Molding resin composition and electronic component device

MYPI2026000120A0Undetermined Publication Date: 2025-01-10RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2026000120
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-10
Filing Date
2024-07-09
Publication Date
2025-01-10

AI Technical Summary

Technical Problem

Resin compositions containing alumina as an inorganic filler for electronic component devices face challenges with poor mold releasability and surface staining, which affect production efficiency and product quality.

Method used

A molding resin composition incorporating epoxy resin, a phenol curing agent, and a mold release agent containing polyethylene oxide with specific molecular weight and acid value ranges, along with alumina as the inorganic filler, to enhance mold releasability and prevent surface staining.

Benefits of technology

The composition achieves improved mold releasability and reduced surface staining, enhancing the production efficiency and quality of electronic component devices.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A molding resin composition contains an epoxy resin, a curing agent, a release agent containing oxidized polyethylene, and an inorganic filler containing alumina, in which a parameter P calculated by formula A below based on the weight average molecular weight of the oxidized polyethylene and the content of the oxidized polyethylene with respect to 100 parts by mass of the epoxy resin is 300 to 1500. In formula A below, Mi represents a weight average molecular weight of an i-th type of oxidized polyethylene, and Ri represents the content of the i-th type of oxidized polyethylene with respect to 100 parts by mass of the epoxy resin.
Need to check novelty before this filing date? Find Prior Art

Description

Molding resin composition and electronic component device

[0001] The present disclosure relates to a molding resin composition and an electronic component device.

[0002] In the field of element encapsulation of electronic component devices such as transistors, ICs (integrated circuits), and LSIs (large-scale integrations), resin encapsulation has traditionally been mainstream from the standpoints of productivity, cost, etc., and epoxy resin compositions have been widely used as encapsulants because epoxy resins have an excellent balance of various properties, such as electrical properties, moisture resistance, heat resistance, mechanical properties, and adhesion to insert products.

[0003] On the other hand, with the recent progress in higher output and higher density of electronic component devices, the amount of heat generated by electronic component devices tends to increase. Therefore, there is a demand for improving the thermal conductivity of encapsulants to enhance the heat dissipation properties of electronic component devices. For example, Patent Document 1 discloses an encapsulating epoxy resin composition in which 60 volume % or more of the inorganic filler is alumina in order to enhance thermal conductivity.

[0004] Patent Document 1: Japanese Patent Application Laid-Open No. 2014-31460

[0005] However, resin compositions containing alumina as an inorganic filler may have inferior fluidity compared to resin compositions containing silica as an inorganic filler. Furthermore, resin compositions containing alumina as an inorganic filler tend to cause surface contamination of molded products more easily compared to resin compositions containing silica as an inorganic filler. Therefore, in order to improve the production efficiency of electronic component devices and achieve good continuous moldability, it is desirable to further improve the mold release properties of resin compositions containing alumina as an inorganic filler and suppress surface contamination of molded products. The present disclosure has been made in consideration of the above-mentioned conventional circumstances, and aims to provide a molding resin composition containing alumina as an inorganic filler, which has excellent mold release properties and can suppress surface contamination of molded products, and an electronic component device using the same.

[0006] Specific means for achieving the above object are as follows: <1> A molding resin composition comprising an epoxy resin, a curing agent, a release agent containing polyethylene oxide, and an inorganic filler containing alumina, wherein a parameter P calculated by the following formula A based on the weight-average molecular weight of the polyethylene oxide and the content of the polyethylene oxide relative to 100 parts by mass of the epoxy resin is 300 to 1500:

[0007]

[0008] In Formula A, Mi represents the weight-average molecular weight of the ith polyethylene oxide, and Ri represents the content of the ith polyethylene oxide per 100 parts by mass of the epoxy resin. <2> The molding resin composition according to <1>, wherein the polyethylene oxide has a weight-average molecular weight of 3,500 or more. <3> The molding resin composition according to <1> or <2>, wherein the polyethylene oxidized has an acid value of 2 mg KOH / g to 50 mg KOH / g. <4> The molding resin composition according to any one of <1> to <3>, wherein the polyethylene oxidized comprises a linear polyethylene oxide. <5> The molding resin composition according to any one of <1> to <4>, wherein the polyethylene oxidized comprises a branched polyethylene oxide. <6> The molding resin composition according to any one of <1> to <5>, wherein the epoxy resin comprises a biphenyl-type epoxy resin. <7> The molding resin composition according to <6>, wherein the biphenyl-type epoxy resin accounts for 50% by mass or more of the total epoxy resins. <8> The molding resin composition according to any one of <1> to <7>, wherein the curing agent comprises a phenolic curing agent. <9> The molding resin composition according to <8>, wherein the phenolic curing agent accounts for 50% by mass or more of the total curing agents. <10> The molding resin composition according to <8> or <9>, wherein the hydroxyl equivalent of the phenolic curing agent is 70 g / eq to 1000 g / eq. <11> The molding resin composition according to any one of <1> to <10>, wherein the alumina accounts for 50% by volume or more of the total inorganic filler. <12> The molding resin composition according to any one of <1> to <11>, further comprising a copolymer of an α-olefin having 5 to 30 carbon atoms and at least one of maleic anhydride and a maleic anhydride derivative. <13> The molding resin composition according to <12>, wherein the copolymer comprises a structural unit represented by the following general formula (C) and a structural unit represented by the following general formula (D):

[0009]

[0010] (In general formula (C) and general formula (D), R 11 represents a monovalent aliphatic hydrocarbon group having 3 to 28 carbon atoms, and R 12 and R13 each independently represents a hydrogen atom, an alkyl group, or an aryl group.) <14> An electronic component device comprising: a support member; an electronic component placed on the support member; and a cured product of the molding resin composition according to any one of <1> to <13> that encapsulates the electronic component.

[0011] According to the present disclosure, it is possible to provide a molding resin composition that contains alumina as an inorganic filler, has excellent mold releasability, and is capable of suppressing contamination of the surface of a molded product, and an electronic component device using the same.

[0012] The present disclosure will be described in detail below. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless otherwise specified. The same applies to numerical values ​​and their ranges, and do not limit the present disclosure.

[0013] In the present disclosure, the term "process" includes not only processes that are independent of other processes, but also processes that cannot be clearly distinguished from other processes as long as the purpose of the process is achieved. In the present disclosure, numerical ranges indicated using "to" include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in the present disclosure, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in numerical ranges described in the present disclosure, the upper or lower limit value of that numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple corresponding substances. When multiple substances corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, particles corresponding to each component may contain multiple types of particles. When multiple types of particles corresponding to each component are present in a composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified.

[0014] <Molding Resin Composition> The molding resin composition of the present disclosure contains an epoxy resin, a curing agent, a release agent containing polyethylene oxide, and an inorganic filler containing alumina, and has a parameter P calculated by the following formula A based on the weight-average molecular weight of the polyethylene oxide and the content of the polyethylene oxide relative to 100 parts by mass of the epoxy resin, of 300 to 1500.

[0015]

[0016] In formula A, Mi represents the weight average molecular weight of the i-th type of polyethylene oxide, and Ri represents the content (parts by mass) of the i-th type of polyethylene oxide relative to 100 parts by mass of the epoxy resin.

