or more and 10% by mass or less, more preferably 1% by mass or more and 7% by mass or less, based on the total amount of the conductive paste. When the content of the binder resin is in the above range, the conductive paste has excellent conductivity and dispersibility.

[0044] The content of the binder resin is preferably 1 part by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 14 parts by mass or less, relative to 100 parts by mass of the conductive powder.

[0045] (Organic Solvent) As the organic solvent, a known organic solvent capable of dissolving the binder resin can be used. In addition, the organic solvent preferably contains a terpene-based solvent (a) and one or more solvents (b) selected from hydrocarbon-based solvents, acetate-based solvents, ether-based solvents, and ketone-based solvents. By containing these organic solvents, excellent compatibility with the binder resin, excellent dispersibility of the filler, and sheet attack on the green sheet can be suppressed.

[0046] Examples of the terpene solvent (a) include dihydroterpineol, terpineol, dihydroterpinyl acetate, and the like, and among these, dihydroterpineol is preferred.

[0047] Examples of the hydrocarbon solvent (b1) include solvents containing tridecane, nonane, cyclohexane, etc., mineral spirits, naphthenic solvents, etc. Among these, mineral spirits are preferred. The content of the hydrocarbon solvent may be 10% by mass or more and 50% by mass or less, or 20% by mass or more and 40% by mass or less, based on the total amount of the organic solvent.

[0048] Examples of the acetate solvent (b2) include isobornyl acetate, isobornyl propionate, isobornyl butyrate, and isobornyl isobutyrate; glycol ether acetates such as ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, 3-methoxy-3-methylbutyl acetate, and 1-methoxypropyl-2-acetate; glycol diacetates such as propylene glycol diacetate, 1,4-butanediol diacetate, 1,3-butylene glycol diacetate, and 1,6-hexanediol diacetate; and cyclohexanol acetate.

[0049] Examples of the ether-based solvent (b3) include propylene glycol monoalkyl ethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether; ethylene glycol ethers such as diethylene glycol mono-2-ethylhexyl ether, ethylene glycol mono-2-ethylhexyl ether, diethylene glycol monohexyl ether, and ethylene glycol monohexyl ether; dipropylene glycol methyl-n-propyl ether, dipropylene glycol methyl-n-butyl ether, and dipropylene glycol dimethyl ether.

[0050] Examples of the ketone solvent (b4) include methyl isobutyl ketone, diisobutyl ketone, etc. When a ketone solvent is contained, it is possible to adjust the viscosity and improve the drying property without impairing the dispersibility.

[0051] The content of the organic solvent (total) is preferably 20% by mass or more and 60% by mass or less, and more preferably 25% by mass or more and 45% by mass or less, based on the total amount of the conductive paste. When the content of the organic solvent is within the above range, the conductive paste has excellent conductivity and dispersibility. The content of the ether-based solvent is preferably 30% by mass or less.

[0052] The content of the organic solvent is preferably 50 parts by mass or more and 130 parts by mass or less, more preferably 60 parts by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the organic solvent is within the above range, the conductive powder has excellent conductivity and dispersibility.

[0053] Furthermore, one type of organic solvent may be used for each type of solvent, or two or more types may be used. The organic solvent may include, for example, a terpene solvent (a) and a hydrocarbon solvent (b1), or may include dihydroterpineol (a) and mineral spirits (b1). When the terpene solvent (a) and the hydrocarbon solvent (b1) are included, it is preferable that the terpene solvent (a) account for 60% by mass to 80% by mass and the hydrocarbon solvent (b1) account for 40% by mass to 20% by mass, based on the total amount of organic solvents.

[0054] The organic solvent may also include at least three types of organic solvents, for example, a terpene solvent (a), a hydrocarbon solvent (b1), and an acetate solvent (b2). Specifically, the organic solvent may include dihydroterpineol (a), mineral spirits (b1), and diethylene glycol monobutyl ether acetate (b2), or may include dihydroterpineol (a), mineral spirits (b1), and isobornyl acetate (b2). When these organic solvents are included, in addition to the above-mentioned effects, the surface smoothness of the dried film is further improved, and the dispersibility of the conductive paste is improved. When at least three types of solvents, namely, the terpene solvent (a), the hydrocarbon solvent (b1), and the acetate solvent (b2), are contained, it is preferable that the terpene solvent (a) is contained in an amount of 30% by mass to 70% by mass, the hydrocarbon solvent (b1) is contained in an amount of 40% by mass to 20% by mass, and the acetate solvent (b2) is contained in an amount of 30% by mass to 10% by mass, relative to the total amount of organic solvents (100% by mass).

