Gas tungsten arc-welded joint and production method thereof
Patent Information
- Application Number
- MYPI2026000190
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-13
- Filing Date
- 2024-05-28
- Publication Date
- 2025-01-13
AI Technical Summary
Gas tungsten arc welding of high Mn steel for cryogenic applications faces challenges with hot cracking and limited strength enhancement using conventional methods, particularly due to impurity segregation and the need for expensive materials.
The use of nitrogen as a shielding gas and filler metal additive to control the solid-liquid coexistence temperature range, combined with specific chemical compositions in the steel and weld metal, enhances the strength and suppresses hot cracking in gas tungsten arc welding joints for high Mn steel.
This approach results in weld metals with improved yield stress, tensile strength, and cryogenic impact toughness, effectively preventing hot cracking and increasing the strength of the weld joints, while maintaining economic viability.
Smart Images

Figure PI2026000190_DRAWING_001 
Figure PI2026000190_DRAWING_002 
Figure PI2026000190_DRAWING_003
Abstract
Description
Gas tungsten arc welded joint and manufacturing method thereof
[0001] The present invention relates to a gas tungsten arc welded joint and a manufacturing method thereof, and in particular to a welded joint of a high Mn-containing austenitic steel material used in an extremely low temperature environment and a manufacturing method thereof. The numerical range "x to y" means x or more and y or less, and includes the boundary value. The unit of volume "L" is 10 -3 m 3 means.
[0002] Gas tungsten arc welding is a welding method that uses tungsten, a non-consumable material, as an electrode rod, and melts a filler material (filler rod) in an arc while blocking the atmosphere by spraying inert gases, typically argon gas or helium gas. This welding method is also called Tungsten Inert Gas (hereinafter abbreviated as "TIG welding"). This TIG welding can be applied to various alloy steels, non-ferrous metals, and other more complex shapes, and can produce excellent weld quality.
[0003] In recent years, environmental regulations have become stricter. Among these, liquefied natural gas (hereinafter also referred to as LNG) is said to be a clean fuel that does not generate air pollutants such as sulfur oxides because it does not contain sulfur, and demand for LNG is increasing. For the transportation or storage of LNG, containers (tanks) that transport or store LNG are required to maintain excellent cryogenic impact toughness at temperatures of −162°C or lower, which is the liquefaction temperature of LNG.
[0004] Because of the need to maintain this excellent cryogenic impact toughness, aluminum alloys, 9% Ni steel, austenitic stainless steel, etc. have conventionally been used as materials for containers (tanks) and the like.
[0005] However, aluminum alloys have low tensile strength, which requires the plate thickness of the structure to be large, and also has the problem of poor weldability.Furthermore, 9% Ni steel requires the use of expensive Ni-based materials as welding materials, which is economically disadvantageous.
[0006] Therefore, TIG welding techniques using austenitic stainless steel are being considered.
[0007] For example, Patent Document 1 discloses an austenitic steel weld joint obtained by welding a base material of austenitic steel having a specific composition by a gas tungsten arc welding method using a welding material of austenitic steel having a specific composition. The main composition of this weld metal is C≦0.1%, Si≦0.8%, Mn: 1.5 to 5.5%, Ni: 8 to 15%, Cr: 18 to 24%, Al<0.05%, and N: 0.15 to 0.35%, and the amount of ferrite in the weld metal is 20% or less in area ratio. Furthermore, in gas tungsten arc welding, N is used as a shielding gas in addition to Ar gas. 2 It also describes mixing gases at 50% by volume or less.
[0008] However, austenitic stainless steel has problems such as being expensive and having low base metal strength. For these reasons, the application of high-Mn austenitic steel (hereinafter also referred to as "high-Mn steel") containing approximately 10 to 35 mass% Mn has recently been considered as a material for containers (tanks) for transporting or storing LNG. The metal structure of high-Mn steel has an austenite phase even at extremely low temperatures, and brittle fracture does not occur. High-Mn steel is also characterized by having higher strength than austenitic stainless steel. Therefore, there has been a demand for the development of welding materials that can stably weld such high-Mn steel.
[0009] In response to such demands, for example, Patent Document 2 discloses a "high-manganese steel for cryogenic use." This steel contains, by mass, 0.001 to 0.80% C, 15.0 to 35.0% Mn, 0.001 to 0.01% S, 0.01 to 10.0% Cr, 0.001 to 0.05% Ti, 0.0001 to 0.10% N, and 0.001 to 0.010% O. Furthermore, P is limited to 0.02% or less, and contains one or both of 0.001 to 5.00% Si and 0.001 to 2.0% Al, and contains a total of 0.0002% or more of one or more of 0.01% or less Mg, 0.01% or less Ca, and 0.01% or less REM. The steel satisfies the following formulas: 30C + 0.5Mn + Ni + 0.8Cr + 1.2Si + 0.8Mo ≥ 25 (Equation 1), O / S ≥ 1 (Equation 2), with the balance being Fe and unavoidable impurities. The high-Mn steel for cryogenic use has an austenite volume fraction of 95% or more, a grain size of the austenite of 20 to 200 μm, and a carbide coverage rate at the austenite grain boundaries of 50% or less. The steel of Patent Document 2 controls the austenite grain size to an appropriate size, appropriately adjusts the amounts and balance of alloying elements, as well as the amounts of S and O, and adds Mg, Ca, and REM, so that carbides formed at the grain boundaries do not become fracture initiation points or crack propagation paths. This appropriately adjusts the austenite grain size and also makes it possible to suppress coarsening of the grain size in the weld heat-affected zone.
[0010] Patent Document 3 discloses a "thick steel plate for low temperature use." This thick steel plate contains, by mass, C: 0.30 to 0.65%, Si: 0.05 to 0.30%, Mn: more than 20.00% but less than 30.00%, Ni: 0.10% to less than 3.00%, Cr: 3.00% to less than 8.00%, and Al: 0.005 to 0.100%. The steel plate also contains N: 0.0050% to less than 0.0500%, P: 0.0040% or less, S: 0.020% or less, and O: 0.0050% or less, with the balance being Fe and impurities. Furthermore, the steel plate is described as having a Mn segregation ratio XMn (XMn = Mn1 / Mn0) calculated from the Mn concentration Mn1 in the Mn-enriched portion and the Mn concentration Mn0 in the Mn-lean portion of 1.6 or less. The yield stress at room temperature (25°C) is 400 MPa or more, the tensile stress is 800 MPa or more, and the Charpy impact absorption energy of the weld heat affected zone ( v E -196 ) is 70 J or more. According to the technology described in Patent Document 3, it is described that the steel can be provided as it is hot-rolled as a material for containers (tanks) for transporting or storing LNG.
[0011] Generally, in the design of welded structures, design stresses based on the strength characteristics of the base metal or weld metal are used. In recent years, many welded structures, including LNG tanks, have tended to become larger, which requires higher strength joints.
[0012] However, according to the inventors' investigations, there was a problem in that hot cracking could occur if the weld metal had high strength, even if the TIG welding method described in Patent Document 1 was applied to the welding of high-Mn steel materials described in Patent Documents 2 and 3. Furthermore, when high strength weld metal is required, it is necessary to change the composition of the base metal or welding material, and it has been difficult to increase the strength of the weld metal by the welding method alone.
[0013] Therefore, as disclosed in Patent Document 4, the inventors have developed a TIG welded joint for high Mn steel that can suppress the occurrence of hot cracking during welding and has high strength and excellent cryogenic impact toughness.
[0014] WO 2013 / 005570 JP 2016-196703 A JP 2017-071817 A WO 2022 / 186097 A
[0015] As described above, in the design of welded structures, design stresses based on the strength characteristics of the base metal or the weld metal are generally used. However, in recent years, many welded structures, including LNG tanks, have tended to become larger in size, which has led to a demand for even higher strength in joints. In response to the recent demand for even higher strength and improved hot cracking resistance, the inventors have investigated further improvements to the gas tungsten arc welding method for high-Mn steel.
[0016] An object of the present invention is to provide a gas tungsten arc welded joint that can further improve the strength of the weld metal and further suppress the occurrence of hot cracking as a welded joint for high-Mn steel used in cryogenic environments, and a method for manufacturing the same.
[0017] In order to achieve the above-mentioned object, the inventors first conducted extensive research into factors that affect hot cracking during TIG welding of high-Mn steel. As a result, they found that one of the factors that causes hot cracking is the segregation of impurity elements in the final solidification portion of the weld metal. Furthermore, they found that the segregation of impurity elements becomes more pronounced when the temperature range from the start of solidification to the end of solidification is large during solidification of the weld metal. Furthermore, they found that when the weld metal reaches a temperature above the solidus due to the thermal influence of welding from the next welding pass onward and liquefies, the segregation becomes more pronounced when the temperature range from the start of resolidification to the end of resolidification (hereinafter also referred to as the "solid-liquid coexistence temperature range") is large.