[0017] As a result of extensive research, the present inventors have found that when alumina, which has inferior mold releasability compared to silica, is used as an inorganic filler, by setting parameter P, calculated by the above formula A based on the weight-average molecular weight of polyethylene oxide and the content of polyethylene oxide relative to 100 parts by mass of epoxy resin, in the range of 300 to 1500, it is possible to improve mold releasability and suppress contamination of the surface of a molded product, and have completed the present invention.

[0018] Each component constituting the molding resin composition will be described below. The molding resin composition of the present disclosure contains an epoxy resin, a curing agent, a release agent containing polyethylene oxide, and an inorganic filler containing alumina, and may optionally contain other components such as a copolymer of an α-olefin having 5 to 30 carbon atoms with at least one of maleic anhydride and a maleic anhydride derivative (hereinafter, sometimes referred to as a specific copolymer).

[0019] (Epoxy Resin) The molding resin composition of the present disclosure contains an epoxy resin. The type of epoxy resin is not particularly limited as long as it has an epoxy group in the molecule.

[0020] Specific examples of epoxy resins include novolac epoxy resins (phenol novolac epoxy resins, o-cresol novolac epoxy resins, etc.) obtained by epoxidizing novolac resins obtained by condensing or co-condensing, under an acid catalyst, at least one phenolic compound selected from the group consisting of phenolic compounds such as phenol, cresol, xylenol, resorcinol, catechol, bisphenol A, bisphenol F, etc., and naphthol compounds such as α-naphthol, β-naphthol, dihydroxynaphthalene, etc., with an aliphatic aldehyde compound such as formaldehyde, acetaldehyde, propionaldehyde, etc.; triphenylmethane epoxy resins obtained by epoxidizing triphenylmethane phenolic resins obtained by condensing or co-condensing, under an acid catalyst, the above-mentioned phenolic compound with an aromatic aldehyde compound such as benzaldehyde, salicylaldehyde, etc.; and novolac resins obtained by co-condensing, under an acid catalyst, the above-mentioned phenolic compound and naphthol compound with an aldehyde compound. diphenylmethane-type epoxy resins which are diglycidyl ethers of bisphenol A, bisphenol F, or the like; biphenyl-type epoxy resins which are diglycidyl ethers of alkyl-substituted or unsubstituted biphenols; stilbene-type epoxy resins which are diglycidyl ethers of stilbene-based phenolic compounds; sulfur-containing epoxy resins which are diglycidyl ethers of bisphenol S, or the like; epoxy resins which are glycidyl ethers of alcohols such as butanediol, polyethylene glycol, and polypropylene glycol; glycidyl ester-type epoxy resins which are glycidyl esters of polycarboxylic acids such as phthalic acid, isophthalic acid, and tetrahydrophthalic acid; glycidylamine-type epoxy resins in which active hydrogen bonded to nitrogen atoms of aniline, diaminodiphenylmethane, isocyanuric acid, or the like is substituted with a glycidyl group; dicyclopentadiene-type epoxy resins in which a co-condensation resin of dicyclopentadiene and a phenolic compound is epoxidized;Alicyclic epoxy resins such as vinylcyclohexene diepoxide, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, and 2-(3,4-epoxy)cyclohexyl-5,5-spiro(3,4-epoxy)cyclohexane-m-dioxane, which are produced by epoxidizing an intramolecular olefin bond; paraxylylene-modified epoxy resins, which are glycidyl ethers of paraxylylene-modified phenolic resins; metaxylylene-modified epoxy resins, which are glycidyl ethers of metaxylylene-modified phenolic resins; terpene-modified epoxy resins, which are glycidyl ethers of terpene-modified phenolic resins; and dicyclopentadiene-modified phenolic resins, which are glycidyl ethers of dicyclopentadiene-modified phenolic resins. Examples of the epoxy resin include pentadiene-modified epoxy resins, cyclopentadiene-modified epoxy resins which are glycidyl ethers of cyclopentadiene-modified phenolic resins, polycyclic aromatic ring-modified epoxy resins which are glycidyl ethers of polycyclic aromatic ring-modified phenolic resins, naphthalene-type epoxy resins which are glycidyl ethers of naphthalene ring-containing phenolic resins, halogenated phenol novolac-type epoxy resins, hydroquinone-type epoxy resins, trimethylolpropane-type epoxy resins, linear aliphatic epoxy resins obtained by oxidizing olefin bonds with peracids such as peracetic acid, and aralkyl-type epoxy resins obtained by epoxidizing aralkyl-type phenolic resins such as phenol aralkyl resins and naphthol aralkyl resins. Epoxidized acrylic resins are also examples of the epoxy resin.

[0021] The epoxy resin may include an epoxy resin having a mesogenic skeleton. In the present disclosure, the mesogenic skeleton refers to a molecular structure that may exhibit liquid crystallinity. Specific examples include biphenyl, phenyl benzoate, cyclohexyl benzoate, azobenzene, stilbene, and derivatives thereof. Epoxy resins having a mesogenic skeleton are prone to forming higher-order structures, and tend to achieve higher thermal conductivity when cured. Here, the term "higher-order structure" refers to a state in which its components are microscopically arranged, such as a crystalline phase or a liquid crystal phase. The presence of such a higher-order structure can be easily determined by observation with a polarizing microscope. That is, when observed in a crossed Nicol state, the presence of a higher-order structure can be determined if an interference pattern due to depolarization is observed. The higher-order structure typically exists in the resin in the form of islands, forming a domain structure. Each island forming the domain structure is referred to as a "higher-order structure." The structural units constituting the higher-order structure are generally bonded to each other by covalent bonds.

[0022] Specific examples of epoxy resins having a mesogenic skeleton are described in, for example, Japanese Patent No. 4118691. Specific examples of epoxy resins having a mesogenic skeleton are shown below, but the present disclosure is not limited to these.

[0023] Examples of epoxy resins having a mesogenic skeleton include biphenyl-type epoxy resins, 1-(3-methyl-4-oxiranylmethoxyphenyl)-4-(4-oxiranylmethoxyphenyl)-1-cyclohexene, and 1-(3-methyl-4-oxiranylmethoxyphenyl)-4-(4-oxiranylmethoxyphenyl)-benzene. Biphenyl-type epoxy resins can be obtained by reacting biphenol with epichlorohydrin using a known method. Examples of such biphenyl-type epoxy resins include 4,4'-bis(2,3-epoxypropoxy)biphenyl.

[0024] The epoxy resin having a mesogenic skeleton may be in a prepolymer state, in which a portion of the resin has been partially reacted with a curing agent or the like. Epoxy resins having a mesogenic skeleton generally tend to crystallize easily and often have low solubility in solvents. By partially polymerizing the epoxy resin having a mesogenic skeleton, crystallization can be suppressed. This may improve moldability.

[0025] These epoxy resins may be used alone or in combination of two or more. The epoxy resin preferably contains a biphenyl-type epoxy resin from the viewpoint of improving thermal conductivity and being easily available. When two or more epoxy resins are used in combination as the epoxy resin, the proportion of the biphenyl-type epoxy resin in the total epoxy resins is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. The proportion of the biphenyl-type epoxy resin in the total epoxy resins may be 100% by mass or less.