[0055] (Additives)

[0056] (a) Phosphate-Based Additive The conductive paste according to this embodiment contains, as an additive, a phosphate-based additive having a structure represented by the following formula (1).

[0057]

[0058] In the above formula (1), R 1 contains at least one of an alkyl group having 6 or more carbon atoms, an ether group having 6 or more carbon atoms, a polyether group, and a polyester group, and R 2 , R 3 are each independently hydrogen or an ammonium salt group, or contain at least one of an alkyl group, an ester group, and an ether group.

[0059] R 1 R contains at least one of an alkyl group having 6 or more carbon atoms, an ether group having 6 or more carbon atoms, a polyether group, and a polyester group. 1Preferably, the alkyl group and the ether group contain a polyether group and a polyester group. Examples of polyether groups include those having an oxyalkylene repeating unit such as oxymethylene, oxyethylene, and oxypropylene. The polyether group and the polyester group may have a polyether structure and a polyester structure, and may also contain other structures. The alkyl group and the ether group may each have one or more methylenes substituted with oxygen, or a portion of the hydrogen atoms constituting the alkyl group and the ether group may be substituted with a substituent. The polyether group and the polyester group may each have 6 or more carbon atoms.

[0060] R 2 , R 3 R are each independently hydrogen or an ammonium salt group, or contain at least one of an alkyl group, an ester group, and an ether group. 2 , R 3 may be hydrogen. The ammonium base may be an alkylammonium base. The alkyl group, ester group, and ether group may have one or more methylenes substituted with oxygen, and some of the hydrogen atoms constituting the alkyl group, ester group, and ether group may be substituted with a substituent. For example, some of the hydrogen atoms constituting the alkyl group may be substituted with a phosphate ester group. 2 , R 3 may each independently be hydrogen, an alkyl group, an ammonium salt group, or an alkyl phosphate ester group.

[0061] The additive may also include a phosphoric acid-based additive having one or more structures selected from the following formulas (2) and (3).

[0062]

[0063]

[0064] In the above formulas (2) and (3), R 1 each independently contains at least one of an alkyl group having 6 or more carbon atoms, an ether group having 6 or more carbon atoms, a polyether group, and a polyester group; R 2’is hydrogen, an ammonium salt group, an alkyl group, or an alkyl phosphate group. 1 The preferred range of R in the above formula (1) is 1 is the same as:

[0065] When the conductive paste contains the phosphoric acid-based additive, the difference in thermal shrinkage of the conductive film is reduced when the pressed body of the conductive film and the green sheet is sintered, and the sintering of the conductive film proceeds relatively slowly. Although the details of the reason for this are unclear, it is thought that, for example, the phosphoric acid ester inhibits the combustion of the binder resin, forming a carbonized layer, which raises the temperature at which the binder resin completely decomposes.

[0066] The weight-average molecular weight of the phosphate additive is preferably 200 or more and 3000 or less. When the molecular weight of the phosphate additive is within the above range, the difference in thermal shrinkage behavior with the green sheet is smaller. The lower limit of the weight-average molecular weight of the phosphate additive may be, for example, 200 or more, 300 or more, 500 or more, or 1000 or more. When the lower limit of the weight-average molecular weight of the phosphate additive is within the above range, the difference in thermal shrinkage may be reduced and dispersibility may be further improved. The upper limit of the weight-average molecular weight of the phosphate additive may be 2500 or less, 2300 or less, or 2000 or less.

[0067] The content of the phosphate additive is preferably 0.03 mass% or more and 1.5 mass% or less with respect to the entire conductive paste. When the content of the phosphate additive is within the above range, sinterability is good and the difference in thermal shrinkage behavior between the conductive film and the ceramic green sheet is reduced. From the viewpoint of further reducing the difference in thermal shrinkage, the content of the phosphate additive may be 0.1 mass% or more with respect to the entire conductive paste. From the viewpoint of the sinterability of the conductive film and the influence of decomposition of the additive on thermal shrinkage, the content of the phosphate additive is preferably 1 mass% or less, more preferably 0.8 mass% or less, with respect to the entire conductive paste. The content of the phosphate additive may be 0.5 mass% or less, or may be 0.3 mass% or less. If the content of the phosphate additive is too high, the sintering behavior may be excessively delayed.

[0068] (b) Dispersant When the conductive paste contains a dispersant, the dispersibility of the conductive powder and ceramic powder can be improved. Examples of dispersants include acidic dispersants, basic dispersants, nonionic dispersants, and amphoteric dispersants. It is preferable to contain at least one of an acidic dispersant and a basic dispersant, and it is more preferable to contain an acidic dispersant. It is also possible to not contain a basic dispersant. These dispersants may be used alone or in combination of two or more.