[0018] Next, they investigated the weld metal composition required for welded joints produced by TIG welding in accordance with the provisions of JIS Z 3121:2013 to have the desired high strength. As a result, they found that when N is included in the weld metal composition of high-Mn steel, the strength of the weld metal and welded joint is improved by solid solution strengthening. Furthermore, they found that increasing the N content in the weld metal to the range of 0.0400 to 0.4000 mass% has the effect of narrowing the solid-liquid coexistence temperature range, and that N in the weld metal composition is an additive element that suppresses the occurrence of hot cracking in high-Mn steel.
[0019] Therefore, N is N under normal temperature and pressure. 2 Since nitrogen gas is a stable element that forms molecules and is gaseous, 0.5 to 10.0% by volume of nitrogen gas (hereinafter simply referred to as "N") is used during TIG welding. 2 The inventors have found that this allows stable solid solution of N in the weld metal in a range of 0.0400 to 0.4000 mass%.
[0020] Furthermore, it was discovered that by setting the N content of the filler metal to 0.400 mass% or less, N can be stably dissolved in the weld metal not from the nitrogen gas contained in the shielding gas but also from the N in the filler metal.
[0021] The present invention was completed based on these findings and further investigations.
[0022] That is, the gist of the present invention is as follows. [1] A gas tungsten arc welded joint of a steel material using a shielding gas and a filler metal, wherein the steel material is a high-Mn-containing austenitic steel, and the chemical composition of the steel material contains, in mass%, C: 0.10 to 0.70%, Si: 0.05 to 1.00%, Mn: 18.0 to 30.0%, P: 0.030% or less, S: 0.007% or less, Al: 0.010 to 0.070%, Cr: 2.5 to 7.0%, N: 0.0050 to 0.0500%, and O (oxygen): 0.0050% or less, and optionally Mo: 0.01 to 2.00%, V: 0.01 to 2.00%, W: 0.01 to 2.00%, Ni: 0.01 to 4.00%, The weld metal contains at least one selected from REM: 0.0010 to 0.0200%, and B: 0.0005 to 0.0020%, with the balance consisting of Fe and unavoidable impurities, and the chemical composition of the weld metal contains, in mass%, C: 0.15 to 0.80%, Si: 0.10 to 1.00%, Mn: 17.0 to 30.0%, P: 0.030% or less, S: 0.030% or less, Al: 0.005 to 0.100%, Cr: 0.4 to 5.5%, Mo: 0.01 to 3.50%, Ni: 0.01 to 10.00%, and N: 0.0400 to 0.4000%, and optionally V: 0.01 to 1.00%, [2] A gas tungsten arc welded joint containing at least one selected from Ti: 0.010 to 1.000%, Nb: 0.010 to 1.000%, W: 0.01 to 1.00%, Cu: 0.01 to 1.00%, and B: 0.0010% or less, with the balance consisting of Fe and unavoidable impurities. [3] In the above [1], the weld metal has a yield stress (0.2% proof stress) of 400 MPa or more, a tensile strength of 600 MPa or more, and a Charpy impact absorption energy ( v E -196) is 28 J or more. [3] A method for manufacturing a gas tungsten arc welded joint by using a shielding gas and a filler metal on a steel material having the chemical composition described in [1] above to form a weld metal having the chemical composition described in [1] above, wherein the shielding gas contains 0.5 to 10.0% by volume of nitrogen gas, with the remainder consisting of an inert gas and unavoidable impurities. [4] A method for manufacturing a gas tungsten arc welded joint in [3] above, wherein the N content of the filler metal is 0.1200% by mass or less. [5] A method for manufacturing a gas tungsten arc welded joint in which a steel material having the composition described in [1] above is used with a shielding gas and a filler metal to form a weld metal having the composition described in [1] above, wherein the shielding gas contains less than 0.5% by volume of nitrogen gas, with the balance consisting of an inert gas and inevitable impurities, and the N content of the filler metal is 0.4000% by mass. [6] In any one of [3] to [5] above, the weld metal has a yield stress (0.2% proof stress) of 400 MPa or more, a tensile strength of 600 MPa or more, and a Charpy impact absorption energy ( v E -196 ) is 28J or more.
[0023] According to the present invention, it is possible to easily manufacture a welded joint for high-Mn steel used in an extremely low-temperature environment, which further improves the strength of the weld metal and further suppresses the occurrence of hot cracking, thereby achieving significant industrial effects.
[0024] Fig. 1 is a schematic diagram showing an example of a groove shape in a TIG welded joint of the present invention. Fig. 2 is a schematic diagram showing an example of a test piece sampling position for a Charpy impact test. Fig. 3 is a diagram showing a change in 0.2% proof stress versus N content in the weld metal with a change in nitrogen gas content. Fig. 4 is a diagram showing a change in tensile strength versus N content in the weld metal with a change in nitrogen gas content. Fig. 5 is a diagram showing a change in 0.2% proof stress versus N content in the weld metal with a change in N content of a filler metal. Fig. 6 is a diagram showing a change in tensile strength versus N content in the weld metal with a change in N content of a filler metal.
[0025] One embodiment of the present invention is a welded joint for high-Mn steel used in cryogenic environments, and is a TIG-welded joint that further improves the strength of the weld metal and further suppresses the occurrence of hot cracking. That is, the welded joint of this embodiment is a welded joint produced by TIG welding in accordance with the provisions of JIS Z 3001-7:2018 (excluding the type of shielding gas). Furthermore, compared to a typical TIG-welded joint that uses 99.5% or more inert gas as the shielding gas, the yield stress (0.2% proof stress) and tensile strength at room temperature (25°C) in a tensile test of the welded metal produced in accordance with the provisions of JIS Z 3111:2005 are improved by an average of 10 MPa or more. Furthermore, the absorbed energy (hereinafter referred to as "absorbed energy") of the welded metal of a welded joint produced in accordance with the provisions of JIS Z 3128:2017 in a Charpy impact test at a test temperature of -196°C is also improved. v E -196 ") is 28J or more, has excellent cryogenic impact toughness, and is free from hot cracking.
[0026] [Gas Tungsten Arc Welding (TIG Welding)] As mentioned above, TIG welding is a welding method in which tungsten is used as an electrode rod, and a filler material is melted in the arc as needed while blocking air by spraying an inert gas, typically argon gas or helium gas, as a shielding gas. This TIG welding method can be applied to various alloy steels and non-ferrous metals, and can also weld complex shapes, achieving excellent weld quality, so it is used to weld all kinds of metals. Specific welding conditions will be described later.
[0027] [High Mn Steel (High Mn-Containing Austenitic Steel)] First, the steel material that serves as the base material will be described. Any steel material may be used as long as it is a high-Mn-containing austenitic steel having the chemical composition described below. In the present invention, the high Mn content of high-Mn-containing austenitic steel means that the steel composition contains 18.0 to 30.0% Mn, in mass %. Furthermore, the austenitic steel of high-Mn-containing austenitic steel refers to a steel material whose base phase (metal structure) is an austenitic phase.
[0028] That is, if the crystal structure of a steel material is a body-centered cubic (bcc) structure, the steel material may undergo brittle fracture in a low-temperature environment. Therefore, the steel material is not suitable for use in a low-temperature environment. When considering use in a low-temperature environment, the base phase of the metal structure of the steel material must be an austenite structure with a face-centered cubic (fcc) crystal structure. Note that "the base phase is an austenite phase" means that the austenite phase accounts for 90% or more of the area. The remainder other than the austenite phase is a ferrite phase, a martensite phase, or precipitates such as carbides. More preferably, the austenite phase accounts for 95% or more, and even more preferably 100%.
[0029] [Basic Composition of Steel] The chemical composition of the steel according to this embodiment will now be described. In this specification, "%" in "chemical composition" means "mass %" unless otherwise specified.
[0030] The steel used in this embodiment is the aforementioned high-Mn steel containing 18.0 to 30.0% Mn, and other basic components are as follows: C: 0.10 to 0.70%, Si: 0.05 to 1.00%, P: 0.030% or less, S: 0.007% or less, Al: 0.010 to 0.070%, Cr: 2.5 to 7.0%, N: 0.0050 to 0.0500%, O (oxygen): 0.0050% or less. The remainder is a high-Mn steel having a chemical composition consisting of Fe, arbitrarily selected components, and unavoidable impurities. The reasons for limiting the chemical composition are as follows.
[0031] [C: 0.10 to 0.70%] C is an inexpensive and important element that stabilizes the austenite phase and improves cryogenic impact toughness. To achieve this effect, the C content is set to 0.10% or more. Preferably, it is set to 0.20% or more, more preferably, 0.25% or more, even more preferably, 0.30% or more, and most preferably, 0.35% or more. On the other hand, if the C content exceeds 0.70%, Cr carbides are excessively formed, resulting in a decrease in cryogenic impact toughness. Therefore, the C content is set to 0.70% or less. Preferably, it is set to 0.65% or less, more preferably, 0.63% or less, even more preferably, 0.61% or less, and most preferably, 0.60% or less.
