Preparation method for solid electrolyte containing anderson-type polyoxometalate and use of solid electrolyte

MYPI2026000447A0Undetermined Publication Date: 2025-07-24SHANGHAI FIRM LITHIUM NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2026000447
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-01-24
Filing Date
2024-09-14
Publication Date
2025-07-24

AI Technical Summary

Technical Problem

The existing sulfide solid electrolytes have problems such as unstable lithium metal negative electrodes, poor compatibility with oxide positive electrode materials, and insufficient conductivity in all-solid state batteries, which limit their application.

Method used

The Anderson type polyoxylate salt is used as an additive to treat the modified sulfide solid electrolyte by ball milling and calcining to form a dense polyoxylate salt to fill the void, improving the ionic conductivity and interface contact performance of the electrolyte.

Benefits of technology

The modified solid electrolyte is denser, improving the electrochemical performance and cycling stability of the entire battery, enhancing electrode interface contact, and improving ionic conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2026000447_DRAWING_001
    Figure PI2026000447_DRAWING_001
  • Figure PI2026000447_DRAWING_002
    Figure PI2026000447_DRAWING_002
Patent Text Reader

Abstract

A preparation method for a solid electrolyte containing an Anderson-type polyoxometalate as an additive and a use of the solid electrolyte in a solid-state battery. The specific preparation method comprises: mixing a certain mass percentage of a polyoxometalate with a solid electrolyte, and then carrying out ball milling; next, carrying out pressing and then carrying out calcining to finally obtain a solid electrolyte modified by using the polyoxometalate as a filler. A polyoxometalate having excellent electrochemical performance is used as a filler to fill gaps of solid electrolytes, improving interfaces between electrolytes and electrodes, and thus improving the performance of solid electrolytes in all-solid-state batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Preparation method and application of solid electrolyte containing Anderson type polyoxometalate Technical Field

[0001] The present invention belongs to the field of solid electrolytes, and in particular relates to a preparation method and application of a solid electrolyte containing Anderson-type polyoxometalate. Background Art

[0002] In recent years, lithium-ion batteries have been widely used in consumer electronics and electric (automobile) vehicles due to their high energy density. However, their liquid electrolytes are flammable and have caused many safety accidents. Therefore, it is imperative to develop all-solid-state lithium batteries with better safety. As the core of solid-state batteries, electrolytes have developed rapidly. Among all solid electrolytes, sulfide solid electrolytes have better mechanical properties, electrode interface compatibility and the highest room-temperature lithium ion conductivity, and have received widespread attention. However, sulfide electrolytes still have problems such as instability towards lithium metal negative electrodes, poor compatibility with oxide positive electrode materials and insufficient conductivity, which limit their further application.

[0003] Polyoxometalates (POMs) are composed of structurally diverse cation and polyanion clusters and are characterized by MO x The basic structural unit is the polyoxometalate polyhedron. According to the unique structure of polyoxometalates, the polyanions in polyoxometalates are characterized by large size and a large amount of negative charge. In addition, there are abundant oxygen atoms on the surface of the polyanion, which can provide electrons to the electron acceptor, so the polyanion can be regarded as a soft base. Furthermore, the metal ions on the polyanion skeleton have unoccupied orbitals that can accept electrons. In this way, the polyanion can be regarded as a Lewis acid. Therefore, under different conditions, polyanions can be used as both Lewis acids and Lewis bases. In addition, because polyanions have a strong ability to carry and release electrons, they are often considered to be electron storage bodies, which shows that they have good redox properties.

[0004] At present, the application of polyoxometalates in the field of batteries is still in its initial stage, and is mainly used in the modification of positive and negative electrode materials (CN104051734A, CN107946592A, CN110752344A, and the polyoxometalates involved are not Anderson type). There are few reports on the use of polyoxometalates as a filler for solid electrolyte modification. In 2018, Xiamen University reported a patent for the use of polyoxometalates for modifying polymer solid electrolytes (CN108306046A), but due to the defects of low ionic conductivity and good ductility of polymer solid electrolytes, its application in all-solid-state batteries is limited. However, this work provides a theoretical basis for the use of polyoxometalates as fillers to modify sulfide solid electrolytes.