[0069] The acid dispersant may include a carboxylic acid dispersant such as a higher fatty acid, a polycarboxylic acid dispersant, an acid dispersant having an acidic group such as a polymer surfactant, etc., and preferably includes a polycarboxylic acid dispersant. The polycarboxylic acid dispersant may also be a comb-shaped carboxylic acid having a comb structure.

[0070] The higher fatty acid may be either an unsaturated carboxylic acid or a saturated carboxylic acid, and is not particularly limited, but examples thereof include those having 11 or more carbon atoms, such as stearic acid, oleic acid, myristic acid, palmitic acid, linoleic acid, lauric acid, and linolenic acid. Of these, oleic acid or stearic acid is preferred.

[0071] The acid dispersant may be, for example, oleoyl sarcosine, which is a compound of glycine and oleic acid, or an alkyl monoamine salt type, which is an amide compound using a higher fatty acid such as stearic acid or lauric acid instead of oleic acid.

[0072] Furthermore, from the viewpoint of further improving the effect of suppressing separation between the conductive powder and the ceramic powder, a dicarboxylic acid may be contained. The dicarboxylic acid is a carboxylic acid having two carboxyl groups (COO- groups). The average molecular weight of the dicarboxylic acid is not particularly limited, but may be, for example, 200 or more and 1,000 or less.

[0073] Examples of basic dispersants include aliphatic amines such as laurylamine, rosinamine, cetylamine, myristylamine, and stearylamine. When the conductive paste contains the acid dispersant and the basic dispersant, the conductive paste may have better dispersibility and viscosity stability over time.

[0074] The dispersant is contained in an amount of, for example, 0.01% by mass or more and 3% by mass or less with respect to the entire conductive paste. The upper limit of the dispersant content may be 2% by mass or less, 1% by mass or less, or 0.7% by mass or less. When the dispersant content is within the above range, the dispersibility of the conductive paste can be improved and sheet attack can be suppressed. When the dispersant content is high, the difference in thermal shrinkage behavior with the dielectric increases. However, in this embodiment, since the phosphate-based additive is contained, the difference in thermal shrinkage of the conductive film during sintering can be reduced, and the difference in thermal shrinkage behavior with the dielectric can be reduced, even when the dispersant content is high.

[0075] (c) Other Additives The conductive paste of the present embodiment may contain other additives in addition to the above components, as necessary. Examples of other additives that can be used include conventionally known additives such as antifoaming agents, plasticizers, surfactants, and thickeners.

[0076] (Characteristics of the Conductive Paste) (a) Surface Roughness) The conductive paste according to this embodiment is applied to a substrate using an applicator to a wet film thickness of 10 μm, and the surface roughness (Sa) of the dried film obtained by drying at 120° C. for 10 minutes may be 0.10 μm or less, 0.07 μm or less, or 0.05 μm or less. The surface roughness Sa (arithmetic mean roughness) of the dried film is also one of the indicators of the dispersibility of the conductive paste. The lower limit of the surface roughness Sa is not particularly limited, but a value greater than 0 and a smaller value is preferable.

[0077] [Method for Producing Conductive Paste] The method for producing the conductive paste according to this embodiment is not particularly limited, and a conventionally known method can be used. The conductive paste can be produced, for example, by stirring and kneading the above-mentioned components using a triple-roll mill, a ball mill, a mixer, a high-pressure homogenizer, or the like.

[0078] [Thermal Shrinkage Behavior] The present inventors conducted extensive research to solve the above-mentioned problems, and as a result, they found that a conductive paste containing a conductive powder, a ceramic powder, an additive, a resin, and an organic solvent, when having a specific composition, can suppress a rapid dimensional change during sintering of a conductive film formed using the conductive paste, i.e., can reduce the difference in thermal shrinkage, even when the particle size of the conductive powder is small, and thus completed the present invention.

[0079] It has been thought that a large difference between the thermal shrinkage onset temperature (sintering onset temperature) of the conductive powder and the thermal shrinkage onset temperature (sintering onset temperature) of the green sheet results in a difference in thermal shrinkage due to sintering over a wider temperature range. Therefore, as shown in Patent Document 1 and other publications, efforts have been made to bring the thermal shrinkage onset temperature of the conductive powder closer to the thermal shrinkage onset temperature of the ceramic dielectric. Cracks can occur, for example, due to gases generated when organic matter is decomposed during binder removal. Furthermore, cracks can occur due to the decomposition of remaining organic matter during firing and the difference in thermal shrinkage due to the sintering of the conductive powder. However, the influence of organic matter on the thermal shrinkage of the conductive film has not received much attention.