[0026] The epoxy equivalent (molecular weight / number of epoxy groups) of the epoxy resin is not particularly limited. From the viewpoint of a balance of various properties such as moldability, reflow resistance, and electrical reliability, the epoxy equivalent of the epoxy resin is preferably 100 g / eq to 1000 g / eq, and more preferably 150 g / eq to 500 g / eq. When two or more epoxy resins are used in combination, the epoxy equivalent of the mixture of two or more epoxy resins is preferably within the above range. The epoxy equivalent of the epoxy resin is a value measured by a method in accordance with JIS K 7236:2009.

[0027] When the epoxy resin is solid, the softening point or melting point of the epoxy resin is not particularly limited. The softening point or melting point of the epoxy resin is preferably 40°C to 180°C from the viewpoint of moldability and reflow resistance, and more preferably 50°C to 130°C from the viewpoint of handleability during preparation of the molding resin composition. The melting point or softening point of the epoxy resin is a value measured by differential scanning calorimetry (DSC) or a method in accordance with JIS K 7234:1986 (ring and ball method).

[0028] (Curing Agent) The molding resin composition of the present disclosure contains a curing agent. The curing agent preferably contains a phenolic curing agent from the viewpoint of moldability and reliability. As the curing agent, a curing agent other than the phenolic curing agent may be used. Examples of other curing agents include acid anhydride curing agents, amine curing agents, and active ester compounds. The molding resin composition may contain only one type of curing agent, or may contain two or more types. When the molding resin composition contains two or more types of curing agents, the proportion of the phenolic curing agent in the total curing agents is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. The proportion of the phenolic curing agent in the total curing agents may be 100% by mass or less.

[0029] -Phenol Curing Agent- Specific examples of the phenol curing agent include polyhydric phenol compounds such as resorcinol, catechol, bisphenol A, bisphenol F, and substituted or unsubstituted biphenols; novolak-type phenolic resins obtained by condensing or co-condensing at least one phenolic compound selected from the group consisting of phenolic compounds such as phenol, cresol, xylenol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol, and naphthol compounds such as α-naphthol, β-naphthol, and dihydroxynaphthalene, with an aldehyde compound such as formaldehyde, acetaldehyde, or propionaldehyde, under an acidic catalyst; and resins synthesized from the above phenolic compounds and dimethoxyparaxylene, bis(methoxymethyl)biphenyl, or the like. terpene-modified phenolic resins; dicyclopentadiene-type phenolic resins and dicyclopentadiene-type naphthol resins synthesized by copolymerization of the above-mentioned phenolic compounds with dicyclopentadiene; cyclopentadiene-modified phenolic resins; polycyclic aromatic ring-modified phenolic resins; biphenyl-type phenolic resins; triphenylmethane-type phenolic resins obtained by condensation or co-condensation of the above-mentioned phenolic compounds with an aromatic aldehyde compound such as benzaldehyde or salicylaldehyde in the presence of an acid catalyst; and phenolic resins obtained by copolymerization of two or more of these.

[0030] These phenolic curing agents may be used alone or in combination of two or more. As the phenolic curing agent, triphenylmethane-type phenolic resins are preferred from the viewpoint of improving thermal conductivity by increasing the crosslink density of the cured product. When two or more phenolic curing agents are used in combination as the phenolic curing agent, the proportion of triphenylmethane-type phenolic resins in the entire phenolic curing agent is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. The proportion of triphenylmethane-type phenolic resins in the entire phenolic curing agent may be 100% by mass or less. When two or more curing agents are used in combination as the curing agent, the proportion of triphenylmethane-type phenolic resins in the entire curing agent is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. The proportion of triphenylmethane-type phenolic resins in the entire curing agent may be 100% by mass or less.

[0031] The hydroxyl equivalent of the phenolic curing agent is not particularly limited. From the viewpoint of balancing various properties such as moldability, reflow resistance, and electrical reliability, the hydroxyl equivalent of the phenolic curing agent is preferably 70 g / eq to 1000 g / eq, more preferably 80 g / eq to 500 g / eq, and from the viewpoint of improving thermal conductivity by increasing the crosslink density of the cured product, it is even more preferably 90 g / eq to 300 g / eq. When two or more phenolic curing agents are used in combination, it is preferable that the hydroxyl equivalent of the mixture of two or more phenolic curing agents be within the above range. The hydroxyl equivalent of the phenolic curing agent is a value measured by a method in accordance with JIS K 0070:1992.

[0032] The softening point or melting point of the phenolic curing agent is not particularly limited. From the viewpoints of moldability and reflow resistance, the softening point or melting point of the phenolic curing agent is preferably 40°C to 180°C, and from the viewpoint of handleability during production of the molding resin composition, it is more preferably 50°C to 130°C. The melting point or softening point of the phenolic curing agent is a value measured in the same manner as the melting point or softening point of the epoxy resin.

[0033] The equivalent ratio of the epoxy resin to the curing agent, i.e., the ratio of the number of functional groups in the curing agent to the number of functional groups in the epoxy resin (number of functional groups in the curing agent / number of functional groups in the epoxy resin), is not particularly limited. From the viewpoint of minimizing unreacted components, it is preferably set in the range of 0.5 to 2.0, more preferably in the range of 0.6 to 1.3. From the viewpoint of moldability and reflow resistance, it is even more preferably set in the range of 0.8 to 1.2.

[0034] (Inorganic filler) The molding resin composition contains an inorganic filler containing alumina. By including an inorganic filler in the molding resin composition, the moisture absorption of the molding resin composition tends to be reduced and the strength in a cured state tends to be improved.

[0035] The inorganic filler may be used alone or in combination of two or more. When two or more inorganic fillers are used in combination, for example, two or more inorganic fillers with different components, average particle diameters, shapes, etc. may be used. The shape of the inorganic filler is not particularly limited, and examples thereof include powder, spheres, fibers, etc. From the viewpoint of fluidity during molding of the molding resin composition and mold wear resistance, a spherical shape is preferred.

[0036] The inorganic filler may contain alumina, and may be entirely alumina or may contain alumina in combination with other inorganic fillers. When the inorganic filler contains alumina, the thermal conductivity of the molding resin composition tends to be improved. Examples of other inorganic fillers that can be used in combination with alumina include silica such as spherical silica and crystalline silica, zircon, magnesium oxide, calcium silicate, calcium carbonate, potassium titanate, silicon carbide, silicon nitride, boron nitride, beryllia, and zirconia. Furthermore, examples of inorganic fillers with flame retardant properties include aluminum hydroxide and zinc borate.

[0037] When alumina and other inorganic fillers are used in combination as inorganic fillers, it is preferable to use silica as the other inorganic filler in view of its spherical shape.When alumina and other inorganic fillers such as silica are used in combination as inorganic fillers, the content of alumina in the entire inorganic filler is preferably 50% by volume or more, more preferably 60% by volume or more, and even more preferably 70% by volume or more.In addition, the content of alumina in the entire inorganic filler may be 100% by volume or less, and preferably 99% by volume or less.

[0038] From the viewpoints of moisture absorption, reduction of the linear expansion coefficient, improvement of strength, and solder heat resistance, the content of the inorganic filler is preferably 70% by volume or more, more preferably 71% by volume or more, and even more preferably 72% by volume or more, based on the total volume of the molding resin composition. The content of the inorganic filler is preferably 85% by volume or less, more preferably 80% by volume or less, and even more preferably 78% by volume or less. The content of the inorganic filler may be 70% by volume to 85% by volume.