[0005] Summary of the Invention

[0006] The purpose of the present invention is to address the problems existing in the prior art and provide a method for preparing a solid electrolyte containing Anderson-type polyoxometalate and its application, wherein the polyoxometalate is added as an additive to the solid electrolyte.

[0007] The purpose of the present invention can be achieved by the following solutions:

[0008] In a first aspect, the present invention provides a method for preparing a solid electrolyte containing an Anderson-type polyoxometalate, comprising the following steps:

[0009] S1. Mixing a polyoxometalate and a solid electrolyte, and ball milling the mixture to obtain a mixed electrolyte;

[0010] S1. calcining the mixed electrolyte to obtain a solid electrolyte modified with polyoxometalate.

[0011] In step S1, the polyoxometalate is an Anderson-type polyoxometalate, and the preparation method is as follows:

[0012] Add the metal salt into deionized water and stir until dissolved to obtain a metal salt solution; add ammonium molybdate ((NH4)6Mo7O 24 ) or ammonium molybdate tetrahydrate ((NH4)6Mo7O 24 4H2O) is dissolved in water, heated to boiling and maintained, and the obtained metal salt solution is added dropwise. After the addition is complete, the reaction is carried out at a constant temperature, filtered while hot, and allowed to stand at a constant temperature before recrystallization to obtain pure Anderson-type polyoxometallate.

[0013] The metal salt in the metal salt solution includes one or more metal nitrates and sulfates; the metal includes one of iron, nickel, copper, chromium, and cobalt. The metal salt is specifically one of Fe2(SO4)3, Ni(NO3)2, CuSO4, Cr(NO3)3, and CoSO4. The mass ratio of the metal salt to ammonium molybdate or ammonium molybdate tetrahydrate is (2-4):(4-8). The metal salt solution is obtained by adding the metal salt to deionized water and stirring until dissolved.

[0014] The ratio of the metal salt to the deionized water used for dissolving the metal salt is 1-5 g: 20-100 ml. The ratio of ammonium molybdate or ammonium molybdate tetrahydrate to the deionized water used for dissolving the metal salt is 3-10 g: 50 ml-160 ml.

[0015] During the addition of the metal salt solution, HCl was added in real time to adjust the pH to 2-5.

[0016] The temperature of the constant temperature reaction is 90° C.-110° C., and the constant temperature reaction time is 20 min-60 min.

[0017] The constant temperature placement time is 10-12 hours, and the number of recrystallizations is 2-4 times.

[0018] The structural formula of the obtained Anderson type polyoxometalate is: (MH4) x [MMo6O 18 (OH)6] (6-x)- (X=1, 2, 3, 4, 5), M=one of Fe, Ni, Cu, Cr, Co.

[0019] In step S1, the stoichiometric ratio of the polyoxometalate to the solid electrolyte is (1-5): (70-95). The solid electrolyte is a sulfide electrolyte including Li6PS5Cl.

[0020] In step S1, the ball milling speed is 300r / min-600r / min, and the ball milling time is 2h-8h. The ball milling is carried out under sealed conditions, the ball-to-material ratio of the ball milling is (30-50):1, a high-energy planetary ball mill is used for ball milling, and the diameter of the zirconia ball milling beads is 2mm-5mm. The preferred material weight during ball milling is 1g-10g. The ball milling method belongs to the solid phase method, and the solvent mixing belongs to the liquid phase method. The solvent is introduced into the liquid phase method. Although it has been dried, it is inevitable that residual solvent molecules will remain in the electrolyte system, thereby affecting the ionic conductivity of the electrolyte. The solid phase method of the present invention does not require a binder or other polymer macromolecules, which completely solves this problem.

[0021] In step S2, the calcination temperature is 400℃-700℃, and the time is 6h-9h; the heating rate during calcination is 0.1℃ / min-1℃ / min. The purpose of calcination is to remove the impurity phase produced by the preparation of polyoxometalates and form a dense solid electrolyte. If the temperature is too low, the impurities cannot be completely removed. After calcination, what is obtained is a sulfide solid electrolyte modified by polyoxometalates filling the gaps. Since the solid electrolyte particles are in solid-solid contact with each other, gaps will inevitably form, leading to interface problems. The nano-scale polyoxometalates of the present invention just fill the gaps during the ball milling process, which solves the interface problem to a certain extent, thereby improving the electrochemical performance of the full battery. Control the heating rate. On the one hand, considering safety issues, if the heating rate is too fast, the quartz tube may explode; on the other hand, the heating rate will directly affect the purity of the product.