[0032] [Si: 0.05 to 1.00%] Si acts as a deoxidizer and is an element that dissolves in steel to contribute to increasing the strength of the steel material through solid solution strengthening. To achieve this effect, the Si content is set to 0.05% or more. Preferably, it is set to 0.07% or more, more preferably, 0.10% or more, even more preferably, 0.15%, and most preferably, 0.20% or more. On the other hand, if the Si content exceeds 1.00%, weldability decreases. Therefore, the Si content is set to 1.00% or less. Preferably, it is set to 0.80% or less, more preferably, 0.70% or less, even more preferably, 0.65% or less, and most preferably, 0.60% or less.
[0033] [Mn: 18.0 to 30.0%] Mn is a relatively inexpensive element that stabilizes the austenite phase and is an important element for achieving both high strength and excellent cryogenic impact toughness. To achieve this effect, a Mn content of 18.0% or more is required. Therefore, the Mn content is set to 18.0% or more. Preferably, it is set to 20.0% or more, more preferably, 22.0% or more, and even more preferably, 24.0% or more. On the other hand, even if the Mn content exceeds 30.0%, the effect of improving cryogenic impact toughness saturates, and the expected effect commensurate with the content cannot be expected, which is economically disadvantageous. Furthermore, a large Mn content exceeding 30.0% leads to a decrease in cuttability and promotes Mn segregation, which promotes the occurrence of stress corrosion cracking. Therefore, the Mn content is set to 30.0% or less. Preferably, it is set to 29.0% or less, more preferably, 28.5% or less, and even more preferably, 28.0% or less.
[0034] [P: 0.030% or less] P is an impurity element that segregates at grain boundaries and becomes the initiation point of stress corrosion cracking. In this embodiment, it is desirable to reduce the P content as much as possible. A P content of 0.030% or less is acceptable. Therefore, the P content is set to 0.030% or less. Preferably, it is set to 0.028% or less, more preferably 0.024% or less, even more preferably 0.020% or less, and most preferably 0.015% or less. On the other hand, extremely reducing the P content to less than 0.002% requires long refining times, which increases refining costs. Therefore, from an economical point of view, the P content is preferably set to 0.002% or more.
[0035] [S: 0.007% or less] S exists in steel as sulfide-based inclusions and reduces the ductility and cryogenic impact toughness of steel and weld metal. For this reason, it is desirable to reduce S as much as possible. Note that a S content of 0.007% or less is acceptable. Therefore, the S content is set to 0.007% or less. Preferably, it is set to 0.005% or less, and more preferably, it is set to 0.004% or less. On the other hand, extremely reducing S to less than 0.0005% requires long refining times, which increases refining costs. For this reason, from an economical viewpoint, the S content is preferably set to 0.0005% or more.
[0036] [Al: 0.010 to 0.070%] Al acts as a deoxidizer and is the most commonly used element in the molten steel deoxidation process. To achieve this effect, the Al content is set to 0.010% or more. Preferably, it is set to 0.020% or more, and more preferably, it is set to 0.030% or more. On the other hand, if the Al content exceeds 0.070%, Al is mixed into the weld metal during welding, reducing the toughness of the weld metal. For this reason, the Al content is set to 0.070% or less. Preferably, it is set to 0.060% or less, and more preferably, it is set to 0.050% or less.
[0037] [Cr: 2.5 to 7.0%] Cr is an element that stabilizes the austenite phase and effectively contributes to improving cryogenic impact toughness and steel strength. It is also an effective element for forming a fine crystal region. To achieve this effect, the Cr content is set to 2.5% or more. It is preferably set to 3.0% or more, more preferably set to 3.3% or more, even more preferably set to 3.5% or more, and most preferably set to 4.0% or more. On the other hand, if the Cr content exceeds 7.0%, Cr carbides are formed, resulting in a decrease in cryogenic impact toughness and stress corrosion cracking resistance. Therefore, the Cr content is set to 7.0% or less. It is preferably set to 6.8% or less, more preferably set to 6.5% or less, and even more preferably set to 6.0% or less.
[0038] [N: 0.0050 to 0.0500%] N is an element that stabilizes the austenite phase and effectively contributes to improving cryogenic impact toughness. To achieve this effect, the N content is set to 0.0050% or more. Preferably, it is set to 0.0060% or more, more preferably, it is set to 0.0070% or more, and even more preferably, it is set to 0.0080% or more. On the other hand, if the N content exceeds 0.0500%, nitrides or carbonitrides will coarsen during the steel manufacturing process, resulting in a decrease in cryogenic impact toughness. For this reason, the N content is set to 0.0500% or less. Preferably, it is set to 0.0450% or less, more preferably, it is set to 0.0400% or less, and even more preferably, it is set to 0.0350% or less.
[0039] [O (oxygen): 0.0050% or less] O (oxygen) exists in steel as oxide-based inclusions and reduces the cryogenic impact toughness of the steel material. For this reason, it is preferable to reduce O (oxygen) as much as possible, but 0.0050% or less is acceptable. For this reason, the O (oxygen) content is set to 0.0050% or less. Preferably, it is set to 0.0045% or less, and more preferably, it is set to 0.0040% or less. On the other hand, to drastically reduce O (oxygen) to less than 0.0005%, long refining times are required, which increases refining costs. For this reason, from the viewpoint of economy, O (oxygen) is preferably set to 0.0005% or more, and more preferably, it is set to 0.0006% or more.
[0040] [Optional Composition of Steel] The chemical composition described above is the preferred basic composition of high-Mn steel, but in addition to this basic composition, optional compositions that may be contained as needed are shown below. These are at least one of Mo: 0.01 to 2.00%, V: 0.01 to 2.00%, W: 0.01 to 2.00%, Ni: 0.01 to 4.00%, REM: 0.0010 to 0.0200%, and B: 0.0005 to 0.0020%. The reasons for limiting each composition are as follows:
[0041] [Mo, V, and W: 0.01 to 2.00%] Mo, V, and W are elements that contribute to stabilizing the austenite phase and also contribute to improving the strength and cryogenic impact toughness of the steel material. At least one of them can be selected and contained as needed. To achieve these effects, it is preferable that the Mo, V, and W contents are each 0.01% or more. On the other hand, if the Mo, V, and W contents exceed 2.00%, the amount of coarse carbonitrides increases, which become the origin of fracture and reduce the cryogenic impact toughness. Therefore, when Mo, V, and W are contained, it is preferable that they be 2.00% or less. More preferably, the Mo, V, and W contents are each 1.70% or less, and even more preferably 1.50% or less.
[0042] [Ni: 0.01 to 4.00%] Ni is an element that contributes to stabilizing the austenite phase and strengthening the austenite grain boundaries, and also contributes to improving the cryogenic impact toughness of steel. To achieve these effects, the Ni content is preferably 0.01% or more. More preferably, it is 0.10% or more, and even more preferably, it is 0.20% or more. On the other hand, Ni is an expensive element, and a Ni content exceeding 4.00% is economically disadvantageous. Therefore, the Ni content is preferably 4.00% or less. More preferably, it is 3.75% or less, and even more preferably, it is 3.50% or less.
[0043] [REM: 0.0010 to 0.0200%] REM is a rare earth element such as Sc, Y, La, or Ce. REM is an element that has the effect of improving the toughness of steel, as well as ductility and sulfide stress corrosion cracking resistance, by controlling the morphology of inclusions. To achieve this effect, the REM content is preferably 0.0010% or more, and more preferably 0.0015% or more. On the other hand, if the REM content exceeds 0.0200%, the amount of nonmetallic inclusions increases, which may result in a decrease in toughness, ductility, and sulfide stress cracking resistance. For this reason, the REM content is preferably 0.0200% or less, and more preferably 0.0180% or less.
[0044] [B: 0.0005 to 0.0020%] B is an element that segregates at grain boundaries and contributes to improving the toughness of steel. To achieve this effect, the B content is preferably 0.0005% or more, and more preferably 0.0008% or more. On the other hand, if the B content exceeds 0.0020%, coarse nitrides and carbides increase, which may reduce toughness. For this reason, the B content is preferably 0.0020% or less, and more preferably 0.0018% or less.
[0045] [Remainder of Steel Composition] The remainder of the composition other than the above-described chemical composition consists of Fe and unavoidable impurities. Examples of unavoidable impurities include Ca, Mg, Ti, Nb, and Cu, and a total of 0.05% or less is acceptable. The inclusion of elements below the lower limit of the optional composition does not affect the properties of high-Mn steel, and is therefore acceptable as an unavoidable impurity. Furthermore, elements other than these may be included as long as they satisfy the basic composition and optional composition described above and do not affect the properties of high-Mn steel, and such embodiments are also within the technical scope of the present invention.
[0046] [Method of manufacturing high Mn steel] Next, a preferred method of manufacturing the high Mn steel used in this embodiment will be described. Note that manufacturing methods other than the method described below may also be used as long as equivalent high Mn steel can be obtained, and the manufacturing method is not limited to the following method.
[0047] Molten steel having the above-described steel composition is produced by a conventional melting method such as a converter or an electric furnace, and then produced into a steel material such as a slab of a predetermined size by a conventional casting method such as a continuous casting method or an ingot making-blooming rolling method. During the production, secondary refining may be carried out using a vacuum degassing furnace or the like.