[0039] The average particle size (volume average particle size) of the inorganic filler is preferably 1 μm to 30 μm, more preferably 3 μm to 20 μm, and even more preferably 5 μm to 15 μm. In the present disclosure, the average particle size of the inorganic filler refers to the average particle size of alumina when alumina is used alone as the inorganic filler, and refers to the average particle size of the inorganic filler as a whole when alumina is used in combination with other inorganic fillers as the inorganic filler.

[0040] The average particle size of an inorganic filler can be measured by the following method. The inorganic filler to be measured is added to a solvent (pure water) in a range of 0.02% to 0.08% by mass, and the mixture is vibrated in a 110W bath-type ultrasonic cleaner for 1 to 10 minutes to disperse the inorganic filler. Approximately 40 mL of the dispersion is poured into a measurement cell and measured at 25°C. A laser diffraction / scattering particle size distribution analyzer (e.g., HORIBA, Ltd., LA920 (trade name)) is used to measure the volumetric particle size distribution. The average particle size is determined as the particle size (D50%) at which the cumulative total from the smallest diameter side in the volumetric particle size distribution reaches 50%. The refractive index used is that of alumina. When the inorganic filler is a mixture of alumina and other inorganic fillers, the refractive index used is that of alumina.

[0041] (Mold Release Agent) The molding resin composition of the present disclosure contains a mold release agent containing polyethylene oxide, from the viewpoint of obtaining good releasability from the mold during molding. The polyethylene oxide may be used alone or in combination of two or more types. In the molding resin composition of the present disclosure, parameter P calculated by the above formula A based on the weight-average molecular weight of the polyethylene oxide and the content of the polyethylene oxide per 100 parts by mass of the epoxy resin is 300 to 1500, preferably 400 to 1300, more preferably 500 to 1100, and even more preferably 600 to 1000.

[0042] In the molding resin composition of the present disclosure, the content of polyethylene oxide per 100 parts by mass of the epoxy resin and curing agent is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 4 parts by mass, and even more preferably 1 to 2.5 parts by mass. When the content of polyethylene oxide per 100 parts by mass of the epoxy resin and curing agent is 0.01 part by mass or more, sufficient mold releasability tends to be obtained. When the content of polyethylene oxidized per 100 parts by mass of the epoxy resin and curing agent is 5 parts by mass or less, contamination of the surface of a molded product tends to be further suppressed.

[0043] The molding resin composition of the present disclosure may contain a release agent other than oxidized polyethylene as a release agent. As the other release agent, conventionally known ones can be used. Specific examples include carnauba wax, higher fatty acids such as montanic acid and stearic acid, higher fatty acid metal salts, ester waxes such as montanic acid esters, and polyolefin waxes such as non-oxidized polyethylene. Among these, ester waxes such as montanic acid esters are preferred. The other release agents may be used alone or in combination of two or more.

[0044] When polyethylene oxide and other release agents are used in combination as a release agent, the proportion of polyethylene oxide in the entire release agent is preferably 15% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more. The proportion of polyethylene oxidized in the entire release agent is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 65% ​​by mass or less. When polyethylene oxidized and other release agents are used in combination as a release agent, the proportion of polyethylene oxidized in the entire release agent is preferably 15% by mass to 80% by mass.

[0045] The oxidized polyethylene may be linear oxidized polyethylene or branched oxidized polyethylene. Linear oxidized polyethylene and branched oxidized polyethylene may be used in combination. Here, linear oxidized polyethylene refers to oxidized polyethylene in which the number of carbon atoms in the side alkyl chain is approximately 10% or less of the number of carbon atoms in the main alkyl chain. Generally, oxidized polyethylene with a penetration of 2 or less is classified as linear oxidized polyethylene. Compared with branched oxidized polyethylene of the same molecular weight and acid value, linear oxidized polyethylene tends to have a higher alkyl chain efficiency, be more likely to bleed out from the base resin, and have higher releasability. This tendency becomes more pronounced the greater the amount of inorganic filler added and the greater the weight-average molecular weight of the linear oxidized polyethylene.

[0046] The weight average molecular weight of the polyethylene oxide is preferably 3,500 or more, more preferably 5,000 or more, and even more preferably 10,000 or more, from the viewpoint of mold releasability. The weight average molecular weight of the polyethylene oxide may be 15,000 or less, and is preferably 3,500 to 15,000, more preferably 4,000 to 14,000, and even more preferably 4,200 to 13,000, from the viewpoint of adhesiveness and prevention of mold and package contamination. Here, the weight average molecular weight of the polyethylene oxide refers to a value measured by high-temperature GPC. The measurement method is as follows. Measuring device: High-temperature GPC manufactured by Waters Column: Two columns of PLgel 10 μm MIXED-B (7.5 mm × 300 mm) manufactured by Polymer Laboratories Flow rate: 1.0 ml / min (sample concentration: 0.3 w / vol%) Injection amount: 100 μl

[0047] From the viewpoint of the balance between package fouling and mold releasability, the acid value of the oxidized polyolefin is preferably 2 mgKOH / g to 50 mgKOH / g, more preferably 10 mgKOH / g to 40 mgKOH / g, and even more preferably 15 mgKOH / g to 30 mgKOH / g. If the acid value is 2 mgKOH / g or more, package fouling tends to be more easily suppressed, and if it is 50 mgKOH / g or less, mold releasability tends to be more improved. When two or more types of oxidized polyethylene are used in combination, the acid value of the mixture of oxidized polyethylenes is preferably within the above range. In the present disclosure, the acid value of the oxidized polyolefin is a value measured by a method in accordance with JIS K 5902:1969.

[0048] The content of the release agent is preferably 0.1 to 10 parts by mass, more preferably 1 to 5 parts by mass, and even more preferably 2 to 4 parts by mass, per 100 parts by mass of the epoxy resin and curing agent combined. When the amount of the release agent is 0.1 part by mass or more per 100 parts by mass of the epoxy resin and curing agent combined, sufficient releasability tends to be obtained. When the amount is 10 parts by mass or less, better adhesion tends to be obtained.

[0049] (Specific Copolymer) The molding resin composition of the present disclosure may contain a specific copolymer. The α-olefin having 5 to 30 carbon atoms used in the specific copolymer is not particularly limited. Specific examples of the α-olefin having 5 to 30 carbon atoms include 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 1-docosene, 1-tricosene, 1-tetracosene, 1-pentacosene, 1 Examples of the maleic anhydride derivatives include linear α-olefins such as 1-hexacosene and 1-heptacosene, and branched α-olefins such as 3-methyl-1-butene, 3,4-dimethyl-pentene, 3-methyl-1-nonene, 3,4-dimethyl-octene, 3-ethyl-1-dodecene, 4-methyl-5-ethyl-1-octadecene, and 3,4,5-triethyl-1-eicosene. These may be used alone or in combination of two or more. Among these, linear α-olefins having 10 to 25 carbon atoms are preferred, and linear α-olefins having 15 to 25 carbon atoms such as 1-eicosene, 1-docosene, and 1-tricosene are more preferred. Examples of the maleic anhydride derivatives used in the specific copolymer include methylmaleic anhydride and dimethylmaleic anhydride.