[0022] In a second aspect, the present invention further provides a use of the solid electrolyte containing an Anderson-type polyoxometalate in preparing a composite cathode material. Specifically, the use comprises ball milling a cathode material, a solid electrolyte containing an Anderson-type polyoxometalate, and vapor-grown carbon fiber (VGCF). The cathode material comprises NCM811.

[0023] In a third aspect, the present invention also provides an application of the solid electrolyte containing Anderson-type polyoxometalate in an all-solid-state battery.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) Compared with traditional solid electrolytes, the modified solid electrolyte is denser, resulting in better interface contact with electrodes in the assembled full battery;

[0026] (2) The ionic conductivity of the modified solid electrolyte is improved;

[0027] (3) Since the modified solid electrolyte is denser and the interface is relatively better, the cycling stability in the full battery is also more stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Other features, objects and advantages of the present invention will become more apparent upon reading the detailed description of non-limiting embodiments with reference to the following drawings:

[0029] FIG1 is an infrared spectrum of FePOM prepared in Example 1;

[0030] FIG2 is an impedance diagram of the solid electrolyte modified in Example 1;

[0031] FIG3 is a 300-cycle graph of a full battery prepared with the material obtained in Example 1 at 0.1C. DETAILED DESCRIPTION

[0032] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments. The following examples are implemented under the premise of the technical solution of the present invention, provide detailed implementation methods and specific operating procedures, and will help those skilled in the art to further understand the present invention. It should be pointed out that the scope of protection of the present invention is not limited to the following embodiments, and a number of adjustments and improvements made under the premise of the concept of the present invention all fall within the scope of protection of the present invention.

[0033] The following steps were used to test the charge and discharge performance of the embodiments and comparative examples of the present invention:

[0034] First, the NCM811 composite cathode material was prepared: NCM811, the prepared modified solid electrolyte, and vapor-grown carbon fiber (VGCF) were weighed into a 25mL zirconia ball mill according to a mass ratio of 16:3:1. The total mass of the materials was 1g, the ball-to-material ratio was controlled to 20:1, and the diameter of the zirconia ball milling beads used was 3mm. The sealed ball mill was then fixed on a high-energy planetary ball mill and ball milled at 400r / min for 4h. Finally, the NCM811 composite cathode material was obtained. Then, Li / In was used as the negative electrode and the modified solid electrolyte was used as the electrolyte to assemble the all-solid-state battery, and the charge and discharge performance was tested.

[0035] Example 1

[0036] This embodiment provides a method for preparing a solid electrolyte containing an Anderson-type polyoxometalate, comprising the following steps:

[0037] (1) Preparation of Fe-based polyoxometalates (FePOM):

[0038] Weigh 1.2g Fe2(SO4)3, add 20ml deionized water, and stir until dissolved to obtain Fe2(SO4)3 solution. 24 4H2O was dissolved in 80mL of water and heated to boiling. Fe2(SO4)3 solution was added dropwise with stirring. As the Fe2(SO4)3 solution was added, the solution gradually changed from colorless to deep red. The pH change was monitored in real time. The solution was adjusted to pH 2.8 with hydrochloric acid. The reaction was kept at this temperature for 1 hour and filtered while hot. After 12 hours, brown-red flaky crystals precipitated. Recrystallization was performed once in an 80°C water bath to obtain pure Fe-based polyoxometalate (4.9g). The infrared spectrum of the prepared FePOM is shown in Figure 1.