[0048] The obtained steel material is either as cast or further heated, hot rolled, and then cooled to a predetermined size. A steel material with excellent cryogenic impact toughness can be obtained by heating at a heating temperature in the range of 1100 to 1300°C, finishing the hot rolling at a finish rolling end temperature of 790 to 980°C, and immediately cooling. Further heat treatments such as annealing may be performed to adjust the steel material properties.
[0049] Next, preferred mechanical properties of the high Mn steel used in this embodiment will be described. The high strength steel for cryogenic use having the above steel composition has a plate thickness of, for example, 5 to 102 mm, a yield stress (0.2% proof stress) YS of 400 MPa or more, and a Charpy impact absorption energy ( v E -196 Preferably, the tensile strength TS is 28 J or more. Furthermore, the tensile strength TS is 660 MPa or more. More preferably, the tensile strength TS is 800 MPa or more.
[0050] [Basic Composition of Weld Metal] In this embodiment, the high-Mn steels described above are welded joints formed by TIG welding to form a weld metal part consisting of a single layer or multiple layers of weld metal. The chemical composition of this weld metal part is a mixture (up to about 50%) of the filler metal composition and the base metal composition of the high-Mn steel.
[0051] The basic composition of the weld metal according to this embodiment is as follows: C: 0.15 to 0.80%, Si: 0.10 to 1.00%, Mn: 17.0 to 30.0%, P: 0.030% or less, S: 0.030% or less, Al: 0.005 to 0.100%, Cr: 0.4 to 5.5%, Mo: 0.01 to 3.50%, Ni: 0.01 to 10.00%, N: 0.0400 to 0.4000%, with the balance being Fe, arbitrarily selected compositions, and unavoidable impurities. The reasons for limiting the chemical composition are as follows:
[0052] [C: 0.15 to 0.80%] C is an element that increases the strength of the weld metal through solid solution strengthening. It also stabilizes the austenite phase and improves the cryogenic impact toughness of the weld metal. To achieve this effect, a C content of 0.15% or more is required. Therefore, the C content is set to 0.15% or more. Preferably, it is set to 0.20% or more, more preferably, 0.25% or more, and even more preferably, 0.28% or more. On the other hand, if the C content exceeds 0.80%, carbides precipitate, reducing the cryogenic impact toughness and increasing the likelihood of hot cracking during welding. Therefore, the C content is set to 0.80% or less. Preferably, it is set to 0.75% or less, more preferably, 0.70% or less, even more preferably, 0.65% or less, and most preferably, 0.63% or less.
[0053] [Si: 0.10 to 1.00%] Si acts as a deoxidizer, increasing the yield of Mn and increasing the viscosity of the molten metal, thereby stably maintaining the bead shape. To achieve this effect, a Si content of 0.10% or more is required. Therefore, the Si content is set to 0.10% or more. Preferably, it is set to 0.15% or more, more preferably 0.20% or more, even more preferably 0.25% or more, and most preferably 0.28% or more. On the other hand, a Si content exceeding 1.00% reduces the cryogenic impact toughness of the weld metal. Furthermore, Si segregates during solidification, forming a liquid phase at the solidification cell interface, thereby reducing hot cracking resistance. Therefore, the Si content is set to 1.00% or less. Preferably, it is set to 0.80% or less, more preferably 0.75% or less, and even more preferably 0.70% or less.
[0054] [Mn: 17.0 to 30.0%] Mn is an inexpensive element that stabilizes the austenite phase, and in this embodiment, a content of 17.0% or more is required. If the Mn content is less than 17.0%, a ferrite phase will form in the weld metal, significantly reducing the cryogenic impact toughness. For this reason, the Mn content is set to 17.0% or more. Preferably, it is set to 18.0% or more, and more preferably, it is set to 19.0% or more. On the other hand, if the Mn content exceeds 30.0%, excessive Mn segregation will occur during solidification, inducing hot cracking. For this reason, the Mn content is set to 30.0% or less. Preferably, it is set to 28.0% or less, and more preferably, it is set to 27.0% or less.
[0055] [P: 0.030% or less] P is an element that segregates at grain boundaries and induces hot cracking. In this embodiment, it is preferable to reduce the P content as much as possible, but 0.030% or less is acceptable. Therefore, the P content is set to 0.030% or less. Preferably, it is 0.020% or less, more preferably 0.018% or less, even more preferably 0.016% or less, and most preferably 0.014% or less. Note that excessive reduction leads to an increase in refining costs. Therefore, the P content is preferably adjusted to 0.002% or more.
[0056] [S: 0.030% or less] S exists in the weld metal as sulfide-based inclusions MnS. MnS acts as a fracture initiation point, reducing cryogenic impact toughness. Therefore, the S content is set to 0.030% or less. Preferably, it is set to 0.025% or less, more preferably, 0.020% or less, and even more preferably, it is set to 0.017% or less. Note that excessive reduction leads to an increase in refining costs. Therefore, the S content is preferably adjusted to 0.001% or more.
[0057] [Al: 0.005 to 0.100%] Al acts as a deoxidizer, increasing the viscosity of the molten metal and playing an important role in stably maintaining the bead shape. Furthermore, Al narrows the temperature range within which the molten metal remains solid and liquid, thereby contributing to the suppression of hot cracking in the weld metal. This effect is significant at an Al content of 0.005% or more, so the Al content is set to 0.005% or more. Preferably, the Al content is set to 0.010% or more, and more preferably, 0.015% or more. On the other hand, if the Al content exceeds 0.100%, the viscosity of the molten metal becomes too high, which in turn prevents the bead from spreading and increases defects such as incomplete fusion. Therefore, the Al content is set to 0.100% or less. Preferably, the Al content is set to 0.060% or less, more preferably, 0.050% or less, and even more preferably, 0.040% or less.
[0058] [Cr: 0.4 to 5.5%] Cr acts as an element that stabilizes the austenite phase at cryogenic temperatures, thereby improving the cryogenic fracture toughness of the weld metal. It also has the effect of improving the strength of the weld metal, the effect of increasing the liquidus temperature of the molten metal to prevent hot cracking of the weld metal during welding, and the effect of improving the corrosion resistance of the weld metal. If the Cr content is too low, these effects cannot be obtained. To achieve these effects, a Cr content of 0.4% or more is required. Preferably, the Cr content is 0.6% or more, and more preferably, 0.8% or more. On the other hand, if the Cr content is too high, Cr carbides precipitate in the weld metal, reducing the cryogenic fracture toughness of the weld metal. Therefore, the Cr content must be 5.5% or less. Preferably, the Cr content is 5.0% or less, and more preferably, 4.5% or less.
[0059] [Mo: 0.01 to 3.50%] Mo is an element that strengthens austenite grain boundaries, segregating at the grain boundaries and improving the strength of the weld metal. It also has the effect of improving the strength of the weld metal through solid solution strengthening. To achieve this effect, the Mo content must be 0.01% or more. Preferably, it is 0.30% or more, more preferably 0.50% or more, and even more preferably 1.00% or more. On the other hand, if it is contained in an amount exceeding 3.50%, it precipitates as carbides, which become the starting point for fracture, resulting in a decrease in cryogenic impact toughness. Therefore, the Mo content is set to 3.50% or less. Preferably, it is 3.20% or less, more preferably 3.00% or less, and even more preferably 2.50% or less.
[0060] [Ni: 0.01 to 10.00%] Ni is an element that strengthens austenite grain boundaries, segregating at the grain boundaries and improving cryogenic impact toughness. Ni also has the effect of stabilizing the austenite phase. Therefore, further increasing the Ni content stabilizes the austenite phase and improves the cryogenic impact toughness of the weld metal. To achieve this effect, a Ni content of 0.01% or more is required. Preferably, the Ni content is 0.02% or more, more preferably 0.05% or more, and even more preferably 1.00% or more. However, Ni is an expensive element, and a Ni content exceeding 10.00% is economically disadvantageous. Therefore, the Ni content is set to 10.00% or less. Preferably, the Ni content is 8.00% or less, more preferably 7.00% or less, even more preferably 6.50% or less, and most preferably 6.00% or less.
[0061] [N: 0.0400 to 0.4000%] N is an element that is inevitably incorporated, but is intentionally incorporated in this embodiment. Like C, N effectively contributes to improving the strength of the weld metal and stabilizes the austenite phase, contributing to a stable improvement in cryogenic impact toughness. Furthermore, increasing the N content narrows the solid-liquid coexistence temperature range, making it an additive element that suppresses the occurrence of hot cracking during welding of high-Mn steel. This effect becomes significant when the N content is 0.0400% or more. Therefore, the N content is set to 0.0400% or more. Preferably, it is 0.0500% or more, more preferably 0.0800% or more, and even more preferably 0.1000% or more. On the other hand, if the N content exceeds 0.4000%, nitrides are formed, which reduces low-temperature toughness and excessive solute N leads to the occurrence of weld defects such as blowholes and pits. Therefore, the N content is set to 0.4000% or less. The content is preferably 0.3500% or less, and more preferably 0.3000% or less.