[0080] However, while the particle size of the conductive powder used in conductive pastes has recently been reduced, lowering the thermal shrinkage onset temperature of the conductive film, the conductive paste of this embodiment not only raises the thermal shrinkage onset temperature, bringing the thermal shrinkage behavior of the conductive film closer to that of the green sheet, but also reduces the difference in thermal shrinkage of the conductive film within a specific temperature range during sintering, thereby allowing the sintering reaction to proceed more slowly and reducing the occurrence of delamination and cracking. When the conductive paste has the above composition, the sintering of the conductive film proceeds slowly, thereby suppressing the occurrence of delamination and cracking. Conventionally, ceramic powder (dielectric powder) such as barium titanate used in green sheets has been added to the conductive paste to bring the thermal shrinkage behavior of the conductive film closer to that of the green sheet. However, the conductive paste of this embodiment allows the amount of ceramic powder added to be reduced.

[0081] (a) Difference in Thermal Shrinkage Rate During Firing For example, when the thermal shrinkage rate (dimensional change rate) of evaluation pellets prepared using the conductive paste of this embodiment by the following method is measured using a thermomechanical analyzer (TMA), the difference in thermal shrinkage rate at 600°C or higher and 900°C or lower is preferably 10% or less. In this specification, the thermal shrinkage rate at a temperature (t°C) refers to the difference in the dimension (L 0 ) means the rate of change (%) of dimension at t ° C. 1 ℃~t 2 The difference in thermal shrinkage at t 1 ℃~t 2 This refers to the difference between the maximum and minimum values ​​of the thermal shrinkage rate between temperatures in °C.

[0082] (Method of Preparing Evaluation Pellets) The conductive paste is dried at 120°C for 40 minutes to obtain a dry conductive sheet. The obtained dry conductive sheet is pulverized to obtain a dry powder sample. 0.15 g of the obtained dry powder sample is placed in a cylindrical mold (bottom diameter 0.5 cm) and subjected to a pressure of 1000 kgf / cm. 2 A pressure of 1.5 mm was applied to prepare a pellet for evaluation (diameter 5 mm x thickness 1.5 mm).

[0083] The prepared pellets for evaluation were fired under nitrogen at 310°C for 3 hours, and then heated from 25°C to 1300°C at a rate of 5°C / min in a mixed gas atmosphere of nitrogen gas containing 0.15% hydrogen and water vapor gas, each at a gas flow rate of 200 ml / min, and the thermal shrinkage (dimensional change rate) was measured using a thermomechanical analyzer.

[0084] Here, the thermal shrinkage rate (dimensional change rate) α at a temperature t°C is calculated by the following formula: α = 100 × (L 0 -L) / L 0 L 0 : Height of test piece (evaluation pellet) before measurement L: Height of test piece (evaluation pellet) during measurement (temperature t°C)

[0085] Furthermore, the difference in thermal shrinkage rate between evaluation pellets produced using the conductive paste of this embodiment at 600°C or higher and 900°C or lower is more preferably 9% or lower, even more preferably 8% or lower, and may be 7% or lower. The lower limit of the thermal shrinkage difference is not particularly limited, and may be, for example, 1% or higher, 2% or higher, 4% or higher, or 5% or higher. If the lower limit of the thermal shrinkage difference is too low, the sintering behavior of the conductive film may be excessively delayed.

[0086] Furthermore, for example, the difference in thermal shrinkage rate of the above-mentioned evaluation pellets at 550°C or higher and 750°C or lower may be 7% or lower, 6% or lower, or 5% or lower. The lower limit of the difference in thermal shrinkage rate is not particularly limited, but may be, for example, 0.5% or higher. Note that for a conductive paste produced under similar conditions except that it does not contain the phosphoric acid-based additive, the difference in thermal shrinkage rate at 550°C or higher and 750°C or lower exceeds 7%.

[0087] Furthermore, for example, the difference in the thermal shrinkage rate of the evaluation pellets at temperatures from 900° C. to 1200° C. may be 5% or more, or may be 7% or more. Since the thermal shrinkage of the dielectric layer (green sheet) increases sharply at around 1000° C., when the difference in the thermal shrinkage rate of the evaluation pellets at temperatures from 900° C. to 1200° C. is within the above range, the thermal shrinkage behavior of the evaluation pellets can be made to approach that of the dielectric layer.