[0050] The specific copolymer preferably contains a structural unit represented by the following general formula (C) and a structural unit represented by the following general formula (D).

[0051]

[0052] In general formula (C) and general formula (D), R 11 represents a monovalent aliphatic hydrocarbon group having 3 to 28 carbon atoms, and R 12 and R 13 Each independently represents a hydrogen atom, an alkyl group, or an aryl group. 11 Specific examples of the monovalent aliphatic hydrocarbon group having 3 to 28 carbon atoms represented by the formula (I) include an ethenyl group (—CH═CH) derived from the α-olefin having 5 to 30 carbon atoms. 2 ) and monovalent residues excluding the moiety R 11is preferably a linear hydrocarbon group having 13 to 23 carbon atoms, more preferably a linear hydrocarbon group having 18 to 21 carbon atoms such as an n-octadecyl group, an n-eicosyl group, or an n-heneicosyl group. 12 or R 13 Examples of the alkyl group represented by the formula (D) include alkyl groups having 1 to 4 carbon atoms, and a methyl group is preferred. 12 or R 13 In general formula (D), the aryl group represented by R is preferably a phenyl group. 12 or R 13 is preferably a hydrogen atom.

[0053] The copolymerization ratio of the structural units represented by general formula (C) and the structural units represented by general formula (D) is not particularly limited, but when the structural units represented by general formula (C) are X moles and the structural units represented by general formula (D) are Y moles, X / Y is preferably 1 / 2 to 10 / 1, more preferably 2 / 3 to 5 / 1, still more preferably 3 / 4 to 2 / 1, and particularly preferably approximately equimolar, about 1 / 1.

[0054] When the structural unit represented by general formula (C) and the structural unit represented by general formula (D) are bonded together, they may be in the form of either general formula (E) or general formula (F). 11 ~R 13 Specific and preferred examples of are the same as those of formula (C) and formula (D).

[0055]

[0056] The specific copolymer may have any structure such as a random, block, or graft copolymer. When the specific copolymer contains a structural unit represented by general formula (C) and a structural unit represented by general formula (D), it may or may not contain other structural units other than the structural unit represented by general formula (C) and the structural unit represented by general formula (D). The proportion of other structural units in the total structural units of the specific copolymer is preferably 0 mol% to 50 mol%, more preferably 0 mol% to 35 mol%, and even more preferably 0 mol% to 20 mol%.

[0057] The specific copolymer may have a carboxy group as a result of hydrolysis of at least a portion of the structural units derived from at least one of maleic anhydride and maleic anhydride derivatives contained in the specific copolymer.

[0058] The method for producing the specific copolymer is not particularly limited, and a general copolymerization method such as reacting raw materials can be used. An organic solvent capable of dissolving α-olefin and maleic anhydride may be used for the reaction. While the organic solvent is not particularly limited, toluene is preferred, and alcohol-based solvents, ether-based solvents, amine-based solvents, etc. can also be used. The reaction temperature varies depending on the type of organic solvent used, but from the standpoints of reactivity and productivity, it is preferably 50°C to 200°C, and more preferably 80°C to 120°C. The reaction time is not particularly limited as long as the specific copolymer is obtained, but from the standpoint of productivity, it is preferably 1 hour to 30 hours, more preferably 2 hours to 15 hours, and even more preferably 4 hours to 10 hours. After completion of the reaction, unreacted components, organic solvent, etc. can be removed, if necessary, by heating under reduced pressure, etc. The reaction conditions are a temperature of 100°C to 220°C, more preferably 120°C to 180°C, and a pressure of 13.3 x 10 3 Pa or less, more preferably 8×10 3 The reaction time is preferably 0.5 to 10 hours at a pressure of 0.05 Pa or less. If necessary, a reaction catalyst such as an amine catalyst or an acid catalyst may be added to the reaction. The pH of the reaction system is preferably about 1 to 10.

[0059] The specific copolymer may be a commercially available product, such as Nissan Electol WPB-1 (trade name, manufactured by NOF Corporation), which uses 1-eicosene, 1-docosene, and 1-tricosene as raw materials.

[0060] From the viewpoint of mold / package contamination prevention and moldability, the weight average molecular weight of the specific copolymer is preferably 5,000 to 100,000, more preferably 10,000 to 70,000, and even more preferably 15,000 to 50,000. If the weight average molecular weight is 5,000 or more, the mold / package contamination prevention effect tends to be sufficient, and if it is 100,000 or less, the softening point of the specific copolymer does not increase too much, and deterioration of kneadability, etc. tends to be suppressed. Here, the weight average molecular weight of the specific copolymer is measured by gel permeation chromatography (GPC) and derived by conversion using a standard polystyrene calibration curve. The GPC conditions are as shown below. - GPC conditions - Pump: Hitachi L-6000 type (manufactured by Hitachi, Ltd.) Column: Three columns in total: Gelpack GL-R420, Gelpack GL-R430, Gelpack GL-R440 (all manufactured by Resonaq Technoservice Co., Ltd., trade names) Eluent: Tetrahydrofuran Measurement temperature: 25°C Flow rate: 2.05 mL / min Detector: Hitachi L-3300 type RI (manufactured by Hitachi, Ltd.)

[0061] The content of the specific copolymer is preferably 0.01 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and even more preferably 1 to 4 parts by mass, per 100 parts by mass of the epoxy resin. When the amount of the specific copolymer is 10 parts by mass or less per 100 parts by mass of the epoxy resin, sufficient mold releasability tends to be obtained. When the amount is 0.01 part by mass or more, sufficient adhesion and the effect of improving mold and package staining tend to be achieved. When the amount is 0.01 part by mass or more, sufficient adhesion and the effect of improving mold and package staining tend to be achieved. The content of the specific copolymer is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the epoxy resin and the curing agent combined. When the amount of the specific copolymer is 0.01 part by mass or more per 100 parts by mass of the epoxy resin and the curing agent combined, sufficient mold releasability tends to be achieved. When the amount is 5 parts by mass or less, sufficient adhesion and the effect of improving mold and package staining tend to be achieved.

[0062] (Curing Accelerator) The molding resin composition of the present disclosure may contain a curing accelerator as needed. The type of curing accelerator is not particularly limited and can be selected depending on the type of epoxy resin, the desired properties of the molding resin composition, and the like.