[0062] As a method for adding N to the weld metal, as will be described later, it is possible to add N by mixing nitrogen gas with the shielding gas used during gas tungsten arc welding, or to add N by increasing the N content in the filler metal, which is the welding material.
[0063] [Optional Composition of Weld Metal] The weld metal of this embodiment has the basic chemical composition described above, but in addition to this basic chemical composition, the weld metal may contain, as optional compositions, at least one element selected from V: 0.01 to 1.00%, Ti: 0.010 to 1.000%, Nb: 0.010 to 1.000%, W: 0.01 to 1.00%, Cu: 0.01 to 1.00%, and B: 0.0010% or less, as needed. The reasons for limiting each of the compositions are as follows.
[0064] [V: 0.01 to 1.00%] V is a carbide-forming element that precipitates fine carbides, thereby contributing to improving the strength of the weld metal. To achieve this effect, when V is contained, it is preferable that it be contained in an amount of 0.01% or more. More preferably, it is contained in an amount of 0.02% or more. On the other hand, when V is contained in an amount of more than 1.00%, the carbides become coarse and become the starting point of fracture, resulting in a decrease in cryogenic impact toughness. Therefore, when V is contained, it is preferable that its content be 1.00% or less. More preferably, it is 0.80% or less, and even more preferably, it is 0.60% or less.
[0065] [Ti: 0.010 to 1.000%] Ti is a carbide-forming element and contributes to improving the strength of the weld metal by precipitating fine carbides. Ti also contributes to suppressing hot cracking by precipitating carbides at the solidification cell interface of the weld metal. To achieve this effect, the Ti content is preferably 0.010% or more. More preferably, it is 0.015% or more. On the other hand, if the Ti content exceeds 1.000%, the carbides become coarse and become the starting point of fracture, resulting in a decrease in cryogenic impact toughness. Therefore, the Ti content is preferably 1.000% or less. More preferably, it is 0.800% or less, and even more preferably, it is 0.600% or less.
[0066] [Nb: 0.010 to 1.000%] Nb is a carbide-forming element that precipitates carbides and contributes to improving the strength of the weld metal. Furthermore, Nb precipitates carbides at the solidification cell interface of the weld metal, contributing to suppressing the occurrence of hot cracking. To achieve this effect, the Nb content is preferably 0.010% or more. More preferably, it is 0.015% or more. On the other hand, if the Nb content exceeds 1.000%, the carbides become coarse and become the starting point of fracture, resulting in a decrease in cryogenic impact toughness. Therefore, the Nb content is preferably 1.000% or less. More preferably, it is 0.800% or less, even more preferably, it is 0.700% or less, and most preferably, it is 0.600% or less.
[0067] [W: 0.01 to 1.00%] W is a carbide-forming element that precipitates carbides, contributing to improving the strength of the weld metal. It also contributes to stabilizing the austenite phase and improving cryogenic impact toughness. W also precipitates carbides at the solidification cell interface of the weld metal, contributing to suppressing hot cracking. To achieve this effect, the W content is preferably 0.01% or more. More preferably, it is 0.02% or more, and even more preferably, it is 0.05% or more. On the other hand, if the W content exceeds 1.00%, the carbides become coarse and become fracture initiation sites, resulting in a decrease in cryogenic impact toughness. Therefore, the W content is preferably 1.00% or less. More preferably, it is 0.80% or less, and even more preferably, it is 0.60% or less.
[0068] [Cu: 0.01 to 1.00%] Cu is an element that stabilizes the austenite phase, stabilizing the austenite phase even at cryogenic temperatures and improving the cryogenic impact toughness of the weld metal. To achieve this effect, the Cu content is preferably 0.01% or more, and more preferably 0.04% or more. On the other hand, if Cu is contained in a large amount exceeding 1.00%, it segregates during solidification and induces hot cracking during welding. Therefore, the Cu content is preferably 1.00% or less, and more preferably 0.80% or less.
[0069] [B: 0.0010% or less] B is an element that segregates at grain boundaries and contributes to improving the toughness of steel materials. However, if the B content exceeds 0.0010%, the amount of coarse nitrides and carbides increases, resulting in a decrease in toughness. Therefore, the B content is preferably 0.0010% or less. More preferably, it is 0.0008% or less, and even more preferably, it is 0.0007% or less.
[0070] [Remainder of Weld Metal Composition] The balance other than the above-described chemical composition consists of Fe and unavoidable impurities. Examples of unavoidable impurities include H, O, Mg, Ca, Zn, Re, and REM, and a total of 0.0100% or less is acceptable. The inclusion of elements below the lower limit of the optional composition does not affect the properties of the weld metal, and is therefore acceptable as an unavoidable impurity. Furthermore, elements other than these may be included as long as they satisfy the basic composition and optional composition described above and do not affect the properties of the weld metal, and such embodiments are also within the technical scope of the present invention.
[0071] The chemical composition of the weld metal is determined mainly by the inflow ratio of the base metal and the welding material such as the TIG welding filler metal.
[0072] [Welding method and welding conditions] Next, a specific example of a TIG welding method suitable for producing a welded joint according to this embodiment will be described. One embodiment is shown in Figure 1. The plate thickness t of the steel material that serves as the base material 1 is 5 to 102 mm.
[0073] When preparing the test specimens described below, the base materials 1 are butted together in accordance with JIS Z 3111:2005 to form a V-groove with a groove angle θ in the range of 35 to 60°. A pure tungsten rod and filler metal are used as electrodes for TIG welding, and preheating is not required. A pure tungsten rod with a diameter of 2.5 to 4.0 mm can be used. A wire or filler rod with a diameter of 1.5 to 2.5 mm can be used as the filler metal.
[0074] Other welding conditions include a current of 180 to 250 A, a voltage of 10 to 20 V, a welding speed of 5 to 30 cm / min, and a welding heat input of 7.0 to 40.0 kJ / cm. A welding heat input of less than 7.0 kJ / cm results in insufficient deposition, prone to welding defects, and low efficiency, making it unsuitable for practical use. On the other hand, a heat input of more than 40.0 kJ / cm results in rapid electrode wear, requiring frequent electrode replacement, which reduces efficiency and decreases arc stability, making welding defects more likely. A more preferred range is 8.0 to 30.0 kJ / cm, and even more preferred is 8.0 to 25.0 kJ / cm. The interpass temperature is 100 to 150°C.
[0075] Examples of welding positions include downward, horizontal, upward, and vertical upward welding. The groove shape may be a V-groove as shown in Fig. 1, or a square groove, K-groove, or X-groove. As mentioned above, the groove angle θ is preferably 35 to 60°, and more preferably 40 to 55°.
[0076] Under the above-described welding conditions, a weld metal 2 is formed in the V-groove by single-layer or multi-layer welding, and the weld metal 2 has a form in which multiple weld metal layers 2a are stacked one on top of the other. Note that, with the welding method of this embodiment, that is, when the above-described welding conditions are not met, welding defects such as solidification cracks 4 occur in part of the weld metal layers 2a. On the other hand, with the welding method of this embodiment, such welding defects such as solidification cracks 4 do not occur.
[0077] [Shielding Gas] In this embodiment, in addition to general TIG welding, a gas containing 0.5 to 10.0% nitrogen (N) by volume is used as a shielding gas for TIG welding. 2 It is preferable to use an arc welding shielding gas containing an inert gas and an inert gas as the remainder, with the remainder being an inert gas and unavoidable impurities. Note that, hereinafter, "%" in the gas component contents means "volume %."
[0078] In this embodiment, the "inert gas" used as a shielding gas refers to argon (Ar) gas, helium (He) gas, or a mixture thereof. The content of this inert gas is preferably in the range of 90.0 to 99.5%, more preferably in the range of 93.0 to 99.5%, even more preferably in the range of 93.0 to 98.0%, and most preferably in the range of 95.0 to 98.0%.
[0079] The inevitable impurities are gases other than nitrogen gas and the above-mentioned inert gases, and oxygen (O 2 ) gas, hydrogen (H 2 ) gas, carbon dioxide (CO 2 ) gas, etc.
[0080] N is an element that, when dissolved in the weld metal of high-Mn steel, improves the strength of the weld metal and weld joint through solid solution strengthening. Furthermore, as the N content in the weld metal increases, it tends to narrow the solid-liquid coexistence temperature range, improving hot cracking susceptibility. To achieve this effect, 0.5% or more of nitrogen (N) should be added to the shielding gas. 2 ) is required. Therefore, the nitrogen content in the shielding gas is set to 0.5% or more. Preferably, it is set to 0.8% or more, and more preferably, it is set to 1.0% or more. On the other hand, if the nitrogen content in the shielding gas is 10.0% or more, the arc becomes unstable and welding defects such as blowholes and pits occur. Therefore, the nitrogen content in the shielding gas is set to 10.0% or less. Preferably, it is set to 8.0% or less, more preferably, it is set to 6.0% or less, even more preferably, it is set to 5.0% or less, and most preferably, it is set to 4.5% or less.