[0088] As described above, the conductive film using the conductive paste of this embodiment has a small difference in thermal shrinkage during sintering and undergoes gentle thermal shrinkage. Furthermore, the conductive paste of this embodiment has a final thermal shrinkage amount that is similar to the final thermal shrinkage amount of the green sheet (thermal shrinkage: approximately 20%), so delamination and cracking are effectively suppressed. For example, the difference in thermal shrinkage between 25°C and 1300°C for evaluation pellets using the conductive paste of this embodiment may be, for example, 15% to 25%, or 17% to 23%. Furthermore, the difference in thermal shrinkage between 25°C and 1300°C for the green sheet used in the multilayer ceramic capacitor of this embodiment may also be the same as the range for the evaluation pellets.

[0089] (b) Sintering Start Temperature The sintering start temperature (thermal shrinkage start temperature) of the evaluation pellets produced using the conductive paste of this embodiment may be, for example, 500°C to 700°C, or 500°C to 650°C. The conductive paste of this embodiment has a relatively high thermal shrinkage start temperature compared to a conductive paste produced under similar conditions except that it does not contain a phosphate-based additive. Furthermore, the conductive paste of this embodiment reduces the amount of change in thermal shrinkage (dimensional change rate) from the start of sintering to approximately 900°C, for example, so that sintering proceeds slowly, thereby suppressing the occurrence of delamination and cracks. The thermal shrinkage start temperature refers to the temperature at which the thermal shrinkage rate reaches 5% on the thermal shrinkage curve.

[0090] [Multilayer Ceramic Capacitor] The conductive paste of this embodiment can be suitably used in electronic components such as multilayer ceramic capacitors. The multilayer ceramic capacitor has, for example, dielectric layers formed using dielectric green sheets and internal electrode layers formed using the conductive paste.

[0091] Hereinafter, embodiments of the multilayer ceramic capacitor of the present invention will be described with reference to the drawings. The drawings may be represented schematically or at a different scale as appropriate. The positions and directions of components will be described with reference to an XYZ Cartesian coordinate system shown in FIG. 1 and other figures. In this XYZ Cartesian coordinate system, the X and Y directions are horizontal, and the Z direction is vertical (up-down).

[0092] 1A and 1B are diagrams showing a multilayer ceramic capacitor 1. The multilayer ceramic capacitor 1 includes a ceramic laminate 10 in which dielectric layers 12 and internal electrode layers 11 are alternately stacked, and external electrodes 20.

[0093] A method for manufacturing a multilayer ceramic capacitor using the above-described conductive paste will now be described. First, the conductive paste is screen-printed on ceramic green sheets and dried to form a dry film. A plurality of ceramic green sheets, each having this dry film on its upper surface, are laminated by pressure bonding to obtain a laminate, which is then fired and integrated to produce a ceramic laminate 10 in which internal electrode layers 11 and dielectric layers 12 are alternately laminated. A pair of external electrodes 20 is then formed on both ends of the ceramic laminate 10 to produce a multilayer ceramic capacitor 1. This method will now be described in more detail.

[0094] First, a green sheet, which is an unfired ceramic sheet, is prepared. For example, this green sheet can be prepared by adding a binder resin such as polyvinyl butyral and an organic solvent such as terpineol to a predetermined ceramic raw material powder such as barium titanate to form a dielectric layer paste. The paste is then applied to a support film such as a PET film in a sheet form and dried to remove the solvent. The thickness of the dielectric layer made of the green sheet is not particularly limited, but is preferably 0.05 μm or more and 3 μm or less in view of the demand for miniaturization of multilayer ceramic capacitors.

[0095] Next, the above-mentioned conductive paste is printed and applied to one side of a green sheet, and then dried to prepare multiple green sheets each having a dry film (conductive film) formed on one side. The thickness of the dry film formed from the conductive paste is preferably 1 μm or less after drying, in consideration of the need to thin the internal electrode layers 11. Next, the green sheets are peeled from the support film, and the green sheets and the conductive film formed on one side thereof are stacked alternately, followed by a heat and pressure treatment to obtain a laminate. Protective ceramic green sheets not coated with the conductive paste may also be placed on both sides of the laminate.

[0096] Next, the laminate is cut to a predetermined size to form green chips, and the green chips are subjected to a binder removal treatment and fired in a reducing atmosphere to produce a fired laminated ceramic body (ceramic laminate 10). The atmosphere in the binder removal treatment is air or N 2 It is preferable to use a gas atmosphere. The temperature during the binder removal treatment is, for example, 200°C or higher and 400°C or lower. Furthermore, it is preferable to hold the above temperature for 0.5 hours or higher and 24 hours or lower during the binder removal treatment. Furthermore, the firing is performed in a reducing atmosphere to suppress oxidation of the metal used in the conductive film, and the temperature during firing of the laminate is, for example, 1000°C or higher and 1350°C or lower, and the temperature holding time during firing is, for example, 0.5 hours or higher and 8 hours or lower.