[0063] Examples of the curing accelerator include diazabicycloalkenes such as 1,5-diazabicyclo[4.3.0]nonene-5 (DBN) and 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), cyclic amidine compounds such as 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 2-ethyl-4-methylimidazole, and 2-heptadecylimidazole; derivatives of the cyclic amidine compounds; phenol novolac salts of the cyclic amidine compounds or their derivatives; and the addition of maleic anhydride to these compounds, 1,4-benzoquinone, 2,5-toluquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, and phenyl-1,4-benzoquinone. compounds having intramolecular polarization obtained by adding a compound having a π bond, such as a quinone compound or diazophenylmethane; cyclic amidinium compounds such as the tetraphenylborate salt of DBU, the tetraphenylborate salt of DBN, the tetraphenylborate salt of 2-ethyl-4-methylimidazole, and the tetraphenylborate salt of N-methylmorpholine; tertiary amine compounds such as pyridine, triethylamine, triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; derivatives of the above tertiary amine compounds; ammonium salt compounds such as tetra-n-butylammonium acetate, tetra-n-butylammonium phosphate, tetraethylammonium acetate, tetra-n-hexylammonium benzoate, and tetrapropylammonium hydroxide;Organic phosphines such as primary phosphines such as ethylphosphine and phenylphosphine, secondary phosphines such as dimethylphosphine and diphenylphosphine, and tertiary phosphines such as triphenylphosphine, diphenyl(p-tolyl)phosphine, tris(alkylphenyl)phosphine, tris(alkoxyphenyl)phosphine, tris(alkyl alkoxyphenyl)phosphine, tris(dialkylphenyl)phosphine, tris(trialkylphenyl)phosphine, tris(tetraalkylphenyl)phosphine, tris(dialkoxyphenyl)phosphine, tris(trialkoxyphenyl)phosphine, tris(tetraalkoxyphenyl)phosphine, trialkylphosphine, dialkylarylphosphine, alkyldiarylphosphine, trinaphthylphosphine, and tris(benzyl)phosphine; phosphine compounds such as complexes of the organic phosphines with organic borons; and the organic phosphines or the phosphine compounds, which may be combined with maleic anhydride, 1,4-benzoquinone, 2,5-toluquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone. quinone compounds such as 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, phenyl-1,4-benzoquinone, and anthraquinone, and compounds having intramolecular polarization obtained by adding a compound having a π bond such as diazophenylmethane; a compound having intramolecular polarization, which is obtained by reacting a halogenated phenol compound such as 1-iodophenol, 2-iodophenol, 4-bromo-2-methylphenol, 4-bromo-3-methylphenol, 4-bromo-2,6-dimethylphenol, 4-bromo-3,5-dimethylphenol, 4-bromo-2,6-di-tert-butylphenol, 4-chloro-1-naphthol, 1-bromo-2-naphthol, 6-bromo-2-naphthol, or 4-bromo-4'-hydroxybiphenyl with the halogenated phenol compound, followed by a dehydrohalogenation step;Examples of the curing accelerator include tetra-substituted phosphonium compounds such as tetraphenylphosphonium, tetraphenylborate salts of tetra-substituted phosphonium such as tetraphenylphosphonium tetra-p-tolylborate, and salts of tetra-substituted phosphonium with phenolic compounds; salts of tetraalkylphosphonium with partial hydrolysates of aromatic carboxylic acid anhydrides; phosphobetaine compounds; and adducts of phosphonium compounds with silane compounds. One type of curing accelerator may be used alone, or two or more types may be used in combination.

[0064] Among these, the curing accelerator is preferably a curing accelerator containing an organic phosphine. Examples of the curing accelerator containing an organic phosphine include the above-mentioned organic phosphines, phosphine compounds such as complexes of the above-mentioned organic phosphines and organoborons, and compounds having intramolecular polarization formed by adding a compound having a π bond to the above-mentioned organic phosphines or the above-mentioned phosphine compounds. Among these, particularly suitable curing accelerators include triphenylphosphine, an adduct of triphenylphosphine and a quinone compound, an adduct of tributylphosphine and a quinone compound, and an adduct of tri-p-tolylphosphine and a quinone compound.

[0065] When the molding resin composition contains a curing accelerator, the amount thereof is preferably 0.1 to 30 parts by mass, and more preferably 1 to 15 parts by mass, per 100 parts by mass of the epoxy resin and curing agent combined. When the amount of curing accelerator is 0.1 part by mass or more per 100 parts by mass of the epoxy resin and curing agent combined, the composition tends to cure well in a short time. When the amount of curing accelerator is 30 parts by mass or less per 100 parts by mass of the epoxy resin and curing agent combined, the curing speed is not too fast, and a good molded product tends to be obtained.

[0066] (Stress Relaxant) The molding resin composition of the present disclosure may contain a stress relaxation agent. By including a stress relaxation agent, warpage of the package and the occurrence of package cracks can be further reduced. Examples of the stress relaxation agent include commonly used known stress relaxation agents (flexibilizers). Specific examples include thermoplastic elastomers such as silicone-based, styrene-based, olefin-based, urethane-based, polyester-based, polyether-based, polyamide-based, and polybutadiene-based elastomers; indene-styrene-coumarone copolymers; organic phosphorus compounds such as triphenylphosphine oxide and phosphate esters; rubber particles such as NR (natural rubber), NBR (acrylonitrile-butadiene rubber), acrylic rubber, urethane rubber, and silicone powder; and rubber particles having a core-shell structure such as methyl methacrylate-styrene-butadiene copolymer (MBS), methyl methacrylate-silicone copolymer, and methyl methacrylate-butyl acrylate copolymer. One type of stress relaxation agent may be used alone, or two or more types may be used in combination. Examples of silicone-based stress relaxation agents include those having an epoxy group, those having an amino group, and those obtained by modifying these with polyether. Silicone compounds such as silicone compounds having an epoxy group (epoxy-modified silicone particles) and polyether-based silicone compounds are more preferred.

[0067] When the molding resin composition contains a stress relaxation agent, the amount thereof is, for example, preferably 1 to 35 parts by mass, and more preferably 2 to 20 parts by mass, per 100 parts by mass of the epoxy resin and curing agent in total.

[0068] [Various Additives] In addition to the components described above, the molding resin composition of the present disclosure may contain various additives such as coupling agents, ion exchangers, flame retardants, colorants, etc. The molding resin composition of the present disclosure may contain various additives known in the technical field as needed, in addition to the additives exemplified below.

[0069] (Coupling Agent) The molding resin composition of the present disclosure may contain a coupling agent. From the viewpoint of improving the adhesion between the epoxy resin and the curing agent and the inorganic filler, the molding resin composition preferably contains a coupling agent. Examples of the coupling agent include known coupling agents such as silane-based compounds such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, vinylsilane, and disilazane, titanium-based compounds, aluminum chelate-based compounds, and aluminum / zirconium-based compounds.

[0070] When the molding resin composition contains a coupling agent, the amount of the coupling agent is preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 2.5 parts by mass, per 100 parts by mass of the inorganic filler. When the amount of the coupling agent is 0.05 parts by mass or more per 100 parts by mass of the inorganic filler, the adhesiveness tends to be further improved. When the amount of the coupling agent is 5 parts by mass or less per 100 parts by mass of the inorganic filler, the moldability of the package tends to be further improved.

[0071] (Ion Exchanger) The molding resin composition of the present disclosure may contain an ion exchanger. The molding resin composition preferably contains an ion exchanger from the viewpoint of improving the moisture resistance and high-temperature storage characteristics of an electronic component device including an encapsulated electronic component. The ion exchanger is not particularly limited, and conventionally known ion exchangers can be used. Specific examples include hydrotalcite compounds and hydrous oxides of at least one element selected from the group consisting of magnesium, aluminum, titanium, zirconium, and bismuth. The ion exchangers may be used alone or in combination of two or more. Among these, hydrotalcites represented by the following general formula (A) are preferred:

[0072] Mg (1-X) Al X (OH) 2 (CO 3 ) X/2 ・mH 2 O ……(A) (0<X≦0.5, m is a positive number)

[0073] When the molding resin composition contains an ion exchanger, the content thereof is not particularly limited as long as it is an amount sufficient to capture ions such as halogen ions, etc. For example, the content of the ion exchanger is preferably 0.1 to 30 parts by mass, and more preferably 1 to 10 parts by mass, per 100 parts by mass of the epoxy resin and curing agent combined.