[0081] As described above, by using a shielding gas containing 0.5 to 10.0% by volume of nitrogen gas, with the remainder being an inert gas and unavoidable impurities, the N content in the weld metal of high-Mn steel becomes 0.0400 to 0.4000%, N dissolves in the weld metal, and the strength of the weld metal and welded joint can be improved.
[0082] The flow rate of the shielding gas is preferably in the range of 10 to 30 L / min, and more preferably in the range of 15 to 25 L / min.
[0083] [Basic Composition of Filler Metal] This embodiment is a welding method for forming a welded joint by TIG welding the above-mentioned high-Mn steels together, forming a weld metal part consisting of a single layer or multiple layers of weld metal. The preferred chemical composition of the filler metal used in this case is shown below. Note that hereinafter, "%" in the "chemical composition" of the filler metal means "mass %."
[0084] The filler metal used in this embodiment preferably has a basic composition as follows: C: 0.20 to 0.80%, Si: 0.15 to 1.00%, Mn: 17.0 to 30.0%, P: 0.030% or less, S: 0.030% or less, Ni: 0.01 to 10.00%, Cr: 0.4 to 4.0%, and Mo: 0.01 to 3.50%. Furthermore, the filler metal has a composition that contains B: 0.0010% or less and N: 0.4000% or less, with the balance consisting of Fe, optional components, and unavoidable impurities. The reasons for limiting each component are as follows:
[0085] [C: 0.20 to 0.80%] C is an element that increases the strength of the weld metal through solid solution strengthening. It is also an inexpensive and important element that stabilizes the austenite phase and improves the cryogenic impact toughness of the weld metal. To achieve this effect, the C content is preferably 0.20% or more. More preferably, it is 0.25% or more, and even more preferably, it is 0.28% or more. On the other hand, if the C content exceeds 0.80%, excessive carbides are formed in the weld metal, which reduces the cryogenic impact toughness and may make hot cracking more likely to occur during welding. Therefore, the C content is preferably 0.80% or less. More preferably, it is 0.75% or less, even more preferably, it is 0.70% or less, and most preferably, it is 0.63% or less.
[0086] [Si: 0.15 to 1.00%] Si acts as a deoxidizer, increasing the yield of Mn and increasing the viscosity of the molten metal, thereby stably maintaining the bead shape. To achieve this effect, the Si content is preferably 0.15% or more. More preferably, it is 0.18% or more, even more preferably, it is 0.20% or more, and most preferably, it is 0.25% or more. On the other hand, if the Si content exceeds 1.00%, the cryogenic impact toughness of the weld metal decreases. Furthermore, Si segregates during solidification, forming a liquid phase at the solidification cell interface, which may deteriorate hot cracking resistance. Therefore, the Si content is preferably 1.00% or less. More preferably, it is 0.80% or less, even more preferably, it is 0.75% or less, and most preferably, it is 0.70% or less.
[0087] [Mn: 17.0 to 30.0%] Mn is an inexpensive element that stabilizes the austenite phase. However, if the Mn content is less than 17.0%, a ferrite phase may form in the weld metal, significantly reducing cryogenic impact toughness. Therefore, the Mn content is preferably 17.0% or more. More preferably, it is 18.0% or more, and even more preferably, it is 18.5% or more. On the other hand, if the Mn content exceeds 30.0%, stacking fault energy increases and resistance during deformation decreases, which may result in a decrease in strength. Therefore, the Mn content is preferably 30.0% or less. More preferably, it is 27.0% or less, and even more preferably, it is 26.0% or less.
[0088] [P: 0.030% or less] P is an element that segregates at grain boundaries and induces hot cracking. In this embodiment, it is preferable to reduce the P content as much as possible, but 0.030% or less is acceptable. Therefore, the P content is preferably 0.030% or less. More preferably, it is 0.020% or less, even more preferably, it is 0.018% or less, and most preferably, it is 0.014% or less. On the other hand, extremely reducing the P content to less than 0.002% requires long refining times, which increases refining costs. Therefore, from an economical point of view, the P content is preferably 0.002% or more.
[0089] [S: 0.030% or less] S exists in the weld metal as sulfide-based inclusions MnS. MnS can act as fracture initiation points, which can reduce cryogenic impact toughness. Therefore, the S content is preferably 0.030% or less. More preferably, it is 0.025% or less, even more preferably, it is 0.020% or less, and most preferably, it is 0.017% or less. On the other hand, excessive reduction leads to an increase in refining costs. Therefore, the S content is preferably 0.001% or more.
[0090] [Ni: 0.01 to 10.00%] Ni is an element that strengthens austenite grain boundaries, segregating at the grain boundaries and improving cryogenic impact toughness. Ni also has the effect of stabilizing the austenite phase. Therefore, further increasing the Ni content stabilizes the austenite phase and improves the cryogenic impact toughness of the weld metal. To achieve this effect, the Ni content is preferably 0.01% or more. More preferably, it is 1.00% or more. However, Ni is an expensive element, and a Ni content exceeding 10.00% is economically disadvantageous. Therefore, the Ni content is preferably 10.00% or less. More preferably, it is 8.00% or less, even more preferably, it is 7.00% or less, and most preferably, it is 6.00% or less.
[0091] [Cr: 0.4 to 4.0%] Cr is an element that stabilizes the austenite phase at cryogenic temperatures and effectively contributes to improving cryogenic impact toughness and weld metal strength. Cr also narrows the temperature range of the solid-liquid coexistence region of the molten metal, effectively suppressing the occurrence of hot cracking. To achieve this effect, the Cr content is preferably 0.4% or more. More preferably, it is 0.8% or more, even more preferably, it is 1.0% or more, and most preferably, it is 1.2% or more. On the other hand, a Cr content exceeding 4.0% may result in the formation of Cr carbides, which may lead to a decrease in cryogenic impact toughness. Therefore, the Cr content is preferably 4.0% or less. More preferably, it is 3.5% or less, even more preferably, it is 3.2% or less, and most preferably, it is 2.8% or less.
[0092] [Mo: 0.01 to 3.50%] Mo is an element that strengthens austenite grain boundaries, segregating at the grain boundaries and improving the strength of the weld metal. It also has the effect of improving the strength of the weld metal through solid solution strengthening. To achieve this effect, the Mo content is preferably 0.01% or more. More preferably, it is 0.50% or more, even more preferably, it is 1.00% or more, and most preferably, it is 1.50% or more. On the other hand, if the Mo content exceeds 3.50%, the effect of increasing the strength of the weld metal becomes limited. Furthermore, Mo precipitates as carbides, which can become the origin of fracture, and this can lead to a decrease in cryogenic impact toughness. Therefore, the Mo content is preferably 3.50% or less. More preferably, it is 3.30% or less, even more preferably, it is 3.10% or less, and most preferably, it is 3.00% or less.
[0093] [B: 0.0010% or less] B is one of the elements that segregate at austenite grain boundaries. If B is mixed in at more than 0.0010%, boron nitride is formed at the austenite grain boundaries, reducing strength. Furthermore, the boron nitride may become the origin of fracture, reducing cryogenic impact toughness. Therefore, the B content is preferably 0.0010% or less. More preferably, it is 0.0008% or less, and even more preferably, it is 0.0005% or less.
[0094] [N: 0.4000% or Less] When a conventional shielding gas consisting solely of an inert gas (less than 0.5% nitrogen by volume) is used to increase the N content in the weld metal, the N content in the weld metal does not increase, so it is preferable to use a filler metal with an increased N content. In this case, the N content of the filler metal is preferably 0.4000% or less. If the N content of the filler metal exceeds 0.4000%, the amount added to the weld metal becomes excessively high, resulting in excessively high intragranular strength compared to intergranular strength, which can lead to fracture at the grain boundaries and reduced cryogenic impact toughness. Therefore, when a conventional inert gas is used as the shielding gas, the N content is preferably 0.4000% or less. More preferably, it is 0.3800% or less, and even more preferably, it is 0.3600% or less. When a conventional inert gas is used as the shielding gas, the N content of the filler metal is preferably 0.0400% or more in order to ensure that the N content in the weld metal is 0.0400% or more. More preferably, it is 0.0800% or more, and even more preferably, it is more than 0.1200%.
[0095] However, in the case of the method of adding N to the weld metal from nitrogen gas by using a shielding gas containing 0.5 to 10.0% nitrogen by volume as the above-mentioned shielding gas, if the N content of the filler metal is high, the N content in the weld metal will be excessive, and the cryogenic impact toughness will deteriorate. To prevent this, it is preferable to keep the N content of the filler metal to 0.1200% or less. More preferably, it is 0.1100% or less, and even more preferably, it is 0.1000% or less.
[0096] N is an element that effectively contributes to improving the intragranular strength of the weld metal, stabilizes the austenite phase, and contributes to a stable improvement in cryogenic impact toughness. To achieve these effects, the N content is preferably 0.0030% or more, more preferably 0.0040% or more, and even more preferably 0.0060% or more.