[0097] By firing the green chip, the organic binder in the ceramic green sheet is completely removed, and the ceramic raw material powder is fired to form the ceramic dielectric layer 12. Also, the organic vehicle in the conductive film is removed, and the nickel powder or the alloy powder mainly composed of nickel is sintered or melted and integrated to form the internal electrode layer 11, thereby forming a multilayer ceramic fired body in which a plurality of dielectric layers 12 and internal electrode layers 11 are alternately stacked. Note that, from the viewpoint of taking oxygen into the dielectric layer to increase reliability and suppressing reoxidation of the internal electrodes, the fired multilayer ceramic fired body may be subjected to an annealing treatment.

[0098] Then, a pair of external electrodes 20 is provided on the produced fired laminated ceramic body, thereby manufacturing the multilayer ceramic capacitor 1. For example, the external electrodes 20 include an external electrode layer 21 and a plating layer 22. The external electrode layer 21 is electrically connected to the internal electrode layer 11. Note that, for example, copper, nickel, or an alloy thereof can be suitably used as the material for the external electrodes 20. The external electrodes 20 may be provided on the laminate before firing. Note that, electronic components other than a multilayer ceramic capacitor can also be used as the electronic component.

[0099] EXAMPLES The present invention will be described in detail below based on examples and comparative examples, but the present invention is not limited to these examples.

[0100] [Evaluation Method] (Evaluation of Thermal Shrinkage Behavior) (i) Preparation of Evaluation Pellets The obtained conductive paste of Example 1 was dried at 120°C for 40 minutes, and the obtained dried conductive sheet was pulverized to obtain a dry powder sample. 0.15 g of the prepared dry powder sample was placed in a cylindrical mold (bottom diameter 0.5 cm) and subjected to a pressure of 1000 kgf / cm 2 A pressure of 1000 psi was applied to prepare pellets for evaluation.

[0101] (ii) Measurement of Thermal Shrinkage Behavior Next, the prepared evaluation pellets were fired in a nitrogen atmosphere at 310°C for 3 hours to remove the binder. The binder removal behavior can be confirmed by TMA. Next, the evaluation pellets were returned to room temperature, and the thermal shrinkage curve was measured by TMA. Here, the sample loading was 10.0 g, the atmosphere was a mixed gas of nitrogen gas containing 0.15% hydrogen and water vapor gas at a gas flow rate of 200 ml / min, the temperature was increased by 5°C / min, and the measurement temperature range was 25°C to 1300°C. From the measurement data, the difference in thermal shrinkage rate between 600°C and 900°C was calculated. The evaluation results are shown in Tables 1 to 3.

[0102] (Evaluation of Film Properties) The dispersibility of the conductive paste was evaluated by the following method.

[0103] A sample was printed on a glass substrate (2 inches) (GAP thickness = 10 μm) and dried. Drying was performed in an air atmosphere at a maximum temperature of 120 to 150 °C in a belt furnace. The dried film (2 cm x 2 cm, thickness 2 μm) obtained after drying was observed at ×100 (eyepiece, objective; each 10x) using an optical microscope (Eclipse LV100D-U, Nikon Solutions Corporation) while illuminating the backside of the glass substrate with light (backlight) to confirm the presence or absence of lumps. If no lumps were observed, the dispersibility of the paste was judged to be good (◯), and if one or more lumps were observed, the dispersibility of the paste was judged to be poor (×).

[0104] (Evaluation of Sheet Attack) The sheet attack of the conductive paste was evaluated as follows: "Sheet attack" refers to a phenomenon in which the binder resin contained in the green sheet is dissolved by the components of the conductive paste, causing holes and wrinkles in the green sheet.

[0105] First, the conductive paste was screen-printed onto a green sheet. A 325-mesh, 1.8 x 1.8 cm pattern screen was used for printing. After printing, the sheet was dried at 75°C for 10 minutes, and then the back side (green sheet side) was checked using an optical microscope (Eclipse LV100D-U, Nikon Solutions Corporation) to check whether holes or thinning had occurred in the green sheet due to dissolution and swelling. Evaluation was based on the following criteria: ◯: No holes or thinning were observed in the green sheet. ×: Some holes or thinning were observed in the green sheet.

[0106] (Evaluation of Surface Roughness) The obtained conductive paste was applied to a glass substrate using an applicator to a wet film thickness of 10 μm, and dried at 120° C. for 10 minutes. The average surface roughness Sa (μm) of the obtained dried film was measured using a laser microscope (OLS-5000, Evident Co., Ltd.).