[0039] (2) Modified Li6PS5Cl solid electrolyte (Li6PS5Cl-FePOM):

[0040] The sample of Example 1 and Li6PS5Cl were weighed in a stoichiometric ratio of 5:95 and mixed evenly in a zirconia ball mill. The total mass of the material was 1 g, the ball-to-material ratio was controlled at 30:1, and the diameter of the zirconia ball mill beads used was 5 mm. The sealed ball mill was then fixed on a high-energy planetary ball mill and ball milled at 550 r / min for 7 hours. The material was then scraped off the wall of the ball mill, and the obtained powder was pressed into tablets and vacuum-sealed in a quartz tube. It was then placed in a muffle furnace and calcined at 550°C for 7 hours at a heating rate of 0.5°C / min. After cooling to room temperature, the modified flaky sulfide solid electrolyte material was taken out of the glove box, ground and bottled for later use.

[0041] (3) Preparation of NCM811 composite cathode material:

[0042] NCM811, the Li6PS5Cl-FePOM prepared in step 2 above, and vapor-grown carbon fiber (VGCF) were weighed into a 25mL zirconia ball mill at a mass ratio of 16:3:1. The total mass was 1g, and the ball-to-material ratio was controlled at 20:1. The diameter of the zirconia milling beads used was 3mm. The sealed ball mill was then fixed in a high-energy planetary ball mill at 400 rpm for 4 hours. The resulting NCM811 composite cathode material was obtained.

[0043] Application Example 1

[0044] Assembly of the all-solid-state battery: 100mg of the modified Li6PS5Cl solid electrolyte (Li6PS5Cl-FePOM) was weighed into a 10mm stainless steel tableting mold and pressed at a pressure of 360MPa. Then, 10mg of the composite cathode material prepared by the above method was added to one side of the electrolyte sheet and pressed again at a pressure of 150MPa. The sheet was then demolded and placed into a custom battery test mold. A 9mm lithium indium sheet (30 and 100 micron thick, respectively) was added to the other side of the electrolyte sheet. Finally, an Al current collector was placed on the positive electrode side and a Cu current collector was placed on the negative electrode side to complete the packaging. The battery mold was removed, placed in a battery fixture, and pressed at a pressure of 50MPa to obtain a sandwich-type all-solid-state battery. The assembled full battery was subjected to capacitance discharge testing. As shown in Figure 2, at room temperature and a 0.1C rate, the first-cycle charge capacity reached 251mAh / g. A 300-cycle cycle diagram at 0.1C is shown in Figure 3.

[0045] Example 2

[0046] This embodiment provides a method for preparing a solid electrolyte containing an Anderson-type polyoxometalate, comprising the following steps:

[0047] (1) Preparation of Cu-based polyoxometalates:

[0048] Weigh 0.48g Cu2(SO4)3, add 20ml deionized water, and stir until dissolved to obtain Cu2SO4 solution. 24 Dissolve 4H2O in 80mL of water, heat to boiling, and add CuSO4 solution dropwise with stirring. With the continuous addition of CuSO4 solution, the solution gradually changes from colorless to light blue. Monitor the pH change in real time and adjust the solution to pH 2.8 with hydrochloric acid. React at this constant temperature for 1 hour and filter while hot. After 12 hours, blue flaky crystals precipitate. Recrystallize once in an 80°C water bath to obtain pure Cu-based polyoxometalate (2.8g).

[0049] (2) Modified Li6PS5Cl solid electrolyte (Li6PS5Cl-CuPOM):

[0050] The sample of Example 1 and Li6PS5Cl were weighed in a stoichiometric ratio of 5:95 and mixed evenly in a zirconia ball mill. The total mass of the material was 1 g, the ball-to-material ratio was controlled at 30:1, and the diameter of the zirconia ball mill beads used was 5 mm. The sealed ball mill was then fixed on a high-energy planetary ball mill and ball milled at 550 r / min for 7 hours. The material was then scraped off the wall of the ball mill, and the obtained powder was pressed into tablets and vacuum-sealed in a quartz tube. It was then placed in a muffle furnace and calcined at 550°C for 7 hours at a heating rate of 0.5°C / min. After cooling to room temperature, the modified flaky sulfide solid electrolyte material was taken out of the glove box, ground and bottled for later use.