[0097] [Optional Composition of Filler Metal] The chemical composition described above is a preferred basic composition for the filler metal used in this embodiment, but in addition to this basic composition, the filler metal may contain the following optional compositions as needed. These are at least one selected from V: 0.01-0.04%, Ti: 0.010-0.040%, Nb: 0.010-0.040%, Cu: 0.01-1.00%, Al: 0.010-0.100%, and W: 0.01-1.00%. The reasons for limiting these optional compositions are as follows.
[0098] [V: 0.01 to 0.04%] V is a carbide-forming element that precipitates fine carbides, contributing to improved strength of the weld metal. To achieve this effect, the V content is preferably 0.01% or more. On the other hand, if the V content exceeds 0.04%, the carbides become coarse and can become the starting point for cracks during wiredrawing of the filler metal, reducing wiredrawability and wire manufacturability. Therefore, the V content is preferably 0.04% or less.
[0099] [Ti: 0.010 to 0.040%] Ti is a carbide-forming element and contributes to improving the strength of the weld metal by precipitating fine carbides. It also contributes to suppressing hot cracking by precipitating carbides at the solidification cell interface of the weld metal. To achieve this effect, the Ti content is preferably 0.010% or more. More preferably, it is 0.015% or more, and even more preferably, it is 0.020% or more. On the other hand, if the Ti content exceeds 0.040%, the carbides become coarse and may become the starting point for cracks during the drawing of the solid wire, thereby reducing the wiredrawability and the manufacturability of the wire. Therefore, the Ti content is preferably 0.040% or less. More preferably, it is 0.035% or less, and even more preferably, it is 0.030% or less.
[0100] [Nb: 0.010 to 0.040%] Nb is a carbide-forming element and contributes to improving the strength of the weld metal by precipitating carbides. It also contributes to suppressing hot cracking by precipitating carbides at the solidification cell interface of the weld metal. To achieve this effect, the Nb content is preferably 0.010% or more. More preferably, it is 0.015% or more, and even more preferably, it is 0.020% or more. On the other hand, if the Nb content exceeds 0.040%, the carbides become coarse and may become the starting point for cracks during the drawing of the solid wire, thereby reducing the wiredrawability and the manufacturability of the wire. Therefore, the Nb content is preferably 0.040% or less. More preferably, it is 0.035% or less, and even more preferably, it is 0.030% or less.
[0101] [Cu: 0.01 to 1.00%] Cu is an element that stabilizes the austenite phase, stabilizing the austenite phase even at cryogenic temperatures and improving the cryogenic impact toughness of the weld metal. To achieve this effect, the Cu content is preferably 0.01% or more. More preferably, it is 0.05% or more, and even more preferably, it is 0.10% or more. On the other hand, if the Cu content exceeds 1.00%, the hot ductility may decrease, and the manufacturability of the wire may decrease. Therefore, the Cu content is preferably 1.00% or less. More preferably, it is 0.70% or less, and even more preferably, it is 0.50% or less.
[0102] [Al: 0.010 to 0.100%] Al acts as a deoxidizer, increases the viscosity of the molten metal, stably maintains the bead shape, and has the important effect of reducing spatter. It also increases the liquidus temperature of the molten metal, contributing to the suppression of hot cracking in the weld metal. To achieve these effects, the Al content is preferably 0.010% or more. More preferably, it is 0.020% or more, and even more preferably, it is 0.025% or more. On the other hand, if the Al content exceeds 0.100%, the viscosity of the molten metal becomes too high, which may increase spatter and defects such as poor bead spreading and incomplete fusion. Therefore, the Al content is preferably 0.100% or less. More preferably, it is 0.060% or less, and even more preferably, it is 0.050% or less.
[0103] [W: 0.01 to 1.00%] W is an element that contributes to stabilizing the austenite phase and also contributes to improving strength and cryogenic impact toughness, and can be contained as needed. To achieve this effect, the W content is preferably 0.01% or more. More preferably, it is 0.02% or more, and even more preferably, it is 0.08% or more. If the W content exceeds 1.00%, the amount of coarse carbonitrides increases, which become the starting point of fracture and reduce the cryogenic impact toughness. Therefore, when W is contained, it is preferably 1.00% or less. More preferably, the W content is 0.80% or less, and even more preferably, it is 0.70% or less.
[0104] [Remainder of the Filler Metal Composition] The remainder of the composition other than the above-described chemical composition consists of Fe and unavoidable impurities. Examples of unavoidable impurities include H, O, Mg, Zn, and Re, and a total of 0.020% or less is acceptable. The inclusion of elements below the lower limit of the optional composition does not affect the filler metal's properties, and is therefore acceptable as an unavoidable impurity. Furthermore, elements other than these may be included as long as they satisfy the basic composition and optional composition described above and do not affect the filler metal's properties, and such embodiments are also within the scope of the present invention.
[0105] The present invention will be further described below with reference to examples. However, the following examples are merely intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention.
[0106] Example 1 Molten steel was produced in a vacuum melting furnace, cast into a mold, and then bloomed into slabs (thickness: 150 mm) having the composition shown in Table 1, thereby obtaining steel materials. The balance consisted of Fe and unavoidable impurities. The obtained steel materials were then charged into a heating furnace, heated to 1250°C, and hot-rolled to a finish rolling temperature of 850°C, followed immediately by water cooling to obtain steel materials (high Mn steel) with plate thicknesses of 12 mm and 30 mm. In the following table, underlined parts indicate results outside the technical scope of the present invention.
[0107]
[0108] Next, molten steel having the composition shown in Table 2 was melted in a vacuum melting furnace and cast into a 1000 kg steel ingot. The balance consisted of Fe and unavoidable impurities. The resulting steel ingot was heated to 1200°C, hot rolled, then cold rolled, and annealed (900°C to 1200°C) as necessary to obtain a 2.0 mm diameter, 1000 mm long TIG welding filler material (filler rod).
[0109]
[0110] Next, the resulting steel sheets (12 mm and 30 mm thick) and TIG welding filler rods were butted together in accordance with JIS Z 3121:2013 to form a V-groove with a groove angle θ of 45°. TIG welding was performed under the conditions shown in Table 3. A weld metal was formed in the groove, yielding a welded joint. The TIG welding was performed in a flat position without preheating, using filler rods (2.0 mm diameter) with the compositions shown in Table 2. The welding conditions were a current of 200 to 230 A, a negative electrode (DCEN), a voltage of 12 to 16 V, a welding speed of 8 to 14 cm / min, and an interpass temperature of 100 to 150°C. The welding conditions used are shown in Table 3. A pure tungsten rod (3.2 mm diameter) was used as the electrode.
[0111]
[0112] [Weld Metal Composition Analysis] A 5 mm square block was taken from the center of the plate thickness and the center of the weld line in the weld metal part of the welded joint, and the weld metal composition was analyzed. In addition, the total N content in the weld metal was measured using the inert gas fusion-thermal conductivity method. The results are shown in Table 4.
[0113]
[0114] [Evaluation of Hot Cracking Resistance] After welding, a 10 mm thick macroscopic test piece was taken from the center position in the weld line direction using a microcutter, with the observation surface being a cross section perpendicular to the weld line. The cross section of the weld metal was observed under an optical microscope (30x magnification) to determine whether or not hot cracking occurred. Here, in test pieces where hot cracking was observed, a long, narrow black area measuring 25 μm wide x 80 μm long or more was observed. When hot cracking was observed, it was judged as "present," and when no cracking was observed, it was judged as "absent." The presence or absence of pits or blowholes was also judged.
[0115] Furthermore, flat test specimens measuring 5 (t) mm × 50 (w) mm × 100 (l) mm were cut from the welded joints. The surface of the test specimen was ground 1 mm from the joint surface, and the remaining thickness was ground from the back surface to a thickness of 5 mm. The hot cracking susceptibility of the weld metal of the joint was then evaluated using a trans-Varestraint test. This test involved melt-run welding using a TIG arc, and simultaneously with extinguishing the arc, the yokes at both ends of the test specimen were suddenly dropped to impart tensile strain and forcibly induce hot cracking on the bead surface. The imparted strain was in the range of 2.4 to 5.8%, which corresponds to the saturation strain value for the maximum crack length. The solidification brittleness temperature range [BTR (K)] was calculated from the saturation value of the maximum cracking strain obtained at each strain, and the hot cracking susceptibility of each material was evaluated.
[0116] [Evaluation of Weld Metal Properties] Tensile test pieces (parallel portion diameter 6 mmφ) of the weld metal were taken from the obtained weld joints and subjected to a tensile test in accordance with the provisions of JIS Z 3111: 2005. The tensile test was performed on three pieces at room temperature, and the average values obtained (0.2% proof stress, tensile strength) were taken as the tensile properties of the weld metal of the weld joint.