[0074] (Flame Retardant) The molding resin composition of the present disclosure may contain a flame retardant. The flame retardant is not particularly limited, and conventionally known flame retardants can be used. Specific examples include organic or inorganic compounds containing halogen atoms, antimony atoms, nitrogen atoms, or phosphorus atoms, and metal hydroxides. The flame retardants may be used alone or in combination of two or more.

[0075] When the molding resin composition contains a flame retardant, the amount thereof is not particularly limited as long as it is an amount sufficient to obtain the desired flame retardant effect. For example, the amount of the flame retardant is preferably 1 to 30 parts by mass, and more preferably 2 to 20 parts by mass, per 100 parts by mass of the epoxy resin and curing agent combined.

[0076] (Colorant) The molding resin composition of the present disclosure may contain a colorant. Examples of the colorant include known colorants such as carbon black, organic dyes, organic pigments, titanium oxide, red lead, and red iron oxide. The content of the colorant can be appropriately selected depending on the purpose, etc. The colorant may be used alone or in combination of two or more types.

[0077] (Method for Preparing Molding Resin Composition) The method for preparing the molding resin composition is not particularly limited. A typical method includes thoroughly mixing predetermined amounts of components using a mixer or the like, melt-kneading the mixture using a mixing roll, extruder, or the like, cooling, and pulverizing the mixture. More specifically, a method includes stirring and mixing predetermined amounts of the components described above, kneading the mixture using a kneader, roll, extruder, or the like that has been preheated to 70°C to 140°C, cooling, and pulverizing the mixture. The release agent may be a masterbatch prepared by mixing the epoxy resin and a specific copolymer, etc., as needed, in advance.

[0078] The molding resin composition of the present disclosure is preferably solid at room temperature and normal pressure (e.g., 25°C, atmospheric pressure). When the molding resin composition is solid, its shape is not particularly limited, and examples include powder, granules, tablets, etc. When the molding resin composition is in tablet form, it is preferable that the dimensions and mass of the tablet-shaped molding resin composition be such that they are suitable for the molding conditions of the package, from the viewpoint of handleability.

[0079] The electronic component device of the present disclosure includes a support member, an electronic component disposed on the support member, and a cured product of the molding resin composition described above that seals the electronic component. Examples of the electronic component device include a support member such as a lead frame, a pre-wired tape carrier, a wiring board, glass, a silicon wafer, or an organic substrate, on which electronic components (active elements such as semiconductor chips, transistors, diodes, and thyristors, passive elements such as capacitors, resistors, and coils, and antennas) are mounted, and the resulting electronic component region is sealed with the molding resin composition.

[0080] The type of the support member is not particularly limited, and a support member commonly used in the manufacture of electronic component devices can be used. Furthermore, in the electronic component device of the present disclosure, if necessary, other electronic components may be disposed on the surface of the support member opposite to the surface on which the electronic components are disposed. The other electronic components may be encapsulated with the molding resin composition described above, with another resin composition, or may not be encapsulated.

[0081] (Method for manufacturing an electronic component device) The method for manufacturing an electronic component device of the present disclosure includes a step of placing an electronic component on a support member and a step of encapsulating the electronic component with the molding resin composition. The method for carrying out each of the above steps is not particularly limited, and can be carried out by a general method. Furthermore, the types of support member and electronic component used in manufacturing the electronic component device are not particularly limited, and support members and electronic components commonly used in manufacturing electronic component devices can be used.

[0082] Methods for encapsulating electronic components using the molding resin composition include low-pressure transfer molding, injection molding, compression molding, etc. Among these, low-pressure transfer molding is the most common.

[0083] The above-described embodiment will be specifically described below using examples, but the scope of the above-described embodiment is not limited to these examples.

[0084] <Preparation of molding resin compositions> The molding resin compositions of Examples, Comparative Examples, and Reference Examples were prepared by mixing the components shown below in the blending ratios (parts by mass) shown in Table 1. These molding resin compositions were solid at room temperature and normal pressure. Table 1 also shows the volumetric content (vol %) of the inorganic filler relative to the total molding composition.

[0085] Epoxy resin 1: biphenyl type epoxy resin (epoxy equivalent: 173 g / eq) Epoxy resin 2: biphenyl type epoxy resin (epoxy equivalent: 186 g / eq) Mold release agent 1: linear polyethylene oxide, weight average molecular weight 11,000, oxidation 24.5 mg KOH / g Mold release agent 2: linear polyethylene oxide, weight average molecular weight 7,500, oxidation 24.5 mg KOH / g Mold release agent 3: branched polyethylene oxide, weight average molecular weight 4,300, oxidation 17 mg KOH / g Mold release agent 4: branched polyethylene oxide, weight average molecular weight 3,100, oxidation 24.5 mg KOH / g Mold release agent 5: montanic acid ester Specific copolymer 1: containing a structural unit represented by general formula (C) and a structural unit represented by general formula (D), wherein the molar ratio X / Y of the structural unit represented by general formula (C) and the structural unit represented by general formula (D) is 1 / 1, and R in general formula (C) 11 is an n-octadecyl group, an n-eicosyl group, or an n-heneicosyl group, and R in general formula (D) 12 and R 13 is a hydrogen atom. Specific copolymer 2: A copolymer using 1-eicosene, 1-docosene, and 1-tricosene as raw materials (weight average molecular weight: 20,400). Specific copolymer 3: A copolymer containing a structural unit represented by general formula (C) and a structural unit represented by general formula (D), wherein R in general formula (C) is a hydrogen atom. 11 is an alkyl group having 8 or more carbon atoms, and R in general formula (D)12 and R 13 is a hydrogen atom. Curing agent: triphenylmethane type phenol resin (hydroxyl group equivalent: 106 g / eq) Curing accelerator: phosphorus-based curing accelerator Coupling agent 1: 3-methacryloxypropyltrimethoxysilane Coupling agent 2: N-phenyl-3-aminopropyltrimethoxysilane Colorant: carbon black Stress relaxation agent: epoxy-modified silicone particles Inorganic filler 1: silica particles (volume average particle diameter: 11.2 μm, top cut 20 μm) Inorganic filler 2: silica particles (volume average particle diameter: 0.63 μm) Inorganic filler 3: alumina particles (volume average particle diameter: 6.2 μm, top cut 25 μm) Inorganic filler 4: alumina particles (volume average particle diameter: 0.39 μm)

[0086] The parameter P calculated by formula A for Examples 1 to 6, Comparative Examples 1 to 5, and Reference Example was as shown in Table 1.