[0051] (3) Preparation of NCM811 composite cathode material:

[0052] NCM811, the Li6PS5Cl-CuPOM prepared in step 2 above, and vapor-grown carbon fiber (VGCF) were weighed into a 25mL zirconia ball mill at a mass ratio of 16:3:1. The total mass was 1g, and the ball-to-material ratio was controlled at 20:1. The diameter of the zirconia milling beads used was 3mm. The sealed ball mill was then fixed in a high-energy planetary ball mill at 400 rpm for 4 hours. The resulting NCM811 composite cathode material was obtained.

[0053] Application Example 2

[0054] Assembly of the all-solid-state battery: 100mg of the modified Li6PS5Cl solid electrolyte (Li6PS5Cl-CuPOM) was weighed into a 10mm stainless steel tablet mold and pressed at a pressure of 360MPa. 10mg of the composite cathode material prepared by the above method was then added to one side of the electrolyte sheet and pressed again at a pressure of 150MPa. The sheet was then demolded and placed into a specially designed battery test mold. A 9mm lithium indium sheet (30 and 100 microns thick, respectively) was added to the other side of the electrolyte sheet. Finally, an Al current collector was placed on the positive electrode side and a Cu current collector was placed on the negative electrode side to complete the packaging. The battery mold was removed, placed in a battery fixture, and pressed at a pressure of 50MPa to obtain a sandwich-type all-solid-state battery. The assembled full battery was subjected to a capacitance discharge test. At room temperature and a 0.1C rate, the first cycle charge capacity can reach 184mAh / g.

[0055] Example 3

[0056] This embodiment provides a method for preparing a solid electrolyte containing an Anderson-type polyoxometalate, comprising the following steps:

[0057] (1) Preparation of Ni-based polyoxometalates:

[0058] Weigh 0.55g Ni(NO3)2, add 20ml deionized water, and stir until dissolved to obtain Ni(NO3)2 solution. 24 Dissolve 4H2O in 80mL of water, heat to boiling, and add Ni(NO3)2 solution dropwise with stirring. As the Ni(NO3)2 solution is added, the solution gradually changes from colorless to deep red. Monitor the pH change in real time and adjust the solution to pH 2.8 with hydrochloric acid. React at this constant temperature for 1 hour and filter while hot. After 12 hours, sky-blue flaky crystals precipitate. Recrystallize once in an 80°C water bath to obtain pure Ni-based polyoxometalate (2.1g).

[0059] (2) Modified Li6PS5Cl solid electrolyte (Li6PS5Cl-NiPOM):

[0060] The sample of Example 1 and Li6PS5Cl were weighed in a stoichiometric ratio of 5:95 and mixed evenly in a zirconia ball mill. The total mass of the material was 1 g, the ball-to-material ratio was controlled at 30:1, and the diameter of the zirconia ball mill beads used was 5 mm. The sealed ball mill was then fixed on a high-energy planetary ball mill and ball milled at 550 r / min for 7 hours. The material was then scraped off the wall of the ball mill, and the obtained powder was pressed into tablets and vacuum-sealed in a quartz tube. It was then placed in a muffle furnace and calcined at 550°C for 7 hours at a heating rate of 0.5°C / min. After cooling to room temperature, the modified flaky sulfide solid electrolyte material was taken out of the glove box, ground and bottled for later use.

[0061] (3) Preparation of NCM811 composite cathode material:

[0062] NCM811, the Li6PS5Cl-NiPOM prepared in step 2 above, and vapor-grown carbon fiber (VGCF) were weighed into a 25mL zirconia ball mill at a mass ratio of 16:3:1. The total mass was 1g, and the ball-to-material ratio was controlled at 20:1. The diameter of the zirconia milling beads used was 3mm. The sealed ball mill was then fixed in a high-energy planetary ball mill at 400 rpm for 4 hours. The resulting NCM811 composite cathode material was obtained.