[0107] [Materials Used] (Conductive Powder) Ni powder (SEM average particle size: 0.18 μm) was used as the conductive powder.

[0108] (Ceramic Powder) As the ceramic powder, barium titanate (BaTiO 3 (SEM average particle size: 0.05 μm) was used.

[0109] (Binder Resin) As the binder resin, ethyl cellulose resin (EC) and polyvinyl butyral resin (PVB) were used.

[0110] (Dispersant) In the examples and comparative examples, the dispersant commonly contained was an acid dispersant, which was a polycarboxylic acid dispersant having polyoxyalkylene as a graft chain.

[0111] (Additives) As phosphoric acid-based additives, the following A-1, A-2, A-3, and A-4, and phosphoric acid were used. A-1: ​​Compound of formula (1) in which R 1 contains polyether groups and polyester groups, and R 2 , R 3 A-2: A compound of formula (1) containing a phosphate additive in which R is hydrogen (weight average molecular weight: about 1600). 1contains polyether groups and polyester groups, and R 2 , R 3 A-3: A compound of formula (1) containing a phosphate additive in which R is an alkylol ammonium salt group (weight average molecular weight: about 1400). 1 contains polyether groups and polyester groups, and R 2 is hydrogen, and R 3 A-4: A compound of formula (1) containing a phosphate additive in which R is an alkyl ammonium salt group (weight average molecular weight: about 1800). 1 contains an ether group having 6 or more carbon atoms, and R 2 , R 3 is hydrogen (weight average molecular weight: about 750).

[0112] As comparative examples, the following additives were used in place of the phosphoric acid-based additives used in the examples: Z: oleoyl sarcosine G: oxyethylene lauryl amine

[0113] (Organic Solvent) As the organic solvent, dihydroterpineol (DHT), mineral spirits (MSA), and diethylene glycol monobutyl ether acetate (BCA) were used.

[0114] [Example 1] A conductive paste was prepared by mixing 50% by mass of conductive powder, 4% by mass of ceramic powder, 0.15% by mass of dispersant, 0.25% by mass of the above-mentioned "A-1" as a phosphoric acid-based additive, 3% by mass of binder resin (EC:PVB = 6:4 (mass ratio)), and 42.6% by mass of organic solvent (DHT:MA = 7:3 (mass ratio)) to make a total of 100% by mass. The contents of each material in the conductive paste and the evaluation results of the thermal shrinkage behavior are shown in Table 1 and Figure 2.

[0115] [Examples 2 to 14, Comparative Examples 1 to 5] Conductive pastes were prepared and evaluated in the same manner as in Example 1, except that the particle size of the conductive powder, the content of the ceramic powder, the content of the dispersant, the type and content of the additive, the type and content of the binder resin, and the type and content of the organic solvent were set as shown in Tables 1 to 3. The content of each material in the conductive paste and the evaluation results are shown in Tables 1 to 3.

[0116]

[0117]

[0118]

[0119] (Evaluation Results) Table 1 shows the evaluation results of the conductive pastes of Examples 1 to 9 and Comparative Examples 1 to 5, in which the type and content of additive, the type of binder resin, and the type of organic solvent were changed. Compared to the conductive pastes of Comparative Examples 1 to 3, which do not contain the phosphoric acid-based additive represented by formula (1), the conductive pastes of Examples 1 to 9 had a smaller difference in thermal shrinkage between 600°C and 900°C, did not produce lumps or sheet attack, and had small surface roughness. In the case of Comparative Example 4, which contained phosphoric acid as an additive, lumps were produced, and in the case of Comparative Example 5, which contained only terpineol (TPO, a terpene-based solvent) as the organic solvent, sheet attack occurred.

[0120] In addition, in both Example 4, in which the binder resin is EC only, and Example 5, in which the binder resin is PVB only, the difference in thermal shrinkage can be reduced.

[0121] Table 2 shows the ceramic powder (BaTiO 3 The evaluation results of the conductive pastes of Examples 1, 9, and 10 in which the content of ceramic powder was changed are shown below. As shown in Example 10 in Table 2, when the content of ceramic powder is large, the thermal shrinkage of the internal electrode layers can be further suppressed (compare Example 1 and Example 9 in Table 2). Furthermore, as shown in Examples 11 and 12 in Table 2, it can be seen that rapid thermal shrinkage can be suppressed even when the content of ceramic powder is reduced.