[0117] Charpy impact tests were also conducted on the weld metal in accordance with the provisions of JIS Z 3128:2017. The positions at which the test pieces (V-notches) were taken are shown in Figure 2. The direction of the V-notch 8 of the test piece 6 was perpendicular to the surface of the base metal 1, and the position of the V-notch 8 was set to the midpoint of the fusion line 5 of the weld metal 2 on the center line 7 of the test piece, and the test piece 6 was taken from a position 1 mm below the surface of the base metal 1. Charpy impact tests were also conducted on three pieces of each test piece in the same way, and the absorbed energy ( v E -196 ) was calculated, and the average value was taken as the cryogenic impact toughness of the weld metal of the welded joint.
[0118] As mentioned above, the target values of the present invention are that the yield stress (0.2% proof stress) and tensile strength of the weld metal at room temperature are improved by an average of 10 MPa or more when compared with conventional TIG welded joints in which a filler metal having a normal N content is used and a shielding gas is used in which 99.5% or more of an inert gas and the remainder is unavoidable impurities. Furthermore, the Charpy impact test absorption energy ( v E -196 ) must be 28J or more.
[0119] The results obtained are shown in Table 5.
[0120]
[0121] All of the welded joints shown as examples in the remarks column of Table 5 were welded joints that did not experience hot cracking during welding and had excellent hot cracking resistance. A conventional TIG welded joint (comparison example) in which 99.5% by volume or more of inert gas was used as the shielding gas and the N content of the filler metal was less than 0.0400% by mass was used as the standard, and mechanical properties were compared when nitrogen gas was mixed into the shielding gas or when the N content of the filler metal was increased. As a result, the inventive examples had an average improvement of 10 MPa or more in yield stress (0.2% proof stress) and tensile strength. Furthermore, the BTR was reduced and hot cracking susceptibility was improved. Furthermore, the weld metal had a yield stress (0.2% proof stress) of 400 MPa or more, a tensile strength of 600 MPa or more, and Charpy impact absorption energy ( v E -196 ) of 28 J or more, excellent mechanical properties were obtained.
[0122] For example, weld joint No. 1 (combination of steel No. A and filler metal No. a) uses 100% Ar gas by volume as the shielding gas, while weld joints No. 2 to 4 use the same combination but with the nitrogen gas content in the shielding gas increased to 2%, 5%, and 15% by volume. Weld joint No. 5 is an example in which filler metal No. a was replaced with filler metal No. b, which has a higher N content but is otherwise identical in composition. As a result, the N content in the weld metal increased from 0.012% by mass in weld joint No. 1 to 0.053% by mass in weld joint No. 2, 0.124% by mass in weld joint No. 3, and 0.125% by mass in weld joint No. 5, which was welded with filler metal No. b. None of these showed any hot cracking, pits, or blowholes. However, in welded joint No. 4, in which the N content of the nitrogen gas was increased to 15% by volume, the N content in the weld metal increased to 0.468% by mass, causing blowholes and poor welding, making it impossible to determine whether hot cracking had occurred. Similar results were obtained for welded joints No. 6 to 10.
[0123] Note that welded joint No. 11 (combination of steel No. C and filler metal No. e) lacked strength due to the low carbon content of filler metal No. e, and its high manganese content resulted in low toughness and low Charpy impact energy absorption. However, welded joint No. 12, which contained 2% nitrogen gas by volume in the shielding gas, welded joint No. 13, which contained 5% nitrogen gas by volume, and welded joint No. 15, which was combined with filler metal No. f, which had the same composition as filler metal No. e but a higher nitrogen content, showed improved strength and no hot cracking. These results demonstrate that simply adding nitrogen gas to the shielding gas or increasing the nitrogen content of the filler metal can improve the strength of welded joints without adjusting the composition of the base metal or welding conditions. Welded joint No. 12 also showed improved strength due to the low carbon content of filler metal No. e. Examples 16 to 23 are also examples in which the N content of the filler metal was increased, and similarly, an effect of improving the strength of the weld metal was observed.
[0124] On the other hand, in welded joints No. 24 and 25, the Mn content of the weld metal was low and the weld metal was not austenite single phase, so even if the N content was increased, no improvement in strength or toughness was observed.
[0125] [Relationship between Nitrogen Content of Shielding Gas or N Content of Filler Metal and Strength of Weld Metal] Based on the data in Table 5 above, the changes in 0.2% proof stress and tensile strength relative to the N content in the weld metal were organized for each method of adding N: a method of adding nitrogen by mixing it with a shielding gas, and a method of adding N by increasing the N content in the filler metal.
[0126] Figure 3 shows the change in 0.2% proof stress versus N content in the weld metal with a change in the nitrogen gas content in the shielding gas during welding. Figure 4 shows the change in tensile strength versus N content in the weld metal with a change in the nitrogen gas content in the shielding gas during welding. Figure 5 shows the change in 0.2% proof stress versus N content in the weld metal with a change in N content in the filler metal. Figure 6 shows the change in tensile strength versus N content in the weld metal with a change in N content in the filler metal. In Figures 3 and 4, the nitrogen content of the shielding gas is shown in brackets [ ], and the figures are grouped by level and enclosed in a two-dot chain ellipse. In Figures 5 and 6, the figures are grouped by high and low N content in the filler metal and enclosed in a two-dot chain ellipse.
[0127] As can be seen from Figure 3, when the nitrogen gas content in the shielding gas is changed for the same steel and filler metal combination, the 0.2% proof stress is higher when the nitrogen gas content is 2% by volume than when inert gas is used alone, and is even higher when the nitrogen gas content is 5% by volume. The same is true for the tensile strength shown in Figure 4, where the tensile strength increases as the nitrogen gas content increases from 2% to 5% by volume. Figures 5 and 6 also show that strength improves as the N content of the filler metal increases. The data in Table 5 show that, for all combinations, the 0.2% proof stress and tensile strength improve by 10 MPa or more when the N content in the weld metal is increased compared to the reference conditions. These results also confirm that the technology of increasing the N content in the weld metal according to the present invention is effective in improving the strength of the weld metal.
[0128] REFERENCE SIGNS LIST 1 Base metal (steel material) 2 Weld metal 2a Weld metal layer 3 Groove face 4 Solidification crack 5 Fusion line 6 Test piece 7 Center line of test piece 8 V-notch t Plate thickness θ Groove angle
Claims
1. A gas tungsten arc welded joint of a steel material using a shielding gas and a filler metal, wherein the steel material is a high Mn-containing austenitic steel, and the chemical composition of the steel material contains, in mass%, C: 0.10 to 0.70%, Si: 0.05 to 1.00%, Mn: 18.0 to 30.0%, P: 0.030% or less, S: 0.007% or less, Al: 0.010 to 0.070%, Cr: 2.5 to 7.0%, N: 0.0050 to 0.0500%, and O (oxygen): 0.0050% or less, and optionally Mo: 0.01 to 2.00%, V: 0.01 to 2.00%, W: 0.01 to 2.00%, Ni: 0.01 to 4.00%, REM: 0.0010-0.0200%, and B: 0.0005-0.0020%, with the balance being Fe and unavoidable impurities; and the chemical composition of the weld metal is, in mass %, C: 0.15-0.80%, Si: 0.10-1.00%, Mn: 17.0-30.0%, P: 0.030% or less, S: 0.030% or less, Al: 0.005-0.100%, Cr: 0.4-5.5%, Mo: 0.01-3.50%, Ni: 0.01-10.00%, and N: 0.0400-0.4000%, and optionally V: 0.01-1.00%, A gas tungsten arc welded joint containing at least one selected from Ti: 0.010-1.000%, Nb: 0.010-1.000%, W: 0.01-1.00%, Cu: 0.01-1.00%, and B: 0.0010% or less, with the balance being Fe and unavoidable impurities.
2. The weld metal has a yield stress (0.2% proof stress) of 400 MPa or more, a tensile strength of 600 MPa or more, and a Charpy impact absorption energy ( v E -196 2. The gas tungsten arc welded joint according to claim 1, wherein the weld strength is 28 J or more.
3. A method for manufacturing a gas tungsten arc welded joint, in which a steel material having the composition as defined in claim 1 is treated with a shielding gas and a filler metal to form a weld metal having the composition as defined in claim 1, wherein the shielding gas contains 0.5 to 10.0% nitrogen gas by volume, with the remainder consisting of an inert gas and unavoidable impurities.
4. A method for manufacturing a gas tungsten arc welded joint as described in claim 3, wherein the N content of the filler metal is 0.1200% or less, by mass percent.
5. A method for manufacturing a gas tungsten arc welded joint, which comprises using a shielding gas and a filler metal on a steel material having the composition as defined in claim 1 to form a weld metal having the composition as defined in claim 1, wherein the shielding gas contains less than 0.5% nitrogen gas by volume, with the remainder consisting of inert gases and unavoidable impurities, and the N content of the filler metal is 0.4000% or less by mass.
6. The weld metal shall have a yield stress (0.2% yield strength) of 400 MPa or more, a tensile strength of 600 MPa or more, and a Charpy impact absorption energy ( v E -196 The method for producing a gas tungsten arc welded joint according to any one of claims 3 to 5, wherein the weld strength is 28 J or more.