[0063] Application Example 3

[0064] Assembly of all-solid-state batteries:

[0065] 100mg of modified Li6PS5Cl solid electrolyte (Li6PS5Cl-NiPOM) was weighed into a 10mm stainless steel tablet mold and pressed at a pressure of 360MPa. Then 10mg of the composite positive electrode material prepared by the above method was added to one side of the electrolyte sheet and pressed again at a pressure of 150MPa. It was then demolded and placed in a special battery test mold. Then a 9mm lithium indium sheet (the thickness of the lithium indium sheet was 30 and 100 microns respectively) was added to the other side of the electrolyte sheet. Finally, an Al sheet current collector was placed on the positive electrode side and a Cu current collector was placed on the negative electrode side to complete the packaging. The battery mold was removed, placed in a battery fixture, and pressed at a pressure of 50MPa to obtain a sandwich-type all-solid-state battery. The assembled full battery was subjected to a capacitance discharge test. At room temperature and a rate of 0.1C, the first cycle charge capacity can reach 191mAh / g.

[0066] Comparative Example 1

[0067] This example provides a method for preparing a solid electrolyte containing an Anderson-type polyoxometalate. The steps are essentially the same as those in Example 1, differing only in that a wet ball milling method is employed. Following the same process, Fe-based polyoxometalate (FePOM) and Li₆PS₅Cl₄ are mixed, 10 mL of acetonitrile solvent is added to the mill, and the mixture is vacuum dried for 12 hours to remove the solvent, followed by calcination.

[0068] Comparative Example 2

[0069] This embodiment provides a method for preparing a solid electrolyte containing Anderson-type polyoxometalate. The steps are basically the same as those in Example 1, except that no calcination treatment is performed after ball milling.

[0070] Comparative Example 3

[0071] This embodiment provides a method for preparing a solid electrolyte containing Anderson-type polyoxometalate. The steps are basically the same as those in Example 1, with the only difference being that the calcination temperature is 200°C.

[0072] The electrolyte sheets prepared in the embodiments and comparative examples were tested using the same test method as in the application examples, and the test results were as follows:

[0073] Table 1

[0074] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various variations or modifications within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A preparation method of a solid electrolyte containing Anderson-type polyoxometalate, characterized in that, It includes the following steps: S1. Mix the polyoxometalate with the solid electrolyte and perform ball milling to obtain a mixed electrolyte; S2. Calcinate the mixed electrolyte to obtain a solid electrolyte modified with polyoxometalate.

2. The preparation method according to claim 1, wherein In step S1, the polyoxometalate is an Anderson-type polyoxometalate, and the preparation method is as follows: Dissolve ammonium molybdate or ammonium molybdate tetrahydrate in water, heat to boiling and maintain, dropwise add the metal salt solution, after dropping, carry out a constant-temperature reaction, filter while it is hot, and perform recrystallization after constant-temperature standing to obtain the Anderson-type polyoxometalate.

3. The preparation method according to claim 2, wherein The metal salt in the metal salt solution includes one or more of metal nitrates and sulfates; among them, the metal includes one or more of iron, nickel, copper, chromium, and cobalt; the mass ratio of the metal salt to ammonium molybdate tetrahydrate is (2-4):(4-8).

4. The preparation method according to claim 2, wherein The temperature of the constant-temperature reaction is 90°C - 110°C, and the time of the constant-temperature reaction is 20 min - 60 min.

5. The preparation method according to claim 2, characterized in that, The structural formula of the Anderson-type polyoxometalate is: (MH4) x [MMo6O 18 (OH)6] (6-x)- , where X takes values of 1, 2, 3, 4 or 5, and M includes one of Fe, Ni, Cu, Cr, Co.

6. The preparation method according to claim 1, characterized in that, In step S1, the stoichiometric ratio of the polyoxometalate to the solid electrolyte is (1-5):(70-95).

7. The preparation method according to claim 1, characterized in that, In step S1, the rotation speed of the ball milling is 300 r / min - 600 r / min, and the ball milling time is 2 h - 8 h.

8. The preparation method according to claim 1, characterized in that, In step S2, the calcination temperature is 400°C - 700°C, and the time is 6 h - 9 h; the heating rate during calcination is 0.1°C / min - 1°C / min.

9. Application of a solid electrolyte containing Anderson-type polyoxometalate as described in claim 1 in a all-solid-state battery.

10. Application of a solid electrolyte containing Anderson-type polyoxometalate as described in claim 1 in the preparation of a composite cathode material. The specific application is: obtaining by mixing and ball milling a cathode material, a solid electrolyte containing Anderson-type polyoxometalate, and vapor-grown carbon fibers.