[0122] Table 3 shows the evaluation results of the conductive pastes of Examples 1, 13, and 14, in which the particle size of the conductive powder (Ni powder) was changed. Table 3 shows that the larger the particle size of the Ni powder, the smaller the difference in thermal shrinkage, but even in Example 14, which has a small particle size, the difference in thermal shrinkage was sufficiently reduced.

[0123] The thermal shrinkage curve of the evaluation pellets of Example 1 is shown in Figure 2. As can be seen from Figure 2, in the case of the evaluation pellets of Example 1, the thermal shrinkage initiation temperature at which the thermal shrinkage rate (dimensional change rate) becomes 5% is relatively low at 550°C. However, in the temperature range of 550°C to 750°C, the thermal shrinkage curve is upwardly convex, and the thermal shrinkage difference, i.e., the degree of shrinkage, is small. Furthermore, in the temperature range of 600°C to 900°C, the thermal shrinkage curve is also generally upwardly convex, and is particularly upwardly convex in the temperature range of 800°C to 900°C, and the thermal shrinkage difference is small.

[0124] Fig. 3 shows an image of the cross section of the evaluation pellet of Example 1 taken by SEM (scanning electron microscope) at 800°C, and Fig. 4 shows an image of the cross section of the evaluation pellet of Comparative Example 1 taken by SEM at 800°C. It was confirmed that the evaluation pellet of Example 1 (Fig. 3) had more voids at 800°C in the firing step than the evaluation pellet of Comparative Example 1 (Fig. 4), and sintering proceeded more slowly.

[0125] When the conductive paste of the present invention is used to form internal electrodes of a multilayer ceramic capacitor, a highly reliable multilayer ceramic capacitor can be obtained with high productivity. Therefore, the conductive paste of the present invention is particularly suitable for use as internal electrodes of multilayer ceramic capacitors, which are chip components in electronic devices such as mobile phones and digital devices that are becoming increasingly miniaturized.

[0126] The technical scope of the present invention is not limited to the aspects described in the above-mentioned embodiments. One or more of the requirements described in the above-mentioned embodiments may be omitted. Furthermore, the requirements described in the above-mentioned embodiments may be combined as appropriate. Furthermore, to the extent permitted by law, the disclosures of all documents cited in the above-mentioned embodiments are incorporated by reference into this specification. Furthermore, to the extent permitted by law, the contents of Japanese Patent Application No. 2023-110358 are incorporated by reference into this specification.

[0127] REFERENCE SIGNS LIST 1 Multilayer ceramic capacitor 10 Ceramic laminate 11 Internal electrode layer 12 Dielectric layer 20 External electrode 21 External electrode layer 22 Plated layer

Claims

1. A conductive paste comprising a conductive powder, a ceramic powder, an additive, a binder resin and an organic solvent, wherein the additive comprises a phosphoric acid-based additive having a structure represented by the following structural formula (1) in an amount of 0.03 mass% to 1.5 mass% based on the total amount of the conductive paste, the organic solvent comprises a terpene-based solvent (a) and at least one solvent (b) selected from a hydrocarbon-based solvent, an acetate-based solvent, an ether-based solvent, and a ketone-based solvent, and the binder resin comprises at least one of a cellulose-based resin and an acetal-based resin. (However, R 1 contains at least one of an alkyl group having 6 or more carbon atoms, an ether group having 6 or more carbon atoms, a polyether group, and a polyester group; R 2 , R 3 are each independently hydrogen or an ammonium salt group, or contain at least one of an alkyl group, an ester group, and an ether group.

2. The conductive paste according to claim 1, wherein the conductive powder has an average particle size of 0.05 μm or more and 1.0 μm or less.

3. The conductive paste according to claim 1 or 2, wherein the conductive powder contains at least one metal powder selected from the group consisting of Ni, Pd, Pt, Au, Ag, Cu and alloys thereof.

4. The conductive paste according to claim 1 or 2, wherein the ceramic powder is contained in an amount of 1 mass % or more based on the total amount of the conductive paste.

5. The conductive paste according to claim 1 or 2, wherein the ceramic powder contains barium titanate.

6. The conductive paste according to claim 5, wherein the ceramic powder has an average particle size of 0.01 μm or more and 0.5 μm or less.

7. The conductive paste according to claim 1 or 2, further comprising an acidic dispersant or a basic dispersant.

8. The conductive paste according to claim 1 or 2, which is used for internal electrodes of multilayer ceramic parts.

9. An electronic component formed using the conductive paste according to claim 1 or 2.

10. A multilayer ceramic capacitor comprising at least a laminate in which dielectric layers and internal electrode layers are laminated, the internal electrode layers being formed using the conductive paste according to claim 8.