[0087] (Evaluation of releasability) A wax-coated sealant (CEL-PR41, manufactured by Resonac Co., Ltd.) was compression-molded into a disk shape on a ferroic plate (35 mm × 50 mm × 0.5 mm) whose surface was hard chrome-plated, and a disk area of ​​3.14 cm was formed. 2 A cured product of 10 ... 2A cured product of the above formula was produced. The cured product was produced at a molding temperature of 175°C, a molding time of 90 seconds, and a molding pressure of 10 MPa. Next, the cured product was fixed using a surface adsorption machine, and the cured product was peeled off from the ferromagnetic plate by pulling the ferromagnetic plate horizontally relative to the interface between the cured product and the ferromagnetic plate. The shear release force (shear stress) required to peel the cured product from the ferromagnetic plate was read using a push-pull gauge (manufactured by Imada Co., Ltd., maximum scale 500 (N)). After the shear release force measurement was completed, the molding resin composition was again compression molded into a disk shape at the site where the cured product was peeled off the ferromagnetic plate, and then the shear release force was measured. This process was repeated a total of 10 times. The difference between the shear release force at the 5th time and the shear release force at the 10th time (the shear release force at the 10th time minus the shear release force at the 5th time) is shown in Table 1 as the shear release force increase. The smaller the shear release force increase, the better the release property.

[0088] (Evaluation of Hot Hardness) The hot hardness of the molding resin composition was evaluated as follows. The molding resin composition was molded into test pieces (disks with a diameter of 50 mm and a thickness of 3 mm) for measuring hot hardness using a transfer molding machine under conditions of 175°C, a molding pressure of 6.9 MPa, and 120 seconds. Immediately after molding, the hot hardness (Shore D) of the test pieces was measured using a Shore D hardness tester. The results are shown in Table 1.

[0089] (Melt Viscosity) The molding resin composition was heated to melt, and the melt viscosity (poise) was measured at 175° C. using a Koka type flow tester. The results are shown in Table 1.

[0090] (Evaluation of Spiral Flow (SF)) Using a spiral flow measurement mold conforming to EMMI-1-66, the molding resin composition was molded with a transfer molding machine under conditions of a mold temperature of 175°C, a molding pressure of 6.9 MPa, and a curing time of 120 seconds, and the flow distance (inches) was determined. The results are shown in Table 1.

[0091] (Evaluation of Gel Time (GT)) Measurement was carried out at a temperature of 175°C using a Curelastometer manufactured by JSR Trading Co., Ltd. The time until the torque curve rose was taken as the gel time (GT, seconds). The results are shown in Table 1.

[0092] (Evaluation of Flexural Strength (25°C)) The molding resin composition was cured using a transfer molding machine under conditions of a mold temperature of 180°C, a molding pressure of 6.9 MPa, and a curing time of 90 seconds. Subsequently, post-curing was performed at 175°C for 6 hours. Test specimens measuring 10 mm x 70 mm x 3 mm were obtained from the resulting molded product. The resulting test specimens were subjected to a three-point bending test in accordance with JIS K6911:2006 using a bending tester (manufactured by A&D Co., Ltd., product name: Tensilon) while being maintained at 25°C in a thermostatic chamber, and the flexural modulus (flexural strength, MPa) at 25°C was calculated using the following formula. The results are shown in Table 1. In the formula, "E" represents the flexural modulus (Pa), "P" represents the load cell value (N), "y" represents the displacement (mm), "l" represents the span (= 48 mm), "w" represents the width (= 10 mm), and "h" represents the thickness (= 3 mm) of the test specimen.

[0093]

[0094] (Evaluation of Flexural Strength (175° C.)) The flexural strength (175° C.) was evaluated in the same manner as in "Flexural Strength (25° C.)" except that the temperature of the thermostatic bath was set to 175° C. The results are shown in Table 1.

[0095] (Evaluation of post-shear film thickness) The film thickness of the deposit attached to the surface of the ferroelectric plate was measured using an ellipsometer manufactured by J. A. Woollam. In the "evaluation of releasability," the film thickness of the deposit was measured before the shear release force evaluation at the site where the cured product produced using the wax-coated sealant on the ferroelectric plate was peeled off. Next, the film thickness of the deposit after the 10th shear release force measurement was measured. The value obtained by subtracting the film thickness of the deposit after the 10th shear release force measurement from the film thickness of the deposit before the shear release force evaluation was determined as the post-shear film thickness increase. The results are shown in Table 1. The smaller the post-shear film thickness increase, the more the contamination of the molded product surface is suppressed. If the post-shear film thickness increase is 0 nm or less, there is no problem in practical use.

[0096]

[0097] Table 1 shows that the molding resin compositions of Comparative Examples 1, 3, and 5, in which the parameter P calculated by Formula A is less than 300, have a high increase in shear release force and are poor in releasability. Table 1 shows that the molding resin compositions of Comparative Examples 2 and 4, in which the parameter P calculated by Formula A is more than 1500, have a high increase in film thickness after shear and are prone to staining on the surface of molded products. Table 1 shows that the molding resin compositions of Examples, in which the parameter P calculated by Formula A is 300 to 1500, have excellent releasability and are able to suppress staining on the surface of molded products.

[0098] The disclosure of Japanese Patent Application No. 2023-113363, filed on July 10, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated by reference into this specification to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. A molding resin composition comprising an epoxy resin, a curing agent, a release agent containing polyethylene oxide, and an inorganic filler containing alumina, wherein a parameter P calculated by the following formula A based on the weight average molecular weight of the polyethylene oxide and the content of the polyethylene oxide relative to 100 parts by mass of the epoxy resin is 300 to 1500. In formula A, Mi represents the weight average molecular weight of the i-th type of polyethylene oxide, and Ri represents the content of the i-th type of polyethylene oxide relative to 100 parts by mass of the epoxy resin.

2. The molding resin composition according to claim 1, wherein the weight average molecular weight of said polyethylene oxide is 3,500 or more.

3. The molding resin composition according to claim 1, wherein the acid value of the oxidized polyethylene is 2 mg KOH / g to 50 mg KOH / g.

4. The molding resin composition according to claim 1, wherein said oxidized polyethylene comprises a linear oxidized polyethylene.

5. The molding resin composition according to claim 1, wherein said oxidized polyethylene comprises a branched oxidized polyethylene.

6. The molding resin composition according to claim 1, wherein said epoxy resin comprises a biphenyl type epoxy resin.

7. The molding resin composition according to claim 6, wherein the proportion of said biphenyl type epoxy resin in the total epoxy resin is 50 mass % or more.

8. The molding resin composition according to claim 1, wherein said hardener comprises a phenolic hardener.

9. The molding resin composition according to claim 8, wherein the proportion of said phenolic curing agent in the total curing agent is 50 mass % or more.

10. The molding resin composition according to claim 8, wherein the hydroxyl equivalent of said phenolic curing agent is from 70 g / eq to 1000 g / eq.

11. The molding resin composition according to claim 1, wherein the proportion of said alumina in the entire inorganic filler is 50 volume % or more.

12. The molding resin composition according to claim 1, further comprising a copolymer of an α-olefin having 5 to 30 carbon atoms and at least one of maleic anhydride and a maleic anhydride derivative.

13. The molding resin composition according to claim 12, wherein the copolymer contains a structural unit represented by the following general formula (C) and a structural unit represented by the following general formula (D): (In general formula (C) and general formula (D), R 11 represents a monovalent aliphatic hydrocarbon group having 3 to 28 carbon atoms; R 12 and R 13 each independently represents a hydrogen atom, an alkyl group, or an aryl group.

14. An electronic component device comprising a support member, an electronic component placed on the support member, and a cured product of the molding resin composition according to any one of claims 1 to 13 that encapsulates the electronic component.